A rare earth-modified TA18 aerospace hydraulic titanium tube and its preparation method
By combining Nd-Ce mixed rare earth modification and multi-pass cold rolling with segmented gradient aging process, the problem of insufficient texture control precision of TA18 aerospace hydraulic titanium tubes was solved, realizing the preparation of high-performance and consistent TA18 aerospace hydraulic titanium tubes, and improving circumferential load-bearing and fatigue resistance.
Patent Information
- Application Number
- CN202611304509.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the texture control precision of TA18 aviation hydraulic titanium tube is limited, resulting in large fluctuations in the finished product's CSR and high performance dispersion. Furthermore, conventional annealing processes cannot achieve precise shaping and correction of the texture, affecting its service performance.
By employing Nd-Ce mixed rare earth modification combined with multi-pass cold rolling and low-temperature gradient aging processes, and controlling the Q value and segmented gradient aging treatment, the radial base surface texture of the pipe is precisely controlled, ensuring that the shrinkage strain ratio (CSR) remains stable at 1.70–1.80.
It significantly improves the circumferential load-bearing and fatigue resistance of TA18 aviation hydraulic titanium tubes, ensuring the performance consistency of batch products. The circumferential tensile strength reaches 860MPa or above, and the fatigue life is ≥2.5×107 cycles.
Smart Images

Figure CN123102786A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of non-ferrous metals and processing technology, specifically to a rare earth modified TA18 aviation hydraulic titanium pipe and its preparation method. Background Technology
[0002] TA18 titanium alloy (Ti-3Al-2.5V) is a key material widely used in aviation hydraulic piping systems. It has good room temperature and high temperature mechanical properties, corrosion resistance, and excellent cold and hot working plasticity, formability and weldability. It has been widely used in hydraulic piping systems of Boeing series aircraft and spacecraft.
[0003] TA18 titanium alloy has a hexagonal close-packed (hcp) crystal structure with low crystal symmetry and significant mechanical anisotropy. During cold working, the grains are prone to preferential orientation, forming a strong rolling texture. The type and strength of the tube texture directly determine its service mechanical properties. Studies have shown that high-performance TA18 tubes require radial texture on the {0001} basal plane as the dominant texture feature. Contraction strain ratio (CSR) is a core indicator for quantitatively characterizing the tube texture state and evaluating its overall service performance. Its physical meaning is the ratio of the true radial strain to the true strain in the wall thickness direction under axial tensile load. Current aerospace tube standards stipulate that CSR should be greater than 1.3. Further research has found that the circumferential yield strength of the tube is at a relatively high level in the CSR range of 1.72 to 1.78, with the best overall performance observed when CSR ≈ 1.75.
[0004] Currently, the texture control of cold-rolled high-strength titanium alloy tubes is mainly achieved by adjusting the overall Q value (the ratio of relative wall reduction to relative diameter reduction). When Q > 1, compressive strain in the wall thickness direction dominates the deformation, and the grain orientation preferentially deflects along the radial direction of the tube, which is conducive to the formation of radial texture. When Q < 1, the tangential strain component dominates, and circumferential texture is easily formed. Based on this principle, existing literature has reported methods for controlling the texture of titanium alloy tubes by adjusting the cold-rolling Q value. For example, Chinese patent application CN110158005A discloses a method for controlling the texture of cold-rolled high-strength titanium alloy tubes, which controls the texture by adjusting the overall Q value and equivalent strain during the cold rolling process, and points out that when the overall Q > 1, the finished tube exhibits radial texture.
[0005] However, the traditional single Q-value control method has limited precision in texture control. Uneven texture distribution easily occurs along the wall thickness and depth of the pipe, resulting in large fluctuations in the finished product's CSR and high performance dispersion in batch products. At the same time, the method in CN110158005A only controls texture by adjusting the rolling deformation parameters. The texture state is determined after cold rolling, and subsequent heat treatment is only used to eliminate residual stress. It does not have the ability to accurately shape and correct the formed texture.
[0006] On the other hand, cold-rolled TA18 tubes only undergo a recovery process during conventional stress-relief annealing at around 500℃, retaining a large amount of cold-rolling deformation characteristics and the original rolling texture in their microstructure. Conventional single-stage annealing processes control annealing temperature and time at a single point, resulting in a narrow process window. They lack effective means to correct the texture delamination problem caused by cold rolling, and even more so, they lack the ability to actively control the texture to a target state. Furthermore, there are reports in the prior art of improving the microstructure of titanium alloys by adding rare earth elements. For example, Chinese patent application CN102605224A discloses aluminum-titanium alloy wire containing Ce and Nd and its manufacturing method, indicating that Ce and Nd have a grain-refining effect. However, when this technology is applied to aluminum-titanium alloy wire, the mechanism of rare earth action and process conditions are fundamentally different from those of TA18 aerospace hydraulic tubing, and it does not involve the directional control of the tubing texture.
