Si-doped AlCoCrFeNi2.1 Six eutectic high-entropy alloy and preparation method for synergistically improving strength and plasticity of Si-doped AlCoCrFeNi2.1 Six eutectic high-entropy alloy

By doping Si elements in eutectic high-entropy alloys and performing thermal mechanical treatment, a refined eutectic structure is formed, which solves the problem of difficulty in balancing strength and plasticity in the existing technology, and achieves efficient synergistic improvement of strong plasticity. Suitable for a variety of high-strength structural applications.

CN119040723AActive Publication Date: 2024-11-29FUJIAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411261220.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-29
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing eutectic high-entropy alloys often sacrifice plasticity when increasing their strength, and there are few researches on doping designs of non-metallic elements, making it difficult to achieve synergistic improvement of strong plasticity.

Method used

By doping trace Si elements, the composition of AlCoCrFeNi2.1Six eutectic high-entropy alloy is adjusted, and combined with thermomechanical treatment methods, a micro-nano ultrafine scale biphasic (FCC+BCC) with a refined eutectic structure and mechanical properties matched by mechanical properties is formed. ) Heterostructure.

Benefits of technology

The coordinated improvement of the strong plasticity of the alloy has been achieved, the tensile strength is increased by 45%, and the fracture toughness is increased by 47%. The strength is further improved without sacrificing plasticity. It is suitable for aerospace and marine equipment and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040723A_ABST
    Figure CN119040723A_ABST
Patent Text Reader

Abstract

The invention relates to a eutectic high-entropy alloy, in particular to a Si-doped AlCoCrFeNi2.1 Six eutectic high-entropy alloy and a preparation method for synergistically improving the strength and plasticity of the Si-doped AlCoCrFeNi2.1 Six eutectic high-entropy alloy, the chemical formula of the eutectic high-entropy alloy is AlCoCrFeNi2.1 Six, and x is larger than or equal to 0 and smaller than or equal to 0.5; the preparation method comprises the following steps: weighing the raw materials according to the proportion; as-cast alloy is obtained through vacuum arc melting, and eutectic high-entropy alloy is obtained through thermal mechanical treatment; the thermal mechanical treatment method comprises a twice rolling process and a twice annealing process, the rolling process adopts multi-pass non-fixed deformation cold rolling, the total rolling amount of the first-time multi-pass non-fixed deformation cold rolling of the as-cast alloy is 30%, and high-temperature annealing is carried out; and then secondary multi-pass non-fixed deformation cold rolling is carried out, the total rolling amount is 0-40%, and high-temperature annealing is carried out again so that crystal grains in the alloy can be refined and recrystallized. Compared with an as-cast AlCoCrFeNi2.1 eutectic high-entropy alloy, the fracture toughness of the alloy treated through the thermal mechanical method can be improved by 47% at most, the fracture toughness can be improved by 110% at most, and synergistic improvement of strength and plasticity is further achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of eutectic high entropy alloy materials, and in particular to a Si-doped AlCoCrFeNi 2.1 Si x Eutectic high entropy alloy and preparation method of synergistically improved strength and plasticity. Background Art

[0002] Since Lu Yiping et al. proposed the concept of eutectic high entropy alloys in 2014, more and more people have begun to pay attention to the field of eutectic high entropy alloys. Eutectic high entropy alloys combine the advantages of traditional eutectic alloys and high entropy alloys, and usually show excellent comprehensive properties, such as good strength and plasticity combination, high oxidation resistance, superior high temperature creep resistance, excellent fluidity and uniform microstructure. Nowadays, the eutectic high entropy alloy system is constantly developing and growing. However, there are few existing eutectic high entropy alloy systems with good strength-plasticity balance, and post-treatment is required to improve their performance. However, the traditional method of improving the mechanical properties of alloys often sacrifices plasticity to improve the strength of the alloy. Experimental studies have shown that by adjusting the proportion of eutectic high entropy alloy components or doping with trace elements, the synergistic improvement of strength and plasticity can be directly achieved. As for the eutectic high entropy alloy components reported so far, the selected elements are mostly based on metal elements or doped with trace rare earth elements to improve the comprehensive mechanical properties of eutectic high entropy alloys, while there are few studies on the non-metallic design of eutectic high entropy alloys. As an inorganic non-metallic element, Si has excellent advantages in oxidation resistance, corrosion resistance and friction resistance, and has low density and low price. Therefore, it has been widely studied and applied in traditional alloys. Based on this, this paper prepared AlCoCrFeNi by adding trace non-metallic element Si. 2.1 Si x Eutectic high entropy alloy directly achieves the synergistic improvement of strength and plasticity; in addition, the alloy is subjected to thermomechanical treatment, and multiple passes of non-fixed deformation cold rolling treatment and recrystallization heat treatment are performed in sequence, and its comprehensive mechanical properties are further improved. The alloy can be processed into various forms of products and has a wide range of applications in the preparation of high-strength structural parts for aerospace, future marine equipment, and petrochemical fields. Summary of the invention

[0003] In order to solve the problems of the prior art, the present invention provides a Si-doped AlCoCrFeNi 2.1 Si x Eutectic high-entropy alloys and their preparation methods and uses for synergistically improved strength and plasticity are widely used in high-strength structural parts in aerospace, future marine equipment, petrochemical industry, etc., and have good theoretical guidance and reference significance for the development of metal materials.

