Methods to improve the quality of ceramic cores for gas turbine blades

By employing techniques such as zoned shrinkage compensation, targeted support reinforcement, and dual compensation at positioning points, the dimensional accuracy and structural stability issues of ceramic cores have been resolved, improving the manufacturing quality and yield of gas turbine blades and achieving high-efficiency process compatibility.

CN123102938APending Publication Date: 2026-11-17AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611578401.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ceramic cores suffer from quality defects such as dimensional deviations, structural deformation, and cracking failures during the preparation and casting process, making it difficult to meet the high precision requirements of gas turbine blades. Furthermore, their poor process compatibility affects the casting qualification rate.

Method used

By employing techniques such as zoned shrinkage compensation, targeted support reinforcement, and dual compensation at positioning points, the shrinkage rate and support ribs of different parts of the ceramic core are set and arranged separately. Combined with hot press molding process, the positioning method is optimized to improve dimensional accuracy and structural stability.

Benefits of technology

It significantly improves the dimensional accuracy and structural stability of ceramic cores, meets the high precision requirements of gas turbine blades, reduces the technical implementation threshold and promotion cost, and improves the qualification rate of castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102938A_ABST
    Figure CN123102938A_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the quality of ceramic cores for gas turbine blades, comprising the following steps: setting a reference shrinkage rate along the length extension direction and the cross-sectional thickness direction respectively; dividing the length direction into several shrinkage compensation sections, and adjusting the shrinkage rate of each shrinkage compensation section in the thickness direction accordingly; arranging several support ribs inside the straight hole channel, the cover plate area, the corner area of ​​the curved channel, and the large cross-section channel respectively; setting main positioning points and auxiliary positioning points on the ceramic core, and setting a thermal deformation compensation coefficient at the contact surface between the positioning points and the forming mold; preparing the ceramic core and testing it to determine whether the forming accuracy, internal integrity, and mechanical properties of the ceramic core meet the preset usage requirements. This invention solves the problems of low dimensional accuracy, frequent deformation and cracking, insufficient positioning accuracy, and poor process adaptability of existing ceramic cores, thereby improving the manufacturing quality and dimensional qualification rate of ceramic cores for gas turbine blades.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of precision casting technology for gas turbine blades, and specifically relates to a method for improving the quality of ceramic cores for gas turbine blades. Background Technology

[0002] As a core hot-end component of a gas turbine, the geometric accuracy of the internal cavity structure of turbine blades directly affects the engine's performance and reliability. The ceramic core, as the key forming medium for creating the complex hollow internal cavity of the blade, directly determines the metallurgical quality and yield of the final casting through its dimensional accuracy and structural stability. However, existing ceramic cores still face numerous technical bottlenecks in their preparation and casting processes. Quality defects such as dimensional deviations, structural deformation, and cracking failures have long remained unresolved, making it difficult to improve the yield of the final blade castings. These quality defects manifest themselves as follows: Firstly, there is the deformation problem caused by inconsistent shrinkage rates. Existing large-size ceramic cores typically employ a uniform shrinkage rate design. However, due to structural differences, uneven wall thickness, and uneven temperature field distribution, the actual shrinkage rates of different parts of the ceramic core (such as tenons, blades, and blade tips) vary significantly. When the shrinkage rate does not match the structural design, it can easily lead to stress concentration inside the core, resulting in deformations such as warping and twisting, or even cracking, severely affecting the dimensional accuracy of the blade's internal cavity.

[0003] Secondly, there is insufficient support for easily deformable parts. For large-sized, thin-walled, or cantilevered ceramic cores, existing designs lack effective support and reinforcement measures for easily deformable parts (such as long cantilever sections, large-span corner areas, and thin-walled areas). During core fabrication, due to their own weight and significant dimensional differences in different parts, ceramic cores are highly susceptible to plastic deformation or fracture, resulting in a high core scrap rate and affecting the casting yield.

[0004] Third, insufficient positioning accuracy and poor adaptability. Existing ceramic core positioning methods often suffer from insufficient positioning accuracy or positioning failure due to unreasonable positioning point layout and mismatch between the positioning structure and the core's thermal expansion coefficient. Specifically, the number, layout, and gap settings of positioning points lack scientific basis, failing to effectively constrain the core's thermal deformation and displacement under high-temperature environments; the gap design between the positioning points and the core body does not fully consider the differences in material thermal expansion, easily leading to interference jamming or instability due to excessive gaps; and the positioning reference transmission chain of complex internal cavity structures is too long, resulting in significant cumulative errors and making it difficult to meet the ±0.1mm dimensional tolerance requirements of high-precision blades.

[0005] Fourth, there are bottlenecks in process compatibility and efficiency. Traditional solutions often improve yield by increasing the overall strength of the core or simplifying the core structure, but this often comes at the cost of sacrificing process flexibility or increasing manufacturing costs, and it is difficult to meet the structural diversity requirements of different blade models.

