A casting method for eliminating sand adhesion defects in large frequency tuning wheel castings
By pre-embedding a venting rope in the relief groove to guide gas pressure, the problems of sand adhesion and associated defects in large frequency-modulated wheel castings were solved, resulting in a significant improvement in casting quality and production efficiency.
Patent Information
- Application Number
- CN202611352673.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
The sand adhesion defect in the relief groove of large frequency-modulated wheel castings is difficult to eliminate. Traditional measures have little effect, affecting the surface quality and dimensional accuracy of the castings, and accompanied by frequent porosity and void defects.
Ventilation ropes are pre-embedded in the relief groove area and arranged along the outer upper circumference. Both ends of the ventilation ropes lead to the outside of the sand mold. In combination with the optimization of the molding sand quality and the pouring system, the gas pressure inside the molding sand is relieved and the driving force of interface boiling is cut off.
It completely eliminated the sand adhesion defect in the relief groove area, simultaneously improved porosity and void defects, significantly reduced the cleaning workload, and improved production efficiency and casting quality.
Smart Images

Figure CN123102923A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of casting technology, specifically to a casting method for large frequency-modulating wheel castings, and more particularly to a casting method for eliminating sand adhesion defects in large frequency-modulating wheel castings. Background Technology
[0002] Large frequency-regulating impellers are a key component of large marine diesel engines, and their casting quality directly affects the engine's operational reliability and service life. These castings are typically made of high-strength gray cast iron (such as HT350), with strict requirements on material properties, internal density, and surface finish. The casting process usually employs furan resin sand molding and medium-frequency induction furnace melting, with the furnace charge including pig iron, scrap steel, carbon raisers, and alloys. Due to the particularly thick and large balance block area of the frequency-regulating impeller, chills are installed on the sides and risers on the top surface during casting, based on the metal solidification principles, to ensure the part's mechanical properties and internal density.
[0003] However, under the aforementioned conventional casting process, severe sand adhesion defects frequently occur in the undercut groove area of the frequency tuning wheel. This defect results in a huge amount of cleaning work, seriously affecting not only the surface quality of the casting but also the dimensional accuracy near the undercut groove, thus hindering the normal production of frequency tuning wheels for a long time. Traditional theory classifies surface sand adhesion into two categories: mechanical sand adhesion and chemical sand adhesion. Mechanical sand adhesion is believed to be caused by molten iron penetrating into the voids on the surface of the molding sand; chemical sand adhesion is caused by a chemical reaction between molten iron and molding sand. Traditional methods to address the above-mentioned sand adhesion phenomenon include: compacting the molding sand in the problem area during molding, applying coatings multiple times or even using high-temperature resistant zircon powder coatings, and lowering the pouring temperature. However, these traditional measures have little effect on improving sand adhesion in the undercut groove area. Observation shows that sand adhesion in the undercut groove area often occurs in conjunction with defects such as surface porosity and riser root holes. While there are existing records of installing ventilation ropes in sand molds to remove gas, these are mainly used to prevent porosity defects. There are no reports of using ventilation ropes to eliminate sand adhesion defects, let alone technical solutions that systematically solve the sand adhesion problem based on the special gas behavior mechanism of the cutter relief groove.
[0004] Therefore, how to re-understand the formation cause of sand adhesion in the relief groove from a mechanistic perspective, and develop a casting method that can fundamentally eliminate the sand adhesion defect in this area, has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] To address the technical problem of the difficulty in completely eliminating sand adhesion defects in the relief groove area of large frequency-modulating wheel castings in existing technologies, this invention provides a casting method for eliminating sand adhesion defects in large frequency-modulating wheel castings. The purpose of this invention is to provide a casting method that can fundamentally eliminate sand adhesion defects in large frequency-modulating wheel castings, thereby solving the technical problem that traditional mechanical sand adhesion prevention measures (such as compacting molding sand, applying coatings, lowering pouring temperature, and increasing the density of chills) have little or no effect on sand adhesion in the relief groove area.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A casting method for eliminating sand adhesion defects in large frequency-modulating wheel castings includes the step of molding with furan resin sand. The frequency-modulating wheel casting has a relief groove and a balance block. During casting, chills are placed on the side of the balance block and risers are placed on the top surface. The method further includes the following steps: During the sand filling process, a ventilation rope is pre-embedded in the sand mold at the relief groove. The ventilation rope is arranged along the outer upper circumferential direction of the relief groove, and both ends of the ventilation rope lead to the outside of the sand mold.
