A continuous casting protective mold flux and a method for producing the same

By employing differentiated pretreatment and synergistic batching mechanisms, the free carbon in the carbon-containing waste electrolyte from CO2 circulating alumina electrolysis reacts with magnesium slag to form a gray silicate calcium stone mineral phase. This solves the problems of performance instability and component loss of fluorine-containing solid waste from aluminum electrolysis and magnesium slag in the preparation of continuous casting protective slag, achieving stable performance and environmentally friendly utilization in the continuous casting process of low-carbon steel.

CN123102945APending Publication Date: 2026-11-17XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611396426.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing continuous casting protective slag using fluorine-containing solid waste from aluminum electrolysis and magnesium slag have difficulty in stably controlling key properties such as melting temperature, viscosity, and alkalinity, and also suffer from problems such as loss of effective components and increased load on fluorine-containing wastewater treatment.

Method used

By using differentiated pretreatment and synergistic batching mechanisms, free carbon in carbon-containing waste electrolyte is electrolyzed using CO2 circulating alumina and reacted with magnesium slag to form a gray silica-calcium mineral phase, thus preparing a low-free-carbon fluorine-containing composite base material. This base material is then combined with conventional conditioning materials to prepare a low-carbon steel continuous casting protective slag.

Benefits of technology

It achieves stable and controllable melting temperature, viscosity and alkalinity of protective slag, reduces the loss of effective components, lowers the treatment load of fluoride-containing wastewater, and is suitable for continuous casting processes of low carbon steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of comprehensive utilization in iron and steel smelting, and particularly to a method for preparing continuous casting protective slag. The method involves mixing aluminum electrolysis waste electrolyte containing carbonaceous components and fluorinated electrolyte components such as NaF and cryolite with magnesium slag. First, under controlled oxygen conditions, some free carbon is oxidized to generate CO2. Then, under a CO2-enriched atmosphere, the CO2 reacts with Ca2SiO4 and CaO in the magnesium slag to pre-form a Ca5(SiO4)2CO3 gray silica-calcium stone crystal phase before the final batching of the protective slag. The resulting composite base material retains fluorinated electrolyte components and an appropriate amount of residual free carbon. After composition correction, slurry preparation, spray granulation, and drying, a low-carbon steel continuous casting protective slag is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of comprehensive utilization of iron and steel smelting, and specifically relates to a continuous casting protective slag and its preparation method. The method involves reacting carbonaceous components and fluorine-containing electrolyte components from aluminum electrolysis carbon-containing waste electrolyte with components from magnesium slag to prepare a protective slag for low-carbon steel continuous casting crystallizers. Background Technology

[0002] The protective slag applied to the surface of molten steel in the mold serves several functions, including isolating the molten steel from air to prevent secondary oxidation, adsorbing inclusions in the steel, forming a slag layer through melting, and providing lubrication and heat transfer regulation to the gap between the billet and the mold. The melting behavior, high-temperature viscosity, and slag film formation ability of the protective slag depend on the compatibility of the basic oxides, alkali metal components, boron-based components, fluorine-containing components, and carbonaceous components in the system.

[0003] Chinese invention patent CN101468386B discloses a continuous casting protective slag and its preparation method, which is composed of calcium-containing compounds, aluminum-containing compounds, and additives containing sodium, magnesium, barium, and carbon. Its performance is improved by controlling the melting point and viscosity at 1300℃, meeting the continuous casting needs of specific steel grades. This scheme is based on conventional commercial raw materials such as lime, bauxite, carbonates, magnesia, and carbonaceous materials, and does not involve the synergistic resource utilization of fluorine-containing solid waste from aluminum electrolysis and magnesium slag. Chinese invention patent CN110040687B discloses a waste cathode carbon block treatment system and its treatment method, which recovers sodium fluoride and obtains carbonaceous materials through crushing, alkali treatment, screening, and acid treatment. This scheme focuses on the harmless disposal and component separation of waste cathode carbon blocks, with the obtained fluoride salts and carbonaceous products mainly used as independent recycling products. It does not conduct synergistic batching design around key indicators such as melting temperature, viscosity, alkalinity, and melting rate of the continuous casting protective slag.