[0007] In summary, there is currently a lack of a preparation method that can accurately and stably control the texture of TA18 titanium tubes to the ideal radial base surface texture state and keep the CSR stable in the optimal range. Summary of the Invention
[0008] In view of this, to solve the above problems, the purpose of this invention is to provide a rare-earth modified TA18 aerospace hydraulic titanium tube and its preparation method, aiming to overcome the defects of existing TA18 aerospace hydraulic titanium tubes, such as poor controllability of texture, large performance dispersion, and insufficient fatigue life. Its core innovation lies in: using Nd-Ce mixed rare-earth micro-modification, combined with multi-pass cold rolling and low-temperature gradient aging processes, to achieve precise and stable control of the radial base surface texture of the tube, so that the shrinkage strain ratio (CSR) is stably controlled at 1.70–1.80, thereby significantly improving the circumferential load-bearing capacity and fatigue resistance of the tube, and ensuring the performance consistency of batch products.
[0009] The method for preparing rare earth-modified TA18 aerospace hydraulic titanium tube proposed in this invention includes the following steps: S1, using TA18 titanium alloy as the matrix, adding Nd-Ce mixed rare earth, and obtaining a titanium alloy ingot through melting; S2, forging the titanium alloy ingot in multiple passes to obtain a titanium alloy billet; S3, processing the titanium alloy billet into a rough tube, and performing multi-pass decreasing deformation rolling using the Pilger cold rolling process, with the Q value of each pass controlled at 1.90~2.20, to obtain a cold-rolled titanium tube; S4, placing the cold-rolled titanium tube in a protective atmosphere and performing segmented gradient low-temperature aging treatment, the first stage being held at 380~420℃ for 1.5~2.5h, and then heating to the second stage at a rate of 1~3℃ / min to 530~580℃ for 1~1.5h, followed by cooling; S5, performing post-treatment on the aging titanium tube to obtain the finished aerospace hydraulic titanium tube.
[0010] In some embodiments, the amount of Nd-Ce mixed rare earth added in step S1 is 0.05wt% to 0.20wt% by mass, and the mass ratio of Nd to Ce is 1:(0.9 to 1.1).
[0011] In some embodiments, the melting in step S1 employs multiple vacuum self-consuming arc melting, with the vacuum degree of the melting chamber ≤5×10 -1 Pa, the melting working current is controlled at 2800~3200A, and after melting, the furnace is cooled and held for 2~4 hours to obtain titanium alloy ingots with specifications of Φ200~350mm.
[0012] In some embodiments, the specific process of forging in step S2 is as follows: heating the titanium alloy ingot to 950~980℃ for the first forging in the β phase region, air cooling to room temperature and then reheating to 900~920℃, followed by 3~4 forgings, with the deformation amount controlled at 20%~30% per forging, the total forging deformation amount at 65%~75%, the final forging temperature not lower than 850℃, and air cooling to room temperature to obtain a titanium alloy billet with a diameter of 80~150mm.
[0013] In some embodiments, in step S3, the outer diameter of the rough tube is Φ40~60mm and the wall thickness is 4~6mm.
[0014] In some embodiments, in step S3, the multi-pass decreasing deformation rolling is completed in 5 to 7 passes, with a total rolling deformation of 70% to 85%; the deformation per pass decreases from 30% to 12% in stages; and there is no intermediate annealing during the entire rolling process.
[0015] In some embodiments, in step S3, the Q value for the first 3 passes is controlled between 2.05 and 2.20, and the Q value for the remaining passes is controlled between 1.90 and 2.05, with the Q value decreasing with each pass.
[0016] In some embodiments, in step S4, the protective atmosphere is a vacuum or argon atmosphere, and the cooling is achieved by cooling the furnace to room temperature.
[0017] In some embodiments, in step S5, the finished aviation hydraulic titanium tube has an outer diameter of Φ6~25mm, a wall thickness of 0.5~2.0mm, and a single length of 3000~6000mm.
