A method for reducing strip breakage rate in cold-rolled chrome steel based on whole-process collaborative control

By employing a full-process collaborative control method, the problem of high strip breakage rate in cold rolling of 430 series ferritic stainless steel was solved, achieving a reduction of strip breakage rate by 83%, thereby reducing production costs and improving the quality of finished products.

CN123102743APending Publication Date: 2026-11-17SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235861.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the current cold rolling process of 430 series ferritic stainless steel, the strip breakage rate remains high, resulting in low production efficiency and high costs.

Method used

The entire process is controlled by a collaborative approach, including ultrapure raw material smelting, hot rolling microstructure homogenization, bell-type furnace annealing temperature homogenization, and matching of the crown of cold rolling rolls of different specifications. The molten steel is treated by EAF electric arc furnace + LF ladle refining + RH vacuum degassing, calcium-modified inclusions are added, the equiaxed crystal ratio of the billet is controlled, induction heating before finishing rolling is used to compensate for temperature differences, laminar flow cooling and low-temperature water spraying are used, the bell-type furnace is kept at a constant temperature, and the appropriate crown of the cold rolling roll system is configured.

Benefits of technology

A breakthrough reduction in cold-rolled strip breakage rate was achieved, with a decrease of over 83%, significantly reducing production costs and downtime, and improving the yield rate and uniformity of mechanical properties of finished products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of cold-rolled chromium steel rolling, and discloses a method for reducing the strip breakage rate of cold-rolled chromium steel based on full-process collaborative control. The method employs four collaborative processes: raw material ultrapure smelting control, hot rolling microstructure homogenization control, bell-type furnace annealing temperature homogenization control, and specification-specific cold rolling roll system crown matching control. Raw material ultrapure smelting control utilizes a triple refining process of EAF electric arc furnace + LF ladle refining + RH vacuum degassing, controlling the [H] content in the cold-rolled chromium steel at the vacuum endpoint to be ≤1.5ppm and [O] to ≤15ppm. This invention provides a closed-loop collaborative coupling control method for the four processes of steelmaking, hot rolling, bell-type annealing, and cold rolling, eliminating various strip breakage causes such as inclusions, billet porosity, hot-rolled edge microcracks, annealing performance dispersion, and cold-rolled transverse tension imbalance, achieving a breakthrough reduction in the cold-rolled strip breakage rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cold-rolled chromium steel rolling, and particularly to the field of 430 series ferritic stainless steel rolling. Background Technology

[0002] 430 series ferritic cold-rolled chromium steel is nickel-free, inexpensive, and exhibits excellent atmospheric corrosion resistance, making it widely used in appliance panels, kitchen and bathroom fixtures, and building decoration. However, current conventional production processes employ a segmented, independently controlled model, leading to the cumulative effect of defects across processes and frequent interruptions in cold rolling, a common pain point in the industry. Defects in the steelmaking process: Traditionally, an EAF electric arc furnace + LF ladle refining is used without RH vacuum degassing, resulting in steel with [H] ≤ 2.5ppm and high total oxygen content; without precise calcium treatment, the deoxidation products are long strip-shaped hard aluminate inclusions with an aspect ratio of 3-8, which are very easy to form crack sources when subjected to rolling stress; continuous casting only uses a single box-type electromagnetic stirring, resulting in well-developed columnar crystals in the billet, with an equiaxed crystal ratio of only 45%-48%, and the billet center is loose and has severe central segregation, with internal defects inherited to cold rolling and inducing tearing.

[0003] Defects in the hot rolling process: The heat dissipation rate at the edge of the slab is much greater than that at the center, and the hardness difference between the edge and the center after finishing rolling is as high as 25HV, resulting in significant deterioration of the plasticity at the edge of the strip; only single laminar flow cooling is used without subsequent auxiliary low-temperature water spraying, resulting in abnormal coarsening of the grains at the edge; air cooling after coiling results in insufficient cooling rate, poor uniformity of transverse structure, and the hot-rolled strip has a large number of microcracks.

[0004] Annealing process defects: Conventional bell furnaces directly heat to the target annealing temperature, resulting in large differences in the heating rate of the outer, middle and inner rings of the steel coil. The hardness and plasticity of the whole coil are significantly dispersed, with insufficient plasticity in some areas, leading to preferential fracture under cold rolling stress.