[0004] The salt-enriched waste electrolyte, waste tank lining, and waste cathode carbon blocks generated during aluminum electrolysis production contain usable fluorine-containing components such as NaF, cryolite, and fluoroaluminates. Magnesium slag contains CaO, MgO, SiO2, and a small amount of Al2O3. These components provide a potential basis for the synergistic preparation of continuous casting protective slag. However, the fluorine occurrence forms and contents of fluorine-containing wastes from different sources vary significantly. Using a uniform process can easily lead to the loss of effective fluoride salts and increase the load on fluorine-containing wastewater treatment. Furthermore, directly mixing untreated fluorine-containing waste with magnesium slag, whose composition fluctuates greatly, for protective slag production makes it difficult to stably control key properties such as melting temperature, viscosity, and basicity of the finished product. Summary of the Invention

[0005] To address the compositional characteristics of fluorine-containing solid waste from aluminum electrolysis and magnesium slag, a differentiated pretreatment and synergistic batching mechanism is established. This mechanism ensures the stable and controllable performance of key properties of continuous casting protective slag, such as melting temperature, high-temperature viscosity, basicity, and melting rate, while achieving high-value utilization of solid waste. The invention provides a continuous casting protective slag and its preparation method. By implementing controlled oxidation of some free carbon and CO2 recycling before final batching of the protective slag, excess free carbon in the carbon-containing waste electrolyte from aluminum electrolysis is appropriately reduced. Furthermore, some of the generated CO2 further participates in the Ca-Si mineral phase reconstruction of magnesium slag, while retaining the F-Na-Al components and a suitable amount of residual free carbon in the waste electrolyte, thus obtaining a low-free-carbon fluorine-containing composite base material.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing continuous casting protective slag, comprising the following steps: (1) Select aluminum electrolysis carbon-containing waste electrolyte that contains both carbonaceous components and fluorine-containing electrolyte components, and perform impurity removal, crushing, drying and homogenization treatment on it; (2) The magnesium slag is crushed, iron removed, dried and homogenized; (3) The aluminum electrolysis carbon-containing waste electrolyte is mixed with the magnesium slag and subjected to a first-stage carbon conversion treatment under oxygen-containing conditions, so that some of the free carbon in the aluminum electrolysis carbon-containing waste electrolyte is oxidized to generate CO2; (4) The CO2-containing gas generated in step (3) is introduced into the second-stage mineral phase control zone. Under the CO2 atmosphere, the CO2 reacts with CaO and SiO2 in the magnesium slag to form a gray silicate calcium stone crystal phase containing Ca5(SiO4)2CO3, thereby obtaining a low-free carbon fluorine-containing composite base material. The first-stage carbon conversion treatment temperature is 500-750 ℃, the O2 volume fraction in the reaction atmosphere is 5%-15%, and the treatment time is 10-60 min. The second-stage mineral phase control temperature is 730-900 ℃, the CO2 volume fraction is 20%-100%, and the heat preservation time is 20-120 min. (5) Based on the actual content of CaO, SiO2, MgO, Al2O3, F, Na and residual free carbon in the low free carbon fluorine composite base material, add protective slag component adjustment material, and mix, slurry, granulate and dry to obtain low carbon steel continuous casting protective slag.

[0007] In a preferred embodiment of the present invention, the aluminum electrolysis carbon-containing waste electrolyte in step (1) is one or more of aluminum electrolysis anode carbon slag, carbon-containing electrolyte cleaning material, carbon-containing crust material and carbon-containing electrolyte screened material, wherein the carbon content of the aluminum electrolysis carbon-containing waste electrolyte is 5% to 35% by mass and the F content is 10% to 45% by mass.

[0008] In a preferred embodiment of the present invention, the fluorinated electrolyte component in step (1) includes one or more of NaF, cryolite, and fluoroaluminate.

[0009] In a preferred embodiment of the present invention, the magnesium slag in step (2) contains 50% to 65% CaO, 25% to 38% SiO2, and 3% to 10% MgO.

[0010] In a preferred embodiment of the present invention, the mass ratio of magnesium slag to carbon-containing waste electrolyte from aluminum electrolysis in step (3) is 75:25 to 90:10.