[0006] Therefore, there is an urgent need to develop a method to improve the quality of ceramic cores for gas turbine blades. This method should systematically solve the problems of low dimensional accuracy, frequent deformation and cracking, and poor process adaptability of existing ceramic cores by using techniques such as precise matching of differentiated shrinkage rates, targeted strengthening of easily deformable parts, high-precision positioning optimization, and gap adaptive compensation. This will significantly improve the dimensional qualification rate and production stability of gas turbine blade castings. Summary of the Invention

[0007] To address the problems existing in the prior art, the present invention provides a method for improving the quality of ceramic cores for gas turbine blades, the method comprising the following steps: Step 1: Based on the length and thickness dimensions of the ceramic core, set the reference shrinkage rate along the length extension direction and the reference shrinkage rate along the thickness direction of the cross section, respectively; divide the ceramic core into several shrinkage compensation sections along the length direction, and adjust the shrinkage rate of each shrinkage compensation section in the thickness direction according to the differences in the geometric configuration and wall thickness distribution of each shrinkage compensation section, so that each shrinkage compensation section has an independent thickness shrinkage rate parameter, thereby achieving segmented and precise control of dimensional shrinkage behavior during the sintering of the ceramic core and the casting of the blade; Step 2: Based on the length of the internal channel of the ceramic core, arrange several support ribs in the straight hole channel along the direction perpendicular to the straight hole channel. At the same time, arrange several support ribs in the cover plate area, the corner area of ​​the curved channel, and the large cross-section channel. Remove all support ribs after the ceramic core has completed the sintering process. Step 3: Set the main positioning point and the auxiliary positioning point on the ceramic core, and set the thermal deformation compensation coefficient at the contact surface between the main positioning point and the auxiliary positioning point and the forming mold, so that the actual position of the main positioning point and the auxiliary positioning point after the ceramic core is sintered and the blade is cast matches the design position. Step 4: Prepare the ceramic core using hot press injection molding process, and test the overall performance of the ceramic core. Based on the test results, determine whether the molding accuracy, internal integrity and mechanical properties of the ceramic core meet the preset usage requirements.

[0008] Preferably, in step one, the reference shrinkage rate along the length extension direction is set segment by segment according to the length of the ceramic core: the reference shrinkage rate is 1.2-1.5% for ceramic core lengths of 300-500mm; 1.5-1.8% for ceramic core lengths of 500-700mm; and 1.8-2.2% for ceramic core lengths of 700-900mm.

[0009] In any of the above schemes, it is preferred that, in step one, the reference shrinkage rate along the cross-sectional thickness direction is set in segments according to the thickness of the ceramic core: the reference shrinkage rate is 2.0-2.2% for ceramic core thickness of 3-12mm; 2.2-2.4% for ceramic core thickness of 12-18mm; and 2.4-2.6% for ceramic core thickness of 18-25mm.

[0010] In any of the above schemes, it is preferred that, in step one, the shrinkage compensation section divided along the length direction of the ceramic core includes a tenon area, a blade area, a blade tip area, and an internal channel; the tenon area has a larger wall thickness, the blade area has a more uniform wall thickness, the blade tip area has a thinner wall thickness, and the internal channel includes a straight hole channel, a curved channel, and a large cross-section channel.

[0011] In any of the above schemes, preferably, in step one, the final shrinkage rate of each shrinkage compensation section in the thickness direction is adjusted as follows: the final shrinkage rate of the tenon area is equal to the reference shrinkage rate of the ceramic core along the cross-sectional thickness direction plus 0.2%, to compensate for insufficient shrinkage in this area due to the large structural thickness, and to ensure that it matches the design dimensions after shrinkage; the final shrinkage rate of the blade area is equal to the reference shrinkage rate of the ceramic core along the cross-sectional thickness direction, to maintain the dimensional stability and straightness of this area; the final shrinkage rate of the blade tip area is equal to the reference shrinkage rate of the ceramic core along the cross-sectional thickness direction minus 0.1%, to avoid dimensional deviations in this thin-walled area due to over-compensation.

[0012] In any of the above schemes, it is preferred that, in step one, the final shrinkage rate of each type of channel in the thickness direction in the tenon area, blade area, and tip area is adjusted as follows: the final shrinkage rate of the straight hole channel is equal to the final shrinkage rate of the area; the final shrinkage rate at the corner of the curved channel is equal to the final shrinkage rate of the area plus 0.1-0.2%; and the final shrinkage rate of the large cross-section channel is equal to 1.1 times the final shrinkage rate of the area.

[0013] In any of the above solutions, it is preferred that, in step two, when the length of the internal channel of the ceramic core is greater than or equal to 80mm, a support rib is required to be arranged inside the straight hole channel. The horizontal distance between two adjacent support ribs is 40-60mm. The support rib is cuboid in shape, with a length equal to the hole diameter of the channel, a width of 5-8mm, and a thickness of 3-5mm. Its material is the same as that of the ceramic core.

[0014] In any of the above solutions, preferably, in step two, triangular support ribs are arranged in the corner area of ​​the curved channel. The two right-angled sides of the support ribs have a contact length with the channel wall of greater than or equal to 15mm, a thickness of 3-5mm, and are made of alumina-based ceramic material; cylindrical support ribs are arranged in the cover plate area. The diameter of the support ribs is 2-3mm, and they are made of alumina-based ceramic material; the cross-sectional area of ​​the inner cavity is not less than 50cm². 2 The large cross-section channel is equipped with cylindrical support ribs with a diameter of 20-30mm, and the material is alumina-based ceramic material.

