A method for superplastic forming of large-cavity irregular titanium alloy sheet by blow molding with punch.

By using pre-variable thickness titanium alloy sheet and punch blow molding superplastic forming method, the problems of uncontrollable forming path and low material utilization of large deep cavity irregular titanium alloy sheet are solved, achieving uniform wall thickness and lightweight effect, which is suitable for the manufacturing of parts in aerospace engines, gas turbines and other fields.

CN123102830APending Publication Date: 2026-11-17HARBIN YUHANG JINGCHUANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611399839.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing superplastic forming processes for preparing large-cavity, irregularly shaped titanium alloy sheets suffer from uncontrollable forming paths, poor deformation uniformity, and low material utilization, making it difficult to meet the high precision and lightweight requirements of the aerospace field.

Method used

Pre-variable thickness titanium alloy sheet is used, combined with punch blow-applied superplastic forming method. By gradually blowing and deforming on the punch, the material flow is controlled by the support and constraint of the punch. The air pressure is optimized by segmented or gradient pressurization strategy to ensure uniform wall thickness and material utilization.

Benefits of technology

It achieves uniform wall thickness and structural integrity of large deep-cavity irregular titanium alloy cladding sheets, reduces material waste, improves forming accuracy and material utilization, and meets the lightweight requirements of aerospace parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102830A_ABST
    Figure CN123102830A_ABST
Patent Text Reader

Abstract

This invention provides a method for superplastic forming of large-deep-cavity irregular-shaped titanium alloy sheets using a punch, relating to the field of precision forming technology for titanium alloys. The method includes the following steps: preparing a pre-variable thickness titanium alloy sheet, the thickness distribution of which is negatively correlated with the deformation amount of the corresponding part, i.e., the initial thickness is larger for parts with larger expected deformation; cleaning and stress-relieving annealing of the sheet material; then placing the sheet material on the punch surface, and lowering the die to close and seal the die with the punch, forming a closed cavity; placing the closed die in a superplastic forming device, heating it to the superplastic forming temperature, and then introducing high-pressure gas from the die side into the closed cavity, pushing the sheet material upwards along the punch surface to gradually deform and adhere to the punch surface, thus completing the forming of the large-deep-cavity irregular-shaped titanium alloy sheet. This invention solves the problems of difficult precise control of the forming path, poor deformation uniformity, and low material utilization in existing superplastic forming processes for preparing large-deep-cavity irregular-shaped titanium alloy sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of precision forming technology of titanium alloys, and in particular to a method for superplastic forming of large-cavity irregular titanium alloy sheet punches by blow molding. Background Technology

[0002] Large-cavity irregularly shaped titanium alloy cladding sheets are key structural components in aerospace engines, gas turbines, and high-end equipment. They are characterized by large cavity depths, complex cross-sectional shapes, thin walls, and high height-to-diameter ratios. These parts must withstand high temperatures, high pressures, and complex alternating loads during service, placing extremely stringent requirements on forming accuracy, wall thickness uniformity, and structural integrity. With the continuous increase in aircraft speed and the growing urgency for lightweight structures, the integrated precision forming of large-cavity irregularly shaped titanium alloy cladding sheets has become a core technological bottleneck restricting the development of related equipment.

[0003] Currently, the forming of large, deep-cavity, irregularly shaped titanium alloy sheets mainly relies on superplastic forming (SPF) technology. Superplastic forming is a processing method that utilizes the ultra-high elongation characteristics of metals at specific temperatures and strain rates. Gas pressure is used to force the sheet metal into a mold cavity, thereby manufacturing complex parts. Traditional superplastic forming typically employs an "inward die blowing" method, where the sheet metal is placed above a punch, and high-pressure gas is introduced from above, causing the sheet metal to deform downwards and conform to the mold cavity. For large, deep-cavity annular structures, sometimes positive and negative pressure superplastic forming (i.e., applying pressure to one side first, then to the other) is used to improve wall thickness uniformity.