[0011] In a preferred embodiment of the present invention, the residual free carbon content in the low free carbon fluorinated composite matrix obtained in step (4) is 0.5% to 3.0%.

[0012] In a preferred embodiment of the present invention, the protective slag composition conditioning material in step (5) includes one or more of the following: siliceous conditioning material, aluminous conditioning material, alkali metal melting conditioning material, boron-based melting conditioning material, and binder.

[0013] In a preferred embodiment of the present invention, in step (5), the silica modifier is one or more of quartz powder, silica micro powder and waste glass powder, the alumina modifier is one or more of alumina, bauxite and kaolin, the alkali metal melting modifier is one or more of sodium carbonate, potassium carbonate and lithium carbonate, and the boron-based melting modifier is one or more of borax, boric acid and B2O3.

[0014] The low-carbon steel continuous casting protective slag prepared by this invention has a CaO / SiO2 mass ratio of 0.9~1.20, an F mass content of 3%~8%, a free carbon mass content of 0.5%~1.5%, a melting temperature of 1050~1160 ℃, a viscosity of 0.20~0.40 Pa·s at 1300 ℃, and a melting time of 20~40 s.

[0015] The advantages of this invention compared to existing technologies are as follows: (1) Instead of completely separating the carbon-containing waste electrolyte from aluminum electrolysis, the carbon components and fluorine-containing electrolyte components such as NaF and cryolite are introduced into the reaction system as a whole, reducing the process increase and loss of effective components caused by flotation decarbonization, large amount of water washing and separate recovery of fluoride salts.

[0016] (2) Controlled oxidation is used to reduce the excess free carbon in the waste electrolyte, so that the free carbon content in the final protective slag is more suitable for continuous casting of low carbon steel, while retaining some residual free carbon to continue to play the role of isolating the powder slag layer, inhibiting sintering and regulating the melting rate.

[0017] (3) The CO2 generated in the first stage is not simply emitted as exhaust gas, but is at least partially recycled for the Ca-Si-CO2 mineral phase reaction in the second stage, so that the Ca2SiO4 and CaO in the magnesium slag are pre-converted into anhydrous Ca5(SiO4)2CO3 gray calcium silicate before the final protective slag is added, so as to realize the joint utilization of the reaction between carbon-containing waste electrolyte and magnesium slag. Detailed Implementation

[0018] In the technical solution described in this invention, unless otherwise specified, the proportions of each raw material are by mass; the equipment, mixing method, molding equipment, heating equipment, and phase and performance testing equipment can be conventional equipment capable of achieving the same technical purpose; and the "%" in this invention refers to mass percentages unless otherwise specified.

[0019] This invention provides a method for preparing continuous casting protective slag, comprising the following steps: (1) Select aluminum electrolysis carbon-containing waste electrolyte that contains both carbonaceous components and fluorine-containing electrolyte components, and perform impurity removal, crushing, drying and homogenization treatment on it; (2) The magnesium slag is crushed, iron removed, dried and homogenized; (3) The aluminum electrolysis carbon-containing waste electrolyte is mixed with the magnesium slag and subjected to a first-stage carbon conversion treatment under oxygen-containing conditions, so that some of the free carbon in the aluminum electrolysis carbon-containing waste electrolyte is oxidized to generate CO2; (4) The CO2-containing gas generated in step (3) is introduced into the second-stage mineral phase control zone. Under the CO2 atmosphere, the CO2 reacts with CaO and SiO2 in the magnesium slag to form a gray silicate calcium stone crystal phase containing Ca5(SiO4)2CO3, thereby obtaining a low-free carbon fluorine-containing composite base material. The first-stage carbon conversion treatment temperature is 500-750 ℃, the O2 volume fraction in the reaction atmosphere is 5%-15%, and the treatment time is 10-60 min. The second-stage mineral phase control temperature is 730-900 ℃, the CO2 volume fraction is 20%-100%, and the heat preservation time is 20-120 min. (5) Based on the actual content of CaO, SiO2, MgO, Al2O3, F, Na and residual free carbon in the low free carbon fluorine composite base material, add protective slag component adjustment material, and mix, slurry, granulate and dry to obtain low carbon steel continuous casting protective slag.