[0007] In a preferred embodiment of the present invention, the aperture of the venting rope is 12-16 mm. Controlling the aperture of the venting rope within the above range ensures sufficient venting capacity while preventing excessively large apertures from affecting the strength of the sand mold or causing molten iron to enter the venting rope during casting.
[0008] In a preferred embodiment of the present invention, the sand penetration between the venting rope and the surface of the relief groove is 15-20 mm. Controlling the sand penetration within this range ensures that the venting rope is not exposed on the cavity surface, while also ensuring that the gas in the molding sand can smoothly reach the venting rope and be discharged.
[0009] In a preferred embodiment of the present invention, an iron wire is threaded through the ventilation rope, and the iron wire is selected from one of #8, #10, or #12 iron wire. The function of the iron wire is to maintain the shape and position stability of the ventilation rope during the sand filling process and to prevent the ventilation rope from shifting or deforming when the molding sand is compacted.
[0010] In a preferred embodiment of the present invention, the number of ventilation ropes is one or more. Depending on the difference in gas dispersion capacity of the local sand mold, at least one additional ventilation rope is added to areas with insufficient gas dispersion capacity. Both ends of the additional ventilation rope extend outwards from the mold. For larger diameter frequency-adjusting wheels or areas with high sand compaction, multiple ventilation ropes can be provided to enhance gas dispersion capacity.
[0011] In a preferred embodiment of the present invention, after the sand mold surface is coated with a paint, the sand mold in the relief groove area is baked using gas for 20-25 minutes. The purpose of baking is to pre-evaporate the moisture and small organic molecules on the surface of the sand mold before pouring, thereby reducing the instantaneous gas generation when the sand mold comes into contact with the high-temperature molten iron.
[0012] In a preferred embodiment of the present invention, hot air at 150-180°C is introduced into the mold cavity after molding and maintained for 60-90 minutes. Hot air baking is gentler and more uniform than gas baking, and can preheat and dry the entire mold cavity, while also reducing gas generation.
[0013] In a preferred embodiment of the present invention, the mud content of the molding sand is controlled to be less than 0.3%, the sand particle size is controlled to be 40 / 70 mesh or 50 / 100 mesh, the loss on ignition is controlled to be less than 3.0%, and the resin addition is controlled to be within the range of 0.8% to 1.2%. These molding sand quality control parameters can reduce the gas evolution of the molding sand and improve its permeability from the source.
[0014] In a preferred embodiment of the present invention, a chill is placed on the side of the balance block, a core is set in the sand layer below the chill, and a venting rope is set in the sand layer. The venting rope is arranged in conjunction with the core, and its two ends are connected to the outside of the sand mold. This solution provides an additional venting and drainage measure for the thin sand layer below the chill, which is also a weak point where gas may be difficult to escape.
[0015] In a preferred embodiment of the present invention, a bottom-pouring gating system is used for casting. The bottom-pouring gating system is characterized by molten metal being poured from the bottom of the mold, with the liquid level rising steadily. This effectively reduces the chance of gas entrapment forming bubbles in the molten iron, preventing or reducing the difficulty of gas generated in the sand mold intruding into the molten iron.
[0016] It should be noted that, in order to better understand the technical solution and technical effects of the present invention, the technical principles on which the present invention is based will be explained below.
[0017] Traditional theory classifies surface sand adhesion into two categories: mechanical sand adhesion and chemical sand adhesion. However, after long-term observation and in-depth research, the inventors of this application discovered that sand adhesion in the relief groove cannot be fully explained by traditional theory—the sand blocks removed from the inner surface of the relief groove are a mixture of molten iron and molding sand, with a clear interface with the relief groove surface, and there is no sand adhesion in other parts, ruling out the possibility of chemical sand adhesion; however, various measures taken according to the traditional mechanical sand adhesion theory cannot completely eliminate the sand adhesion phenomenon.