[0004] However, for large, deep-cavity irregularly shaped titanium alloy cladding sheets, the existing "inward die blowing" forming process has the following technical bottlenecks: (1) Uncontrollable forming path and poor deformation uniformity: When the sheet metal is deformed into the deep cavity under the drive of high-pressure gas, there is a long free suspension deformation stage in the middle area. During this stage, the sheet metal lacks effective support, the deformation path is uncontrollable, resulting in uneven material flow. In particular, it will undergo severe thinning at the bottom of the deep cavity and the transition fillet of the side wall, which is very easy to crack and fail. Although the existing technology attempts to improve this by optimizing the mold temperature field (such as zone heating) or combining processes (such as thermoforming + superplastic forming), none of them have fundamentally solved the problem of uncontrollable thinning of the sheet metal due to lack of constraint during the free deformation stage.

[0005] (2) Low material utilization rate, which is not conducive to lightweighting: In order to compensate for the severe thinning of the deep cavity area, the traditional process usually requires an overall increase in the initial thickness of the sheet metal, resulting in an increase in the weight of the parts and serious material waste, which is contrary to the increasingly stringent lightweight design requirements in the aerospace field. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a superplastic forming method for large deep-cavity irregular titanium alloy cladding sheets by punching and bonding. This method solves the problems of difficult precise control of the forming path, poor deformation uniformity, and low material utilization in existing superplastic forming processes for preparing large deep-cavity irregular titanium alloy cladding sheets.

[0007] According to an embodiment of the present invention, a method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding includes the following steps: Pre-variable thickness titanium alloy sheet is prepared. The thickness distribution of the pre-variable thickness titanium alloy sheet is negatively correlated with the forming deformation of the corresponding part. That is, the initial sheet thickness is larger in the part with a larger expected deformation. The pre-thickness titanium alloy sheet is pretreated, and after pretreatment, the pre-thickness titanium alloy sheet is placed on the surface of the convex mold, and then the concave mold is lowered to close and seal the concave mold with the convex mold, forming a closed cavity. The pretreatment includes surface cleaning and stress-relieving annealing. The lower surface of the concave mold is provided with a sealing groove, which is arranged along the outer contour of the concave mold cavity. A high-temperature resistant sealing ring is installed in the sealing groove. After the mold is closed, it is placed in a superplastic forming equipment and heated to the superplastic forming temperature. Then, high-pressure gas is introduced from the concave mold side into the closed cavity, pushing the pre-variable thickness titanium alloy sheet to gradually deform and adhere to the convex mold surface. The forming process adopts a segmented pressure increase or gradient pressure increase strategy, gradually increasing the gas pressure according to the forming state of different areas of the large deep cavity, to complete the forming of the large deep cavity irregular titanium alloy sheet. After the forming is completed, heating is stopped and gas pressure is maintained. After cooling to below 200°C, the gas pressure is released, the mold is opened, and the formed large deep cavity irregular titanium alloy sheet is taken out. The ratio of the depth of the punch cavity to the minimum width of the cross section is 0.5-3.0, and the depth-to-diameter ratio of the formed large deep cavity irregular titanium alloy cladding is 0.5-3.0.

[0008] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention overturns the traditional forming path of "blowing air into the concave mold" and changes it to the forming method of "blowing onto the convex mold". The titanium alloy sheet is driven by air pressure to adhere to the convex mold. Under the full support and constraint of the convex mold surface, the material flows orderly along the convex mold surface. The deformation path is clear and controllable. This fundamentally avoids the problem of excessive thinning and cracking at the bottom of the deep cavity and the transition rounded corners of the side wall caused by the free suspension deformation of the sheet in the traditional concave mold blowing process. It greatly improves the uniformity of wall thickness and structural integrity of the deep cavity area.

[0009] (2) By using pre-variable thickness titanium alloy plates, the initial thickness of the plates is designed according to the difference in deformation of each part. Thickness compensation is carried out for areas that still have a tendency to thin during the punch blow-on process. Combined with the forming path characteristics of punch blow-on, the uniformity of wall thickness is guaranteed in two ways. This fundamentally avoids the problem of serious material waste in the traditional die blow-on process. It does not require an overall increase in the initial thickness of the plate, thereby reducing material waste and meeting the lightweight requirements of the parts.

