Die-casting method for magnesium alloy gearbox housing, magnesium alloy gearbox housing and vehicle

By employing vacuum die casting, mold temperature balancing technology, and local extrusion or spot cooling technology, the casting defects of magnesium alloy gearbox housings for commercial vehicles have been solved, achieving high-quality molding and lightweighting of the housing, reducing the scrap rate, and meeting the usage requirements of commercial vehicles.

CN123102958APending Publication Date: 2026-11-17FAW CASTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611204008.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing die-casting process for magnesium alloy gearbox housings in commercial vehicles is prone to casting defects such as shrinkage porosity, air holes, and cold shuts, resulting in excessive weight and increased costs.

Method used

Vacuum die casting combined with mold temperature balancing technology and local extrusion or local spot cooling technology is used to improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, thereby enhancing the internal density and appearance quality of the casting.

Benefits of technology

It effectively improves casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, enhances the internal density and appearance quality of magnesium alloy gearbox housings, meets the load-bearing, shock absorption, and long-term service requirements of commercial vehicle gearbox housings, and achieves vehicle lightweighting and reduces casting scrap rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102958A_ABST
    Figure CN123102958A_ABST
Patent Text Reader

Abstract

This application discloses a die-casting method for a magnesium alloy gearbox housing, a magnesium alloy gearbox housing, and a vehicle. The method includes: (1) placing a magnesium alloy ingot in a melting furnace and melting it under a protective atmosphere to obtain a magnesium alloy melt; (2) injecting the magnesium alloy melt into a die-casting machine cup, filling the mold cavity with the magnesium alloy melt by injection and solidifying it, and die-casting it to obtain a magnesium alloy gearbox housing blank; (3) performing post-processing on the magnesium alloy gearbox housing blank to obtain a magnesium alloy gearbox housing; wherein, the preheating temperature of the mold is 100℃~150℃, and the temperature of the mold during the die-casting process is 150℃~200℃; the mold is evacuated after the mold is closed; during the solidification of the magnesium alloy melt in the mold cavity, the thick parts of the solidified magnesium alloy blank are subjected to extrusion treatment or spot cooling treatment. This application utilizes vacuum die casting + mold temperature balancing technology + local extrusion technology or local spot cooling technology to effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, enhance the internal density and appearance quality of the magnesium alloy gearbox housing, and simultaneously achieve vehicle lightweighting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of magnesium alloy gearbox housing technology, and more specifically, to a die-casting method for a magnesium alloy gearbox housing, a magnesium alloy gearbox housing, and a vehicle. Background Technology

[0002] The rapid rise of new energy vehicles has created an increasingly urgent demand for lightweighting. Lightweighting, as a crucial pathway to low-carbon development in the automotive industry, has become a major trend. Traditional commercial vehicle transmission housings are mostly made of cast iron, resulting in significant weight. With the increasing demand for vehicle lightweighting, the application of aluminum alloy die-casting technology in commercial vehicle transmission housings is gradually increasing, but the issue of excessive weight remains. Furthermore, rising aluminum alloy prices have significantly increased the cost of aluminum alloy commercial vehicle transmission housings. Magnesium alloys, being the lightest structural metal material, possess advantages such as low density, high strength, excellent rigidity, good die-casting performance, excellent noise reduction, electromagnetic shielding and vibration damping properties, and recyclability, enabling the ultimate lightweighting of automobiles.

[0003] However, existing die-casting processes for magnesium alloy gearbox housings in commercial vehicles are prone to casting defects such as shrinkage porosity, air holes, and cold shuts. To address these issues, this invention proposes a die-casting method for magnesium alloy gearbox housings. Summary of the Invention

[0004] This application aims to at least partially address one of the technical problems in the related art. Therefore, the purpose of this application is to propose a die-casting method for a magnesium alloy gearbox housing, a magnesium alloy gearbox housing, and a vehicle. By employing vacuum die casting + mold temperature balancing technology + local extrusion technology or local spot cooling technology, this application can effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, enhance the internal density and appearance quality of the magnesium alloy gearbox housing, and simultaneously achieve vehicle lightweighting.