[0018] The inventors of this application propose a novel hypothesis on the sand adhesion mechanism, namely the "interfacial pressure fusion-interfacial boiling" mechanism: When high-temperature molten iron is poured into the mold, the small molecule products of the decomposition of moisture and high molecular weight binders such as furan resin in the molding sand of the relief groove instantly vaporize, generating a large amount of gas; due to the poor venting of the molding sand in the relief groove, the gas pressure increases dramatically in an instant; when the gas pressure exceeds the surface tension of the molten iron, the gas bursts into the molten iron, forming bubbles; the pressure inside the molding sand drops sharply due to the release of gas, and the molten iron is drawn into the voids of the molding sand under negative pressure; the high-temperature molten iron reheats the binder on the surface of the molding sand, causing a large amount of gas to be generated instantly, and the gas pressure in the molding sand rises again, breaking through the interfacial tension and rushing into the molten iron—thus, intermittent pressure fusion leading to interfacial boiling occurs repeatedly at the mold-liquid interface, and finally the molten iron occupies the voids of the molding sand, forming a sand adhesion layer that is difficult to remove.
[0019] Based on the aforementioned novel mechanism, this invention employs a "dredging instead of blocking" technical approach—pre-embedding venting ropes in the cutter relief groove to promptly release the gas pressure accumulated within the molding sand. The venting ropes are arranged along the upper circumference of the cutter relief groove, maximizing the collection of gas generated in this area (gas naturally rises after being heated), with both ends leading to the outside of the mold for smooth discharge of high-pressure gas. After the gas pressure within the molding sand is promptly released, it remains at a low level, unable to overcome the surface tension of the molten iron, thereby cutting off the driving force for interfacial boiling and fundamentally eliminating sand adhesion defects.
[0020] The present invention has the following advantages over the prior art: 1. Complete elimination of sand adhesion defects. After adopting the method of this invention, the severe sand adhesion phenomenon in the retraction groove of the frequency tuning wheel is completely eliminated. By pre-embedding venting ropes in the retraction groove to guide the gas pressure inside the molding sand, the driving force of interface boiling is fundamentally cut off, preventing the sand adhesion defect from recurring.
[0021] 2. Simultaneous improvement of associated defects. Porosity defects near the relief groove are completely eliminated, and porosity defects at the riser root also disappear, thus reducing the riser body size.
[0022] 3. The workload for cleaning is significantly reduced. Since the sand adhesion defect is completely eliminated, the workload for cleaning is significantly reduced, basically the same as cleaning other parts, which significantly reduces labor intensity and time consumption.
[0023] 4. Significant improvement in production efficiency and economic benefits. The quality of individual parts has been significantly improved, the quality of mass production has been stable, production efficiency has been greatly increased, production input has been significantly reduced, and economic benefits have been significantly improved.
[0024] 5. Excellent universality and promotional value. When this method was applied to other similar flywheel products, the severe sand adhesion problem was also eliminated; similar sand adhesion problems were also eliminated in other products with similar sand adhesion mechanisms.
[0025] In summary, this invention provides a casting method based on a novel sand adhesion mechanism that can fundamentally eliminate sand adhesion defects in large frequency-modulated wheel castings, and has significant industrial application value and promising prospects for promotion. Attached Figure Description
[0026] Figure 1 This is a top view schematic diagram of the sand mold for casting the large frequency modulation wheel of the present invention; Figure 2 for Figure 1 AA section view; Figure 3 for Figure 1 BB cross-sectional view.
[0027] Explanation of icon numbers: Detailed Implementation The specific embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0028] The large frequency-modulated wheel involved in this invention is one of the main components of a large marine diesel engine, and its material is high-strength gray cast iron HT350. It is cast using furan resin sand molding and smelted in a medium-frequency induction furnace. The furnace charge includes pig iron, scrap steel, carbon raiser, and alloys.
[0029] like Figures 1 to 3 As shown, a frequency-modulating wheel cavity 2 is formed in sand mold 1. The balance block portion 7 of the frequency-modulating wheel casting is particularly thick, so chills 5 are provided on the side of the balance block 7 and risers 6 are provided on the top surface to ensure the mechanical properties and internal density of the part. The relief groove 3 is located at the corresponding position of the frequency-modulating wheel and is the area where sand adhesion defects are most concentrated.