[0004] The alloy is composed of FCC phase and BCC phase. With the increase of Si content, its microstructure gradually evolves from the typical lamellar eutectic structure to a structure in which lamellar eutectic structure and irregular petal-shaped structure coexist, and finally to a completely irregular petal-shaped structure. Si element can promote the formation of BCC phase and regulate the volume ratio of hard BCC phase and tough FCC phase in the organization. The volume change of the two phases is as follows: Figure 2 As shown in the figure, it has a significant effect on the microhardness and wear resistance of the alloy. On the other hand, the increase in Si concentration accelerates the growth of grains, gradually increases the average grain size in the alloy, and improves the work hardening ability of the alloy. The change of the two-phase grain size in the alloy with Si content is shown in Figure 3 As shown. In summary, the addition of Si solves the key problem that is difficult to break through in the synergistic improvement of strength and plasticity of eutectic high entropy alloy materials, and improves the comprehensive mechanical properties of the alloy. In addition, the alloy is subjected to thermomechanical treatment to obtain a refined eutectic structure, and then by regulating the heat treatment time and temperature, a micro-nano ultrafine scale dual-phase (FCC+BCC) heterogeneous structure with matching mechanical properties can be formed. The change of the two-phase grain size in the alloy after thermomechanical treatment with Si content is shown in Figure 4 shown.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A Si-doped AlCoCrFeNi 2.1 Si x Eutectic high entropy alloy, general formula AlCoCrFeNi 2.1 Si x , where 0≤x≤0.5, x is the molar percentage of the corresponding element. The Si-modified cast alloy with synergistically improved strength and plasticity is obtained by vacuum arc melting process, wherein the cast alloy AlCoCrFeNi 2.1 Si 0.15 It has the best strength-plastic matching, compared with the matrix AlCoCrFeNi 2.1 Its strength and plasticity are both increased by 45%. When x>0.2, the plasticity of the cast alloy begins to decrease significantly, especially when x=0.3, with only about 5% plasticity. Figure 1 As shown. On this basis, a eutectic high entropy alloy with further synergistic improvement in strength and plasticity is obtained through a thermomechanical treatment method. Compared with the cast AlCoCrFeNi2.1 eutectic high entropy alloy, the alloy treated by the thermomechanical method can improve the fracture toughness by up to 47% and the tensile strength by up to 110%, further achieving the improvement of strength. Fig.14 shown.

[0006] A Si-doped AlCoCrFeNi 2.1 Si xThe method for synergistically improving the strength and plasticity of eutectic high entropy alloys comprises the following steps: S1: Master alloy preparation: Al, Co, Cr, Fe, Ni and non-metallic Si raw materials are accurately weighed according to the molar percentage of eutectic high entropy alloy, and then AlCoCrFeNi is obtained through a casting process. 2.1 Si x Eutectic high entropy alloy master alloy; S2: First cold deformation: The AlCoCrFeNi obtained in step S1 is 2.1 Si x The eutectic high entropy alloy master alloy is cold rolled to reduce the total thickness by 30%; S3: First heat treatment: AlCoCrFeNi after cold rolling in step S2 2.1 Si x The eutectic high entropy alloy is annealed and water quenched to remove internal stress and casting defects of the alloy; S4: Second cold deformation: AlCoCrFeNi annealed in step S3 2.1 Si x The eutectic high entropy alloy is cold rolled to reduce the thickness again by 0-40%; S5: Second annealing treatment: The cold-rolled AlCoCrFeNi 2.1 Si x The eutectic high entropy alloy is annealed and water quenched to refine and recrystallize the grains in the alloy, thereby obtaining the eutectic high entropy alloy with synergistically improved strength and plasticity.

[0007] In step S1, the purity of metals Al, Co, Cr, Fe, and Ni is greater than or equal to 99.95%, and the purity of non-metal Si is greater than or equal to 99.999%.

[0008] A Si-doped AlCoCrFeNi 2.1 Si x A method for synergistically improving the strength and plasticity of eutectic high entropy alloys, wherein the casting process is arc melting under inert gas protection, comprising the following steps: evacuating the vacuum arc melting furnace to 1×10 -3 Pa, then inert gas is injected into the furnace, and then the alloy is melted. After the arc is struck, the titanium ingot is first melted to absorb the residual oxygen in the furnace, and then the weighed raw materials in S1 of claim 2 are put into the furnace in order from low to high melting points of the elements. After the sample is melted and thoroughly cooled, it is turned over and repeatedly melted for more than 8 times to ensure the uniformity of the alloy ingot composition. After the melting is completed, the alloy ingot is obtained.