[0005] In a first aspect of this application, a die-casting method for a magnesium alloy gearbox housing is proposed. According to an embodiment of this application, the method includes: (1) Place the magnesium alloy ingot in a melting furnace and melt it under a protective atmosphere to obtain a magnesium alloy melt; (2) The magnesium alloy melt is injected into the die casting machine cup, and the magnesium alloy melt is filled into the mold cavity and solidified by injection, and die casting is performed to obtain a magnesium alloy gearbox housing blank. (3) The magnesium alloy gearbox housing blank is post-processed to obtain a magnesium alloy gearbox housing; The preheating temperature of the mold is 100℃~150℃, and the temperature of the mold during the die casting process is 150℃~200℃. After the mold is closed, a vacuum is drawn from the mold. During the solidification of the magnesium alloy melt in the mold cavity, the thicker parts of the solidified magnesium alloy billet are subjected to extrusion or spot cooling.

[0006] The die-casting method for magnesium alloy gearbox housings according to the above embodiments of this application, by employing vacuum die casting + mold temperature balancing technology + local extrusion technology or local spot cooling technology, can effectively improve casting defects such as shrinkage porosity, gas holes, and cold shuts during the casting process, and improve the internal density and appearance quality of the magnesium alloy gearbox housing; the mechanical properties of the housing are guaranteed, meeting the requirements of commercial vehicle gearbox housings for load bearing, shock absorption, and long-term service; the low density advantage of magnesium alloys is fully utilized to achieve vehicle lightweighting, reducing the weight by about 30% compared to aluminum alloy commercial vehicle gearbox housings, contributing to low carbon emissions and reduced energy consumption in vehicles; the die-casting process is stabilized, the casting scrap rate is reduced, production efficiency is improved, and the industrial mass production of magnesium alloy gearbox housings is facilitated.

[0007] In addition, the die-casting method for the magnesium alloy gearbox housing according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the mold uses circulating heated oil as the medium for controlling the mold preheating and mold temperature during the die casting process.

[0008] In some embodiments of this application, after the mold is closed, the mold is evacuated to make the vacuum degree in the mold cavity <100mbar.

[0009] In some embodiments of this application, during the solidification of the magnesium alloy melt in the mold cavity, when the thickness of the thick portion of the solidified magnesium alloy billet is ≥10mm, the thick portion of the magnesium alloy billet is subjected to extrusion treatment or spot cooling treatment.

[0010] In some embodiments of this application, the pressure for extruding the thicker parts of the magnesium alloy billet is 100 bar to 120 bar, and the time is 2 to 3 seconds.

[0011] In some embodiments of this application, the temperature for spot cooling of the thicker parts of the magnesium alloy billet is 15°C to 25°C.

[0012] In some embodiments of this application, before placing the magnesium alloy ingot in the melting furnace, the die casting method further includes: drying and preheating the magnesium alloy ingot; and / or, in step (3), the post-processing includes: water cooling the magnesium alloy gearbox housing blank, removing it from the gating system, and marking it.

[0013] In some embodiments of this application, during the process of filling the mold cavity with molten magnesium alloy by injection, the temperature of the punch is 40°C to 70°C; and / or, during the process of filling the mold cavity with molten magnesium alloy by injection, the low speed of the punch is 0.2 m / s to 0.8 m / s, the high speed of the punch is 4 m / s to 5 m / s, the holding time is 10 s to 15 s, the rapid energy storage is 120 bar to 160 bar, and the pressurized energy storage is 100 bar to 150 bar.

[0014] In a second aspect of this application, a magnesium alloy gearbox housing is proposed. According to an embodiment of this application, the aforementioned magnesium alloy gearbox housing is prepared using the die-casting method of the first aspect. Therefore, this application can effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, enhance the internal density and appearance quality of the magnesium alloy gearbox housing; ensure the mechanical properties of the housing, meeting the load-bearing, shock absorption, and long-term service requirements of commercial vehicle gearbox housings; fully utilize the low-density characteristics of magnesium alloys to achieve lightweighting, reducing weight by approximately 30% compared to aluminum alloy commercial vehicle gearbox housings, contributing to low carbon emissions and reduced fuel consumption in vehicles; simultaneously, it can stabilize the die-casting process, reduce casting scrap rate, improve production efficiency, and facilitate the industrial-scale mass production of magnesium alloy gearbox housings.