[0020] The preferred carbon-containing waste electrolyte for aluminum electrolysis is aluminum electrolysis anode carbon slag. Before the raw materials enter the reaction system, obvious metallic aluminum, iron foreign matter, and other large inclusions are removed, and the materials are crushed to a particle size of no more than 1 mm. They are then dried at 100–150 °C until the moisture content is no more than 1.0%, and subsequently homogenized. The pretreatment does not employ flotation aimed at removing graphite carbon, nor does it use large-volume water washing to dissolve NaF and cryolite, in order to maintain the integrity of the CF-Na-Al composition.

[0021] The magnesium slag is preferably the reduction slag from the silicothermic magnesium smelting process. The magnesium slag is first crushed and magnetically separated to remove iron, then dried and ground to a particle size of no more than 3 mm. XRF is preferably used to detect the contents of CaO, SiO2, MgO, and Al2O3, and XRD is used to analyze the mineral phases such as Ca2SiO4, Ca3MgSi2O8, Ca2MgSi2O7, and free CaO. The amount of carbon-containing waste electrolyte to be added for aluminum electrolysis is determined based on the measured composition.

[0022] The first stage of carbon conversion treatment can be carried out in a rotary kiln, fluidized bed, belt roasting device, or other reaction apparatus with atmosphere conditioning and continuous exhaust functions. Preferably, the mixture is heated to 550–680 °C, and an oxygen-containing gas prepared from air, circulating flue gas, and / or inert gas is introduced to control the O2 volume fraction at 6%–12%. The degree of partial oxidation is determined by online measurement of the CO and CO2 concentrations in the exhaust gas, the free carbon content before and after treatment, or the weight loss rate.

[0023] After high-temperature dust removal, the exhaust gas from the first stage enters a gas buffer and circulation system, with at least a portion of the CO2-containing gas being transported to the second-stage mineral phase control zone. The second stage can be located in a different temperature zone within the same rotary reactor as the first stage, or two reactors can be used in series. Preferably, the material temperature in the second stage is controlled at 780–880 °C, the CO2 volume fraction is controlled at 30%–80%, and the O2 volume fraction is not higher than 3%, to reduce further oxidation of residual free carbon.

[0024] In the second stage, Ca2SiO4, CaO, and CO2 react to form Ca5(SiO4)2CO3. This reaction can be represented as: 2Ca2SiO4 + CaO + CO2 → Ca5(SiO4)2CO3. Since NaF, cryolite, and fluoroaluminates from the carbon-containing waste electrolyte of aluminum electrolysis enter the second stage along with the solid phase, the fluorine-containing components can act as mineralizing components, reducing the resistance to the Ca-Si solid-phase reaction and promoting the formation of siliceous calcium silicate. After the second stage, a low-oxygen atmosphere is used for cooling to prevent further oxidation of the remaining free carbon.

[0025] The mineralogical name of Ca5(SiO4)2CO3 described in this invention is gray silicate calcium silicate. It differs from the fluorine-containing gunmetallic Ca4Si2O7F2 commonly found in continuous casting protective slag. The key point of this invention is that, before the final batching of the protective slag, gray silicate calcium silicate is pre-formed using CO2 generated from carbon-containing waste electrolyte and the Ca-Si components in the magnesium slag, rather than relying on the protective slag to form fluorine-containing gunmetallic crystals during the crystallization process.

[0026] The content of gray silicate in the composite matrix is ​​preferably quantified using X-ray diffraction combined with Rietveld full-spectrum fitting; the free carbon content is determined using combustion-infrared spectroscopy or equivalent methods; the fluorine (F) content can be determined using ion-selective electrode method, ion chromatography, or other analytical methods suitable for fluorine-containing solid samples. The F retention rate is calculated as the ratio of the actual F retention in the composite matrix after two-stage treatment to the total F entering the treatment system.