[0010] (3) By keeping the pre-thickness titanium alloy sheet in contact with the convex mold surface during the convex mold blowing process, the molding process is gradual and orderly, avoiding the uncontrollability problem of the free deformation stage in the traditional concave mold blowing process. This results in a high degree of fit between the formed large deep cavity irregular titanium alloy sheet and the convex mold surface, and the bending rate and dimensional accuracy are effectively guaranteed.

[0011] (4) The superplastic forming method used in this invention is particularly suitable for large deep cavity irregular titanium alloy cladding with large depth-to-diameter ratio and complex cross-sectional shape. It can be widely used in the forming and manufacturing of various large deep cavity irregular parts such as aerospace engine combustion chamber bushings, gas turbine hot end components, and high-end equipment irregular protective covers.

[0012] (5) The superplastic forming method used in this invention does not require complicated intermediate processes and special auxiliary devices. The process flow of plate placement-mold closing-blowing-cooling demolding is simple and clear, easy to achieve automated control, high production efficiency and controllable production cost. Attached Figure Description

[0013] Figure 1 This is a flowchart illustrating the superplastic forming method for a large deep-cavity irregular titanium alloy sheet punching die in Embodiment 1 of the present invention.

[0014] Figure 2 This is a schematic diagram showing the design of the pre-variable thickness plate and the comparison of wall thickness before and after forming in Embodiment 1 of the present invention.

[0015] Figure 3 This is a flow chart of the punch blow molding process according to Embodiment 1 of the present invention.

[0016] Figure 4 This is a schematic diagram of the pre-variable thickness titanium alloy plate according to Embodiment 2 of the present invention.

[0017] Figure 5 This is a schematic diagram of the formed large-cavity irregular titanium alloy cladding sheet according to Embodiment 2 of the present invention. Detailed Implementation

[0018] The technical solutions of the present invention will be further described below with reference to the accompanying drawings and embodiments.

[0019] Example 1 like Figures 1-3As shown, this embodiment of the invention proposes a punch blow molding superplastic forming method for a large deep-cavity irregular-shaped titanium alloy cladding sheet for an aero-engine (depth-to-diameter ratio 1.5, cross-sectional dimensions 200mm × 150mm, cavity depth 80mm, wall thickness 0.6mm), including the following steps: S1. Prepare a pre-thickness titanium alloy plate. The thickness distribution of the pre-thickness titanium alloy plate is negatively correlated with the forming deformation of the corresponding part. That is, the initial plate thickness is larger in the part with a larger expected deformation. Specifically, the preparation of the pre-variable thickness titanium alloy plate includes: Based on the cavity depth, cross-sectional shape, and deformation requirements of various parts of the deep-cavity irregular titanium alloy cladding, and combined with the finite element simulation prediction results, a thickness distribution scheme for the titanium alloy sheet is designed. Based on the thickness distribution scheme, the titanium alloy sheet is machined or chemically milled to prepare a pre-variable thickness titanium alloy sheet.

[0020] The thickness difference of the pre-variable thickness titanium alloy plate is 0.1-0.8 mm, and the overall thickness is controlled between 0.3-1.5 mm; the titanium alloy is selected from TC4, TA15 or TA32. The punch blow forming process was simulated and analyzed by finite element simulation, and the thickness distribution scheme of the titanium alloy sheet was iteratively optimized to ensure that the wall thickness uniformity error of the formed large deep cavity irregular titanium alloy sheet is ≤ ±0.06mm.