[0015] In a third aspect of this application, a vehicle is proposed. According to an embodiment of this application, the vehicle includes a magnesium alloy gearbox housing as described in the second aspect. It should be noted that the vehicle possesses the aforementioned advantages of the magnesium alloy gearbox housing, which will not be elaborated further here.

[0016] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0017] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic diagram of a die-casting method for a magnesium alloy gearbox housing according to some embodiments of this application; Figure 2 This is a diagram showing the X-ray flaw detection results of Example 1; Figure 3 This is a diagram of the X-ray flaw detection results for Comparative Example 1. Detailed Implementation

[0018] The embodiments of this application are described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application.

[0019] In a first aspect of this application, a die-casting method for a magnesium alloy gearbox housing is proposed. According to an embodiment of this application, refer to the appendix... Figure 1 The above method includes: S100: placing a magnesium alloy ingot in a melting furnace and melting it under a protective atmosphere to obtain a magnesium alloy melt; S200: injecting the magnesium alloy melt into a die-casting machine cup, filling the mold cavity with the magnesium alloy melt through injection and solidifying it, then die-casting it to obtain a magnesium alloy gearbox housing blank; S300: performing post-processing on the magnesium alloy gearbox housing blank to obtain a magnesium alloy gearbox housing; wherein, the preheating temperature of the mold is 100℃~150℃ (for example, it can be 100℃, 110℃, 120℃, 130℃, 1... The temperature of the mold during die casting is 150℃~200℃ (e.g., 150℃, 160℃, 170℃, 180℃, 190℃, 200℃ or any range between two), which is the mold temperature balancing technology; after the mold is closed, the mold is evacuated, which is vacuum die casting; during the solidification of the magnesium alloy melt in the mold cavity, the thick parts of the solidified magnesium alloy billet are subjected to extrusion treatment (i.e., local extrusion technology) or spot cooling treatment (i.e., local spot cooling technology).

[0020] The beneficial effects achievable by the die-casting method for the magnesium alloy gearbox housing proposed in this application will be described in detail below: This application utilizes vacuum die casting + mold temperature balancing technology + local extrusion technology or local spot cooling technology to effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, thereby enhancing the internal density and appearance quality of the magnesium alloy gearbox housing. The mechanical properties of the housing are guaranteed, meeting the requirements for load-bearing, shock absorption, and long-term service of commercial vehicle gearbox housings. It fully leverages the low density advantage of magnesium alloys to achieve vehicle lightweighting, reducing the weight of commercial vehicle gearbox housings by approximately 30% compared to aluminum alloy housings, contributing to low carbon emissions and reduced fuel consumption. The stable die casting process reduces casting scrap rates, improves production efficiency, and facilitates the industrial-scale mass production of magnesium alloy gearbox housings.

[0021] In vacuum die casting technology, after the mold is closed, a vacuum is drawn into the mold to create negative pressure. This prevents the molten magnesium from oxidizing when it encounters air in the mold, reducing the formation of oxide slag. At the same time, it also prevents air entrapment between the molten magnesium and the air in the mold during the filling process, reducing the formation of porosity in the casting. Finally, the negative pressure also helps the molten magnesium fill the mold, improving the overall filling quality. In summary, this can effectively improve the overall quality of casting.

[0022] In mold temperature balancing technology, the preheating temperature of the mold is 100℃~150℃, and the temperature of the mold during the die casting process is 150℃~200℃. The balanced mold temperature can avoid the occurrence of cold shut defects at the far end on the one hand, and effectively achieve sequential solidification on the other hand, ensuring the smooth flow of the feeding channel and effectively reducing defects such as shrinkage porosity, shrinkage cavity and cracking.

[0023] In local extrusion / local spot cooling technology, during the solidification of magnesium alloy melt in the mold cavity, the thick parts of the solidified magnesium alloy billet are extruded. Under pressure, the microstructure at the extrusion location is made denser, avoiding shrinkage porosity and effectively improving the internal quality of the casting.

[0024] Specifically, see the attached document. Figure 1 The above methods include: S100: Magnesium alloy ingots are placed in a melting furnace and melted under a protective atmosphere to obtain magnesium alloy melt; As some specific embodiments, AS41B magnesium alloy ingots can be used, which include 3.7wt%~4.8wt% Al, 0.35wt%~0.6wt% Mn, 0.10wt%~0.40wt% Zn, 0.6wt%~1.4wt% Si, and the remainder being Mg.