[0015] In any of the above schemes, it is preferred that, in step two, the alumina support rib can also be designed as a spiral groove interlocking structure or an end conical positioning interlocking structure; the spiral groove interlocking structure is provided with at least three parallel spiral grooves on the outer surface of the cylindrical support rib, the upper opening width of the groove is 4-5mm, the lower opening width is 3-4mm, the depth is 1.5-2mm, and the distance between two adjacent spiral grooves is 1-3mm; the end conical positioning interlocking structure is provided with a conical positioning section at each end of the cylindrical support rib, the conical positioning section is embedded in the ceramic core, its bottom diameter is equal to the diameter of the cylindrical support rib, and its axial height is greater than or equal to 3mm.

[0016] In any of the above schemes, it is preferred that, in step two, the cylindrical alumina support ribs need to be roughened by sandblasting, and the surface roughness after sandblasting is 3.2-6.3μm, so as to enhance the interfacial bonding strength between them and the ceramic slurry.

[0017] In any of the above schemes, preferably, in step three, the main positioning point is set in the tenon area and the blade tip area of ​​the ceramic core, and the auxiliary positioning point is set in the middle area of ​​the blade of the ceramic core; the main positioning point adopts a conical embedded positioning structure or a frustum-shaped positioning structure; when the conical embedded positioning structure is a conical positioning hole or a conical positioning groove, its taper is 5-10° and the hole diameter or groove width is 5-10mm; the small end diameter of the frustum-shaped positioning structure is 5-15mm, the height is 3-6mm, and the taper is 5-10°; the auxiliary positioning point adopts a hemispherical positioning structure with a diameter of 2-8mm.

[0018] In any of the above schemes, it is preferred that, in step three, the thermal deformation compensation coefficients at the contact surfaces of the main positioning point and the auxiliary positioning point with the forming mold are both set to 1.05-1.1, that is, the final shrinkage rate of the main positioning point and the auxiliary positioning point is equal to 1.05-1.1 times the final shrinkage rate along the thickness direction of their respective shrinkage compensation sections; the roots of the main positioning point and the auxiliary positioning point are provided with rounded corners for smooth transition, with a rounded corner radius greater than or equal to 1.5 mm and a surface roughness less than or equal to 1.6 μm; the gap between the main positioning point and the forming mold is 0.05-0.1 mm, and the gap between the auxiliary positioning point and the forming mold is 0.1-0.3 mm.

[0019] In any of the above schemes, it is preferred that, in step four, the inspection items include dimensional inspection, defect inspection and strength inspection, and the inspection covers the entire structural area of ​​the ceramic core, including the ceramic core body, the internal channel area, the area below the cover plate, the positioning point area and the support rib area.

[0020] In this invention, if the test results of the ceramic core meet the following standards, it can be determined that the molding accuracy, internal integrity, and mechanical properties of the ceramic core meet the preset usage requirements.

[0021] Dimensional inspection: A laser tracker (measurement accuracy ±0.01mm) and a 3D optical scanner (scanning accuracy ±0.02mm) are used to inspect the overall external dimensions of the ceramic core, the cross-sectional dimensions of the channel, the coordinates of the positioning points, and the spacing of the support ribs. The acceptable threshold is ±0.4mm.

[0022] Defect detection: X-ray flaw detector (sensitivity ≥1.5%) and industrial CT scanner (resolution 0.1mm) are used to detect internal pores (pore diameter ≤0.5mm is acceptable), cracks (length ≤1.0mm is acceptable) and peeling defects at the joint between the support rib and the core matrix. There are no gaps, pores or inclusions ≥0.1mm within a ≤3mm range of the support rib area.

[0023] Strength testing: The strength of the ceramic core is tested using a four-point bending test, and the overall bending strength is ≥15 MPa.

[0024] Positioning point inspection: The coaxiality between the tapered positioning point and the core substrate is ≤ φ0.3mm.

[0025] Support rib inspection: There are no gaps, pores, or inclusions of ≥0.1mm within the ≤3mm area of ​​the support rib (flaw detection sensitivity ≥1.5%); Two samples are randomly selected from each batch, and a torque of 5-10N・m is applied to the alumina support rib. The alumina support rib does not rotate relative to the others, and the shear bond strength is ≥3MPa.

[0026] This invention primarily focuses on the dimensional changes of ceramic cores in the length and thickness directions, while the dimensional changes in the width direction are negligible. The overall shrinkage characteristics of different ceramic cores are distinguished based on the shrinkage changes in the length direction, while the local shrinkage behavior of different parts of the same ceramic core is distinguished based on the shrinkage changes in the thickness direction.

[0027] This invention uses hot press injection molding to prepare ceramic cores. The hot press injection molding process and subsequent processes such as sintering, dewaxing, and impregnation strengthening can be carried out using existing technologies, and there are no special requirements for process parameters.

[0028] Compared with the prior art, the method for improving the quality of ceramic cores for gas turbine blades of the present invention has the following beneficial effects: (1) Improve dimensional accuracy through zoned shrinkage compensation. In step one of this invention, several shrinkage compensation sections are divided along the length of the ceramic core. Different final shrinkage rates are set for different parts such as tenon, blade body, and blade tip. This overcomes the problem of mismatch in shrinkage behavior in different areas caused by the traditional uniform shrinkage rate design. It effectively avoids stress concentration, warping, twisting and cracking caused by shrinkage mismatch, and significantly improves the dimensional accuracy and wall thickness uniformity of the blade's internal flow channel.