[0009] Furthermore, the inert gas is argon, the current of the arc melting is 400-600A, and each melting time is not less than 3 minutes.

[0010] Furthermore, in step S2 and step S4, the rolling process adopts multiple passes of non-fixed deformation cold rolling, that is, the deformation of the early single pass is maintained at about 5%, the plastic deformation of the material is fully utilized, the edge crack rate of the billet is reduced, and the deformation of the later single pass is not higher than 2%, thereby improving the sample quality and thickness accuracy.

[0011] Furthermore, the annealing temperature in step S3 is 1000-1200°C.

[0012] Furthermore, the annealing temperature in step S5 ranges from 600 to 900°C.

[0013] Compared with the prior art, the invention has the following beneficial effects: (1) The high-strength and high-plasticity AlCoCrFeNi modified by doping with trace Si elements 2.1 Si x Eutectic high entropy alloys are composed of six elements: Al, Co, Cr, Fe, Ni and Si. The melting points of the six elements are relatively low, making them easy to smelt. In addition, the alloy has good casting properties and is suitable for industrial large-scale production applications.

[0014] (2) The present invention increases the volume fraction of the BCC phase by doping a trace amount of Si element, and fine particles are precipitated in the BCC phase, which plays a role of precipitation strengthening; in addition, the increase in Si concentration accelerates the growth of grains, gradually increases the average grain size in the alloy, improves the work hardening ability of the alloy, and achieves a synergistic improvement in the strength and plasticity of the alloy, so that the alloy has excellent comprehensive mechanical properties in the cast state. The cast tensile strength is increased from 765.5MPa to 1112MPa, and the plasticity is increased from 13.5% to 19.5%, which is higher than that of the matrix AlCoCrFeNi 2.1 The tensile strength and plasticity were both increased by 45%. Further, by combining the thermomechanical treatment process, the tensile strength of the alloy was further increased to 1347.47MPa without sacrificing plasticity, and the maximum tensile strength could reach 1601.15MPa.

[0015] (3) The high-strength and high-plasticity AlCoCrFeNi modified by doping with trace Si elements in the present invention 2.1 Si x The elements in the eutectic high entropy alloy system are easy to obtain, non-toxic and harmless, and the preparation method is simple, using vacuum arc melting.

[0016] (4) AlCoCrFeNi of the present invention 2.1 Si x The inorganic non-metallic element Si selected for eutectic high entropy alloy not only reduces the overall density and manufacturing cost of the alloy, but also has excellent corrosion resistance, oxidation resistance and friction resistance.

[0017] In summary, the high-strength and high-plasticity AlCoCrFeNi modified by doping a trace amount of Si element in the present invention 2.1 Si x Eutectic high-entropy alloys not only exhibit excellent comprehensive mechanical properties, casting fluidity and uniform microstructure, but also have potential wear resistance, oxidation resistance and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Other features, objectives and advantages of the present invention will become more apparent from a reading of the detailed description of non-limiting embodiments made with reference to the following accompanying drawings.

[0019] Figure 1 As-cast AlCoCrFeNi 2.1 Si x (x=0, 0.05, 0.1, 0.15, 0.2, 0.3) Stress-strain curves of eutectic high-entropy alloy.

[0020] Figure 2 As-cast AlCoCrFeNi 2.1 Si x (x=0, 0.05, 0.1, 0.15, 0.2) Bar graph of the volume of FCC and BCC phases in eutectic high entropy alloys changing with Si content.

[0021] Figure 3 AlCoCrFeNi 2.1 Si x (x=0, 0.05, 0.1, 0.15, 0.2) Line graph of FCC and BCC grain size variation with Si content in cast eutectic high entropy alloy.

[0022] Figure 4 AlCoCrFeNi 2.1 Si x (x=0, 0.05, 0.1, 0.15, 0.2) Line graph of FCC and BCC grain size changes with Si content after thermomechanical treatment of eutectic high entropy alloy.

[0023] Figure 5 AlCoCrFeNi in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 Microstructure of eutectic high entropy alloy in the as-cast state; Figure 6 AlCoCrFeNi in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 XRD pattern of eutectic high entropy alloy in cast state; Figure 7 For AlCoCrFeNi in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 DSC differential thermal analysis of eutectic high entropy alloy in cast state; Figure 8 AlCoCrFeNi in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 Tensile engineering stress-strain curve of eutectic high entropy alloy in cast state; Fig. 9 For AlCoCrFeNi in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 Microstructure of eutectic high entropy alloy in the as-cast state; Fig.10 AlCoCrFeNi in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 XRD pattern of eutectic high entropy alloy in cast state; Fig.11 AlCoCrFeNi in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 DSC differential thermal analysis of eutectic high entropy alloy in cast state; Fig.12 For AlCoCrFeNi in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 Tensile engineering stress-strain curve of eutectic high entropy alloy in the cast state.

