A high surface quality high-speed steel composite roll and its preparation method

By adding boron (B) and nitrogen (Nb) elements to the outer layer of high-speed steel and combining this with optimized smelting and heat treatment processes, high-surface-quality high-speed steel composite rolls were prepared. This solved the problems of surface roughening and insufficient toughness of rolls during high-surface-quality rolling, achieving a balance between high wear resistance and impact toughness, and extending the service life of the rolls.

CN123102971APending Publication Date: 2026-11-17SINOSTEEL XINGTAI MACHINERY & MILL ROLL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611292969.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-speed steel rolls are prone to problems such as surface roughening, insufficient toughness, and increased roll wear during high surface quality rolling processes, making it difficult to simultaneously meet the requirements of high wear resistance and impact toughness.

Method used

High-temperature red hardness and impact toughness of high-speed steel were improved by adding boron to the outer layer of high-speed steel, and Nb was added to the core to refine the carbide morphology. Combined with optimized smelting and heat treatment processes, high-surface-quality high-speed steel composite rolls were prepared.

Benefits of technology

It significantly improves the impact toughness and high-temperature oxidation resistance of the rolls, enhances the ability to maintain roll surface roughness, extends roll service life, reduces roll consumption, and meets the requirements of high surface quality rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102971A_ABST
    Figure CN123102971A_ABST
Patent Text Reader

Abstract

This invention discloses a high-surface-quality high-speed steel composite roll and its preparation method, belonging to the field of roll manufacturing. The method includes: smelting outer and core molten steel separately in an intermediate frequency furnace, tapping the steel after it meets the required standards; heating the outer molten steel to 1600–1750℃ and holding for 30–50 minutes, then cooling to 1350–1450℃ and pouring it into a ladle; heating the core molten steel to 1500–1650℃ and holding for 10–20 minutes, adding 2%–4% spheroidizing agent to the bottom of the ladle before pouring; cooling for 120–240 hours before unpacking; rough machining of the blank leaving a radial allowance of 6–15 mm and an axial allowance of ≥10 mm; followed by high-temperature quenching and tempering heat treatment, and finishing to obtain the finished product. This invention, while ensuring wear resistance, adds boron (B) to improve red hardness and impact toughness, and adds nitrogen (Nb) to refine carbides, promoting coordinated and balanced wear on the roll surface, enhancing oxide film retention and anti-coarsening ability, thus meeting the requirements for high-surface-quality rolling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of roll manufacturing technology, and in particular to a high-surface-quality high-speed steel composite roll and its preparation method. Background Technology

[0002] Rolls are core components of steel rolling equipment, coming into direct contact with the high-temperature workpiece during rolling and enduring enormous rolling forces and thermal shock. High-speed steel composite rolls, due to their excellent wear resistance and red hardness of the outer layer, have been widely used in vertical rolls, roughing mill stands, and finishing mill stands in hot strip rolling lines. To meet the demands of increased capacity and product upgrades in the steel industry, the application of high-speed strip steel rolls across the entire production line is becoming increasingly urgent.

[0003] Currently, conventional high-nickel-chromium indefinite chilled cast iron rolls are still used in some rolling lines for the finishing mill stage and finished product stands due to their good resistance to thermal fatigue. However, with the rapid development of industries such as new energy vehicles, the requirements for plate surface quality are constantly increasing. When rolling plates with high surface requirements, the surface of conventional high-nickel-chromium rolls is prone to roughening, resulting in a rough surface of the hot-rolled plate. When used as cold-rolled base material, this produces surface defects similar to pitting, seriously affecting the surface quality of the finished product. If conventional high-speed steel rolls are directly applied to the finishing mill stage, their insufficient toughness makes them prone to abnormal wear on the roll surface when subjected to sudden accidents such as tailing and sticking, resulting in a significant increase in roll wear and a substantial rise in rolling costs.