[0029] (2) Improve structural stability through targeted support reinforcement. In step two of this invention, support ribs with different configurations such as cuboids, cylinders and triangles are arranged for different easily deformable parts such as straight hole channels, cover plate areas, corners of curved channels and large cross-section channels. During sintering and casting, these ribs form effective support for weak parts, which significantly enhances the core's resistance to deformation under high temperature and load conditions. The support ribs are removed after sintering to avoid adverse effects on the accuracy of the final casting cavity.

[0030] (3) Improve positioning accuracy through dual compensation of positioning points. In step three of this invention, a precise positioning constraint relationship is established through the synergistic effect of the main positioning point and the auxiliary positioning point. A thermal deformation compensation coefficient is set at the contact surface between the positioning point and the forming mold, which eliminates the displacement interference between the thermal expansion of the mold and the shrinkage of the core. This avoids the problem of interference jamming or instability due to the mismatch of thermal expansion coefficients in the traditional positioning method, and meets the requirements of high-precision blades for positioning consistency.

[0031] (4) The process compatibility problem has been solved. Steps one to three of this invention are independent of each other and complementary to each other. The parameters of each step can be flexibly adjusted according to the structural characteristics of different types of blades, which has good process compatibility and scalability. Each step can be implemented independently or in combination, and can be achieved without large-scale modification of existing production equipment, which significantly reduces the technical implementation threshold and promotion cost.

[0032] (5) Achieve full-process quality control through comprehensive performance testing. In step four of this invention, the dimensional inspection, defect inspection and strength inspection are carried out on the molded ceramic core. The inspection range covers the core body, internal channels, under the cover plate, positioning points and the area where the support ribs are located. The implementation effect of each previous step is comprehensively verified to ensure that the molding accuracy, internal integrity and high temperature mechanical properties of the core meet the preset usage requirements, forming a complete closed loop from process control to quality verification.

[0033] In summary, this invention, through a systematic technical solution of zoned shrinkage compensation, targeted support reinforcement, and positioning point compensation, effectively solves the problems of low dimensional accuracy, frequent deformation and cracking, insufficient positioning accuracy, and poor process adaptability of existing ceramic cores. It significantly improves the manufacturing quality and dimensional qualification rate of ceramic cores for gas turbine blades, and has significant economic benefits and application value. Attached Figure Description

[0034] Figure 1 This is a CT scan of the interior of a ceramic core (no internal defects) prepared according to a preferred embodiment of the method for improving the quality of ceramic cores for gas turbine blades of the present invention. Figure 2 CT scan of the interior of a ceramic core prepared using traditional methods (indicating internal defects). Detailed Implementation

[0035] To further understand the invention, the following detailed description of the invention will be provided in conjunction with specific embodiments.

[0036] Example 1:

[0037] According to a preferred embodiment of the method for improving the quality of ceramic cores for gas turbine blades of the present invention, the improvement method includes the following steps: Step 1: Based on the length and thickness dimensions of the ceramic core, set the reference shrinkage rate along the length extension direction and the reference shrinkage rate along the thickness direction of the cross section, respectively; divide the ceramic core into several shrinkage compensation sections along the length direction, and adjust the shrinkage rate of each shrinkage compensation section in the thickness direction according to the differences in the geometric configuration and wall thickness distribution of each shrinkage compensation section, so that each shrinkage compensation section has an independent thickness shrinkage rate parameter, thereby achieving segmented and precise control of dimensional shrinkage behavior during the sintering of the ceramic core and the casting of the blade; Step 2: Based on the length of the internal channel of the ceramic core, arrange several support ribs in the straight hole channel along the direction perpendicular to the straight hole channel. At the same time, arrange several support ribs in the cover plate area, the corner area of ​​the curved channel, and the large cross-section channel. Remove all support ribs after the ceramic core has completed the sintering process. Step 3: Set the main positioning point and the auxiliary positioning point on the ceramic core, and set the thermal deformation compensation coefficient at the contact surface between the main positioning point and the auxiliary positioning point and the forming mold, so that the actual position of the main positioning point and the auxiliary positioning point after the ceramic core is sintered and the blade is cast matches the design position. Step 4: Prepare the ceramic core using hot press injection molding process, and test the overall performance of the ceramic core. Based on the test results, determine whether the molding accuracy, internal integrity and mechanical properties of the ceramic core meet the preset usage requirements.

[0038] In step one, the reference shrinkage rate is set segment by segment along the length extension direction according to the ceramic core length. In this embodiment, the ceramic core length is 400mm and the reference shrinkage rate is 1.4%. The reference shrinkage rate is also set segment by segment along the cross-sectional thickness direction according to the ceramic core thickness. In this embodiment, the ceramic core thickness is 8mm and the reference shrinkage rate is 2.1%.

[0039] The shrinkage compensation section divided along the length of the ceramic core includes a tenon area, a blade area, a blade tip area, and an internal channel; the tenon area has a larger wall thickness, the blade area has a more uniform wall thickness, the blade tip area has a thinner wall thickness, and the internal channel includes a straight hole channel, a curved channel, and a large cross-section channel.

[0040] The final shrinkage rate of each shrinkage compensation section in the thickness direction is adjusted as follows: The final shrinkage rate of the tenon area is equal to the reference shrinkage rate of the ceramic core along the thickness direction of the cross section plus 0.2% to compensate for insufficient shrinkage caused by the large structure in this area, and to ensure that it matches the design dimensions after shrinkage; the final shrinkage rate of the blade area is equal to the reference shrinkage rate of the ceramic core along the thickness direction of the cross section to maintain the dimensional stability and straightness of this area; the final shrinkage rate of the blade tip area is equal to the reference shrinkage rate of the ceramic core along the thickness direction of the cross section minus 0.1% to avoid dimensional deviations in this thin-walled area due to over-compensation.