[0024] Fig.13 For AlCoCrFeNi in Examples 1 and 2 2.1 Si x Vickers hardness of alloy system in cast state.

[0025] Fig.14 AlCoCrFeNi in Example 3 2.1 Si 0.1 Tensile engineering stress-strain curves of a eutectic high-entropy alloy after thermomechanical treatment (exploring the second heat treatment temperature).

[0026] Fig.15The AlCoCrFeNi obtained in Example 4 after thermomechanical treatment (investigating the second deformation amount) 2.1 Si 0.1 Tensile engineering stress-strain curves of eutectic high entropy alloys.

[0027] Fig.16 The AlCoCrFeNi obtained in Example 4 after thermomechanical treatment (investigating the second deformation amount) 2.1 Si 0.1 Tensile engineering stress-strain curves of eutectic high entropy alloys II.

[0028] Fig.17 The AlCoCrFeNi obtained in Example 4 after thermomechanical treatment (investigating the second deformation amount) 2.1 Si 0.1 Tensile engineering stress-strain curves of eutectic high entropy alloys III.

[0029] Fig.18 This is the tensile engineering stress-strain curve of the alloy structure sample produced when the arc melting current is 400-600A.

[0030] Fig.19 The sample has a single-pass deformation much greater than 5%.

[0031] Fig. 20 This is a sample that has undergone multiple small deformations (the deformation of a single pass in the early stage is about 5%, and the deformation of a single pass in the later stage is not higher than 2%) used in this patent. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below by examples, which are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0033] The present invention relates to a eutectic high entropy alloy, in particular to a Si-doped AlCoCrFeNi 2.1 Si x Eutectic high entropy alloy and preparation method and use thereof for synergistically improving strength and plasticity, the chemical formula of the eutectic high entropy alloy is AlCoCrFeNi 2.1 Si x, where 0≤x≤0.5. The method comprises the following steps: S1: preparation of a master alloy: Al, Co, Cr, Fe, Ni and Si are weighed respectively according to the proportion, and then a Si-modified master alloy with synergistically improved strength and plasticity is obtained through a smelting process; S2: first cold deformation: cold rolling the master alloy to reduce the thickness by 30%; S3: first heat treatment: annealing the eutectic high entropy alloy after the first cold rolling; S4: second cold deformation: cold rolling the eutectic high entropy alloy after the first annealing for the second time to reduce the final thickness by 0-40% again, so as to obtain a eutectic high entropy alloy with further synergistically improved strength and plasticity.

[0034] Original eutectic high entropy alloy AlCoCrFeNi 2.1 It is composed of FCC phase and BCC phase, showing a typical lamellar eutectic structure. A small amount of Si element doping transforms the lamellar eutectic structure into a lamellar structure and an irregular petal-like structure. With the further increase of Si content, its structure is completely transformed into an irregular petal-like structure. This not only causes lattice distortion of FCC phase and BCC phase, but also increases the volume fraction of hard BCC phase, achieving a synergistic improvement of strength and plasticity. Analysis shows that the addition of Si makes AlCoCrFeNi 2.1 The stable mixed structure of FCC and BCC is destroyed, thus generating lattice distortion energy. In order to balance this energy change, obvious lattice distortion will occur. According to the calculation of atomic density, the atomic density of BCC (i.e., the volume percentage of atoms in the unit cell) is 68%, and the atomic density of FCC is 74%. The formation of a lower atomic density can release part of the lattice distortion energy, making the structure tend to be stable. Microscopically, the lattice distortion of the FCC phase and the BCC phase is caused, and the volume fraction of the hard BCC phase is increased, and the synergistic improvement of strength and plasticity is achieved macroscopically. Compared with the prior art, the high-strength and high-plasticity eutectic high-entropy alloy of the present invention has excellent yield strength, tensile strength and elongation, and achieves a synergistic improvement of strength and plasticity; and has excellent casting fluidity and uniform microstructure, so it has broad application prospects in the field of engineering structures. In this scheme, the alloy is composed of FCC phase and BCC phase. With the increase of Si content, its microstructure gradually evolves from the typical lamellar eutectic structure to a structure in which lamellar eutectic structure and irregular petal-shaped structure coexist, and finally evolves into a completely irregular petal-shaped structure. Si element can promote the formation of BCC phase and regulate the volume ratio of hard BCC phase and tough FCC phase in the organization. The volume change of the two phases is as follows: Figure 2 As shown in the figure, it has a significant effect on the microhardness and wear resistance of the alloy. On the other hand, the increase in Si concentration accelerates the growth of grains, gradually increases the average grain size in the alloy, and improves the work hardening ability of the alloy. The change of the two-phase grain size in the alloy with Si content is shown in Figure 3As shown. In summary, the addition of Si solves the key problem that is difficult to break through in the synergistic improvement of strength and plasticity of eutectic high entropy alloy materials, and improves the comprehensive mechanical properties of the alloy. In addition, the alloy is subjected to thermomechanical treatment to obtain a refined eutectic structure, and then by regulating the heat treatment time and temperature, a micro-nano ultrafine scale dual-phase (FCC+BCC) heterogeneous structure with matching mechanical properties can be formed. The change of the two-phase grain size in the alloy after thermomechanical treatment with Si content is shown in Figure 4 shown.