[0027] The final protective slag is prepared by wet pulping and spray granulation after batching. The preferred particle size for spray granulation is 0.10–1.20 mm, and the moisture content of the finished product is not higher than 0.5%. The melting temperature of the protective slag is determined by the hemispherical point method or equivalent method, the viscosity at 1300 °C is determined by the rotational viscosity method, and the melting time is determined by conventional melting characteristic testing methods.

[0028] To evaluate the suitability of this invention for low-carbon steel, a simulated slag-steel contact test was conducted at 1550 °C for 20 min with the protective slag and low-carbon steel with an initial C content of 0.04%–0.08%, and the change in C content of the steel samples before and after the test was compared. The following examples use this method to evaluate the carbon-increasing tendency of the protective slag.

[0029] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0030] Example 1

[0031] Carbon slag from aluminum electrolysis anodes was selected as the carbon-containing waste electrolyte. After removing metallic impurities, crushing, drying at 120 °C for 2 h, and homogenizing, it was used. Its main components were: C 18.6 wt%, F 30.8 wt%, Na 17.4 wt%, Al 12.5 wt%, Ca 2.1 wt%, Si 1.4 wt%, with the remainder being O and unavoidable trace impurities. Magnesium slag was also used, with the main chemical composition being: CaO 58.71 wt%, SiO2 32.61 wt%, MgO 4.75 wt%, Fe2O3 2.91 wt%, Al2O3 0.82 wt%. This slag was crushed, subjected to 0.8 T magnetic separation for iron removal, dried, and ground before use.

[0032] 82 wt% magnesium slag-based material was mixed with 18 wt% carbon-containing waste electrolyte from aluminum electrolysis. The mixture was heated to 620℃ and held for 30 min in a circulating atmosphere with an O2 volume fraction of 10% for the first stage of carbon conversion treatment. The resulting CO2-containing tail gas was refrigerated and then recycled into the second stage reaction zone after dust removal. Subsequently, the material was heated to 830℃, and the CO2 volume fraction was controlled at 50% and the O2 volume fraction was below 3% for the second stage, and held for 60 min for mineral phase regulation. After the reaction, it was cooled to below 300℃ in a low-oxygen atmosphere to obtain a low-free-carbon fluorine-containing composite material. X-ray diffraction and Rietveld full-spectrum fitting analysis showed that the Ca5(SiO4)2CO3 gray silicate calcium silicate content in the obtained composite material was 5.2 wt%, while retaining crystalline phases such as Ca2SiO4, Ca3MgSi2O8, and Ca2MgSi2O7; the residual free carbon content of the composite material was 0.55 wt%, and the F retention rate was 86.0%. Based on the total mass of the dry raw materials for the protective slag, weigh out the following: 75 wt% of the above composite base material, 10 wt% of waste glass powder, 5 wt% of quartz powder, 3 wt% of alumina powder, 3 wt% of sodium carbonate, 3 wt% of borax, and 1 wt% of binder. The waste glass powder used contains approximately 70 wt% SiO2, approximately 14 wt% Na2O, and approximately 10 wt% CaO. Mix the raw materials, prepare a slurry, spray granulate, dry, and sieve to obtain a low-carbon steel continuous casting protective slag.

[0033] The resulting protective slag had a CaO / SiO2 mass ratio of 1.16, an F content of 3.6 wt%, and a free carbon content of 0.51 wt%. The melting temperature was 1112 ℃, the viscosity at 1300 ℃ was 0.29 Pa·s, and the melting time was 28 s. After a 20-minute slag-steel contact test at 1550 ℃ with low-carbon steel having an initial C content of approximately 0.06 wt%, the C content of the steel sample increased by 0.004 wt%.

[0034] Example 2

[0035] The carbon slag from aluminum electrolysis anodes was selected, and after impurity removal, crushing, drying at 120 ℃ for 2 h, and homogenization, its main components were: C 20.1 wt%, F 29.6 wt%, Na 17.9 wt%, Al 11.8 wt%, Ca 1.8 wt%, Si 1.6 wt%, with the remainder being O and unavoidable impurities. The magnesium slag used had the following main chemical composition: CaO 60.12 wt%, SiO2 30.86 wt%, MgO 5.36 wt%, Fe2O3 2.54 wt%, Al2O3 1.12 wt%, and was used after crushing, magnetic separation to remove iron, drying, and grinding.