[0041] In the tenon area, blade area, and blade tip area, the final shrinkage rate of each type of channel in the thickness direction is adjusted as follows: the final shrinkage rate of a straight channel is equal to the final shrinkage rate of the area; the final shrinkage rate at the corner of a curved channel is equal to the final shrinkage rate of the area plus 0.15%; and the final shrinkage rate of a large cross-section channel is equal to 1.1 times the final shrinkage rate of the area.

[0042] In step two, when the length of the internal channel of the ceramic core is greater than or equal to 80mm, a support rib needs to be installed inside the straight hole channel. The horizontal distance between two adjacent support ribs is 50mm. The support rib is cuboid in shape, with a length equal to the hole diameter of the channel, a width of 7mm, and a thickness of 4mm. Its material is the same as that of the ceramic core.

[0043] Triangular support ribs are installed at the corners of the curved passage. Each rib has two right-angled sides that adhere to the passage wall for 15mm, and its thickness is 4mm. The ribs are made of alumina-based ceramic material. Cylindrical support ribs with a diameter of 2.5mm are installed in the cover plate area. The cross-sectional area of ​​the inner cavity is not less than 50cm². 2 The large cross-section channel is equipped with cylindrical support ribs with a diameter of 25mm, which are made of alumina-based ceramic material.

[0044] For alumina support ribs, a spiral groove interlocking structure or an end-conical positioning interlocking structure can also be designed. The spiral groove interlocking structure consists of three parallel spiral grooves on the outer surface of the cylindrical support rib. The upper opening width of the groove is 4.5 mm, the lower opening width is 3.5 mm, and the depth is 1.8 mm. The distance between two adjacent spiral grooves is 2 mm. The end-conical positioning interlocking structure consists of a conical positioning section at each end of the cylindrical support rib. The conical positioning section is embedded inside the ceramic core, and its bottom diameter is equal to the diameter of the cylindrical support rib, with an axial height of 3 mm.

[0045] For cylindrical alumina support ribs, their surfaces need to be roughened by sandblasting. The surface roughness after sandblasting is 4.8μm to enhance the interfacial bonding strength between them and the ceramic slurry.

[0046] In step three, the main positioning points are located in the tenon area and blade tip area of ​​the ceramic core, and the auxiliary positioning points are located in the middle area of ​​the blade body of the ceramic core. The main positioning points adopt a conical embedded positioning structure or a frustum-shaped positioning structure; when the conical embedded positioning structure is a conical positioning hole or a conical positioning groove, its taper is 8° and the hole diameter or groove width is 8mm; the small end diameter of the frustum-shaped positioning structure is 10mm, the height is 4.5mm, and the taper is 8°; the auxiliary positioning points adopt a hemispherical positioning structure with a diameter of 5mm.

[0047] The thermal deformation compensation coefficients at the contact surfaces of the main and auxiliary positioning points with the forming mold are both set to 1.08, meaning that the final shrinkage rate of the main and auxiliary positioning points is equal to 1.08 times the final shrinkage rate along the thickness direction of their respective shrinkage compensation sections. The roots of the main and auxiliary positioning points are rounded for a smooth transition, with a radius of 1.5 mm and a surface roughness of 1.6 μm. The gap between the main positioning point and the forming mold is 0.08 mm, and the gap between the auxiliary positioning point and the forming mold is 0.2 mm.

[0048] In step four, the inspection items include dimensional inspection, defect inspection, and strength inspection. The inspection covers all structural areas of the ceramic core, including the ceramic core body, internal channel area, area under the cover plate, positioning point area, and support rib area.

[0049] In this embodiment, if the test results of the ceramic core meet the following standards, it can be determined that the molding accuracy, internal integrity, and mechanical properties of the ceramic core meet the preset usage requirements.

[0050] Dimensional inspection: A laser tracker (measurement accuracy ±0.01mm) and a 3D optical scanner (scanning accuracy ±0.02mm) are used to inspect the overall external dimensions of the ceramic core, the cross-sectional dimensions of the channel, the coordinates of the positioning points, and the spacing of the support ribs. The acceptable threshold is ±0.4mm.

[0051] Defect detection: X-ray flaw detector (sensitivity ≥1.5%) and industrial CT scanner (resolution 0.1mm) are used to detect internal pores (pore diameter ≤0.5mm is acceptable), cracks (length ≤1.0mm is acceptable) and peeling defects at the joint between the support rib and the core matrix. There are no gaps, pores or inclusions ≥0.1mm within a ≤3mm range of the support rib area.

[0052] Strength testing: The strength of the ceramic core is tested using a four-point bending test, and the overall bending strength is ≥15 MPa.

[0053] Positioning point inspection: The coaxiality between the tapered positioning point and the core substrate is ≤ φ0.3mm.

[0054] Support rib inspection: There are no gaps, pores, or inclusions of ≥0.1mm within the ≤3mm area of ​​the support rib (flaw detection sensitivity ≥1.5%); Two samples are randomly selected from each batch, and a torque of 5-10N・m is applied to the alumina support rib. The alumina support rib does not rotate relative to the others, and the shear bond strength is ≥3MPa.