[0018] The rare earth modified TA18 aerospace hydraulic titanium tube proposed in the second aspect of the present invention is prepared by the preparation method described in any of the above embodiments. The α phase of the rare earth modified TA18 aerospace hydraulic titanium tube is mainly radially textured on the {0001} basal plane, and the shrinkage strain ratio CSR is 1.70~1.80.
[0019] The beneficial effects of this invention are as follows: This invention provides a method for preparing rare-earth modified TA18 aerospace hydraulic titanium tubes and its products. By adding Nd-Ce mixed rare earth elements to TA18 titanium alloy as the matrix, the grain boundary pinning effect of Ce and the solid solution strengthening and microstructure homogenization effect of Nd are synergistically refined to refine the as-cast microstructure. Combined with multi-pass Pilger cold rolling with decreasing deformation (Q value decreasing step by step and controlled at 1.90~2.20 overall), the tube accumulates sufficient deformation energy storage and forms a preferred orientation under the stress state dominated by radial compressive stress. Furthermore, the segmented gradient low-temperature aging process (the first stage is held at 380~420℃ to store energy) is further enhanced. The process involves graded stress release to eliminate stress while preserving the advantages of texture orientation, followed by a second stage of heat treatment at 530~580℃ to achieve precise shaping and microstructure stabilization of the radial basal surface texture. The synergistic effect of these three methods overcomes the limitations of traditional single-Q-value control in terms of texture precision, uneven distribution along wall thickness and depth, and the inability of single-stage annealing to correct texture delamination. This results in TA18 aerospace hydraulic titanium tubes with the α-phase dominated by the {0001} basal surface radial texture, a shrinkage strain ratio (CSR) stably controlled between 1.70 and 1.80 (covering the optimal range of 1.72~1.78), a circumferential tensile strength exceeding 860 MPa, and a fatigue life ≥2.5 × 10⁻⁶. 7 The batch products exhibit good performance consistency, and the entire process can be achieved using existing Pilger cold rolling and vacuum heat treatment equipment without the need for additional special equipment, demonstrating promising prospects for industrial application. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other embodiments can be obtained based on these drawings without creative effort.
[0021] Figure 1 A flowchart illustrating a method for preparing rare-earth modified TA18 aerospace hydraulic titanium tube according to an embodiment of the present invention; Figure 2 This is the pole figure corresponding to Example 1; Figure 3 This is the pole figure corresponding to Example 2; Figure 4 This is the pole figure corresponding to Comparative Example 1. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0023] To facilitate understanding of this invention, the meanings of the key detection methods and parameters involved in this invention will be explained below.
[0024] Contraction strain ratio (CSR) is a core indicator for quantitatively characterizing the texture of pipes. Physically, it represents the ratio of true radial strain to true wall strain under axial tensile load. The CSR value directly reflects the pipe's texture type and preferred orientation: when CSR > 1, it indicates that the pipe's radial texture is dominated by the {0001} basal plane; the closer the CSR value is to 1.75, the higher the circumferential yield strength and the better the overall service performance. In this invention, the CSR value is calculated by measuring the changes in outer diameter and wall thickness under axial tension, and the specific testing method follows the ASTM E8M standard.
[0025] Texture type was detected using electron backscatter diffraction (EBSD) technique, with the crystallographic preferred orientation of the α phase characterized by a pole figure ({0001} basal plane pole figure). When the {0001} poles are concentrated in the radial direction (RD direction) of the tube, it indicates that a texture type dominated by the radial texture of the {0001} basal plane has been formed.
[0026] An embodiment of the present invention provides a method for preparing rare-earth modified TA18 aerospace hydraulic titanium tubing, such as... Figure 1 As shown, it includes the following steps: S1: Batching and Melting. Using TA18 titanium alloy (Ti-3Al-2.5V, mass percentage) as the matrix, 0.05%~0.12wt% of Nd-Ce mixed rare earth elements are added, with a Nd to Ce mass ratio of 1:(0.9~1.1). Melting is carried out using a three-stage vacuum arc melting process, with a vacuum degree in the melting chamber ≤5×10⁻⁶. -1 Pa, the melting current is controlled at 2800~3200A. After melting, the furnace is cooled and held for 2~4 hours to obtain a uniform titanium alloy ingot with a diameter of Φ200~350mm. The mechanism of action is as follows: Ce has low solid solubility in titanium and mainly agglomerates at grain boundaries, effectively inhibiting as-cast grain growth and purifying grain boundary impurities through the Zener pinning effect; Nd has a certain solid solubility in α-Ti, which can produce a solid solution strengthening effect and promote microstructure homogenization. The two work synergistically in a 1:(0.9~1.1) ratio to refine the as-cast microstructure and homogenize the composition distribution, providing a microstructure basis for the formation of subsequent cold-rolled deformation texture and the precise shaping of gradient aging texture. Three vacuum self-consuming arc melting processes are combined with a vacuum degree ≤5×10 -1 Under conditions of Pa and a melting current of 2800~3200A, gases and low-melting-point impurities in the alloy can be effectively removed, avoiding metallurgical defects such as porosity and inclusions in the ingot. Holding the ingot at a temperature of 2~4 hours after melting can homogenize the temperature field of the ingot, eliminate thermal stress, and prevent ingot cracking.