[0036] 80 wt% magnesium slag base material was mixed with 20 wt% carbon-containing waste electrolyte from aluminum electrolysis. The first stage was held at 650 ℃ for 40 min with an O2 volume fraction of 12%. The CO2-containing gas generated in the first stage was precipitated and then introduced into the second stage reaction zone. The second stage temperature was 850 ℃ with a CO2 volume fraction of 60% for 60 min. After treatment, the mixture was cooled in a low-oxygen atmosphere. XRD-Rietveld analysis of the resulting composite base material showed a Ca5(SiO4)2CO3 gray silicate content of 6.6 wt%, a residual free carbon content of 0.85 wt%, and an F retention rate of 82.5%. Based on the total dry mass of the protective slag raw materials, a low-carbon steel continuous casting protective slag was obtained by mixing the above composite base material (72 wt%), waste glass powder (12 wt%), quartz powder (5 wt%), alumina powder (3 wt%), sodium carbonate (3 wt%), borax (3 wt%), and binder (2 wt%), followed by pulping, spray granulation, drying, and sieving.

[0037] The resulting protective slag had a CaO / SiO2 mass ratio of 1.12, an F content of 3.5 wt%, and a free carbon content of 0.67 wt%. The melting temperature was 1098 ℃, the viscosity at 1300 ℃ was 0.27 Pa·s, and the melting time was 26 s. After contact testing with the same slag, the carbon content of the steel sample increased by 0.003 wt%.

[0038] Example 3

[0039] Carbon-containing waste electrolyte from aluminum electrolysis was selected. After impurity removal, crushing, drying, and homogenization, its main components were: C 17.2 wt%, F 33.4 wt%, Na 16.8 wt%, Al 12.3 wt%, Ca 2.4 wt%, Si 1.3 wt%, with the remainder being O and unavoidable impurities. The magnesium slag used had the following main chemical composition: CaO 56.92 wt%, SiO2 33.98 wt%, MgO 5.08 wt%, Fe2O3 2.76 wt%, Al2O3 1.26 wt%. It was used after crushing, magnetic separation to remove iron, drying, and grinding.

[0040] 84 wt% magnesium slag base material was mixed with 16 wt% carbon-containing waste electrolyte from aluminum electrolysis. The first stage was held at 580 ℃ for 25 min with an O2 volume fraction of 8%; the second stage was held at 800 ℃ for 90 min with a CO2 volume fraction of 40%. The CO2-containing exhaust gas from the first stage was precipitated and recycled for the second stage. After the second stage, the mixture was cooled in a low-oxygen atmosphere. XRD-Rietveld analysis of the resulting composite base material showed a Ca5(SiO4)2CO3 gray silicate content of 4.2 wt%, a residual free carbon content of 1.35 wt%, and an F retention rate of 90.0%. Based on the total dry weight of the protective slag raw materials, a protective slag was obtained by mixing the above composite base material (78 wt%), waste glass powder (8 wt%), quartz powder (5 wt%), alumina powder (2 wt%), sodium carbonate (3 wt%), borax (3 wt%), and binder (1 wt%), followed by pulping, spray granulation, drying, and sieving.

[0041] The resulting protective slag had a CaO / SiO2 mass ratio of 1.18, an F content of 3.7 wt%, and a free carbon content of 1.17 wt%. The melting temperature was 1124 ℃, the viscosity at 1300 ℃ was 0.31 Pa·s, and the melting time was 30 s. After contact testing with the same slag, the carbon content of the steel sample increased by 0.005 wt%.

[0042] Comparative Example 1 The only difference from Example 1 is that the magnesium slag base material and the carbon-containing waste electrolyte of aluminum electrolysis are not subjected to the first stage carbon conversion treatment and the second stage gray silica-calcium mineral phase regulation. Instead, the magnesium slag, carbon-containing waste electrolyte of aluminum electrolysis and other regulating raw materials are directly mixed, pulped, granulated and dried according to the same raw material ratio as in Example 1. All other conditions are the same as in Example 1.