[0030] Before detailing the technical solution of the present invention, the formation mechanism of sand adhering to the relief groove is first explained in order to better understand the technical concept of the present invention.
[0031] Traditional theory categorizes surface sand adhesion into two types: mechanical sand adhesion and chemical sand adhesion. Mechanical sand adhesion is formed when molten iron penetrates the voids on the surface of the molding sand; chemical sand adhesion is caused by a chemical reaction between the molten iron and the molding sand. However, after long-term observation and in-depth research, the inventors of this application have discovered that sand adhesion in the relief groove area cannot be fully explained by traditional theory.
[0032] Specifically, the sand-adhering blocks removed from the inner surface of the relief groove are a mixture of molten iron and molding sand, with a clear interface to the relief groove surface, and no sand adhesion is observed in other areas. This characteristic rules out the possibility of chemical sand adhesion—if it were chemical sand adhesion, the interface should be blurred and exhibit chemical reaction characteristics. However, various measures taken according to the traditional mechanical sand adhesion theory—compacting the molding sand, applying coatings, lowering the pouring temperature, and increasing the size of the chills—cannot completely eliminate sand adhesion. This indicates that the sand adhesion in the relief groove has a unique formation mechanism.
[0033] The inventors of this application propose a novel hypothesis for the sand adhesion mechanism, namely the "interfacial pressure fusion-interfacial boiling" mechanism. The specific process is as follows: When molten iron is poured into the mold, the sand comes into contact with it. The moisture in the molding sand and the small-molecule products from the thermal decomposition of polymer binders such as furan resin instantly vaporize, generating a large amount of gas in the specific area of the relief groove. The relief groove typically has a complex geometry, high sand compaction, and poor gas escape channels, leading to a sudden and dramatic increase in gas pressure within the molding sand. When the gas pressure suddenly exceeds the surface tension of the molten iron, the gas bursts into the molten iron, forming bubbles. After the gas enters the molten iron, the gas pressure in the molding sand drops sharply, creating a localized negative pressure. Under this negative pressure, the molten iron is drawn into the voids between the sand grains. The high-temperature molten iron directly contacts and heats the polymer binder on the molding sand surface, causing another sudden surge in gas production. The gas pressure in the molding sand rises sharply again, once again exceeding the surface tension of the molten iron at the interface. At the mold-liquid interface, this intermittent pressure fusion may repeatedly occur, leading to interfacial boiling. Ultimately, the molten iron occupies the voids in the molding sand, forming a spatial network of metal wires within the sand mold. This is a mixture of molten iron / metal and molding sand. The metal in the numerous voids of the molding sand at the interface is connected to the casting body, making it extremely difficult to remove.
[0034] Therefore, the sand adhering to the relief groove is essentially a product of the repeated "breathing" process driven by dynamic pressure fusion at the mold-liquid interface, rather than a static result of infiltration. It is precisely because of the complexity of this dynamic process that traditional static defense measures (such as applying coatings or increasing the refractoriness of the molding sand) are ineffective.
[0035] Based on the above-mentioned new mechanism, the core solution proposed in this invention is to pre-embed ventilation ropes in the sand mold at the relief groove to timely release the gas pressure accumulated in the molding sand, so that the gas pressure in the molding sand is always lower than the surface tension of the molten iron, thereby cutting off the driving force of interface boiling and fundamentally eliminating the sand adhesion defect.
[0036] like Figures 1 to 3As shown, during the sand filling process, a ventilation rope 4 is pre-embedded in the sand mold 1 at the relief groove 3. The ventilation rope 4 is arranged along the outer upper circumferential direction of the relief groove 3. The advantages of this arrangement are: (1) the arrangement along the circumferential direction can cover the entire circumference of the relief groove, ensuring that the gas in each part can be effectively channeled; (2) located at the outer upper part of the relief groove, it can collect the gas generated in this part to the greatest extent, because the gas naturally moves upward after being heated; (3) it is convenient for the two ends of the ventilation rope to be led out of the sand mold.
