High-thermal-conductivity brazed high-pressure casting aluminum alloy and preparation method thereof
By optimizing the high-pressure casting process and composition of aluminum alloy, the problems of high welding difficulties and low solid-liquid phase line temperature are solved, high solid-liquid phase temperature and good welding performance are achieved, and high efficiency brazing of complex structural components are ensured. Welding capacity and low cost production.
Patent Information
- Application Number
- CN202411151355.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
During the welding process, existing aluminum alloy materials have problems such as high thermal conductivity, low melting point, easy oxidation and pollution-sensitive problems, which makes welding difficult, and the solid-liquid phase line temperature of conventional cast alloys is relatively low, making it difficult to meet the complex structural components. Brazing requirements, and the existing high-pressure casting process has high cost or difficulty in control, resulting in high defect rate.
The composition of high-pressure cast aluminum alloys includes 0.1 to 0.4% manganese, up to 0.12% silicon, 1.0 to 3.5% nickel, 1.2 to 1.8% iron, 0.01 to 0.2% chromium, up to 0.05% titanium, 0.02 to 0.02 to 0.2% vanadium, up to 0.05% boron, up to 0.12% magnesium, 0.15~0.45% cobalt, up to 0.05% zinc, the single impurity element does not exceed 0.05%, the total impurity element is less than 0.15%, copper + magnesium + The total silicon is not higher than 0.15%, the total of manganese + nickel + iron is not lower than 1.8% and not higher than 5.5%, the total of manganese + vanadium + chromium + titanium is less than 0.25%. By controlling the aluminum liquid temperature at 710~745℃, the Gas refining and high-pressure die-casting molding, the vacuum degree of the mold is 20Mbar, the casting pressure is 65±5MPa, the injection speed is 3.5±0.5m/s, and the mold temperature is 150±10℃.
The high solid-liquid phase temperature of aluminum alloy is achieved, with good castability, fluidity and thermal crack resistance, the cast yield strength is greater than 90MPa, the elongation of breaking is above 10.0%, the tensile strength is greater than 150MPa, and brazing is carried at high temperature There are no obvious defects during the process, low gas content, and good welding performance.
Smart Images

Figure CN119020641A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloy materials, and in particular to a high-heat-conductivity brazable high-pressure casting aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum alloys are widely used in aviation, automobile manufacturing, rail transportation, electronic equipment and other fields due to their good physical and chemical properties. However, the welding of aluminum and its alloys is relatively difficult, due to the high thermal conductivity, low melting point, easy formation of oxide film, and sensitivity to pollution. Brazing is an effective connection method. The body does not remelt during the welding process. It has the advantages of stable structure, high efficiency and yield rate. It can achieve the connection of aluminum alloys at a lower temperature, thereby avoiding or reducing possible problems in the welding process. At present, a large number of aluminum alloy brazing parts are produced by rolling / extrusion / forging. Generally speaking, the molding structure will be suitable for simple parts, but not for parts with complex product structures.
[0003] High-pressure casting of liquid metal (die casting for short) refers to a near-net-shape forming technology that fills the mold cavity with liquid or semi-liquid metal at a high speed and solidifies under pressure under the action of the punch movement. During the die casting process, the pressure on the molten metal is generally 30 to 80 MPa, the gate speed during filling reaches 25-50 m / s, and the filling time is only 0.02-0.1 s. It can form parts with complex structures, and has high production efficiency and low manufacturing cost. It is the most widely used process in the current metal liquid forming method. However, the current cast aluminum alloy is mainly based on the aluminum-silicon system. By adding a certain amount of strengthening elements such as Cu, Mg, and Zn to improve the strength, the solid-liquid phase temperature of the aluminum alloy material is low, and the eutectic temperature is 577 degrees, which is much lower than the conventional brazing temperature. Therefore, it is necessary to develop a new casting alloy system to meet the requirements of casting brazing.