[0004] For rolling mills with high surface quality requirements, how to effectively improve the impact toughness and high-temperature oxidation resistance of high-speed steel while maintaining its excellent wear resistance, and how to form a stable and controllable manufacturing process, are all technical challenges that urgently need to be solved. Summary of the Invention

[0005] The technical problem to be solved by this invention is to provide a high-surface-quality high-speed steel composite roll and its preparation method, which is particularly suitable for the finishing mill stand of high-surface-quality plates. This invention, while ensuring the excellent wear resistance of the outer layer of high-speed steel, enhances the high-temperature red hardness and impact toughness of the matrix by adding boron (B), thereby improving its resistance to accidents and oxidation. Furthermore, by adding nitrogen (Nb), the morphology of the carbides is refined, promoting coordinated wear between the matrix and carbides, ensuring good oxide film retention and roll surface anti-roughening ability during finishing mill applications, thus meeting the requirements for high-surface-quality rolling.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Step A: Use an intermediate frequency furnace to smelt the outer layer of molten steel and the core steel separately. Control the smelting temperature of the outer layer of molten steel to be 1500-1650℃ and the smelting temperature of the core steel to be 1400-1580℃. After the chemical composition of the outer layer of molten steel and the core steel reaches the design target value, tap them out separately for later use. Step B: Continue heating the outer layer molten steel obtained in Step A to 1600-1750℃, hold for 30-50 minutes, and then remove it from the furnace. When the temperature of the outer layer molten steel drops to 1350-1450℃, pour it using a ladle with a turning ladle. Continue heating the core molten steel obtained in Step A to 1500-1650℃, hold for 10-20 minutes, and then remove it from the furnace. When removing it from the furnace, add 2%-4% of the total mass of the core molten steel to the bottom of the core ladle, and then pour the core. Step C: After casting is completed, the roll blank is opened after cooling for 120-240 hours. The roll blank is then rough-machined. During rough machining, a radial allowance of 6-15mm is left on one side of the roll body, and a axial allowance of ≥10mm is left on both ends. Step D: The rough-machined rolls undergo heat treatment, which involves high-temperature quenching followed by high-temperature tempering. Step E: After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained.

[0007] A further improvement of the technical solution of the present invention is that, in steps A and B, the chemical composition of the outer layer of molten steel, by mass percentage, is: C 1.0-2.5%, Si 0.3-1.5%, Mn 0.3-1.5%, P≤0.15%, S≤0.1%, Cr 3.0-17.0%, Ni 0.3-1.5%, Mo 0.5-7.5%, V 0.5-7.5%, W 0.5-1.5%, Nb≤1.0%, B 0.3-0.6%, with the balance being Fe and unavoidable impurities; The chemical composition of the core steel, by mass percentage, is: C 2.3-3.8%, Si 1.2-3.5%, Mn 0.3-1.2%, P≤0.18%, S≤0.16%, Cr≤0.5%, Ni≤2.0%, Mo 0.1-0.5%, and the total amount of W+V+Nb ≤0.8%, with the balance being Fe and unavoidable impurities.

[0008] A further improvement of the technical solution of the present invention is that the chemical composition of the outer layer of molten steel also satisfies the following relationship: Cr equivalent (Cr+1.05×Mo+3.33×V+0.55×W+2.17×Nb)≤30%, wherein each element symbol represents its mass percentage value in the outer layer of molten steel.

[0009] A further improvement of the technical solution of the present invention is that: in step A, the amount of scrap steel added to the furnace charge used for smelting the outer layer of molten steel does not exceed 30% of the total mass of the outer layer furnace charge by mass percentage; the furnace charge used for smelting the core molten steel and the remaining part of the outer layer furnace charge other than the scrap steel can be made of alloy material or recycled waste.

[0010] A further improvement of the technical solution of the present invention is that: in step B, the core molten steel is poured using a combination of centrifugal pouring and static pouring. Specifically, within 1 to 2 minutes after the outer layer of molten steel is poured, 15% to 25% of the total mass of the core molten steel is poured using centrifugal pouring; when the cavity temperature drops to 960 to 1090°C after pouring, the mold is closed, and then the remaining core molten steel is poured using static pouring.

[0011] A further improvement of the technical solution of the present invention is that: in step C, the axial allowance is adjusted according to the total length of the roll blank and the effective furnace chamber size of the heat treatment furnace, and the allowance at both ends of the axial direction is ≥10mm, and can be increased accordingly according to the furnace chamber length.