[0027] S2: Forging and Billet Opening. The titanium alloy ingot is heated to 950-980℃ for the first forging in the β-phase region, breaking up the coarse as-cast dendrite structure. After the first forging, it is air-cooled to room temperature and reheated to 900-920℃ for subsequent forging. This process is completed in 3-4 forging passes, with each pass controlling the deformation to between 20% and 30%, resulting in a total forging deformation of 65%-75%. The final forging temperature is not lower than 850℃. After forging, it is air-cooled to room temperature to obtain titanium alloy billets with dimensions of Φ80-150mm. Metallographic analysis shows that the billet structure is a uniform equiaxed α+β dual-phase structure. The mechanism is that the first forging in the β-phase region at 950-980℃ fully breaks down the coarse as-cast dendrite structure, eliminating potential component segregation in the ingot. Subsequent forging in the α+β two-phase region at 900~920℃ yields a uniform, equiaxed α+β dual-phase microstructure. This microstructure possesses excellent cold-working plasticity, a prerequisite for the smooth progress of subsequent Pilger cold rolling. Controlling the deformation per forging pass to 20%~30%, with a total deformation of 65%~75%, ensures sufficient fragmentation and recrystallization of the as-cast microstructure. A final forging temperature of no less than 850℃ prevents inhomogeneity or forging cracks caused by excessively low temperatures during forging. Air cooling to room temperature preserves a fine α+β dual-phase microstructure, preventing the formation of martensite and other non-equilibrium structures during rapid cooling, which could negatively impact subsequent cold rolling.
[0028] S3: Multi-pass cold rolling. The above-mentioned titanium alloy billet is drilled and bored to prepare a rough tube with an outer diameter of Φ40~60mm and a wall thickness of 4~6mm. A multi-pass decreasing deformation rolling process is used, with no intermediate annealing. The multi-pass decreasing deformation rolling is completed in 5~7 passes, with a total rolling deformation of 70%~85%; the deformation per pass decreases from 30% to 12% progressively, and the rolling Q value is controlled between 1.90~2.20; the Q value of the first 3 passes is controlled between 2.05~2.20, and the Q value of the remaining passes is controlled between 1.90~2.05, with the Q value decreasing with each pass. This step yields a cold-rolled titanium tube. This step employs multi-pass rolling with decreasing deformation. A larger deformation amount in the early stages allows for rapid accumulation of deformation energy and grain refinement. Gradually decreasing deformation in later stages prevents pipe cracking due to excessive work hardening, while simultaneously ensuring dimensional accuracy and surface quality. The absence of intermediate annealing allows deformation energy to accumulate pass by pass, providing sufficient driving force for the directional evolution of texture during subsequent gradient aging. The Q value (the ratio of relative wall reduction to relative diameter reduction) is controlled between 1.90 and 2.20, ensuring the pipe is under a stress state dominated by radial compressive stress throughout the cold rolling process, promoting a preferred deflection of the {0001} basal plane along the pipe's radial direction. The first three passes use a higher Q value (2.05~2.20) to enhance the preferred orientation of radial texture in the early stages of deformation. The remaining passes slightly decrease the Q value (1.90~2.05) to maintain the dominance of radial compressive stress while adjusting the uniformity of texture distribution and improving pipe dimensional accuracy. Setting the Q value to decrease sequentially allows the texture orientation to gradually stabilize, avoiding texture disorder caused by sudden changes in the Q value.