[0035] A eutectic high entropy alloy with synergistic improvement of strength and plasticity doped with Si, with the general formula of AlCoCrFeNi 2.1 Si x , where 0≤x≤0.5, x is the molar percentage of the corresponding element. 2.1 Si x The cast tensile strength of the eutectic high entropy alloy increased from 765.5MPa to 1111.7MPa, and the plasticity increased from 13.5% to 19.5%, which is relatively 2.1 The tensile strength and plasticity are increased by 45%. Figure 1 As shown; further, by combining the thermomechanical treatment process, the tensile strength of the alloy is further increased to 1347.47MPa without sacrificing plasticity, and the maximum tensile strength can reach 1601.15MPa, as shown Fig.14 It is worth noting that in the cast state, when x=0.15, it has the best mechanical properties. It should be noted that when the Si content is greater than 0.2, the plasticity of the alloy begins to decrease, especially when x=0.3, the plasticity is only about 5%, as shown in Figure 1 As shown; after thermomechanical treatment, when x = 0.1, it has the best mechanical properties, and the best heat treatment process is annealing at 800 ° C after the second cold rolling of 30%, as shown Fig.16 shown.

[0036] The Si-doped AlCoCrFeNi 2.1 Si x The method for synergistically improving the strength and plasticity of eutectic high entropy alloys comprises the following steps: S1: Preparation of master alloy: Al, Co, Cr, Fe, Ni and non-metallic Si raw materials are accurately weighed according to the molar percentage of eutectic high entropy alloy, and the purity of Al, Co, Cr, Fe, Ni and Si is greater than or equal to 99.95wt.%; then AlCoCrFeNi is obtained by casting process. 2.1 Si x Eutectic high entropy alloy master alloy; S2: First cold deformation: The AlCoCrFeNi obtained in step S1 is 2.1 Si x The eutectic high entropy alloy master alloy is cold rolled to reduce the total thickness by 30%; S3: First annealing treatment: The AlCoCrFeNi 2.1 Si x The eutectic high entropy alloy is annealed and water quenched; specifically, the AlCoCrFeNi 2.1 Si x The eutectic high entropy alloy is annealed at 1000-1200°C; preferably 1050°C.

[0037] S4: Second cold deformation: AlCoCrFeNi annealed in step S3 2.1 Si x The eutectic high entropy alloy is cold rolled to reduce the thickness again by 0-40%; S5: Second annealing treatment: The cold-rolled AlCoCrFeNi 2.1 Si x The eutectic high entropy alloy is annealed and water quenched to obtain the Si-modified eutectic high entropy alloy. 2.1 Si x The eutectic high entropy alloy is annealed at 600° C. to 900° C. to obtain the Si-modified eutectic high entropy alloy.

[0038] In step S1, the purity of metals Al, Co, Cr, Fe, and Ni is greater than or equal to 99.95%, and the purity of non-metal Si is greater than or equal to 99.999%.

[0039] The casting process is arc melting under inert gas protection, including the following steps: evacuating the vacuum arc melting furnace to 1×10 -3 Pa, then inert gas is injected into the furnace, and then the alloy is melted. After the arc is struck, the titanium ingot is first melted to absorb the residual oxygen in the furnace, and then the weighed raw materials in S1 of claim 2 are put into the furnace in order from low to high melting points of the elements. After the sample is melted and thoroughly cooled, it is turned over and repeatedly melted for more than 8 times to ensure the uniformity of the alloy ingot composition. After the melting is completed, the alloy ingot is obtained.

[0040] The inert gas is argon, and the arc melting current is 400-600A. In order to ensure the uniformity of the melting composition, the current of each system increases with the increase of Si content. Specifically, with the increase of Si content, the current of 400A can no longer meet the experimental requirements. Increasing the current can ensure the uniformity of the melting composition, make the alloy structure distribution more uniform at the microscopic level, and improve the mechanical properties of the alloy at the macroscopic level ( Fig.18 as shown).