[0021] Specifically, based on the cavity depth, cross-sectional shape, and deformation requirements of the large deep-cavity irregular-shaped cladding, and combined with the finite element simulation prediction results, a thickness distribution scheme for the titanium alloy sheet is designed. Then, based on the thickness distribution scheme, the titanium alloy sheet is machined or chemically milled to prepare a pre-variable thickness titanium alloy sheet. The thickness of the prepared pre-variable thickness titanium alloy sheet is negatively correlated with the forming deformation of the corresponding part, that is, the initial sheet thickness is larger for the part with a larger expected deformation, in order to compensate for the wall thickness reduction during the forming process and ensure that the overall wall thickness of the formed part tends to be uniform.

[0022] Preferably, TC4 titanium alloy sheet is selected. Based on the deep cavity structure characteristics and deformation of each part of the cladding, the punch blow forming process is simulated and analyzed using finite element simulation to predict the wall thickness distribution after forming, and the thickness distribution scheme of the pre-variable thickness sheet is designed: the initial thickness of the deep cavity bottom region (expected to have the largest deformation) is 0.85 mm, the initial thickness of the deep cavity sidewall region is 0.70 mm, the initial thickness of the flange edge region (expected to have the smallest deformation) is 0.50 mm, and the maximum thickness difference is 0.35 mm. Subsequently, the TC4 titanium alloy substrate is chemically milled to prepare the pre-variable thickness titanium alloy sheet that meets the design requirements.

[0023] S2. The pre-thickness titanium alloy plate is pre-treated, and after pre-treatment, the pre-thickness titanium alloy plate is placed on the convex mold surface, and then the concave mold is lowered so that the concave mold and the convex mold are closed and sealed to form a closed cavity. The pre-treatment includes surface cleaning treatment and stress relief annealing treatment. The lower surface of the die cavity is provided with a sealing groove, which is arranged along the outer contour of the die cavity. The sealing groove is fitted with a high-temperature resistant sealing ring, which is made of graphite or metal to maintain a sealing pressure of ≥5MPa in a high-temperature environment of 850-930℃.

[0024] The punch is made of heat-resistant cast steel, high-temperature alloy or ceramic material; the surface roughness Ra of the deep cavity surface of the punch is ≤0.8μm.

[0025] The pretreatment of the pre-thickness-variable titanium alloy plate specifically includes: The surface of the pre-variable thickness titanium alloy sheet is cleaned to remove surface oil and dirt. Subsequently, stress-relief annealing is performed at a temperature of 500-600℃ for 1-2 hours, followed by furnace cooling to room temperature.

[0026] Specifically, firstly, the punch is installed on the lower platform of the mold, and the die is installed on the upper platform of the mold, ensuring the surface fit accuracy of the punch and the die (i.e., the surface roughness of the punch and the die is ≤0.8μm). Then, a release agent (using yttrium oxide or boron nitride) is uniformly coated on the surface of the punch to prevent interface adhesion between the titanium alloy sheet and the punch during superplastic forming. At the same time, the surface of the pre-variable thickness titanium alloy sheet is cleaned to remove surface oil stains, followed by stress-relief annealing at a temperature of 500-600℃ for 1-2 hours, followed by furnace cooling to room temperature to eliminate residual stress inside the sheet and avoid cracking defects during forming.

[0027] After processing, the pre-treated pre-thickness titanium alloy sheet is placed on the convex mold surface, allowing the titanium alloy sheet to naturally adhere to the convex mold surface under gravity and initial positioning. Subsequently, the concave mold is lowered, causing the concave mold, the titanium alloy sheet, and the convex mold to close and seal, forming a closed cavity. The lower surface of the concave mold is provided with a sealing groove, and a high-temperature resistant sealing ring is installed in the sealing groove to ensure the airtightness of the closed cavity under high temperature and high pressure conditions.

[0028] Preferably, the punch is installed on the lower platform of the mold, and the die is installed on the upper platform of the mold. The fitting accuracy of the punch and the die is adjusted. Then, a boron nitride release agent is uniformly coated on the surface of the punch. After stirring evenly, there is no agglomeration or clumping, and it does not fall off after drying. Subsequently, the pre-thickness titanium alloy sheet is wiped clean with a white silk cloth and subjected to stress-relieving annealing treatment at 550°C for 1.5 hours. It is then cooled to room temperature in the furnace. Then, the pre-treated pre-thickness titanium alloy sheet is placed on the surface of the punch, so that the pre-thickness titanium alloy sheet naturally adheres to the surface of the punch under the action of gravity. Finally, the die is lowered, and the high-temperature resistant graphite sealing ring installed in the sealing groove on the lower surface of the die is pressed against the punch table to form a closed cavity, ensuring airtightness.