[0055] This embodiment offers the following advantages: it improves dimensional accuracy through zoned shrinkage compensation; enhances structural stability through targeted support reinforcement; improves positioning accuracy through dual compensation of positioning points; resolves process compatibility issues; and achieves full-process quality control through comprehensive performance testing. This embodiment effectively addresses the problems of low dimensional accuracy, frequent deformation and cracking, insufficient positioning accuracy, and poor process adaptability in existing ceramic cores, significantly improving the manufacturing quality and dimensional pass rate of ceramic cores for gas turbine blades, demonstrating significant economic benefits and application value.

[0056] Example 2:

[0057] Another preferred embodiment of the method for improving the quality of ceramic cores for gas turbine blades according to the present invention has the same process flow, technical principle, and beneficial effects as Embodiment 1, except that: In step one, the reference shrinkage rate along the length extension direction is set segment by segment according to the length of the ceramic core. In this embodiment, the length of the ceramic core is 600mm, and the reference shrinkage rate is 1.7%. The reference shrinkage rate along the cross-sectional thickness direction is set segment by segment according to the thickness of the ceramic core. In this embodiment, the thickness of the ceramic core is 15mm, and the reference shrinkage rate is 2.3%.

[0058] In the tenon area, blade area, and blade tip area: the final shrinkage rate of a straight channel is equal to the final shrinkage rate of the area; the final shrinkage rate at the corner of a curved channel is equal to the final shrinkage rate of the area plus 0.1%; the final shrinkage rate of a large cross-section channel is equal to 1.1 times the final shrinkage rate of the area.

[0059] In step two, when the length of the internal channel of the ceramic core is greater than or equal to 80mm, a support rib needs to be installed inside the straight hole channel. The horizontal distance between two adjacent support ribs is 40mm. The length of the support rib is equal to the hole diameter of the channel, the width is 5mm, and the thickness is 3mm.

[0060] Triangular support ribs are installed at the corners of the curved passage, with each of the two right-angled sides of the rib fitting against the passage wall for 15mm, and the rib thickness is 3mm; cylindrical support ribs with a diameter of 2mm are installed in the cover plate area; the cross-sectional area of ​​the inner cavity is not less than 50cm². 2 The large cross-section channel is equipped with cylindrical support ribs with a diameter of 20mm.

[0061] The spiral groove interlocking structure consists of three parallel spiral grooves on the outer surface of the cylindrical support rib. The grooves have an upper opening width of 4 mm, a lower opening width of 3 mm, and a depth of 1.5 mm. The spacing between two adjacent spiral grooves is 1 mm. For the cylindrical alumina support rib, the surface roughness after sandblasting is 3.2 μm.

[0062] In step three, the main positioning point adopts a conical embedded positioning structure or a frustum-shaped positioning structure; when the conical embedded positioning structure is a conical positioning hole or a conical positioning groove, its taper is 5° and the hole diameter or groove width is 5mm; the small end diameter of the frustum-shaped positioning structure is 5mm, the height is 3mm, and the taper is 5°. The auxiliary positioning point adopts a hemispherical positioning structure with a diameter of 2mm.

[0063] The thermal deformation compensation coefficient at the contact surface between the main positioning point and the auxiliary positioning point and the forming mold is set to 1.05. The gap between the main positioning point and the forming mold is 0.05 mm, and the gap between the auxiliary positioning point and the forming mold is 0.1 mm.

[0064] In step four, the inspection items include dimensional inspection, defect inspection, and strength inspection. The inspection covers all structural areas of the ceramic core, including the ceramic core body, internal channel area, area under the cover plate, positioning point area, and support rib area.

[0065] Example 3:

[0066] Another preferred embodiment of the method for improving the quality of ceramic cores for gas turbine blades according to the present invention has the same process flow, technical principle, and beneficial effects as Embodiment 1, except that: In step one, the reference shrinkage rate is set segment by segment along the length extension direction according to the ceramic core length. In this embodiment, the ceramic core length is 800mm and the reference shrinkage rate is 2.0%. The reference shrinkage rate is also set segment by segment along the cross-sectional thickness direction according to the ceramic core thickness. In this embodiment, the ceramic core thickness is 22mm and the reference shrinkage rate is 2.5%.

[0067] In the tenon area, blade area, and blade tip area: the final shrinkage rate of a straight channel is equal to the final shrinkage rate of the area; the final shrinkage rate at the corner of a curved channel is equal to the final shrinkage rate of the area plus 0.2%; the final shrinkage rate of a large cross-section channel is equal to 1.1 times the final shrinkage rate of the area.

[0068] In step two, when the length of the internal channel of the ceramic core is greater than or equal to 80mm, a support rib needs to be installed inside the straight hole channel. The horizontal distance between two adjacent support ribs is 60mm. The length of the support rib is equal to the hole diameter of the channel, the width is 8mm, and the thickness is 5mm.

[0069] Triangular support ribs are installed at the corners of the curved passage, with each of the two right-angled sides of the rib fitting against the passage wall for 15mm, and the rib thickness is 5mm; cylindrical support ribs with a diameter of 3mm are installed in the cover plate area; the cross-sectional area of ​​the inner cavity is not less than 50cm². 2 The large cross-section channel is equipped with cylindrical support ribs with a diameter of 30mm.