[0041] The cold rolling process in step S2 and step S4 is a multi-pass cold rolling with non-fixed deformation. The deformation of the early single pass is maintained at about 5%, which makes full use of the plastic deformation of the material, reduces the length of the billet scrap, and improves the utilization rate; the deformation of the later single pass is not higher than 2%, which improves the sample quality and thickness accuracy, and finally makes the total deformation after two cold rollings 40% of the original. The alloy of this system has high hardness and overall low plasticity. Multi-pass cold rolling with small deformation can reduce the crack rate and improve the utilization rate of the alloy; in addition, multi-pass cold rolling with small deformation can also control the accuracy of the sample thickness to avoid over-rolling. Fig.19 The sample shown here has a single-pass deformation much greater than 5%. Fig. 20 After the multi-pass small deformation used in this patent (the deformation of a single pass in the early stage is about 5%, and the deformation of a single pass in the later stage is not more than 2%), the cracks of the samples are significantly reduced.

[0042] The annealing temperature range in step S5 is 600~900℃. This process is a key core step in the heat treatment process and one of the original and innovative parts. The heat treatment after two cold rollings, annealing can improve the structure and properties of the cold-rolled alloy. While improving the internal stress, hardness and elastic modulus, it can also improve the tensile strength, ductility and fatigue strength. In addition, annealing can also improve the surface quality of the rolled billet, making it smoother. The experiment explored the optimal second heat treatment temperature at 600-900℃. Taking the Si0.1 system as an example, Fig.14 As shown in the figure, when the temperature is too low, the alloy has the highest strength but the plasticity is less than 10%. When the temperature is too high, it has higher plasticity but the strength is too low, and it is impossible to achieve a good balance between strength and plasticity.

[0043] Implementation Case 1 This example discloses a high-strength, high-plasticity cast eutectic high-entropy alloy modified by doping with trace Si elements, and its general formula is AlCoCrFeNi 2.1 Si 0.1 , abbreviated as AS-Si0.1, matrix AlCoCrFeNi 2.1 Abbreviated as AS-Si0.

[0044] In this embodiment, a Si-doped AlCoCrFeNi 2.1 Si 0.1The method for synergistically improving the strength and plasticity of eutectic high entropy alloys comprises the following steps: accurately weighing Ni, Co, Fe, Cr, Al and non-metallic Si raw materials according to the molar percentage of the eutectic high entropy alloy, wherein the purity of metals Al, Co, Cr, Fe and Ni is greater than or equal to 99.95%, and the purity of non-metallic Si is greater than or equal to 99.999%. Then, the Si-modified AlCoCrFeNi is obtained by vacuum arc melting. 2.1 Si 0.1 Eutectic high entropy alloy. The specific operation is as follows: evacuate the vacuum arc melting furnace to 1×10 -3 Pa, and then inert gas argon is flushed into the furnace, and then the alloy is melted. After the arc is struck, the titanium ingot is first melted to absorb the residual oxygen in the furnace, and then the mixed raw materials are melted, and the melting current is 400~600A. After the sample is melted and thoroughly cooled, it is turned over and repeatedly melted for more than 8 times to ensure the uniformity of the alloy ingot composition. After the melting is completed, the cast alloy ingot is obtained.

[0045] Figure 5 The cast AlCoCrFeNi obtained in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 Microstructure of eutectic high entropy alloy. It can be found that with the addition of Si, the alloy changes from a typical lamellar eutectic microstructure to a lamellar structure and an irregular petal-like structure. The addition of Si reduces the FCC volume fraction and increases the BCC volume fraction. Fine particles precipitate in the BCC phase, which plays a role of precipitation strengthening and achieves a synergistic improvement in the strength and plasticity of the alloy.

[0046] Figure 6 The cast AlCoCrFeNi obtained in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 From the XRD diffraction analysis of the eutectic high entropy alloy, it can be seen that the alloy is composed of FCC and BCC phases, indicating that the change in Si content will not cause changes in the crystal structure. However, it can be found from the figure that the diffraction peak of the BCC phase shifts to the right after adding Si, indicating that due to the small radius of Si atoms, the BCC solid solution lattice shrinks by replacing larger atoms in the solid solution, the lattice constant decreases, and the BCC diffraction peak shifts to the right.

[0047] Figure 7 The cast AlCoCrFeNi obtained in Example 1 2.1 Si 0.1 The DSC differential thermal analysis of the eutectic high entropy alloy in the cast state shows only a single endothermic / exothermic peak, which indicates that the alloy is a eutectic alloy composition.

[0048] Figure 8 The cast AlCoCrFeNi obtained in Example 1 2.1 Si 0.1 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 The tensile engineering stress-strain curve of the eutectic high entropy alloy in the cast state shows that the alloy has achieved a synergistic improvement in strength and plasticity. 2.1 The tensile strength and elongation of the eutectic high entropy alloy are 765.5MPa and 13.5% respectively, and the Vickers hardness is 258HV; AlCoCrFeNi 2.1 Si 0.1 The tensile strength and elongation of the eutectic high entropy alloy are 979.2MPa and 16.7% respectively, and the Vickers hardness is 298HV.