[0004] Invention patent application CN113897519A discloses an Al-Mn-Mg-Si-Ti-Sn casting alloy for vacuum brazing by vacuum die casting and a preparation method thereof. On the basis of the aluminum-manganese eutectic composition, magnesium and silicon are added to improve the toughness of the alloy, and titanium and tin are added to refine the grains and improve the toughness of the alloy; however, the addition of 0.2 to 0.6 wt.% of silicon will significantly increase the solidification range, aggravate the tendency of hot cracking, and affect the casting performance;
[0005] Invention patent application CN116377288A discloses a high-pressure cast aluminum alloy that can be used for brazing. The high-pressure cast aluminum alloy that can be used for brazing includes: up to 0.3% by weight of silicon, 0.6-1.5% by weight of manganese, 0.3-1.0% by weight of magnesium, and 5.0-12.0% by weight of rare earth; wherein the rare earth: 3*Mn weight % ratio is controlled between 2.0 and 3.8; the patented cast aluminum alloy requires the use of a large amount of rare earth, which is relatively expensive;
[0006] Invention patent CN115679159B discloses an aluminum-nickel-manganese alloy material for high-temperature brazing and a rheocasting molding method thereof. The casting performance is improved by adding 3-3.5wt.% nickel and 1.0-1.2wt.% manganese, and rheocasting is used to alleviate shrinkage and thermal cracking. However, in actual operation, the rheological process is difficult to control, and defective products are prone to occur. In addition, excessive nickel addition will significantly increase the cost. Summary of the invention
[0007] In view of the deficiencies in the above-mentioned prior art, the present invention provides a high thermal conductivity brazable high-pressure cast aluminum alloy, which has a high solid-liquid phase temperature and good castability, and can be used to produce a brazable cast aluminum alloy for a closed fluid system.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A high-thermal-conductivity brazable high-pressure cast aluminum alloy, characterized in that: the high-pressure cast aluminum alloy comprises the following components by mass percentage:
[0010] 0.1-0.4 wt. % manganese;
[0011] up to 0.12 wt. % silicon;
[0012] 1.0 to 3.5 wt. % nickel;
[0013] 1.2-1.8 wt. % iron;
[0014] 0.01-0.2 wt. % chromium;
[0015] up to 0.05 wt. % titanium;
[0016] 0.02-0.2 wt. % vanadium;
[0017] Up to 0.05% by weight of boron;
[0018] up to 0.12% by weight of magnesium;
[0019] Up to 0.05% by weight of copper;
[0020] up to 0.05% by weight of calcium;
[0021] 0.15-0.45 wt.% cobalt;
[0022] Up to 0.05% by weight of zinc;
[0023] The maximum amount of a single impurity element is 0.05% by weight, the total amount of impurity elements is less than 0.15% by weight, and the rest is aluminum.
[0024] Furthermore, the total amount of copper+magnesium+silicon is not higher than 0.15 wt %.
[0025] Furthermore, the sum of manganese+nickel+iron is not less than 1.8 wt % and not more than 5.5 wt %.
[0026] Furthermore, the total amount of manganese + vanadium + chromium + titanium is less than 0.25% by weight.
[0027] It is also intended to provide a method for preparing a high-thermal-conductivity brazable high-pressure cast aluminum alloy, characterized in that it comprises the following steps:
[0028] S1, melting aluminum ingots and controlling the temperature of aluminum liquid to be between 710 and 745°C; controlling the composition of aluminum alloy liquid to be:
[0029] 0.1-0.4 wt. % manganese;
[0030] up to 0.12 wt. % silicon;
[0031] 1.0 to 3.5 wt. % nickel;
[0032] 1.2-1.8 wt. % iron;
[0033] 0.01-0.2 wt. % chromium;
[0034] up to 0.05 wt. % titanium;
[0035] 0.02-0.2 wt. % vanadium;
[0036] Up to 0.05% by weight of boron;
[0037] up to 0.12% by weight of magnesium;
[0038] Up to 0.05% by weight of copper;
[0039] up to 0.05% by weight of calcium;
[0040] 0.15-0.45 wt.% cobalt;
[0041] Up to 0.05% by weight of zinc;
[0042] The maximum amount of a single impurity element is 0.05% by weight, the total amount of impurity elements is less than 0.15% by weight, and the rest is aluminum. The added components are melted by heating the aluminum liquid;
[0043] S2, pressing the aluminum alloy sodium-free refining agent into the degasser for refining and degassing, and setting the refining time to 10-20 minutes to remove hydrogen and inclusions in the aluminum liquid;
[0044] S3, the gas content is detected by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, it is die-casted by a pressure casting equipment. The process parameters of pressure casting are as follows: the vacuum degree of the mold cavity is 20Mbar, the casting pressure is 65±5MPa, the injection speed is 3.5±0.5m / s, the mold temperature is 150±10℃, and the aluminum alloy liquid temperature is 710±10℃.
[0045] The beneficial effects of the present invention include: the aluminum alloy has a relatively high solid-liquid phase temperature, and the solidus line is greater than or equal to 620°C. It also has good castability, fluidity and thermal cracking resistance comparable to conventional cast A356 alloy, a cast yield strength greater than 90MPa, and a fracture elongation A greater than 10.0%, and a tensile strength greater than 150MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the metallographic structure diagram (200 times) of Example 2 of the present invention. DETAILED DESCRIPTION
[0047] The present invention will be further described in detail below with reference to specific embodiments and accompanying drawings.