[0005] Defects in the cold rolling process: The roll crown is uniformly fixed and does not match the transverse deformation requirements of strips of different widths. The transverse tension distribution is uneven during the rolling process, and the fluctuation of the roll thermal crown can easily induce local tearing and strip breakage.

[0006] The production of 430 cold-rolled chromium steel using the existing segmented control process has resulted in a cold-rolling strip breakage rate that is consistently greater than 3%. Each strip breakage requires a shutdown of more than 2 hours, and also generates scrap steel loss, roll surface damage, and capacity loss. The comprehensive cost of handling a single strip breakage exceeds 30,000 yuan. Summary of the Invention

[0007] The technical problem to be solved by this invention is: how to solve the problem of high strip breakage rate during cold rolling of existing 430 series ferritic stainless steel.

[0008] The technical solution adopted in this invention is: a method for reducing the strip breakage rate in cold-rolled chromium steel based on full-process collaborative control. This method employs four collaborative processes: raw material ultrapure smelting control, hot rolling microstructure homogenization control, bell-type furnace annealing temperature homogenization control, and cold rolling roll system crown matching control for different specifications. The control steps for each process are as follows: Raw material ultrapure smelting control: A three-stage refining process is employed, using an EAF electric arc furnace + LF ladle refining + RH vacuum degassing, to control the [H] content in the vacuum-finished cold-rolled chromium steel to be ≤1.5ppm and [O] to ≤15ppm. Calcium is added to the molten steel for inclusion modification, controlling the calcium mass percentage content in the vacuum-finished cold-rolled chromium steel to be 0.001%-0.003%, thus modifying the inclusions into spherical shapes with an aspect ratio ≤2.0. Electromagnetic stirring employs roller stirring + box stirring, with an equiaxed crystal ratio of 55%. Hot-rolled microstructure homogenization control: Before finishing rolling, edge induction heating is used to compensate for temperature difference, controlling the edge of the strip at 1080-1100℃ and the core at 1090-1120℃; after laminar flow cooling, low-temperature auxiliary water spray at ≤25℃ is added; the coiling temperature is ≤580℃, and after coiling, forced water cooling is performed with a cooling rate ≥20℃ / s, and the final cooling temperature of the steel coil is 260-300℃; Uniform control of annealing temperature in bell-type furnace: When the steel coil is heated to the range of 680-750℃, it is kept at a constant temperature for 3-6 hours before being raised to the target annealing temperature of the finished product. Crown matching control of cold rolling roll system by specification: The crown of two intermediate drive rolls, two intermediate free rolls, and work rolls is configured according to the difference in strip width.

[0009] The configuration of two intermediate drive rollers, two intermediate free rollers, and work roller crown is based on the strip width, including the following: For cold-rolled chromium steel, which is 430 series ferritic stainless steel, the specific crown matching standard for cold-rolling rolls suitable for its high deformation resistance and easy edge cracking characteristics is as follows: When the strip width is 1000-1199mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 200-300μm, and the crown of the work rollers is 50-150μm. When the strip width is 1200-1300mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 100-200μm, and the crown of the work rollers is 0-100μm. When the strip width is 1301-1550mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 0-100μm, and the crown of the work roller is 0-100μm.

[0010] After the hot rolling process is completed, the hardness difference between the edge and core of the strip is ≤8HV.

[0011] Comparison of key smelting indicators between traditional processes and the present invention

[0012] The beneficial effects of this invention are: This invention provides a closed-loop synergistic coupling control method for four processes: steelmaking, hot rolling, bell-type annealing, and cold rolling. It eliminates various causes of strip breakage, such as inclusions, billet porosity, micro-cracks at the edge of hot rolling, discrete annealing performance, and transverse tension imbalance in cold rolling, thereby achieving a breakthrough reduction in the strip breakage rate in cold rolling.

[0013] Synergistic effects and unexpected technical benefits: Existing technologies only optimize a single process, and the strip breakage rate can only be reduced to a minimum of 1.5%; This invention is the first to propose a parameter coupling and synergistic scheme for the entire process of steelmaking-hot rolling-annealing-cold rolling, eliminating the source of strip breakage defects in each of the four processes in advance, achieving a stable control of the cold rolling strip breakage rate below 0.5%, a reduction of more than 83%, breaking through the existing technical bottleneck in the industry.