[0029] S4: Gradient aging texture control. The above-mentioned cold-rolled titanium tube is placed in a vacuum furnace (vacuum degree 1×10⁻⁶). -3 The process involves a segmented gradient low-temperature aging treatment: the first stage is held at 380–420℃ for 1.5–2.5 h; then, the temperature is increased at a rate of 1–3℃ / min to the second stage at 530–580℃ for 1–1.5 h. After aging, the furnace is cooled to room temperature. This gradient heating method achieves the gradual release of stored energy and the directional evolution of texture, avoiding the texture disorder and performance dispersion caused by traditional direct heating.
[0030] S5: Finishing Process. The aged titanium tubes undergo sequential pressure straightening, inner and outer wall polishing, and deburring. After passing ultrasonic testing, the finished aerospace hydraulic titanium tubes are obtained, with specifications of outer diameter Φ6~25mm, wall thickness 0.5~2.0mm, and single-piece length 3000~6000mm. Straightening eliminates bending deformation caused by cold rolling and aging, ensuring the tube's straightness meets the installation requirements of aerospace hydraulic pipelines. Inner and outer wall polishing reduces surface roughness, decreases stress concentration sources, and helps improve fatigue life. Ultrasonic testing detects internal defects such as cracks, porosity, and inclusions, ensuring the reliability and service safety of the delivered products.
[0031] The α phase of the titanium tube prepared by the above steps is mainly radially textured on the {0001} basal plane, and the shrinkage strain ratio (CSR) is 1.70~1.80.
[0032] The present invention will be further described in detail below with reference to embodiments and comparative examples, but the implementation of the present invention is not limited thereto. Unless otherwise stated, the raw materials and equipment used in the following embodiments are all commercially available products or commonly used equipment in the art, and the detection methods used are all standard detection methods in the art.
[0033] Example 1 This embodiment provides a method for preparing rare earth modified TA18 aerospace hydraulic titanium pipe, including the following steps.
[0034] S1: Batching and Melting. Using TA18 titanium alloy (Ti-3Al-2.5V, mass percentage) as the matrix, 0.12wt% of Nd-Ce mixed rare earth elements were added, with a Nd to Ce mass ratio of 1:1. Melting was carried out using a three-stage vacuum arc melting process, with a vacuum level of 5×10⁻⁶ in the melting chamber. - ¹ Pa, the melting current is 3000A. After melting, the furnace is cooled and held for 3 hours to obtain a uniform titanium alloy ingot with a diameter of Φ250mm.
[0035] S2: Forging and Billet Opening. The aforementioned titanium alloy ingot was heated to 965℃ for the first forging in the β-phase region, breaking up the coarse as-cast dendrite structure. After the first forging, it was air-cooled to room temperature and reheated to 910℃ for subsequent forging. The process was completed in four forging passes, with each pass controlling the deformation between 17% and 20%, resulting in a total forging deformation of 70%. The final forging temperature was 880℃. After forging, it was air-cooled to room temperature to obtain a titanium alloy billet with a diameter of Φ100mm. Metallographic analysis showed that the billet had a uniform, equiaxed α+β dual-phase structure.
[0036] S3: Multi-pass cold rolling. The above-mentioned titanium alloy billet is drilled and bored to prepare a rough tube with an outer diameter of Φ50mm and a wall thickness of 5mm. A multi-pass decreasing deformation rolling process is used, with no intermediate annealing. The process is completed in 6 passes, with a total rolling deformation of 78%, and the deformation per pass decreasing from 28% to 14%. During the rolling process, the Q value is controlled between 2.05 and 2.20 for the first 3 passes and between 1.90 and 2.05 for the last 3 passes, with the Q value decreasing with each pass. This step yields a cold-rolled titanium tube.
[0037] S4: Gradient aging texture control. The above-mentioned cold-rolled titanium tube is placed in a vacuum furnace (vacuum degree 1×10⁻⁶). -3 The process involves a segmented gradient low-temperature aging treatment: the first stage is held at 400℃ for 2.0h; then the temperature is increased at a rate of 2℃ / min to the second stage at 550℃ for 1.2h. After aging, the furnace is cooled to room temperature.
[0038] S5: Finishing process. The aged titanium tubes undergo a series of post-processing steps, such as pressure straightening, inner and outer wall polishing (surface roughness Ra=0.6μm), deburring, and ultrasonic flaw detection. After passing the ultrasonic flaw detection, the finished aviation hydraulic titanium tubes are obtained, with specifications of outer diameter Φ12mm, wall thickness 0.9mm, and single length of 4000mm.