[0037] Both ends of the ventilation rope 4 extend to the outside of the sand mold 1 at the ends of the balance block 7. The purpose of leading both ends of the ventilation rope out of the mold is to allow the high-pressure gas inside the molding sand to be smoothly discharged into the atmosphere, preventing it from accumulating inside the molding sand. In actual operation, one end of the ventilation rope can be led out of the mold and fixed first, and the other end can be led out of the mold after the sand filling is completed.
[0038] The preferred aperture of the venting rope 4 is 12-16 mm. If the aperture is too small, the venting capacity will be insufficient, and the gas pressure inside the molding sand cannot be effectively released; if the aperture is too large, it may affect the strength of the sand mold or allow molten iron to penetrate during the casting process. In a preferred embodiment of the present invention, the aperture of the venting rope is 14 mm, which has been verified by experiments to have good venting effect and process feasibility.
[0039] The sand thickness between the venting rope 4 and the surface of the relief groove 3 is controlled within the range of 15-20mm. Sand thickness refers to the thickness of the sand layer between the outer wall of the venting rope and the cavity surface of the relief groove. If the sand thickness is too small, the venting rope may be exposed on the cavity surface, and molten iron directly contacting the venting rope during pouring could lead to molten iron drilling accidents. If the sand thickness is too large, the gas in the molding sand needs to pass through a thicker sand layer to reach the venting rope, significantly reducing the venting effect. Controlling the sand thickness within the range of 15-20mm ensures that the venting rope is not exposed on the cavity surface while also ensuring good venting and drainage effects.
[0040] In a preferred embodiment of the invention, an iron wire can be threaded through the venting rope 4 to facilitate its placement and positioning. The iron wire can be selected from 8#, 10#, or 12# iron wire. The function of the iron wire is to maintain the shape and position stability of the venting rope during sand filling, preventing displacement or deformation of the venting rope when the molding sand is compacted. After sand filling is completed, the iron wire can be retained in the venting rope or removed. Preferably, the iron wire is retained in the venting rope because it can act as a skeleton, preventing the venting rope from softening and deforming due to heat during casting, thus blocking the venting channels.
[0041] The number of ventilation ropes can be adjusted according to the actual situation. The basic scheme is to set one ventilation rope along the circumference of the upper part of the relief groove. If the local sand mold has poor gas dissipation capacity, ventilation ropes can be added at the relief groove as needed. For example, for a frequency-adjusting wheel with a larger diameter, 2 to 4 ventilation ropes can be evenly arranged in the circumference of the relief groove, with each ventilation rope leading out of the mold to enhance gas conduction capacity.
[0042] To further optimize the technical effects of the present invention, one or more of the following supporting process measures may also be adopted: (a) Sand mold baking After applying the coating to the surface of the sand mold, a gas-fired baking process is used to focus the baking on areas prone to sand adhesion, such as the relief groove, for 20-25 minutes. The purpose of baking is to pre-evaporate the moisture and small organic molecules on the surface of the sand mold before pouring, reducing the instantaneous gas generation when the sand mold comes into contact with the high-temperature molten iron, thereby lowering the peak gas pressure inside the molding sand and helping to reduce the intensity of interface boiling.
[0043] As an alternative, hot air at 150-180℃ can be introduced into the mold cavity after molding for 60-90 minutes. Hot air baking is gentler and more uniform than gas baking, and can preheat and dry the entire mold cavity, while also reducing gas generation. The hot air temperature should be controlled within the range of 150-180℃—too low a temperature will result in poor drying, while too high a temperature may damage the sand mold or cause the coating layer to crack.
[0044] (II) Quality Control of Molding Sand Controlling the quality of molding sand can reduce gas evolution and improve permeability at the source. Specifically: The mud content should be controlled below 0.3%. Excessive mud content will reduce the permeability of the molding sand, making it more difficult for gas to escape and exacerbating pressure buildup.