[0070] The spiral groove interlocking structure consists of three parallel spiral grooves on the outer surface of the cylindrical support rib. The grooves have an upper opening width of 5 mm, a lower opening width of 4 mm, and a depth of 2 mm, with a spacing of 3 mm between adjacent spiral grooves. The surface roughness of the cylindrical alumina support rib after sandblasting is 6.3 μm.

[0071] In step three, the main positioning point adopts a conical embedded positioning structure or a frustum-shaped positioning structure; when the conical embedded positioning structure is a conical positioning hole or a conical positioning groove, its taper is 10° and the hole diameter or groove width is 10mm; the small end diameter of the frustum-shaped positioning structure is 15mm, the height is 6mm, and the taper is 10°. The auxiliary positioning point adopts a hemispherical positioning structure with a diameter of 8mm.

[0072] The thermal deformation compensation coefficient at the contact surface between the main positioning point and the auxiliary positioning point and the forming mold is set to 1.1. The gap between the main positioning point and the forming mold is 0.1 mm, and the gap between the auxiliary positioning point and the forming mold is 0.3 mm.

[0073] In step four, the inspection items include dimensional inspection, defect inspection, and strength inspection. The inspection covers all structural areas of the ceramic core, including the ceramic core body, internal channel area, area under the cover plate, positioning point area, and support rib area.

[0074] The overall performance of the ceramic cores prepared in the above embodiments was tested, and the molding accuracy, internal integrity, and mechanical properties of the ceramic cores were determined based on the test results to meet the preset usage requirements. The main testing equipment included a laser tracker (for measuring dimensions), a 3D optical scanner (for measuring dimensions), an X-ray flaw detector (for detecting internal defects), and an industrial CT scanner (for detecting internal defects). The overall performance test data of the ceramic cores prepared in Example 1 are shown in Tables 1-5.

[0075]

[0076]

[0077]

[0078]

[0079]

[0080] As shown in Tables 1-5, the overall performance test results of the ceramic core prepared by the technical solution of Example 1 meet the preset usage requirements. Furthermore, the internal macroscopic morphology of the ceramic core prepared in Example 1 is as follows: Figure 1 As shown, the internal macroscopic morphology of the ceramic core prepared using traditional processes is as follows. Figure 2 As shown in the comparison, it can be seen that the ceramic core prepared in Example 1 has no internal defects, while the ceramic core prepared by the traditional process has internal defects.

[0081] Special Note: The technical solution of this invention involves numerous parameters, and the synergistic effects between these parameters must be comprehensively considered to achieve the beneficial effects and significant progress of this invention. Furthermore, the value ranges of each parameter in the technical solution were obtained through extensive experimentation. For each parameter and the combinations thereof, the inventors have recorded a large amount of experimental data; however, due to space limitations, the specific experimental data is not disclosed here.

[0082] It will be readily understood by those skilled in the art that this invention includes any combination of the inventive description and specific embodiments outlined in the foregoing specification, as well as the various parts shown in the accompanying drawings. Due to space limitations and for the sake of brevity, not all of these combinations have been described in detail. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A method for improving the quality of ceramic cores for gas turbine blades, characterized in that, The lifting method includes the following steps: Step 1: Based on the length and thickness dimensions of the ceramic core, set the reference shrinkage rate along the length extension direction and the reference shrinkage rate along the thickness direction of the cross section, respectively; divide the ceramic core into several shrinkage compensation sections along the length direction, and adjust the shrinkage rate of each shrinkage compensation section in the thickness direction according to the differences in the geometric configuration and wall thickness distribution of each shrinkage compensation section, so that each shrinkage compensation section has an independent thickness shrinkage rate parameter, thereby achieving segmented and precise control of dimensional shrinkage behavior during the sintering of the ceramic core and the casting of the blade; Step 2: Based on the length of the internal channel of the ceramic core, arrange several support ribs in the straight hole channel along the direction perpendicular to the straight hole channel. At the same time, arrange several support ribs in the cover plate area, the corner area of ​​the curved channel, and the large cross-section channel. Remove all support ribs after the ceramic core has completed the sintering process. Step 3: Set the main positioning point and the auxiliary positioning point on the ceramic core, and set the thermal deformation compensation coefficient at the contact surface between the main positioning point and the auxiliary positioning point and the forming mold, so that the actual position of the main positioning point and the auxiliary positioning point after the ceramic core is sintered and the blade is cast matches the design position. Step 4: Prepare the ceramic core using hot press injection molding process, and test the overall performance of the ceramic core. Based on the test results, determine whether the molding accuracy, internal integrity and mechanical properties of the ceramic core meet the preset usage requirements.

2. The method for improving the quality of ceramic cores for gas turbine blades according to claim 1, characterized in that, In step one, the reference shrinkage rate is set segment by segment along the length extension direction according to the ceramic core length: 1.2-1.5% for ceramic core lengths of 300-500mm; 1.5-1.8% for ceramic core lengths of 500-700mm; and 1.8-2.2% for ceramic core lengths of 700-900mm. The reference shrinkage rate along the thickness direction of the cross section is set according to the thickness of the ceramic core: 2.0-2.2% for ceramic core thickness of 3-12mm; 2.2-2.4% for ceramic core thickness of 12-18mm; and 2.4-2.6% for ceramic core thickness of 18-25mm.