[0039] The finished titanium tubes prepared in Example 1 were tested according to the above testing method, and the results are as follows: The EBSD technology is used to perform {0001} basal plane pole figure inspection on the finished pipes, such as... Figure 2 As shown. From Figure 2 It can be clearly seen that the {0001} poles are concentrated in the radial direction (RD direction) of the pipe, indicating that the α phase of the finished pipe is mainly composed of the radial texture of the {0001} base plane. The texture type is stable and simple, and there is no obvious presence of cylindrical texture or other unfavorable texture.
[0040] According to measurements and calculations, the shrinkage strain ratio (CSR) of the finished pipe is 1.75.
[0041] Tensile testing at room temperature was conducted according to ASTM E8M standard, and the circumferential tensile strength was 868 MPa. Fatigue testing was performed under cyclic loading conditions of a maximum cyclic stress of 680 MPa (78% of the circumferential tensile strength), a stress ratio R=0.1, and a frequency of 10 Hz. The finished pipe achieved a fatigue life of 2.5 × 10⁻⁶ MPa. 7 More than once a week.
[0042] The above results show that the TA18 aviation hydraulic titanium tube prepared in this embodiment has an ideal radial base surface texture and excellent comprehensive mechanical properties.
[0043] Example 2 This embodiment provides a method for preparing rare earth modified TA18 aviation hydraulic titanium tube. The steps are the same as in Embodiment 1, but some process parameters are adjusted as follows.
[0044] S1: Batching and Melting. The amount of Nd-Ce mixed rare earth added is 0.05wt%, and the mass ratio of Nd to Ce is 1:1. Three-stage vacuum consumable arc melting is employed, with a vacuum degree of 5×10⁻⁶ in the melting chamber. -1 Pa, the melting working current is 2800A, after melting, the furnace is cooled and held for 2 hours to obtain a titanium alloy ingot with a specification of Φ200mm.
[0045] S2: Forging and Billet Opening. The titanium alloy ingot is heated to 950℃ for the first forging in the β-phase region. After air cooling to room temperature, it is reheated to 900℃ for subsequent forging cycles. The process is completed in three cycles, with each cycle controlling the deformation between 22% and 25%, resulting in a total forging deformation of 72%. The final forging temperature is 860℃. After forging, the ingot is air cooled to room temperature to obtain a titanium alloy billet with a diameter of Φ80mm.
[0046] S3: Multi-pass cold rolling. The rough tube has an outer diameter of Φ40mm and a wall thickness of 4mm. It is completed in 5 passes using the Pilger cold rolling process, with a total rolling deformation of 70%. The deformation per pass decreases from 30% to 15% in stages. The Q value is controlled between 2.05 and 2.20 for the first 2 passes and between 1.90 and 2.05 for the last 3 passes, with the Q value decreasing in each pass.
[0047] S4: Gradient aging texture control. The first stage is held at 380℃ for 1.5h, and then the temperature is increased to 530℃ for 1.0h at a rate of 1℃ / min. After that, it is cooled in a vacuum furnace.
[0048] S5: Finishing process. After straightening, polishing, deburring, and ultrasonic testing, the finished aviation hydraulic titanium tube is obtained with an outer diameter of Φ10mm, a wall thickness of 0.7mm, and a single tube length of 3500mm.
[0049] The finished pipes prepared in Example 2 were subjected to {0001} basal plane pole figure detection using EBSD technology, such as... Figure 3 As shown. From Figure 3 It can be confirmed that the α phase of the finished pipe is mainly radially textured on the {0001} base plane, and the texture type is consistent with that of Example 1.
[0050] According to measurements and calculations, the shrinkage strain ratio (CSR) of the finished pipe is 1.72.
[0051] Mechanical properties were tested according to the same testing standards as in Example 1. The circumferential tensile strength was 853 MPa, and the fatigue life reached 2.2 × 10⁻⁶ MPa. 7 Week.
[0052] The above results show that even with appropriate adjustments to the rare earth addition amount and process parameters within the preferred range, the method of the present invention can still stably produce TA18 aerospace hydraulic titanium tubes with radial base plane texture as the main feature and excellent comprehensive performance, demonstrating the wide process adaptability and consistent performance of batch products of this method.
[0053] Comparative Example 1 This comparative example provides a method for preparing TA18 aviation hydraulic titanium tube. The purpose is to illustrate, by comparing with Example 1, the superiority of the gradient aging process of the present invention over the conventional single-stage aging process in terms of texture control.