[0029] S3. Place the mold after mold closing in the superplastic forming equipment and heat it to the superplastic forming temperature. Then, high-pressure gas is introduced from the concave mold side into the closed cavity to push the pre-variable thickness titanium alloy sheet to gradually blow and deform along the convex mold surface to fit the convex mold surface, thus completing the forming of the large deep cavity irregular titanium alloy sheet.

[0030] The superplastic forming temperature is determined based on the titanium alloy material. When the titanium alloy is TC4, the superplastic forming temperature is 850-920℃; when the titanium alloy is TA15 or TA32, the superplastic forming temperature is 850-930℃. The heating rate in the superplastic forming equipment is 60-150℃ / h, and the temperature is held for 10-20 minutes after reaching the superplastic forming temperature.

[0031] The superplastic forming equipment includes a hydraulic system, a heating system, and a gas supply system; the maximum gas supply pressure provided by the gas supply system is ≥4MPa; the temperature and pressure parameters are adjusted in real time according to the actual forming state of the part during the forming process; the temperature uniformity of the superplastic forming equipment during the forming process is ≥±10℃; The high-pressure gas is argon with a purity of ≥99.99%, the forming pressure is 0.5-3MPa, the pressure control accuracy is ±0.01MPa, and the holding time is 30-60min; When high-pressure gas is introduced into the closed cavity from the die side, a segmented pressurization or gradient pressurization strategy is adopted to gradually increase the gas pressure according to the forming state of different regions of the deep cavity, so as to optimize the material flow and wall thickness distribution in each region.

[0032] Specifically, the mold (including the punch and the die) after mold closing is sent into the superplastic forming equipment, and the heating system is started to raise the temperature to the superplastic forming temperature at a heating rate of 60℃ / h-150℃ / h (the superplastic forming temperature is determined according to the titanium alloy material; when the titanium alloy is TC4, the superplastic forming temperature is 850-920℃; when the titanium alloy is TA15 or TA32, the superplastic forming temperature is 850-930℃). After reaching the target temperature, it is held for 10-20 minutes to allow the titanium alloy sheet to fully reach the superplastic state. Subsequently, a heating element is introduced into the closed cavity from the die side. High-purity argon gas (purity ≥99.99%) is applied at a forming pressure of 0.5-3 MPa, with a pressure control accuracy of ±0.01 MPa. A segmented or gradient pressure increase strategy is adopted, gradually increasing the gas pressure according to the forming state of different regions of the deep cavity to optimize the material flow and wall thickness distribution in each region. Under the action of gas pressure, the superplastic titanium alloy sheet gradually deforms upward along the surface of the convex mold, closely fitting the deep cavity surface and detailed features of the convex mold. After holding the pressure for 30-60 minutes, the forming of the large deep cavity irregular titanium alloy sheet is completed. During the forming process, the temperature uniformity of the heating furnace (the heating system includes the heating furnace) is ≥±10℃.

[0033] Preferably, the mold after mold closing is sent into the superplastic forming equipment and heated to 900°C at a heating rate of 100°C / h, and held for 15 minutes to allow the titanium alloy sheet to fully reach the superplastic state. Then, 99.99% pure argon gas is introduced into the closed cavity from the side of the concave mold, and a forming pressure of 1.8MPa is applied, with a pressure control accuracy of ±0.01MPa. A segmented pressure increase strategy is adopted: the first stage increases the pressure to 0.5MPa and holds for 10 minutes to allow the titanium alloy sheet to initially fit the upper part of the deep cavity of the punch; the second stage increases the pressure to 1.2MPa and holds for 15 minutes to allow the titanium alloy sheet to gradually fit the middle part of the deep cavity of the punch; the third stage increases the pressure to 1.8MPa and holds for 20 minutes to allow the titanium alloy sheet to completely fit the bottom and all details of the deep cavity of the punch. The total holding time is 45 minutes. During the forming process, the temperature uniformity of the heating furnace is controlled within ±8°C.