[0025] According to some specific embodiments of this application, before placing the magnesium alloy ingot in the melting furnace, the die-casting method further includes: placing the magnesium alloy ingot into a feeding machine for drying and preheating to remove surface moisture. As some specific embodiments, the preheating temperature of the feeding machine is 100℃~120℃.

[0026] According to some specific embodiments of this application, the preheated magnesium alloy ingot is placed in the melting chamber of a magnesium alloy melting furnace and melted under a protective atmosphere at a melting temperature of 700°C to 730°C.

[0027] S200: Magnesium alloy melt is injected into the die casting machine cup, and the magnesium alloy melt is filled into the mold cavity and solidified by injection to form a magnesium alloy gearbox housing blank. In this step, the molten magnesium alloy that has reached the required melting level is injected into the die-casting machine cup; the molten magnesium alloy is then pushed into the mold cavity by low-speed injection and high-speed injection in sequence. After filling, pressure is increased and held to compensate for the solidification shrinkage of the molten magnesium alloy; the molten magnesium alloy cools and solidifies in the mold cavity, and after reaching the process conditions, the mold is opened and the part is ejected to obtain the magnesium alloy gearbox housing blank.

[0028] In the embodiments of this application, the preheating temperature of the mold is 100℃~150℃, and the temperature of the mold during the die casting process is 150℃~200℃. Thus, the balanced mold temperature can avoid the generation of cold shut defects at the far end on the one hand, and effectively achieve sequential solidification on the other hand, ensuring the smooth flow of the feeding channel and reducing defects such as shrinkage porosity, shrinkage cavity and cracking.

[0029] In the embodiments of this application, the mold is evacuated after mold closing to ensure that the cavity vacuum degree is <100mbar. This further reduces the formation of oxide slag and the formation of porosity in the casting, thereby further improving the overall quality of casting.

[0030] In the embodiments of this application, during the solidification of the magnesium alloy melt in the mold cavity, a cooling function is achieved by external extrusion pins or by processing the core, thereby extruding or spot cooling the thick parts of the solidified magnesium alloy billet.

[0031] As some specific embodiments, the mold includes a static mold and a moving mold. Before casting, a layer of water-based release agent is evenly sprayed onto the surfaces of both the moving and static molds for 5 to 15 seconds. As some specific examples, the water-based release agent used is Derunbao or Metformo's special magnesium alloy release agent.

[0032] In some specific embodiments, a 4500-ton high-pressure die-casting machine is used, and the magnesium alloy gearbox housing mold is fixed on the mold frame of the 4500-ton high-pressure die-casting machine.

[0033] In some specific embodiments, during casting, molten magnesium alloy is drawn from below the molten metal surface in the holding furnace, transported via a feed pipe, and injected from above into the die-casting machine's feed cup, where it is then injected through a punch. The temperature of the molten alloy during casting is 680℃~700℃.

[0034] According to some specific embodiments of this application, the above-mentioned mold uses circulating heating oil as the medium to control the mold preheating and mold temperature during the die casting process. The preheating temperature of the mold is controlled to be 100℃~150℃ by the heating oil, and the mold temperature during the die casting process is 150℃~200℃. This can further ensure that the product is free from defects such as cold shuts and guarantee product quality.

[0035] According to some specific embodiments of this application, after the mold is closed, the mold is evacuated. The vacuuming is triggered by position and the vacuuming time is 0.2s to 0.3s, so that the vacuum degree in the mold cavity is <100mbar, thereby further ensuring the internal quality of the product.

[0036] According to some specific embodiments of this application, during the process of filling the mold cavity with magnesium alloy melt by injection, the temperature of the punch is 40℃~70℃, for example, it can be 40℃, 50℃, 60℃, 70℃ or any range between the two. Therefore, it can further effectively improve casting defects such as shrinkage porosity, air holes, and cold shuts during the casting process, and further improve the internal density and appearance quality of the magnesium alloy gearbox housing.