[0054] In this comparative example, except for step S4 (aging treatment), the process parameters for steps S1 to S3 and S5 are exactly the same as in Example 1. Specifically: S1: Same as Example 1, add 0.12wt% of Nd-Ce mixed rare earth (Nd:Ce=1:1), and obtain a Φ250mm titanium alloy ingot through three vacuum consumable arc melting processes.
[0055] S2: Same as Example 1, after the first β-brushing at 965℃ and the subsequent forging at 910℃, the total deformation of the 4 forgings is 70%, and a Φ100mm titanium alloy billet is obtained.
[0056] S3: Same as Example 1, prepare a Φ50mm×5mm rough tube, and perform 6 passes of Pilger cold rolling (deformation decreases from 28% to 14%, Q=2.05~2.20 for the first 3 passes and Q=1.90~2.05 for the last 3 passes), with a total deformation of 78%, to obtain a cold-rolled titanium tube.
[0057] S4 (different from Example 1): The cold-rolled titanium tube is placed in a vacuum furnace and subjected to single-stage aging treatment: directly heated to 550°C and held for 3.2 hours (the total holding time is the same as the total holding time of the two stages in Example 1), and then cooled to room temperature with the furnace.
[0058] S5: Same as in Example 1, after straightening, polishing, deburring and ultrasonic testing, a finished pipe with an outer diameter of Φ12mm and a wall thickness of 0.9mm is obtained.
[0059] The finished pipes obtained in Comparative Example 1 were subjected to {0001} basal plane pole figure inspection using EBSD technology, such as... Figure 4 As shown. From Figure 4 It can be clearly seen that the texture type of the finished pipe is a mixture of base surface texture and cylindrical texture. The {0001} poles are not only distributed in the radial direction, but also have obvious concentrated distribution in the tangential and circumferential directions, indicating that single-stage aging treatment cannot effectively eliminate the non-favorable texture components generated during cold rolling.
[0060] According to measurements and calculations, the shrinkage strain ratio (CSR) of the finished pipe is 1.43.
[0061] Mechanical properties were tested according to the same testing standards as in Example 1. The circumferential tensile strength was 825 MPa, and the fatigue life was approximately 1.6 × 10⁻⁶ MPa. 7 Week.
[0062] By comparing the detection results of Example 1 with those of Comparative Example 1, the following conclusions can be drawn: First, regarding the texture type, Example 1 employs a segmented gradient low-temperature aging treatment (first stage 400℃×2h + second stage 550℃×1.2h), resulting in a finished pipe exhibiting a single {0001} radial texture on the base surface; while Comparative Example 1 employs a single-stage aging treatment (550℃×3.2h), resulting in a finished pipe exhibiting a mixed texture of the base surface and cylindrical surface. This indicates that the segmented gradient aging process used in this invention can achieve graded release of cold-rolled energy, effectively guiding the texture to evolve in a favorable direction and achieving precise shaping, while the single-stage aging treatment, due to the concentrated release of energy during the heating process, cannot achieve selective evolution of the texture.
[0063] Secondly, regarding the CSR value, the CSR value of Example 1 is 1.75, which is within the theoretical optimal range (1.72~1.78); the CSR value of Comparative Example 1 is only 1.43, which, although still meeting the basic requirement of CSR>1.3 in the current aviation tubing standard, is far from the optimal range. This indicates that the CSR value is highly sensitive to the temperature control path of the aging process, and the present invention achieves precise and stable control of the CSR value through gradient aging.
[0064] Third, in terms of mechanical properties, the circumferential tensile strength of Example 1 (868 MPa) is approximately 5.2% higher than that of Comparative Example 1 (825 MPa), and the fatigue life (≥2.5 × 10⁻⁶) is also improved. 7 Weekly) compared to Comparative Example 1 (approximately 1.6 × 10) 7 The number of cycles increased by approximately 56%. This indicates that the purity of the radial base surface texture and the precise control of the CSR value directly determine the circumferential load-bearing capacity and fatigue resistance of the pipe.
[0065] In summary, this invention achieves precise and stable control of the radial texture of the TA18 aerospace hydraulic titanium tube {0001} base surface through the synergistic effect of three technical means: "Nd-Ce rare earth modification - multi-pass cold rolling with decreasing deformation - segmented gradient low temperature aging". It overcomes the technical defects of poor texture controllability and large performance dispersion in traditional single Q value control and single-stage annealing processes, and has significant progress and practical value.
