A manufacturing process for a wheel hub
By using coated sand cores in low-pressure casting molds and combining them with spinning, the hollow structure of the hollow wheel hub can be formed in one step, which solves the problems of long processing time and high cost of hollow wheel hubs in the existing technology, and improves the mechanical properties and material utilization of the hollow wheel hub.
Patent Information
- Application Number
- CN202611524067.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing hollow wheel hub manufacturing process, the hollow structure cannot be directly formed during the casting stage and needs to rely on subsequent CNC side milling, which results in long processing time, high cost, large tool consumption, and high investment in forging equipment.
By using coated sand cores for positioning in low-pressure casting molds and combining them with spinning, a hollow structure can be formed in one step. Spinning also improves the mechanical properties and material utilization of the rim area.
The hollow structure is formed during the casting stage, eliminating the need for subsequent CNC side milling processes. This reduces the processing time of a single product by 80%, improves the performance of the rim, reduces material costs, and increases the product qualification rate.
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy wheel manufacturing technology, and more specifically to a wheel manufacturing process. Background Technology
[0002] As the automotive industry moves towards lightweighting and personalization, hollowed-out car wheels are gradually gaining popularity in the mid-to-high-end vehicle market due to their unique appearance and weight reduction advantages. Hollowed-out wheels feature through-holes in the spokes, which not only create a sporty visual effect but also reduce redundant material in the spoke area.
[0003] However, the manufacturing of hollowed-out wheel hubs has long faced a technological dilemma. Currently, there are two main paths for producing hollowed-out wheel hubs in the industry: one is gravity casting combined with subsequent CNC side milling, and the other is forging milling. Although gravity casting can form the basic outline of the wheel hub, because the demolding direction of the hollow structure is inconsistent with the mold opening and closing direction, the hollow holes on the side of the spokes cannot be directly formed during the casting stage. Subsequent CNC side milling is necessary to remove the material. This side milling requires a special side milling cutter, with a single tool costing approximately 10,000 yuan. Furthermore, the tool life is limited, requiring up to 10 clamping operations, and the processing time for a single product can be as long as 4 hours. The processing cost is as high as 240 for 5 hours. 300 yuan. Although the forging route has better material properties, it also faces the problems of low side milling efficiency and high tool consumption, and the investment in forging equipment is much higher than that in casting equipment. Summary of the Invention
[0004] This invention provides a wheel hub manufacturing process and a steel wire bonding molding device with elastic floating adaptive capability.
[0005] To achieve the above objectives, this application provides the following technical solution: A manufacturing process for a wheel hub includes the following steps: S1. Sand core preparation: Prepare a coated sand core according to the hollow structure shape of the target wheel hub. The outline of the sand core corresponds to the hollow cavity of the wheel hub spoke. S2. Low-pressure casting: The sand core is positioned in the cavity of the low-pressure casting mold, aluminum alloy liquid is filled into the cavity and pressure is maintained and solidified to obtain a wheel hub blank. The spoke part of the wheel hub blank forms a hollow structure occupied by the sand core, and the wall thickness of the rim part of the wheel hub blank is greater than the target rim wall thickness. S3. Demolding and sand removal: Open the mold, remove the wheel hub blank, and remove the residual sand core in the wheel hub blank; S4. Spin forming: Spin forming is performed on the rim part of the wheel hub blank after the sand core is removed, so that the wall thickness of the rim part is reduced to the target wall thickness, and the grains of the rim part are stretched and strengthened along the spinning direction.
[0006] Furthermore, in step S1, the coated sand core is prepared using a hot core box sand-shooting process, with a sand-shooting temperature of 200-320℃ and a curing time of 60-180 seconds.
[0007] Furthermore, in step S2, the outer surface of the sand core undergoes a first spraying, surface polishing, and a second fine spraying before being placed into the mold. The second fine spraying uses fine-grained paint.