[0014] The entire chain addresses the root causes of strip breakage: the smelting process eliminates internal inclusions and defects in the billet; the hot rolling process eliminates poor plasticity and micro-cracks at the edges of the strip; the annealing process unifies the plasticity of the entire coil; and the cold rolling process balances the transverse rolling tension, suppressing strip breakage simultaneously from multiple dimensions, rather than providing temporary relief through a single process.

[0015] Low cost of industrialization: The entire process is compatible with existing 430 chromium steel production lines. The main equipment for steelmaking, hot rolling, bell annealing, and cold rolling does not require large-scale modification. Only process parameters and roll grinding crown need to be adjusted. The modification investment is low and it can be put into large-scale production directly.

[0016] Production costs are significantly reduced: the frequency of strip breakage is greatly reduced, significantly reducing downtime, scrap steel loss, and roll repair losses, resulting in a significant decrease in the annual comprehensive production cost of a single production line; at the same time, the uniformity of the transverse mechanical properties of the strip is improved, and the yield of finished products is increased accordingly.

[0017] Product quality stability improved: the equiaxed crystal ratio of the billet increased, the transverse hardness difference of the strip steel was significantly reduced, the performance dispersion of the whole coil of steel coil decreased, and the surface defects and mechanical property non-compliance rate of finished products decreased simultaneously. Detailed Implementation

[0018] Example 1: 430 series ferritic chromium steel, finished product thickness 0.5mm, strip width 1020mm.

[0019] A method for reducing strip breakage rate in cold-rolled chromium steel based on full-process collaborative control employs four collaborative processes: raw material ultrapure smelting control, hot rolling microstructure homogenization control, bell-type furnace annealing temperature homogenization control, and cold rolling roll system crown matching control for different specifications. The control steps for each process are as follows: Ultra-pure raw material smelting: EAF+LF+RH triple refining, vacuum endpoint [H]=1.2ppm, total oxygen [O]=10ppm; metallic calcium is added to molten steel, vacuum endpoint calcium mass fraction is 0.002%, inclusions are modified into spherical CaO-Al2O3; the billet is simultaneously stirred by roller stirring + box stirring with dual electromagnetic stirring, the billet equiaxed crystal ratio is 55%.

[0020] Hot rolling homogeneity control: An edge induction heating device is set before finishing rolling to control the edge temperature of the strip steel. The edge induction heating is 1080℃, and the core of the slab is 1100℃. After laminar flow cooling, low-temperature auxiliary water spraying at 18℃ is used to suppress abnormal grain growth at the edge of the strip steel. The coiling temperature is 550℃, and the forced water cooling rate after coiling is 25℃ / s. The final cooling temperature of the steel coil is 280℃.

[0021] Bell-type annealing: When the temperature is raised to 720℃, a constant temperature holding platform is set for 2 hours. After the holding is completed, the temperature is raised to the target annealing temperature. The difference in heating rate between the outer ring, middle and inner ring of the steel coil is eliminated by the long constant temperature in the middle section, so as to ensure that the microstructure and mechanical plastic properties of the whole coil are uniform.

[0022] The cold rolling roll system is configured as follows: two intermediate drive rolls with a crown of 250μm, two intermediate free rolls with a crown of 200μm, and work rolls with a crown of 100μm.

[0023] Production verification results: The cold-rolled strip breakage rate was reduced to 0.2%; after the hot-rolling process, the hardness difference between the edge and core of the strip was ≤8HV.

[0024] Example 2: 430 series ferritic chromium steel, finished product thickness 0.8mm, strip width 1240mm.

[0025] A method for reducing strip breakage rate in cold-rolled chromium steel based on full-process collaborative control employs four collaborative processes: raw material ultrapure smelting control, hot rolling microstructure homogenization control, bell-type furnace annealing temperature homogenization control, and cold rolling roll system crown matching control for different specifications. The control steps for each process are as follows: Ultra-pure raw material smelting: EAF+LF+RH triple refining, vacuum endpoint [H]=1.0ppm, total oxygen [O]=8ppm; metallic calcium is added to molten steel, the mass fraction of calcium at the vacuum endpoint is 0.001%, and inclusions are modified into spherical CaO-Al2O3; the billet is simultaneously stirred by roller stirring + box stirring with dual electromagnetic stirring, and the equiaxed crystal ratio of the billet is 52%.