[0049] Implementation Case 2 This example discloses a high-strength, high-plasticity cast eutectic high-entropy alloy modified by doping with trace Si elements, and its general formula is AlCoCrFeNi 2.1 Si 0.15 , abbreviated as AS-Si0.15.

[0050] In this embodiment, a Si-doped AlCoCrFeNi 2.1 Si 0.15 A method for synergistically improving the strength and plasticity of a eutectic high entropy alloy, the preparation of which comprises the following steps: accurately weighing Ni, Co, Fe, Cr, Al and non-metallic Si raw materials according to the molar percentage of the high entropy alloy, wherein the purity of metals Al, Co, Cr, Fe and Ni is greater than or equal to 99.95%, and the purity of non-metallic Si is greater than or equal to 99.999%. Subsequently, the Si-modified AlCoCrFeNi is obtained by vacuum arc melting. 2.1 Si 0.15 High entropy alloy. The specific operation is as follows: evacuate the vacuum arc melting furnace to 1×10 -3 Pa, and then inert gas argon is flushed into the furnace, and then the alloy is melted. After the arc is struck, the titanium ingot is first melted to absorb the residual oxygen in the furnace, and then the mixed raw materials are melted, and the melting current is 400~600A. After the sample is melted and thoroughly cooled, it is turned over and repeatedly melted for more than 8 times to ensure the uniformity of the alloy ingot composition. After the melting is completed, the cast alloy ingot is obtained.

[0051] Fig. 9 The cast AlCoCrFeNi obtained in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1Microstructure of eutectic high entropy alloy. It can be found that when X is greater than 0.1, the layered structure disappears completely, the alloy completely transforms from a typical layered eutectic microstructure to an irregular petal-like structure, and the volume fraction of the hard BCC phase further increases, and the strength of the alloy is further improved.

[0052] Fig.10 The cast AlCoCrFeNi obtained in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 From the XRD diffraction analysis of the eutectic high entropy alloy, it can be seen that the alloy is composed of FCC and BCC phases, indicating that changes in Si content will not cause changes in the crystal structure. However, as the Si content in the alloy increases, the tendency of FCC phase formation is less than the relatively stable BCC structure, and the FCC phase will gradually disappear, and the BCC phase will gradually become the main phase. In addition, due to the small radius of Si atoms, the BCC solid solution lattice shrinks by replacing larger atoms in the solid solution, the lattice constant decreases, and the BCC diffraction peak shifts to the right.

[0053] Fig.11 The cast AlCoCrFeNi obtained in Example 2 2.1 Si 0.15 DSC differential thermal analysis of eutectic high entropy alloy, the image shows two sets of endothermic / exothermic peaks.

[0054] Fig.12 The cast AlCoCrFeNi obtained in Example 2 2.1 Si 0.15 Eutectic high entropy alloy and matrix AlCoCrFeNi 2.1 The tensile engineering stress-strain curve of the eutectic high entropy alloy in the cast state shows that the alloy has achieved a synergistic improvement in strength and plasticity. 2.1 Si 0.15 The tensile strength and elongation of the eutectic high entropy alloy are 1111.7MPa and 19.5% respectively, and the Vickers hardness is 331HV.

[0055] Implementation Case 3 Based on Example 1, this example combines the thermomechanical treatment process (the alloys are abbreviated as CR-Si0.1-600, CR-Si0.1-700, CR-Si0.1-750, CR-Si0.1-800, CR-Si0.1-850, CR-Si0.1-900), so that the strength of the alloy is further improved without sacrificing plasticity.

[0056] In this embodiment, the subsequent thermomechanical treatment process steps are as follows: S1: Cold deformation: Cast AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy master alloy is cold rolled to reduce the thickness by 30%; S2: annealing treatment: the AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy is annealed at 1050°C for 5h; S3: cold deformation: the AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy is cold rolled to reduce the thickness by another 40%; S4: annealing treatment: the cold rolled AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy is annealed at 600°C-900°C for 30 minutes to obtain the eutectic high entropy alloy with further improved strength and plasticity.

[0057] Fig.14 The AlCoCrFeNi obtained in Example 3 after thermomechanical treatment 2.1 Si 0.1 The tensile engineering stress-strain curve of the eutectic high entropy alloy shows that the strength of the alloy is further improved without sacrificing plasticity after thermomechanical treatment. 2.1 Si 0.1 The tensile strength of the eutectic high entropy alloy is 2 times higher than that of the matrix.

[0058] Implementation Case 4 Based on Example 3, this example explores the effect of the second cold rolling amount on the mechanical properties of the alloy (the alloys are abbreviated as CR0%-Si0.1-800, CR10%-Si0.1-800, CR20%-Si0.1-800, CR30%-Si0.1-800, CR40%-Si0.1-800), so that the strength of the alloy is further improved.