[0034] Furthermore, after the forming of the large, deep-cavity irregular titanium alloy cladding sheet is completed, cooling and demolding are required, specifically including: S4. After the forming is completed, stop heating and maintain gas pressure. After cooling to below 200°C, release the gas pressure, then open the mold and take out the formed large deep cavity irregular titanium alloy sheet.

[0035] The ratio of the depth of the punch cavity to the minimum width of the cross section is 0.5-3.0, and the depth-to-diameter ratio of the formed large deep cavity irregular titanium alloy cladding is 0.5-3.0. It is suitable for forming and manufacturing irregular protective covers for aerospace engine combustion chamber bushings, gas turbine hot end components, and high-end equipment.

[0036] Specifically, after forming is completed, heating is stopped, and the inert gas pressure is kept constant. The mold and the large-cavity shaped titanium alloy sheet are allowed to cool naturally to below 200°C in the furnace. The gas pressure is then released, the mold is opened, and the formed large-cavity shaped titanium alloy sheet is removed. It is important to note that rapid cooling should be avoided during the cooling process to prevent cracking of the parts due to excessive thermal stress.

[0037] Preferably, after the forming is completed, heating is stopped, the argon pressure is kept constant, and the furnace is allowed to cool naturally to 180°C. The gas pressure is then released, the mold is opened, and the formed large deep cavity irregular titanium alloy sheet is removed.

[0038] In this embodiment, the superplastic forming method for large deep cavity irregular titanium alloy sheet punching of the present invention adopts a forming path of "punch blowing": air pressure is applied from the die side to push the titanium alloy sheet upward to adhere to the punch. Since the punch is a solid structure, the titanium alloy sheet is effectively supported and constrained by the punch surface during the process of adhering to the punch. The deformation path is clear and controllable, and the material flows uniformly along the punch surface. This avoids the problems of excessive thinning and uncontrollable deformation caused by the free suspension deformation of the sheet in the traditional die blowing process, and fundamentally improves the wall thickness uniformity and forming integrity of the large deep cavity area.

[0039] The large deep cavity irregular titanium alloy cladding sheet formed by the punch blow molding superplastic forming method of the present invention has a deep cavity bottom wall thickness of 0.52mm, a side wall thickness of 0.55mm, and a flange edge wall thickness of 0.48mm. The wall thickness uniformity error is controlled within ±0.05mm, and there are no defects such as cracking, wrinkling, or shrinkage. Compared with the traditional die blow molding process, the thinning rate at the bottom of the deep cavity is reduced from 45% to 14%, and the overall strength of the part is increased by more than 25%, which meets the requirements for use in aero-engines.

[0040] Example 2 like Figure 4 and Figure 5As shown in Example 1, this embodiment of the invention proposes a punch-blown superplastic forming method for another type of large-cavity irregular-shaped titanium alloy hot-end cladding for gas turbines (depth-to-diameter ratio 2.2, cross-sectional dimensions 300mm×200mm, cavity depth 120mm, wall thickness 0.8mm), including the following steps: S1. Prepare a pre-thickness titanium alloy plate. The thickness distribution of the pre-thickness titanium alloy plate is negatively correlated with the forming deformation of the corresponding part. That is, the initial plate thickness is larger in the part with a larger expected deformation. Specifically, TA15 titanium alloy sheet was selected. Based on the characteristics of the large aspect ratio and significant deformation distribution gradient of the cladding, a pre-variable thickness scheme was designed: initial thickness of 1.0 mm at the bottom of the deep cavity, 0.90 mm in the middle section of the deep cavity sidewall, 0.75 mm in the upper transition zone, and 0.60 mm in the flange edge area, with a maximum thickness difference of 0.40 mm. Subsequently, the pre-variable thickness titanium alloy sheet was prepared by machining. Finite element simulation verification ensured that the wall thickness uniformity error after forming was ≤ ±0.05 mm.