[0026] Hot rolling homogeneity control: An edge induction heating device is set before finishing rolling to control the edge temperature of the strip. The edge induction heating is 1090℃, and the core of the slab is 1110℃. After laminar flow cooling, a low-temperature auxiliary water spray at 22℃ is used. The coiling temperature is 560℃, and the forced water cooling rate after coiling is 23℃ / s. The final cooling temperature of the steel coil is 270℃.

[0027] Bell-type annealing: When the temperature is raised to 750℃, a constant temperature holding platform is set for 4 hours. After the holding is completed, the temperature is raised to the target annealing temperature. The difference in heating rate between the outer ring, middle and inner ring of the steel coil is eliminated by the long constant temperature in the middle section, so as to ensure that the microstructure and mechanical and plastic properties of the whole coil are uniform.

[0028] The cold rolling roll system is configured as follows: two intermediate drive rolls with a crown of 250μm, two intermediate free rolls with a crown of 100μm, and work rolls with a crown of 50μm.

[0029] Production verification results: The cold-rolled strip breakage rate was reduced to 0.3%; after the hot rolling process, the hardness difference between the edge and core of the strip was ≤8HV.

Claims

1. A method for reducing the strip breakage rate in cold-rolled chromium steel based on full-process collaborative control, characterized in that: The process employs four collaborative steps: raw material ultrapure smelting control, hot rolling microstructure homogenization control, bell-type furnace annealing temperature homogenization control, and cold rolling roll crown matching control for different specifications. The control steps for each step are as follows: Raw material ultrapure smelting control: EAF electric arc furnace + LF ladle refining + RH vacuum degassing triple refining is adopted to control [H] ≤ 1.5ppm and [O] ≤ 15ppm in the vacuum final cold-rolled chromium steel; calcium is added to the molten steel for inclusion modification, and the calcium mass percentage content in the vacuum final cold-rolled chromium steel is controlled to be 0.001%-0.003%, so that the inclusions are modified into spherical shape with an aspect ratio ≤ 2.0; The electromagnetic stirring method uses roller stirring and box stirring, with an equiaxed crystal ratio of 55%. Hot-rolled microstructure homogenization control: Before finishing rolling, edge induction heating is used to compensate for temperature difference, controlling the edge of the strip at 1080-1100℃ and the core at 1090-1120℃; after laminar flow cooling, low-temperature auxiliary water spray at ≤25℃ is added; the coiling temperature is ≤580℃, and after coiling, forced water cooling is performed with a cooling rate ≥20℃ / s, and the final cooling temperature of the steel coil is 260-300℃; Uniform control of annealing temperature in bell-type furnace: When the steel coil is heated to the range of 680-750℃, it is kept at a constant temperature for 3-6 hours before being raised to the target annealing temperature of the finished product. Crown matching control of cold rolling roll system by specification: The crown of two intermediate drive rolls, two intermediate free rolls, and work rolls is configured according to the difference in strip width.

2. The method for reducing strip breakage rate in cold-rolled chromium steel based on full-process collaborative control according to claim 1, characterized in that: The configuration of two intermediate drive rollers, two intermediate free rollers, and work roller crown is based on the strip width, including the following: For cold-rolled chromium steel, which is 430 series ferritic stainless steel, the specific crown matching standard for cold-rolling rolls suitable for its high deformation resistance and easy edge cracking characteristics is as follows: When the strip width is 1000-1199mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 200-300μm, and the crown of the work rollers is 50-150μm. When the strip width is 1200-1300mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 100-200μm, and the crown of the work rollers is 0-100μm. When the strip width is 1301-1550mm, the crown of the two intermediate drive rollers is 200-300μm, the crown of the two intermediate free rollers is 0-100μm, and the crown of the work roller is 0-100μm.

3. The method for reducing strip breakage rate in cold-rolled chromium steel based on full-process collaborative control according to claim 1, characterized in that: After the hot rolling process is completed, the hardness difference between the edge and core of the strip is ≤8HV.