[0045] The sand particle size is mainly controlled at 40 / 70 mesh and 50 / 100 mesh. If the particle size is too fine, the gaps between the sand particles are small, resulting in poor air permeability and making it difficult for gas to escape; if the particle size is too coarse, the gaps between the sand particles are large, making it easier for molten iron to penetrate. The particle size distribution of 40 / 70 mesh and 50 / 100 mesh can ensure sufficient air permeability while also providing good resistance to molten iron penetration.
[0046] The loss on ignition should be controlled within 3.0%. Loss on ignition reflects the content of organic matter and other volatile components in the molding sand. The lower the loss on ignition, the less gas the molding sand generates at high temperatures.
[0047] The resin addition should be controlled within the range of 0.8% to 1.2%. Resin is the main binder of furan resin sand and one of the main sources of gas generation at high temperatures. If the resin addition is too low, the sand mold strength will be insufficient; if the resin addition is too high, the gas generation will increase and the economy will decrease. Controlling the resin addition within the range of 0.8% to 1.2% can minimize gas generation while ensuring the sand mold strength.
[0048] (III) Venting treatment of the sand layer below the chill When chills 5 are placed on the side of the balance block 7, the sand layer below the chills is usually thin, requiring a core to be placed within it to enhance its strength. In this case, ventilation ropes should also be installed in this sand layer, arranged in conjunction with the core, with both ends of the ventilation ropes connected to the outside of the sand mold. This measure aims to prevent similar gas pressure buildup in the thin sand layer below the chills, which could lead to sand adhesion.
[0049] (iv) Design of the gating system Bottom-pouring gating is preferred for casting. The characteristic of bottom-pouring gating is that the molten metal is poured from the bottom of the mold, and the liquid level rises steadily. Compared to top-pouring or side-pouring systems, bottom-pouring effectively reduces the chance of entrained gas forming bubbles in the molten iron, preventing or reducing the difficulty of gas generated in the sand mold intruding into the molten iron. This, from another perspective, reduces the intensity of gas exchange at the mold-liquid interface, which helps to suppress interfacial boiling.
[0050] The effects of the present invention will be verified through several specific embodiments below.
[0051] Example 1 A large frequency-modulating wheel casting, made of HT350 steel, with an outer diameter of approximately 3200 mm, was molded using furan resin sand. The relief groove area was equipped with a venting rope according to the method of this invention: a 14mm aperture venting rope was arranged along the upper circumference of the relief groove, with a sand intake controlled at 18mm. A #10 iron wire was threaded through the venting rope for auxiliary positioning, and both ends extended out of the mold from the balance block ends. The molding sand had a mud content controlled at 0.25%, a particle size of 50 / 100 mesh, a loss on ignition of 2.8%, and a resin addition of 1.0%. After coating the sand mold, the relief groove area was baked with gas for 22 minutes. A bottom-pouring gating system was used for casting.
[0052] After casting, cleaning and inspection revealed no sand adhesion defects in the relief groove area, and the surface was smooth. The cleaning workload was comparable to that of other areas. There were no porosity defects near the relief groove, and no holes at the riser root. The casting quality was satisfactory, and production efficiency was increased by approximately 30% compared to traditional processes.
[0053] Example 2 A large frequency-modulating wheel casting, made of HT350, has an outer diameter of approximately 3800 mm and a relatively large relief groove diameter. Two ventilation ropes, both with a 16 mm aperture, are evenly arranged around the circumference of the relief groove. The sand intake is controlled at 20 mm, and they are threaded with #8 iron wire. The remaining process parameters are the same as in Example 1.
[0054] After casting, there were no sand adhering defects in the relief groove area. Due to the increased number of ventilation ropes, gas drainage was more thorough, and the surface quality of the casting was better than that of Example 1.
[0055] Example 3 A certain flywheel-type casting, with a structure similar to a frequency tuning wheel and featuring a relief groove, is cast using the method of this invention. The ventilation rope has a 12mm hole diameter, a sand allowance of 15mm, and is threaded with #12 iron wire. After mold assembly, 160℃ hot air is introduced into the mold cavity for 75 minutes before pouring.
[0056] After casting, the sand adhesion in the relief groove area was also eliminated. This indicates that the method of the present invention has good versatility and can be extended to other castings with similar structures.