[0066] The method for preparing rare-earth modified TA18 aerospace hydraulic titanium tubes provided by this invention utilizes existing Pilger cold rolling equipment and vacuum heat treatment equipment, requiring no additional special equipment and can be directly applied to existing titanium alloy tube processing lines. The resulting TA18 aerospace hydraulic titanium tubes exhibit a predominantly radial texture on the {0001} basal plane, with a CSR value stably controlled between 1.70 and 1.80, a circumferential tensile strength exceeding 860 MPa, and a fatigue life ≥ 2.5 × 10⁻⁶. 7 The overall performance of this product is significantly superior to similar products prepared using conventional processes. With the continued growth in global demand for seamless titanium tubes for aerospace applications and the urgent need for high-end titanium tubes due to the accelerated mass production of domestically produced large aircraft, this invention has promising prospects for industrial application and significant economic and social benefits.
[0067] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0068] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A method for producing a rare earth modified TA18 aerospace hydraulic titanium tube, characterized by, Includes the following steps: S1, with TA18 titanium alloy as the matrix, Nd-Ce mixed rare earth is added, and titanium alloy ingot is obtained by melting; S2, the titanium alloy ingot is forged in multiple firings to obtain a titanium alloy billet. S3, the titanium alloy billet is processed into a rough tube, and then rolled in multiple passes with decreasing deformation using the Pilger cold rolling process. The Q value of each pass is controlled between 1.90 and 2.20 to obtain a cold-rolled titanium tube. S4, the cold-rolled titanium tube is placed in a protective atmosphere and subjected to segmented gradient low-temperature aging treatment. The first segment is held at 380~420℃ for 1.5~2.5h, and then the temperature is increased to 530~580℃ at a rate of 1~3℃ / min and held for 1~1.5h, followed by cooling. S5 involves post-processing the aged titanium tube to obtain the finished aerospace hydraulic titanium tube.
2. The production method according to claim 1, characterized by, The amount of Nd-Ce mixed rare earth added in step S1 is 0.05wt%~0.20wt% by mass, and the mass ratio of Nd to Ce is 1:(0.9~1.1).
3. The preparation method according to claim 1, characterized in that, The smelting in step S1 adopts multiple vacuum consumable arc smelting, and the vacuum degree of a smelting cavity is ≤5×10 -1 Pa, the smelting working current is controlled at 2800~3200A, and the titanium alloy ingot with a specification of Φ200~350mm is obtained after smelting, cooling and insulation for 2~4h.
4. The method of claim 1, wherein, In step S2, the specific process of forging blanking is as follows: the titanium alloy ingot is heated to 950~980℃ for the first forging in the β phase region, air-cooled to room temperature and then reheated to 900~920℃, followed by 3~4 forgings, with the deformation amount controlled at 20%~30% per forging, the total forging deformation amount at 65%~75%, the final forging temperature not lower than 850℃, and air-cooled to room temperature to obtain a titanium alloy bar blank with Φ80~150mm.
5. The preparation method according to claim 1, characterized in that, In step S3, the outer diameter of the rough tube is Φ40~60mm and the wall thickness is 4~6mm.
6. The method of claim 1, wherein, In step S3, the multi-pass decreasing deformation rolling is completed in 5 to 7 passes, with a total rolling deformation of 70% to 85%; the deformation per pass decreases from 30% to 12% step by step; there is no intermediate annealing during the entire rolling process.
7. The method of claim 1, wherein, In step S3, the Q value for the first 3 passes is controlled between 2.05 and 2.20, and the Q value for the remaining passes is controlled between 1.90 and 2.05, with the Q value decreasing for each pass.
8. The method of claim 1, wherein, In step S4, the protective atmosphere is a vacuum or argon atmosphere, and the cooling is achieved by cooling the furnace to room temperature.
9. The method of claim 1, wherein, In step S5, the finished aviation hydraulic titanium tube has an outer diameter of Φ6~25mm, a wall thickness of 0.5~2.0mm, and a single length of 3000~6000mm.
10. A rare earth modified TA18 aerospace hydraulic titanium tube characterized by, The titanium tube is prepared by any one of claims 1 to 9, wherein the α phase is mainly composed of radial texture on the {0001} basal plane, and the shrinkage strain ratio (CSR) is 1.70 to 1.80.
Citation Information
Patent Citations
Aluminum-titanium alloy wire containing Ce and Nd, and manufacturing method thereof
CN102605224A
Cold-rolled high-strength titanium alloy pipe texture control method
CN110158005A