[0037] According to some specific embodiments of this application, during the process of filling the mold cavity with magnesium alloy melt by injection, the low speed of the punch is 0.2m / s to 0.8m / s (e.g., it can be 0.2m / s, 0.4m / s, 0.6m / s, 0.8m / s, or any range between the two), the high speed of the punch is 4m / s to 5m / s (e.g., it can be 4m / s, 4.2m / s, 4.4m / s, 4.6m / s, 4.8m / s, 5m / s, or any range between the two), and the holding time is 10s to 15s (e.g., it can be...). The injection time is 10s, 11s, 12s, 13s, 14s, 15s, or any range between these two values. The injection specific pressure is 120bar to 160bar (e.g., 120bar, 130bar, 140bar, 150bar, 160bar, or any range between these two values), and the boost pressure is 100bar to 150bar (e.g., 100bar, 110bar, 120bar, 140bar, 150bar, or any range between these two values). The boost triggering method is position triggering. This can further effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, and further enhance the internal density and appearance quality of the magnesium alloy gearbox housing.

[0038] According to some specific embodiments of this application, during the solidification process of the magnesium alloy melt in the mold cavity, when the thickness of the thick part of the solidified magnesium alloy billet is ≥10mm, the thick part of the magnesium alloy billet is subjected to extrusion treatment or spot cooling treatment. This can further ensure the absence of casting defects such as shrinkage porosity and shrinkage cavities, and improve the internal quality of the product.

[0039] According to some specific embodiments of this application, the die-casting pressure for extruding the thick parts of the magnesium alloy billet is 100 bar to 120 bar (e.g., it can be 100 bar, 105 bar, 110 bar, 115 bar, 120 bar or any range between the two), and the time is 2 s to 3 s (e.g., it can be 2 s, 2.2 s, 2.5 s, 2.8 s, 3 s or any range between the two). This can further ensure the absence of casting defects such as shrinkage porosity and shrinkage cavities, and improve the internal quality of the product.

[0040] According to some specific embodiments of this application, the temperature for spot cooling of the thicker parts of the magnesium alloy billet is 15°C to 25°C (for example, it can be 15°C, 18°C, 20°C, 22°C, 25°C, or any range between the two). This further ensures the absence of casting defects such as shrinkage porosity and shrinkage cavities, improving the internal quality of the product.

[0041] S300: Post-processing of the magnesium alloy gearbox housing blank to obtain the magnesium alloy gearbox housing.

[0042] According to some specific embodiments of this application, the post-processing includes: water cooling of the magnesium alloy gearbox housing blank, removal of the gating system, and marking. Specifically, a robot can be used to pick up the magnesium alloy gearbox housing blank, quench it in water for 2-5 seconds at room temperature, automatically remove the magnesium alloy gearbox housing gating system, slag bag, and venting plate, and perform casting marking to obtain the magnesium alloy gearbox housing. Then, the magnesium alloy gearbox housing is transported to the part removal port by a conveyor belt.

[0043] In a second aspect of this application, a magnesium alloy gearbox housing is proposed. According to an embodiment of this application, the aforementioned magnesium alloy gearbox housing is prepared using the die-casting method of the first aspect. Therefore, this application can effectively improve casting defects such as shrinkage porosity, gas porosity, and cold shuts during the casting process, enhance the internal density and appearance quality of the magnesium alloy gearbox housing; ensure the mechanical properties of the housing, meeting the load-bearing, shock absorption, and long-term service requirements of commercial vehicle gearbox housings; fully utilize the low-density characteristics of magnesium alloys to achieve lightweighting, reducing weight by approximately 30% compared to aluminum alloy commercial vehicle gearbox housings, contributing to low carbon emissions and reduced fuel consumption in vehicles; simultaneously, it can stabilize the die-casting process, reduce casting scrap rate, improve production efficiency, and facilitate the industrial-scale mass production of magnesium alloy gearbox housings.

[0044] In a third aspect of this application, a vehicle is proposed. According to an embodiment of this application, the vehicle includes a magnesium alloy gearbox housing as described in the second aspect. Specifically, the vehicle includes a frame, a transmission system, and a magnesium alloy gearbox housing mounted on the transmission system.

[0045] It should be noted that the vehicle has the aforementioned advantages of a magnesium alloy gearbox housing, which will not be elaborated upon here.

[0046] The embodiments of this application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. In addition, unless otherwise specified, all reagents used in the following embodiments are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also readily available to those skilled in the art.