[0041] S2. The pre-thickness titanium alloy plate is pre-treated, and after pre-treatment, the pre-thickness titanium alloy plate is placed on the convex mold surface, and then the concave mold is lowered so that the concave mold and the convex mold are closed and sealed to form a closed cavity. The pre-treatment includes surface cleaning treatment and stress relief annealing treatment. Specifically, the punch described in Example 1 is disassembled and replaced with the punch adapted to the sheet structure of this embodiment. The punch is made of high-temperature alloy and has a surface roughness Ra=0.5μm in the deep cavity. Then, the release agent is coated and the sheet is subjected to stress-relieving annealing treatment according to the method of Example 1. The annealing temperature is 580℃ and the holding time is 1.2h.

[0042] S3. Place the mold after mold closing in the superplastic forming equipment and heat it to the superplastic forming temperature. Then, high-pressure gas is introduced from the concave mold side into the closed cavity to push the pre-variable thickness titanium alloy sheet to gradually blow and deform along the convex mold surface to fit the convex mold surface, thus completing the forming of the large deep cavity irregular titanium alloy sheet.

[0043] Specifically, the titanium alloy sheet is placed according to the method of Example 1, and the mold is closed and sealed. A high-temperature resistant metal sealing ring is installed in the sealing groove to ensure the sealing reliability at a high temperature of 930℃. Then, the temperature is increased to 930℃ at a heating rate of 100℃ / h and held for 20 minutes to make the titanium alloy sheet reach a superplastic state. Subsequently, argon gas with a purity of 99.99% is introduced from the concave mold side, and a gradient pressure increase strategy is adopted: 0→0.5MPa (10min)→1.0MPa (10min)→1.5MPa (10min)→2.5MPa (25min), with a total holding time of 55min, so that the titanium alloy sheet fully fits the deep cavity surface of the punch. During the forming process, the temperature uniformity of the heating furnace is controlled within ±8℃.

[0044] Furthermore, after the forming of the large, deep-cavity irregular titanium alloy cladding sheet is completed, cooling and demolding are required, specifically including: S4. After the forming is completed, stop heating and maintain gas pressure. After cooling to below 200°C, release the gas pressure, then open the mold and take out the formed large deep cavity irregular titanium alloy sheet.

[0045] Specifically, following the cooling and demolding method of Example 1, the molded parts are removed after being cooled in the furnace to below 200°C.

[0046] In this embodiment, the large deep-cavity irregular titanium alloy cladding sheet formed by the punch blow molding superplastic forming method of the present invention has a depth-to-diameter ratio of 2.2, a bottom wall thickness of 0.72 mm, a side wall thickness of 0.75 mm, and a flange edge wall thickness of 0.58 mm. The wall thickness uniformity meets the design requirements, and there are no cracking defects. Compared with the traditional die blow molding process, the thinning rate at the bottom of the deep cavity is reduced from 55% to 10%, the strength of the part is increased by more than 30%, and the weight is reduced by more than 15%.