[0008] Furthermore, in step S2, the filling pressure of the low-pressure casting is 0.02-0.06 MPa, the filling time is 7-12 seconds, the solidification holding pressure is 0.05-0.08 MPa, and the holding time is 8-15 minutes.
[0009] Furthermore, in step S2, a clearance of 0.1-0.3 mm on one side is provided at the mating surface between the sand core and the mold to accommodate the thermal deformation of the mold.
[0010] Furthermore, in step S2, an exhaust channel is provided at the positioning position of the sand core, and the exhaust channel is connected to a negative pressure device outside the mold.
[0011] Furthermore, in step S3, the method of removing the sand core is at least one of vibration sand removal, heat treatment heating removal, or manual removal.
[0012] Furthermore, in step S4, the spinning process reduces the wall thickness of the rim portion by 1.5-3.0 mm relative to before spinning.
[0013] Furthermore, in step S2, the wheel hub blank is provided with a shrinkage rib at the connection between the spokes and the rim, and the machining allowance of the shrinkage rib is 4-8mm.
[0014] Furthermore, in step S4, the spinning process adopts a three-wheel synchronous spinning method, and the spinning temperature is 200-350℃.
[0015] Working principle and beneficial effects of the present invention: Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Hollow structure is formed in one step: By positioning the coated sand core in the low pressure casting mold, the hollow wheel spokes can obtain the required hollow holes in the casting stage, eliminating the subsequent CNC side milling process. The machining time of a single product is shortened from 4-5 hours to less than 1 hour, and the processing cost is reduced by about 80%.
[0016] (2) Improved mechanical properties of the rim: Spinning process causes plastic deformation of the casting structure of the rim, the grains are stretched and refined along the spinning direction, and casting defects such as porosity and shrinkage are eliminated by compression during the spinning process. The tensile strength and elongation of the rim are significantly improved, thus allowing for thinner rim wall thickness.
[0017] (3) Improved material utilization: Before spinning, the wheel rim blank only needs to reserve a small machining allowance. After spinning, the wall thickness is reduced by 1.5-3.0mm. Taking a 20-inch wheel hub as an example, the weight of a single product can be reduced by 1.2-2.1kg, and the material cost is significantly reduced.
[0018] (4) Improved sand core venting and mold thermal management scheme: By designing the venting channel at the sand core positioning point and the mold insulation measures, the problem of local mold cooling caused by sand core placement and the gas trapping defect during the casting process were solved, and the product qualification rate was improved. Detailed Implementation
[0019] The following detailed description illustrates the specific implementation method: Example 1 This embodiment provides a manufacturing process for a 20-inch sand core-spinning combined hollow automotive wheel hub, the specific steps of which are as follows: Step 1: Sand Core Preparation Coated sand cores were prepared using a hot-box sand-shooting process. The cavity profile of the sand core was designed based on the hollowed-out spoke shape of the target wheel hub HP281885. The profile of the main body of the sand core was consistent with the hollowed-out cavity of the spoke. The sand core was also equipped with a positioning boss and a positioning ring for mating with the lower mold limiting surface of the casting mold.
[0020] The coated sand is made of 70-140 mesh silica sand mixed with thermoplastic phenolic resin, with the resin added at 1.5-2.5% of the sand weight. The working temperature of the hot core box is set to 250℃, the sand injection pressure to 0.3MPa, and the curing time to 120 seconds. After sand injection, the sand core is removed and inspected for cracks and missing corners on the surface. The dimensional tolerance of the positioning boss is controlled within ±0.15mm.
[0021] Sand core surface treatment: First, the sand core is sprayed for the first time (the coating has a Baume degree of about 20). After drying, it is lightly polished to remove spray marks. Then, a second fine spraying is carried out using fine-grained coating (particle size ≤15μm) to ensure that the surface finish of the sand core meets the surface quality requirements of the casting.