[0043] In Comparative Example 1, no pre-formed Ca5(SiO4)2CO3 gray calcium silicate was detected in the finished product. The free carbon content was 2.51 wt%, and the F content was 4.2 wt%. The melting temperature was 1149 ℃, the viscosity at 1300 ℃ was 0.35 Pa·s, and the melting time was 39 s. After contact testing with the same slag steel, the C content of the steel sample increased by 0.016 wt%.

[0044] Comparative Example 2 The only difference from Example 1 is that only the first stage carbon conversion treatment at 620 °C, 10% O2 volume fraction, and 30 min is performed. After the first stage, the second stage CO2 mineral phase regulation at 830 °C is not performed. Instead, it is directly cooled with low oxygen and used for subsequent protective slag batching. All other conditions are the same as in Example 1.

[0045] In Comparative Example 2, no obvious Ca5(SiO4)2CO3 gray silicate was detected in the composite base material. The final protective slag had a free carbon content of 1.24 wt% and a F content of 3.8 wt%. The melting temperature was 1136 ℃, the viscosity at 1300 ℃ was 0.33 Pa·s, and the melting time was 34 s. After contact testing with the same slag, the C content of the steel sample increased by 0.008 wt%.

[0046] Comparative Example 3 The only difference from Example 1 is that the temperature for the second-stage mineral phase regulation is increased from 830 °C to 950 °C, the CO2 volume fraction remains at 50%, and the temperature is maintained for 60 min. All other conditions are the same as in Example 1.

[0047] Testing revealed that the Ca5(SiO4)2CO3 gray calcium silicate content in the composite base of Comparative Example 3 was only 0.9 wt%, and the F retention rate decreased to 67.5%. The final protective slag had an F content of 2.8 wt%, a free carbon content of 1.12 wt%, a melting temperature of 1168 ℃, a viscosity of 0.38 Pa·s at 1300 ℃, and a melting time of 36 s. After contact testing with the same slag, the C content of the steel sample increased by 0.007 wt%.

[0048] Comparative Example 4 The only difference from Example 1 is that the first stage uses an air atmosphere and is kept at 700 °C with an O2 volume fraction of about 21% for 60 min to cause excessive oxidation of the carbonaceous components in the carbon-containing waste electrolyte of aluminum electrolysis; the conditions of the second stage are the same as those of Example 1.

[0049] In Comparative Example 4, the Ca5(SiO4)2CO3 gray silicate calcium stone content in the composite matrix was 2.1 wt%, the F retention rate was 65.8%, and the final protective slag had a free carbon content of only 0.18 wt% and an F content of 2.7 wt%. The melting temperature was 1120 ℃, and the viscosity at 1300 ℃ was 0.30 Pa·s, but the melting time was shortened to 17 s, indicating a significant acceleration in the sintering and melting rate of the slag layer. After the same slag-steel contact test, the C content of the steel sample increased by 0.001 wt%.

[0050] As can be seen from Examples 1-3 and Comparative Examples 1-4, this invention does not simply remove all C from the carbon-containing waste electrolyte of aluminum electrolysis through oxidation treatment, nor does it separate fluorine-containing salts separately and use them as raw materials for protective slag. Instead, it moderately oxidizes free carbon while retaining the F-Na-Al components, and further uses at least part of the generated CO2 for the preconstruction of lime-silica-calcium stone in the Ca-Si components of magnesium slag. When the two-stage treatment is omitted, the finished product has a higher free carbon content and an increased tendency for carbon increase in slag steel; when only the first-stage oxidation is performed, although free carbon can be reduced, preconstructed lime-silica-calcium stone cannot be formed; excessively high temperatures in the second stage will lead to decreased stability of lime-silica-calcium stone and exacerbate F loss; excessively strong oxidation in the first stage will result in excessively low residual free carbon, increased F loss, and excessively rapid melting of the protective slag. Therefore, by synergistically controlling the degree of partial carbon oxidation, CO2 recycling, and lime-silica-calcium stone formation temperature, a low-carbon steel continuous casting protective slag with appropriate residual free carbon, effective fluorine-containing components, and stable melting rheological properties can be obtained.