[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for superplastic forming of large deep-cavity irregularly shaped titanium alloy sheet by blow molding, characterized in that, Includes the following steps: Pre-variable thickness titanium alloy sheet is prepared. The thickness distribution of the pre-variable thickness titanium alloy sheet is negatively correlated with the forming deformation of the corresponding part. That is, the initial sheet thickness is larger in the part with a larger expected deformation. The pre-thickness titanium alloy sheet is pretreated, and after pretreatment, the pre-thickness titanium alloy sheet is placed on the surface of the convex mold, and then the concave mold is lowered to close and seal the concave mold with the convex mold, forming a closed cavity. The pretreatment includes surface cleaning and stress-relieving annealing. The lower surface of the concave mold is provided with a sealing groove, which is arranged along the outer contour of the concave mold cavity. A high-temperature resistant sealing ring is installed in the sealing groove. After the mold is closed, it is placed in a superplastic forming equipment and heated to the superplastic forming temperature. Then, high-pressure gas is introduced from the concave mold side into the closed cavity, pushing the pre-variable thickness titanium alloy sheet to gradually deform and adhere to the convex mold surface. The forming process adopts a segmented pressure increase or gradient pressure increase strategy, gradually increasing the gas pressure according to the forming state of different areas of the large deep cavity, to complete the forming of the large deep cavity irregular titanium alloy sheet. After the forming is completed, heating is stopped and gas pressure is maintained. After cooling to below 200°C, the gas pressure is released, the mold is opened, and the formed large deep cavity irregular titanium alloy sheet is taken out. The ratio of the depth of the punch cavity to the minimum width of the cross section is 0.5-3.0, and the depth-to-diameter ratio of the formed large deep cavity irregular titanium alloy cladding is 0.5-3.

0.

2. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 1, characterized in that, The preparation of the pre-variable thickness titanium alloy plate specifically includes: Based on the cavity depth, cross-sectional shape, and deformation requirements of the large deep cavity irregular titanium alloy cladding, and combined with the finite element simulation prediction results, a thickness distribution scheme for the titanium alloy plate is designed. The titanium alloy is selected from TC4, TA15, or TA32. Based on the thickness distribution scheme, the titanium alloy sheet is machined or chemically milled to prepare a pre-variable thickness titanium alloy sheet. The thickness difference of the pre-variable thickness titanium alloy sheet is 0.1-0.8 mm, and the overall thickness is controlled between 0.3-1.5 mm.

3. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 2, characterized in that, The punch blow forming process was simulated and analyzed by finite element simulation, and the thickness distribution scheme of the titanium alloy sheet was iteratively optimized to ensure that the wall thickness uniformity error of the formed large deep cavity irregular titanium alloy sheet is ≤ ±0.06mm.

4. A method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 2 or 3, characterized in that, The superplastic forming temperature is determined based on the titanium alloy material used in its preparation. Specifically, when the titanium alloy is TC4, the superplastic forming temperature is 850-920℃; when the titanium alloy is TA15 or TA32, the superplastic forming temperature is 850-930℃. The heating rate in the superplastic forming equipment is 60-150℃ / h, and the temperature is held for 10-20 minutes after reaching the superplastic forming temperature.

5. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 1, characterized in that, The superplastic forming equipment includes a hydraulic system, a heating system, and a gas supply system; the maximum gas supply pressure provided by the gas supply system is ≥4MPa; the temperature and pressure parameters are adjusted in real time according to the actual forming state of the part during the forming process; the temperature uniformity of the superplastic forming equipment during the forming process is ≥±10℃; The high-pressure gas is argon with a purity of ≥99.99%, the forming pressure is 0.5-3MPa, the pressure control accuracy is ±0.01MPa, and the holding time is 30-60min.

6. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet punches by blow molding as described in claim 1, characterized in that, The sealing ring is made of graphite or metal to maintain a sealing pressure of ≥5MPa in a high-temperature environment of 850-930℃.

7. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 1, characterized in that, The punch is made of heat-resistant cast steel, high-temperature alloy or ceramic material; The surface roughness Ra of the deep cavity profile of the punch is ≤0.8μm.

8. The method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in claim 1, characterized in that, The pretreatment of the pre-thickness-variable titanium alloy plate specifically includes: The surface of the pre-variable thickness titanium alloy sheet is cleaned to remove surface oil and dirt. Subsequently, stress-relief annealing is performed at a temperature of 500-600℃ for 1-2 hours, followed by furnace cooling to room temperature.

9. A method for superplastic forming of large deep-cavity irregular titanium alloy sheet by blow molding as described in any one of claims 1-8, characterized in that, The deep-cavity irregular titanium alloy cladding is suitable for forming and manufacturing aerospace engine combustion chamber liners, gas turbine hot-end components, and irregular protective covers for high-end equipment.