[0059] In this embodiment, the subsequent thermomechanical treatment process steps are as follows: S1: Cold deformation: Cast AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy master alloy is cold rolled to reduce the thickness by 30%; S2: annealing treatment: the AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy is annealed at 1050°C for 5h; S3: cold deformation: the AlCoCrFeNi 2.1 Si 0.1The eutectic high entropy alloy is cold rolled to reduce the thickness by 0-40%; S4: annealing treatment: the cold rolled AlCoCrFeNi 2.1 Si 0.1 The eutectic high entropy alloy is annealed at 750°C-850°C for 30 minutes to obtain the eutectic high entropy alloy with further improved comprehensive mechanical properties.

[0060] Figure 15-17 The AlCoCrFeNi obtained in Example 4 after thermomechanical treatment 2.1 Si 0.1 From the tensile engineering stress-strain curve of the eutectic high entropy alloy, it can be found that the alloy has the best mechanical properties under the process of the second rolling amount of 30% and the second annealing temperature of 800℃.

[0061] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.

Claims

1. A Si-doped AlCoCrFeNi 2.1 Si x Eutectic high entropy alloy, characterized in that The general formula is AlCoCrFeNi 2.1 Si x , where 0≤x≤0.5, x is the molar percentage of the corresponding element.

2. Preparation of Si-doped AlCoCrFeNi as claimed in claim 1 2.1 Si x A method for synergistically improving the strength and plasticity of a eutectic high entropy alloy comprises the following steps: S1: Master alloy preparation: Al, Co, Cr, Fe, Ni and non-metallic Si raw materials are accurately weighed according to the molar percentage of eutectic high entropy alloy, and then AlCoCrFeNi is obtained through a casting process. 2.1 Si x Eutectic high entropy alloy master alloy; S2: First cold deformation: The AlCoCrFeNi obtained in step S1 is 2.1 Si x The eutectic high entropy alloy master alloy is cold rolled to reduce the total thickness by 30%; S3: First heat treatment: AlCoCrFeNi after cold rolling in step S2 2.1 Si x The eutectic high entropy alloy is annealed and water quenched; S4: Second cold deformation: AlCoCrFeNi after annealing in step S3 2.1 Si x The eutectic high entropy alloy is cold rolled to reduce the thickness again by 0-40%; S5: Second annealing treatment: The AlCoCrFeNi 2.1 Si x The eutectic high entropy alloy is annealed and water quenched to obtain the eutectic high entropy alloy with synergistically improved strength and plasticity.

3. The Si-doped AlCoCrFeNi according to claim 2 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: In step S1, the purity of metals Al, Co, Cr, Fe, and Ni is greater than or equal to 99.95%, and the purity of non-metal Si is greater than or equal to 99.999%.

4. The Si-doped AlCoCrFeNi according to claim 2 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: The casting process is arc melting under inert gas protection, including the following steps: evacuating the vacuum arc melting furnace to 1×10 -3 Pa, then inert gas is injected into the furnace and the alloy is melted.

5. After arcing, first melt the titanium ingot to absorb the residual oxygen in the furnace, and then put the weighed raw materials in S1 in order from low to high melting points. After the sample is melted and thoroughly cooled, turn it over and melt it repeatedly for more than 8 times to ensure the uniformity of the alloy ingot composition. After melting, the alloy ingot is obtained.

6. The Si-doped AlCoCrFeNi according to claim 4 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: The inert gas is argon, the arc melting current is 400-600A, and each melting time is not less than 3 minutes.

7. The Si-doped AlCoCrFeNi according to claim 2 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: The cold rolling process in step S2 and step S4 is a multi-pass cold rolling with non-fixed deformation. The deformation of the early single pass is maintained at about 5%, making full use of the plastic deformation of the material and reducing the length of the head and tail geometric waste. The deformation of the later single pass is not higher than 2%, which improves the sample quality and thickness accuracy.

8. The Si-doped AlCoCrFeNi according to claim 2 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: The annealing temperature in step S3 is 1000-1200°C.

9. The Si-doped AlCoCrFeNi according to claim 2 2.1 Si x A method for synergistically improving strength and plasticity of eutectic high entropy alloys, characterized in that: The annealing temperature in step S5 ranges from 600 to 900°C.

Citation Information

Patent Citations

  • Cold-rolled composite laser additive manufacturing process for gradient structure high-entropy alloy

    CN112222413A

  • Combined AlCoCrFeNi2.1 eutectic high-entropy alloy with ultrahigh strength and plasticity and preparation method thereof

    CN115491565A

  • High-temperature anti-oxidation high-entropy alloy material and preparation method thereof

    CN118516580A

  • High entropy alloy structure and a method of preparing the same

    US20200109467A1

  • Precipitation-hardened high-entropy alloy component design and preparation method based on diffusion multiple technology

    WO2023142863A1