Claims

1. A method for preparing a continuous casting protective slag, characterized in that, Includes the following steps: (1) Select aluminum electrolysis carbon-containing waste electrolyte that contains both carbonaceous components and fluorine-containing electrolyte components, and perform impurity removal, crushing, drying and homogenization treatment on it; (2) The magnesium slag is crushed, iron removed, dried and homogenized; (3) The aluminum electrolysis carbon-containing waste electrolyte is mixed with the magnesium slag and subjected to a first-stage carbon conversion treatment under oxygen-containing conditions, so that some of the free carbon in the aluminum electrolysis carbon-containing waste electrolyte is oxidized to generate CO2; (4) The CO2-containing gas generated in step (3) is introduced into the second-stage mineral phase control zone. Under the CO2 atmosphere, the CO2 reacts with CaO and SiO2 in the magnesium slag to form a gray silicate calcium stone crystal phase containing Ca5(SiO4)2CO3, thereby obtaining a low-free carbon fluorine-containing composite base material. The first-stage carbon conversion treatment temperature is 500-750 ℃, the O2 volume fraction in the reaction atmosphere is 5%-15%, and the treatment time is 10-60 min. The second-stage mineral phase control temperature is 730-900 ℃, the CO2 volume fraction is 20%-100%, and the heat preservation time is 20-120 min. (5) Based on the actual content of CaO, SiO2, MgO, Al2O3, F, Na and residual free carbon in the low free carbon fluorine composite base material, add protective slag component adjustment material, and mix, slurry, granulate and dry to obtain low carbon steel continuous casting protective slag.

2. The method for preparing a continuous casting protective slag according to claim 1, characterized in that, In step (1), the aluminum electrolysis carbon-containing waste electrolyte is one or more of the following: aluminum electrolysis anode carbon slag, carbon-containing electrolyte cleaning material, carbon-containing crust material, and carbon-containing electrolyte screened material. The carbon-containing waste electrolyte contains 5% to 35% C by mass and 10% to 45% F by mass.

3. The method for preparing a continuous casting protective slag according to claim 2, characterized in that, The fluorinated electrolyte component in step (1) includes one or more of NaF, cryolite, and fluoroaluminate.

4. The method for preparing a continuous casting protective slag according to claim 1, characterized in that, In step (2), the magnesium slag contains 50%–65% CaO, 25%–38% SiO2, and 3%–10% MgO.

5. The method for preparing a continuous casting protective slag according to claim 1, characterized in that, In step (3), the mass ratio of magnesium slag to carbon-containing waste electrolyte from aluminum electrolysis is 75:25 to 90:

10.

6. The method for preparing a continuous casting protective slag according to claim 1, characterized in that, The residual free carbon content in the low free carbon fluorinated composite matrix obtained in step (4) is 0.5% to 3.0%.

7. The method for preparing a continuous casting protective slag according to claim 1, characterized in that, The protective slag composition conditioning material in step (5) includes one or more of the following: siliceous conditioning material, aluminous conditioning material, alkali metal melting conditioning material, boron-based melting conditioning material, and binder.

8. The method for preparing a continuous casting protective slag according to claim 7, characterized in that, In step (5), the silica-based conditioning material is one or more of quartz powder, silica powder and waste glass powder; the alumina-based conditioning material is one or more of alumina, bauxite and kaolin; the alkali metal melting conditioning material is one or more of sodium carbonate, potassium carbonate and lithium carbonate; and the boron-based melting conditioning material is one or more of borax, boric acid and B2O3.

9. A low-carbon steel continuous casting protective slag prepared by a method for preparing a continuous casting protective slag according to any one of claims 1 to 8, characterized in that, The protective slag has a CaO / SiO2 mass ratio of 0.9 to 1.20, an F mass content of 3% to 8%, a free carbon mass content of 0.5% to 1.5%, a melting temperature of 1050 to 1160 ℃, a viscosity of 0.20 to 0.40 Pa·s at 1300 ℃, and a melting time of 20 to 40 s.

Citation Information

Patent Citations

  • Continuous casting mould powder and preparation method thereof

    CN101468386B

  • Waste cathode carbon block processing system and processing method

    CN110040687B