[0022] Step 2: Low-pressure casting The prepared sand core is placed into the lower mold cavity of the low-pressure casting mold. The positioning boss of the sand core mates with the limiting surface of the lower mold, and the lower surface of the positioning ring is supported on the positioning outer ring platform of the lower mold. The upper surface of the positioning ring mates with the side mold. A 0.2mm clearance is reserved on each side of the mating surface of the sand core to accommodate the thermal expansion and deformation of the mold during the casting process. Vent holes are set at the positioning positions of the sand core. The vent holes are connected to an external negative pressure device through a channel inside the mold to actively vent the area around the sand core during the filling process.
[0023] The upper mold, lower mold, and side molds are all covered with insulation cotton to ensure that the mold temperature is maintained at 380-420℃. For mold areas with dense sand cores, additional local electric heating rods are installed for temperature compensation.
[0024] The molten aluminum alloy is made of Al-Si-Mg series casting aluminum alloy (such as A356), with a melting temperature of 720-740℃. After refining and degassing, it is held at a constant temperature. The pouring temperature is controlled at 690-710℃. Low-pressure casting parameters: filling pressure 0.03MPa, filling time 9 seconds, solidification holding pressure 0.06MPa, holding time 10 minutes. Under pressure, the molten aluminum alloy fills the mold cavity, and the space occupied by the sand core forms the negative space of the spoke hollow structure. Feeding ribs are provided at the connection between the spokes and the rim, with a machining allowance of 6mm to ensure sufficient feeding channels at the end of the filling process.
[0025] Step 3: Demolding and Sand Removal After the pressure holding period, the pressure is released, and the wheel hub blank is removed from the mold. The spoke area of the wheel hub blank has hollow holes formed by sand cores. Removing the sand cores: First, a high-frequency vibration device is used to apply vibration to the wheel hub blank, causing most of the sand cores to break and fall off. For the small amount of coated sand remaining on the inner wall of the hollow holes, heat treatment is used to remove it. The wheel hub blank is placed in a heat treatment furnace and heated to 480-520℃, held for 2-3 hours to decompose the residual resin adhesive. Then, sandblasting is used to remove the residual sand. Inspection confirms that no residual sand remains on the inner wall of the hollow holes.
[0026] Step 4: Spin forming The cleaned wheel hub blank is clamped onto a spinning machine, and the rim area is simultaneously spun by three spinning wheels. Before spinning, the wheel hub blank is preheated to 280-320℃. The spinning thinning rate is controlled to reduce the rim wall thickness by 2.0 mm, and the spinning feed speed is set to 1.2 mm / r. During the spinning process, the casting structure of the rim area undergoes plastic deformation; the original equiaxed grains are elongated along the spinning direction, forming a fibrous structure. Simultaneously, the micropores and shrinkage porosity remaining from the casting process are compressed and eliminated under the spinning compressive stress.
[0027] Step 5: Follow-up Processing After spinning, the wheel hub undergoes T6 heat treatment (solution treatment at 535℃ for 4 hours, water quenching, and artificial aging at 155℃ for 4 hours), followed by conventional machining (machining of center hole, bolt hole, and valve hole), painting, and dynamic balancing to obtain the finished hollow car wheel hub.
[0028] Performance testing The performance of the wheel hubs produced in Example 1 was tested: tensile strength of the rim: approximately 220 MPa before spinning and over 310 MPa after spinning; elongation of the rim: approximately 4% before spinning and over 8% after spinning; dimensional accuracy of the hollowed-out holes: within ±0.3 mm, meeting appearance and assembly requirements; machining time per piece: reduced from 4-5 hours in the traditional side milling process to approximately 50 minutes; weight reduction of a single 20-inch wheel hub: approximately 1.8 kg.
[0029] Example 2 The difference from Example 1 is that spherical sand (30% by mass) is mixed into the coated sand of the sand core to improve the high-temperature strength and collapsibility of the sand core. The spherical particle morphology of the spherical sand helps to improve the filling and collapsibility of the sand core and reduce the difficulty of sand removal. The remaining process parameters are the same as in Example 1.