[0047] Example 1 This embodiment provides a die-casting method for a magnesium alloy gearbox housing, comprising the following steps: Step 1: Place the AS41B magnesium alloy ingot into the feeder and preheat it at 110℃.

[0048] Step 2: Then, the preheated magnesium alloy ingot is placed in the melting chamber of the magnesium alloy melting furnace for melting at a melting temperature of 720°C to obtain magnesium alloy melt.

[0049] Step 3: The molten magnesium alloy after melting is injected into the die casting machine cup; the molten magnesium alloy is pushed into the mold cavity by low-speed injection and high-speed injection in sequence. After filling, pressure is increased and held to compensate for the solidification shrinkage of the melt; the molten magnesium alloy cools and solidifies in the cavity. After the process conditions are met, the mold is opened and the blank is ejected to obtain the magnesium alloy gearbox housing blank.

[0050] The die-casting machine used is a 4500-ton high-pressure die-casting machine, and the magnesium alloy gearbox housing mold is fixed on the mold frame of the 4500-ton high-pressure die-casting machine. The mold uses circulating heated oil as the medium to control the mold preheating and mold temperature during the die-casting process. The preheating temperature of the mold is controlled at 150℃ by the heated oil, and the temperature of the mold during the die-casting process is 200℃. The die-casting punch is water-cooled, and the temperature is controlled at 70℃.

[0051] Before casting, a layer of Derunbao magnesium alloy water-based release agent is evenly sprayed onto the surfaces of both the moving and stationary molds for 10 seconds. The casting chamber temperature is set to 680℃.

[0052] After the mold is closed, the mold is evacuated. The evacuation is triggered by position and the evacuation time is 0.2s, so that the vacuum degree in the mold cavity is <100mbar.

[0053] The process parameters for the 4500-ton high-pressure casting machine are set as follows: low-speed punch speed 0.5m / s, high-speed punch speed 4.5m / s, holding pressure for 10s, rapid energy storage of 150bar, pressurization energy storage of 120bar, and holding pressure for 12s.

[0054] During the solidification process of the magnesium alloy melt in the mold cavity, when the thickness of the thick part of the solidified magnesium alloy billet is >10mm, the thick part of the magnesium alloy billet is extruded. The extrusion pressure is 100 bar and the time is 2s.

[0055] Step 4: A robot is used to pick up the magnesium alloy gearbox housing blank, quench it in water for 3 seconds at room temperature, and automatically remove the magnesium alloy gearbox housing gating system, slag bag and exhaust wave plate. The casting is then marked to obtain the magnesium alloy gearbox housing. The magnesium alloy gearbox housing is then transported to the picking port by a conveyor belt.

[0056] Example 2 This embodiment provides a die-casting method for a magnesium alloy gearbox housing, which is basically the same as the die-casting method in Embodiment 1, except that: Step 3: The above mold uses circulating heating oil as the medium to control the mold preheating and mold temperature during the die casting process. The preheating temperature of the mold is controlled at 100℃ by the heating oil, and the temperature of the mold during the die casting process is 150℃.

[0057] Example 3 This embodiment provides a die-casting method for a magnesium alloy gearbox housing, which is basically the same as the die-casting method in Embodiment 1, except that: Step 3: After the mold is closed, the mold is evacuated. The vacuuming is triggered by position and the evacuation time is 0.2s, so that the vacuum degree in the mold cavity is <100mbar.

[0058] Example 4 This embodiment provides a die-casting method for a magnesium alloy gearbox housing, which is basically the same as the die-casting method in Embodiment 1, except that: Step 3: During the solidification of the magnesium alloy melt in the mold cavity, when the thickness of the thick part of the solidified magnesium alloy billet is >10mm, the thick part of the magnesium alloy billet is extruded. The extrusion pressure is 120 bar and the time is 3s.

[0059] Example 5 This embodiment provides a die-casting method for a magnesium alloy gearbox housing, which is basically the same as the die-casting method in Embodiment 1, except that: Step 3: Replace "When the thickness of the thick part of the solidified magnesium alloy billet is >10mm, the thick part of the magnesium alloy billet is extruded, the extrusion pressure is 100bar, and the time is 2s" with "Use high-pressure oil spot cooling to spot cool the thick part of the magnesium alloy billet, and the cooling oil temperature is 15℃".