[0057] To verify the technical effectiveness of this invention, a comparative experiment was conducted. Under the conditions of identical castings, materials, and pouring temperatures, casting was performed using both the traditional process (without ventilation ropes) and the process of this invention (with pre-embedded ventilation ropes). Five frequency tuning wheels were cast in each group of experiments. The results are shown in the table below: Table 1. Comparison of casting quality between traditional process and the process of this invention. Comparative test results show that the method of the present invention can completely eliminate the sand adhesion defect in the relief groove, and at the same time eliminate the associated porosity and hole defects, reduce cleaning time by about 86%, and increase the pass rate to 100%.
[0058] In summary, the core technical principle of this invention can be summarized as follows: Traditional mechanical sand adhesion theory views sand adhesion as a static infiltration process, therefore the measures taken are all "blocking"—applying coatings to block pores, increasing refractoriness to prevent melting, and lowering temperature to reduce dynamics. However, sand adhesion in the relief groove is essentially a dynamic "interfacial boiling" process—repeated fusion of gas pressure drives molten iron to repeatedly enter and exit the pores of the molding sand. For a dynamic process, "blocking" is ineffective because a breakthrough can always be found when the pressure is high enough.
[0059] This invention takes a different approach, employing a "draining" strategy—pre-embedding venting ropes in the cutter relief groove to promptly release the gas accumulated within the molding sand. This keeps the gas pressure within the molding sand at a consistently low level, preventing it from exceeding the surface tension of the molten iron and thus cutting off the driving force for interfacial boiling. Without high-pressure gas in the molding sand, the molten iron will not be explosively injected; without negative pressure, the molten iron will not be drawn into the sand's voids; and without the molten iron entering the voids, the binder will not be repeatedly heated, generating more gas. In this way, the vicious cycle of interfacial boiling is completely broken, and the sand adhesion defect is naturally eliminated.
[0060] This "dredging instead of blocking" technical approach is not only applicable to the frequency tuning wheel's relief groove, but can also be extended to other casting structural parts with similar difficulties in gas discharge.
Claims
1. A casting method for eliminating sand adhesion defects in large frequency-modulating wheel castings, comprising the step of molding with furan resin sand, wherein the frequency-modulating wheel casting has a relief groove and a balance block, and chills are provided on the side of the balance block and risers are provided on the top surface during casting, characterized in that: During the sand filling process, a ventilation rope is pre-embedded in the sand mold at the relief groove. The ventilation rope is arranged along the outer upper circumferential direction of the relief groove, and both ends of the ventilation rope lead to the outside of the sand mold.
2. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: The ventilation rope has a hole diameter of 12~16mm.
3. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: The amount of sand absorbed between the ventilation rope and the surface of the cutter groove is 15~20mm.
4. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: The ventilation rope is threaded with an iron wire, which is selected from one of the following: #8 iron wire, #10 iron wire, or #12 iron wire.
5. The casting method for eliminating sand adhesion defects in large frequency-modulating wheel castings according to claim 1, characterized in that: The number of ventilation ropes is one or more. Depending on the difference in the gas evacuation capacity of the local sand mold, at least one additional ventilation rope is added in the local area where the gas evacuation capacity is insufficient. The two ends of the additional ventilation rope lead out of the mold.
6. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: After applying a coating to the surface of the sand mold, the sand mold in the relief groove area is baked with gas for 20-25 minutes.
7. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: After the mold is closed, hot air at 150~180℃ is introduced into the mold cavity and left for 60~90 minutes.
8. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: The mud content of the molding sand is controlled to be within 0.3%, the sand particle size is controlled to be 40 / 70 mesh or 50 / 100 mesh, the loss on ignition is controlled to be within 3.0%, and the amount of resin added is controlled to be within the range of 0.8% to 1.2%.
9. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to claim 1, characterized in that: A chill is placed on the side of the balance block, a core is set in the sand layer below the chill, and a ventilation rope is set in the sand layer. The ventilation rope is arranged in conjunction with the core and the two ends of the ventilation rope are connected to the outside of the sand mold.
10. The casting method for eliminating sand adhesion defects in large frequency tuning wheel castings according to any one of claims 1 to 9, characterized in that: The bottom-pouring gating system was used for pouring.