[0030] Example 3 The difference from Example 1 is that the spinning process uses a two-wheel asymmetric spinning method, with a spinning temperature of 350℃ and a thinning amount of 3.0mm. It is suitable for wheel hub products of 19 inches and below, and can achieve a more significant weight reduction effect on smaller products. All other process parameters are the same as in Example 1.
[0031] Comparative Example 1 Hollowed-out wheel hubs of the same specifications were manufactured using a combination of traditional gravity casting and CNC side milling. After obtaining the wheel hub blank through gravity casting, the spokes were hollowed out using a specialized side milling cutter. The process involved 8 clamping operations, with a single-piece machining time of 4.5 hours and tool consumption of approximately 0.8 tools per piece. The tensile strength of the rim was measured at approximately 220 MPa, and the elongation was approximately 4%.
[0032] Comparative Example 2 The wheel hub is manufactured using a low-pressure casting + CNC side milling process, without introducing sand cores. After low-pressure casting, the spokes are solid, and hollow holes are formed by CNC side milling. The machining time is approximately 3.5 hours. The rim has a tensile strength of approximately 230 MPa and an elongation of approximately 4.5%.
[0033] Comparative Example 3 Sand core casting is used, but spinning is not performed. The hollow spokes are formed in one piece, but the rim retains the cast wall thickness. The rim has a tensile strength of approximately 220 MPa, an elongation of approximately 4%, and the product weight is approximately 1.8 kg heavier than that of Example 1.
[0034] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A manufacturing process for a wheel hub, characterized in that, Includes the following steps: S1. Sand core preparation: Prepare a coated sand core according to the hollow structure shape of the target wheel hub. The outline of the sand core corresponds to the hollow cavity of the wheel hub spoke. S2. Low-pressure casting: The sand core is positioned in the cavity of the low-pressure casting mold, aluminum alloy liquid is filled into the cavity and pressure is maintained and solidified to obtain a wheel hub blank. The spoke part of the wheel hub blank forms a hollow structure occupied by the sand core, and the wall thickness of the rim part of the wheel hub blank is greater than the target rim wall thickness. S3. Demolding and sand removal: Open the mold, remove the wheel hub blank, and remove the residual sand core in the wheel hub blank; S4. Spin forming: Spin forming is performed on the rim part of the wheel hub blank after the sand core is removed, so that the wall thickness of the rim part is reduced to the target wall thickness, and the grains of the rim part are stretched and strengthened along the spinning direction.
2. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S1, the coated sand core is prepared using a hot core box sand-shooting process, with a sand-shooting temperature of 200-320℃ and a curing time of 60-180 seconds.
3. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S2, the outer surface of the sand core undergoes a first spraying, surface polishing, and a second fine spraying before being placed into the mold. The second fine spraying uses fine-grained paint.
4. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S2, the filling pressure of the low-pressure casting is 0.02-0.06 MPa, the filling time is 7-12 seconds, the solidification holding pressure is 0.05-0.08 MPa, and the holding time is 8-15 minutes.
5. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S2, a 0.1-0.3mm clearance is provided on one side at the mating surface of the sand core and the mold to accommodate the thermal deformation of the mold.
6. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S2, an exhaust channel is provided at the positioning position of the sand core, and the exhaust channel is connected to a negative pressure device outside the mold.
7. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S3, the method of removing the sand core is at least one of vibration sand removal, heat treatment heating removal, or manual removal.
8. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S4, the spinning process reduces the wall thickness of the rim portion by 1.5-3.0 mm relative to before spinning.
9. The manufacturing process of the wheel hub according to claim 1, characterized in that, In step S2, the wheel hub blank is provided with a shrinkage rib at the connection between the spoke and the rim, and the machining allowance of the shrinkage rib is 4-8mm.