[0060] Comparative Example 1 This comparative example provides a die-casting method for a magnesium alloy gearbox housing, which is basically the same as the die-casting method in Example 1, except that: no vacuuming is performed during the die-casting process, the mold is not heated, and local extrusion or spot cooling techniques are not used.

[0061] The magnesium alloy gearbox housings prepared in the above embodiments and comparative examples were subjected to X-ray flaw detection and mechanical property testing, and the results are shown in Table 1.

[0062] Table 1

[0063] As can be seen from Table 1, the mechanical properties of Examples 1-5 are all better than those of Comparative Example 1. It is evident that this application, by employing vacuum die casting + mold temperature balancing technology + local extrusion technology or local spot cooling technology, can effectively improve casting defects such as shrinkage porosity, gas holes, and cold shuts during the casting process, and effectively improve the mechanical properties of magnesium alloy gearbox housings.

[0064] Figure 2 This is an image showing the X-ray flaw detection results of Example 1. Figure 3 This is a comparison image of the X-ray flaw detection results (Scale 1). From... Figure 2 and Figure 3 As can be seen, the magnesium alloy gearbox housing of Example 1 has good internal quality and meets the product technical requirements. However, the magnesium alloy gearbox housing of Comparative Example 1 has casting defects such as shrinkage porosity, air holes, and cold shuts.

[0065] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0066] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A die-casting method for a magnesium alloy gearbox housing, characterized in that, include: (1) Place the magnesium alloy ingot in a melting furnace and melt it under a protective atmosphere to obtain a magnesium alloy melt; (2) The magnesium alloy melt is injected into the die casting machine cup, and the magnesium alloy melt is filled into the mold cavity and solidified by injection, and die casting is performed to obtain a magnesium alloy gearbox housing blank. (3) The magnesium alloy gearbox housing blank is post-processed to obtain a magnesium alloy gearbox housing; The preheating temperature of the mold is 100℃~150℃, and the temperature of the mold during the die casting process is 150℃~200℃. After the mold is closed, a vacuum is drawn from the mold. During the solidification of the magnesium alloy melt in the mold cavity, the thicker parts of the solidified magnesium alloy billet are subjected to extrusion or spot cooling.

2. The die-casting method according to claim 1, characterized in that, The mold uses circulating heated oil as the medium to control the mold preheating and mold temperature during the die casting process.

3. The die-casting method according to claim 1, characterized in that, After the mold is closed, the mold is evacuated to make the vacuum degree inside the mold cavity <100mbar.

4. The die-casting method according to claim 1, characterized in that, During the solidification process of the magnesium alloy melt in the mold cavity, when the thickness of the thick part of the solidified magnesium alloy billet is ≥10mm, the thick part of the magnesium alloy billet is subjected to extrusion treatment or spot cooling treatment.

5. The die-casting method according to claim 1, characterized in that, The pressure for extruding the thicker parts of the magnesium alloy billet is 100 bar to 120 bar, and the time is 2 to 3 seconds.

6. The die-casting method according to claim 1, characterized in that, The temperature for spot cooling of the thicker parts of the magnesium alloy billet is 15℃~25℃.

7. The die-casting method according to any one of claims 1 to 6, characterized in that, Before placing the magnesium alloy ingot in the melting furnace, the die-casting method further includes: drying and preheating the magnesium alloy ingot; And / or, in step (3), the post-processing includes: water cooling the magnesium alloy gearbox housing blank, removing it from the gating system, and marking it.

8. The die-casting method according to any one of claims 1 to 6, characterized in that, During the process of filling the mold cavity with magnesium alloy melt by injection, the temperature of the punch is 40℃~70℃; And / or, during the process of filling the mold cavity with magnesium alloy melt by injection, the low speed of the punch is 0.2m / s to 0.8m / s, the high speed of the punch is 4m / s to 5m / s, the holding time is 10s to 15s, the rapid energy storage is 120bar to 160bar, and the pressurized energy storage is 100bar to 150bar.

9. A magnesium alloy gearbox housing, characterized in that, It is prepared by the die-casting method according to any one of claims 1 to 8.

10. A vehicle, characterized in that, Includes the magnesium alloy gearbox housing as described in claim 9.