3. The method for improving the quality of ceramic cores for gas turbine blades according to claim 2, characterized in that, In step one, the shrinkage compensation section divided along the length of the ceramic core includes a tenon area, a blade area, a blade tip area, and an internal channel; the tenon area has a larger wall thickness, the blade area has a more uniform wall thickness, the blade tip area has a thinner wall thickness, and the internal channel includes a straight hole channel, a curved channel, and a large cross-section channel.

4. The method for improving the quality of ceramic cores for gas turbine blades according to claim 3, characterized in that, In step one, the final shrinkage rate of each shrinkage compensation section in the thickness direction is adjusted as follows: the final shrinkage rate of the tenon area is equal to the reference shrinkage rate of the ceramic core along the cross-sectional thickness direction plus 0.2%, to compensate for insufficient shrinkage caused by the large structure in this area, and to ensure that it matches the design dimensions after shrinkage; the final shrinkage rate of the blade area is equal to the reference shrinkage rate of the ceramic core along the cross-sectional thickness direction, to maintain the dimensional stability and straightness of this area; The final shrinkage rate of the blade tip region is equal to the reference shrinkage rate of the ceramic core along the thickness direction of the cross section minus 0.1%, in order to avoid dimensional deviations in this thin-walled region due to overcompensation; In the tenon area, blade area, and blade tip area, the final shrinkage rate of each type of channel in the thickness direction is adjusted as follows: the final shrinkage rate of a straight channel is equal to the final shrinkage rate of its area; the final shrinkage rate at the corner of a curved channel is equal to the final shrinkage rate of its area plus 0.1-0.2%. The final shrinkage rate of a large cross-section channel is equal to 1.1 times the final yield of the region.

5. The method for improving the quality of ceramic cores for gas turbine blades according to claim 4, characterized in that, In step two, when the length of the internal channel of the ceramic core is greater than or equal to 80mm, a support rib needs to be installed inside the straight hole channel. The horizontal distance between two adjacent support ribs is 40-60mm. The support rib is in the shape of a cuboid, with a length equal to the hole diameter of the channel, a width of 5-8mm, and a thickness of 3-5mm. Its material is the same as that of the ceramic core. Triangular support ribs are installed at the corners of the curved passage. The two right-angled sides of each rib have a contact length with the passage wall of at least 15mm, and the ribs are 3-5mm thick, made of alumina-based ceramic material. Cylindrical support ribs are installed in the cover plate area. These ribs have a diameter of 2-3mm and are also made of alumina-based ceramic material. The cross-sectional area of ​​the inner cavity is not less than 50cm². 2 The large cross-section channel is equipped with cylindrical support ribs with a diameter of 20-30mm, and the material is alumina-based ceramic material.

6. The method for improving the quality of ceramic cores for gas turbine blades according to claim 5, characterized in that, In step two, the alumina support rib can also be designed as a spiral groove interlocking structure or an end conical positioning interlocking structure. The spiral groove interlocking structure consists of at least three parallel spiral grooves on the outer surface of the cylindrical support rib. The upper opening width of the groove is 4-5mm, the lower opening width is 3-4mm, and the depth is 1.5-2mm. The spacing between two adjacent spiral grooves is 1-3mm. The end conical positioning interlocking structure consists of a conical positioning section at each end of the cylindrical support rib. The conical positioning section is embedded inside the ceramic core. Its bottom diameter is equal to the diameter of the cylindrical support rib, and its axial height is greater than or equal to 3mm.

7. The method for improving the quality of ceramic cores for gas turbine blades according to claim 6, characterized in that, In step two, the cylindrical alumina support ribs need to be roughened by sandblasting. The surface roughness after sandblasting is 3.2-6.3μm to enhance the interfacial bonding strength between the ribs and the ceramic slurry.

8. The method for improving the quality of ceramic cores for gas turbine blades according to claim 7, characterized in that, In step three, the main positioning point is set in the tenon area and blade tip area of ​​the ceramic core, and the auxiliary positioning point is set in the middle area of ​​the blade body of the ceramic core; the main positioning point adopts a conical embedded positioning structure or a frustum-shaped positioning structure; when the conical embedded positioning structure is a conical positioning hole or a conical positioning groove, its taper is 5-10° and the hole diameter or groove width is 5-10mm; the small end diameter of the frustum-shaped positioning structure is 5-15mm, the height is 3-6mm, and the taper is 5-10°; the auxiliary positioning point adopts a hemispherical positioning structure with a diameter of 2-8mm.

9. The method for improving the quality of ceramic cores for gas turbine blades according to claim 8, characterized in that, In step three, the thermal deformation compensation coefficients at the contact surfaces of the main positioning point and the auxiliary positioning point with the forming mold are both set to 1.05-1.1, meaning that the final shrinkage rate of the main positioning point and the auxiliary positioning point is equal to 1.05-1.1 times the final shrinkage rate along the thickness direction of their respective shrinkage compensation sections. The roots of the main positioning point and the auxiliary positioning point are provided with rounded corners for smooth transition, with a rounded corner radius greater than or equal to 1.5 mm and a surface roughness less than or equal to 1.6 μm. The gap between the main positioning point and the forming mold is 0.05-0.1 mm, and the gap between the auxiliary positioning point and the forming mold is 0.1-0.3 mm.

10. The method for improving the quality of ceramic cores for gas turbine blades according to claim 9, characterized in that, In step four, the inspection items include dimensional inspection, defect inspection, and strength inspection. The inspection covers all structural areas of the ceramic core, including the ceramic core body, internal channel area, area under the cover plate, positioning point area, and support rib area.