[0048] The aluminum alloy casting of the present invention is composed of the following components in weight percentage:
[0049] 0.1-0.4 wt. % manganese;
[0050] up to 0.12 wt. % silicon;
[0051] 1.0 to 3.5 wt. % nickel;
[0052] 1.2-1.8 wt. % iron;
[0053] 0.01-0.2 wt. % chromium;
[0054] up to 0.05 wt. % titanium;
[0055] 0.02-0.2 wt. % vanadium;
[0056] Up to 0.05% by weight of boron;
[0057] up to 0.12% by weight of magnesium;
[0058] Up to 0.05% by weight of copper;
[0059] up to 0.05% by weight of calcium;
[0060] 0.15-0.45 wt.% cobalt;
[0061] Up to 0.05% by weight of zinc;
[0062] The maximum amount of a single impurity element is 0.05% by weight, the total amount of impurity elements is less than 0.15% by weight, and the rest is aluminum.
[0063] The aluminum alloy casting is prepared by following the steps below:
[0064] Step 1: Add an industrial pure aluminum ingot into a crucible resistance furnace and heat it to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then add other components of the preset composition except aluminum in sequence, that is, add other element components in the above mass percentage composition except aluminum to obtain aluminum alloy liquid.
[0065] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;
[0066] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the preset mass percentage.
[0067] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.
[0068] Die casting production verification:
[0069] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;
[0070] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.
[0071] The following are performance tests of die-casting specimens with different composition ratios after being cut according to the GBT228 standard specimen wire using a universal tensile machine equipped with an extensometer.
[0072] The high pressure cast aluminum alloys of the three embodiments were respectively manufactured by the above-mentioned preparation process, and their properties were tested to obtain the mechanical and thermal conductivity properties of the as-cast test bars, as shown in Table 1.
[0073] Table 1
[0074]
[0075]
[0076] The feasibility of brazing the above die-casting materials was tested by gas shielded brazing process. The results showed that after high-temperature brazing, there was no obvious pore bulging and local melting phenomenon. The metallographic structure of Example 2 was polished and observed. Figure 1 This indicates that the casting material has an extremely low gas content and a high solid-liquid phase temperature, and has no obvious defects during high-temperature brazing. This indicates that the alloy material of the present invention has good weldability.
[0077] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A high thermal conductivity brazable high pressure cast aluminum alloy, characterized in that: The high pressure casting aluminum alloy comprises the following components by mass percentage: 0.1-0.4 wt. % manganese; up to 0.12 wt. % silicon; 1.0 to 3.5 wt. % nickel; 1.2-1.8 wt. % iron; 0.01-0.2 wt. % chromium; up to 0.05 wt. % titanium; 0.02-0.2 wt. % vanadium; Up to 0.05% by weight of boron; up to 0.12% by weight of magnesium; Up to 0.05% by weight of copper; up to 0.05% by weight of calcium; 0.15-0.45 wt.% cobalt; Up to 0.05% by weight of zinc; The maximum amount of a single impurity element is 0.05% by weight, the total amount of impurity elements is less than 0.15% by weight, and the rest is aluminum.
2. A high thermal conductivity brazable high pressure casting aluminum alloy according to claim 1, characterized in that: The total of copper+magnesium+silicon is not higher than 0.15 wt %.
3. The high thermal conductivity brazable high pressure casting aluminum alloy according to claim 1, characterized in that: The sum of manganese+nickel+iron is not less than 1.8 wt % and not more than 5.5 wt %.
4. The high thermal conductivity brazable high pressure casting aluminum alloy according to claim 1, characterized in that: The sum of manganese + vanadium + chromium + titanium is less than 0.25% by weight.
5. A method for preparing a high thermal conductivity brazable high pressure casting aluminum alloy, characterized in that: The following steps are included: S1, melting aluminum ingots and controlling the temperature of aluminum liquid to be between 710 and 745°C; controlling the composition of aluminum alloy liquid to be: 0.1-0.4 wt. % manganese; up to 0.12 wt. % silicon; 1.0 to 3.5 wt. % nickel; 1.2-1.8 wt. % iron; 0.01-0.2 wt. % chromium; up to 0.05 wt. % titanium; 0.02-0.2 wt. % vanadium; Up to 0.05% by weight of boron; up to 0.12% by weight of magnesium; Up to 0.05% by weight of copper; up to 0.05% by weight of calcium; 0.15-0.45 wt.% cobalt; Up to 0.05% by weight of zinc; The maximum amount of a single impurity element is 0.05% by weight, the total amount of impurity elements is less than 0.15% by weight, and the rest is aluminum. The added components are melted by heating the aluminum liquid; S2, pressing the aluminum alloy sodium-free refining agent into the degasser for refining and degassing, and setting the refining time to 10-20 minutes to remove hydrogen and inclusions in the aluminum liquid; S3, the gas content is detected by a hydrogen detector, and when the gas content reaches below 0.15ml / 100g, it is die-casted by a pressure casting device.
Citation Information
Cited By
High solidus die-casting aluminum alloy capable of being brazed and preparation method of high solidus die-casting aluminum alloy
CN121137416A
High-strength high-thermal-conductivity cast rare earth aluminum alloy suitable for brazing and preparation method thereof