[0012] A further improvement to the technical solution of the present invention is that the heat treatment process of high-temperature quenching and high-temperature tempering in step D specifically includes the following steps: (1) Temperature uniform treatment: Heat the rough-machined roll to 600-700℃ and keep it at that temperature for 15-50 hours to make the overall temperature of the roll uniform. (2) High temperature heating: The temperature of the uniformly heated roll is raised to the furnace temperature of 1000-1180℃, and the holding time after the furnace temperature is reached is 150-240 min; (3) Quenching and cooling: The air cooling method is adopted, the air pressure is controlled at 0.2-0.45MPa, the air cooling time is 80-200min, and then the roll body is air cooled until the temperature drops to 300-500℃; (4) Tempering treatment: Temper the cooled rolls at a temperature of 500-550℃ and a holding time of 30-50h.

[0013] A high-surface-quality high-speed steel composite roll is composed of an outer layer and a core, wherein the outer layer is made of high-speed steel and the core is made of ductile iron.

[0014] The technological advancements achieved by this invention due to the adoption of the above technical solutions are as follows: 1. This invention addresses the technical challenges of tailing, steel sticking, and abnormal high roll surface wear that are prone to occur in the high surface finish rolling stage and finished stand rolling process. It conducts a systematic study from multiple dimensions, including material composition design, casting process, heat treatment process, and core inoculation treatment, and proposes a high surface quality high-speed steel composite roll and its preparation method.

[0015] 2. This invention is based on the mechanism of action of various alloying elements in the high-speed steel matrix for high-surface rolling, and specifically optimizes the composition of the outer layer material. By adding boron (B) to strengthen the matrix, the high-temperature red hardness and impact toughness of the outer layer of high-speed steel are effectively improved while ensuring good wear resistance. At the same time, adding an appropriate amount of nitrogen (Nb) can refine the carbide morphology and promote coordinated wear between the matrix and carbides, thereby significantly improving the ability to retain roll surface roughness and meeting the requirements of high surface quality rolling.

[0016] 3. This invention adopts a composite manufacturing method. The outer layer is made of high wear-resistant high-speed steel, and the core is made of high-toughness ductile iron. Through a reasonable core spheroidization inoculation process, the roll has both the excellent wear resistance of the outer layer and the good bending roll deformation resistance and impact toughness of the core, which effectively extends the service life of the roll and reduces roll consumption.

[0017] 4. This invention optimizes the composite casting process that combines centrifugal casting and static casting, as well as the heat treatment process of high-temperature quenching and high-temperature tempering, so that the metallurgical quality of the interface between the outer layer and the core is good, the microstructure is highly uniform, and the residual stress is reasonably distributed, thereby further ensuring the overall performance and surface quality of the roll.

[0018] 5. This invention optimizes the fluidity of molten steel by reasonably limiting the Cr equivalent value of each alloying element in high-speed steel, namely (Cr+1.05×Mo+3.33×V+0.55×W+2.17×Nb)≤30%, which promotes the full floating of fine inclusions in the working layer, thereby significantly improving the cleanliness of the working layer and ensuring its excellent ability to maintain high surface quality. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Figure 1 This is a 500x metallographic image of the outer layer of the high surface quality high-speed steel composite roll obtained in Example 1 of this invention; Figure 2 This is a 500x metallographic image of the outer layer of a conventional high-speed steel roll obtained as a comparative example of the present invention. Detailed Implementation

[0020] It should be noted that the terms "comprising" and "having" and any variations thereof in the specification, claims and accompanying drawings of this invention are intended to cover non-exclusive inclusion. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such process, method, product or device.

[0021] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments: Example 1

[0022] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0023] The chemical composition of the outer layer of molten steel, by mass percentage, is: C 1.60%, Si 0.30%, Mn 0.3%, P 0.10%, S 0.10%, Cr 3.0%, Ni 0.9%, Mo 0.5%, V 7.5%, W 0.5%, Nb 0.5%, B 0.35%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 2.95%, Si 1.41%, Mn 1.2%, P 0.08%, S 0.09%, Cr 0.18%, Ni 0.38%, Mo 0.39%, W+V+Nb=0.08%, with the balance being Fe and unavoidable impurities.

[0024] The outer layer of molten steel is melted at 1565℃. After the composition meets the standards, the temperature is raised to 1675℃ before being centrifuged and cast. The core steel is melted at 1490℃. Before the core molten iron is tapped from the furnace, 2% spheroidizing agent is added to the bottom of the ladle. 1.5 minutes after the outer layer of molten steel is cast, 18% of the total mass of the core steel is first poured using centrifugal casting at a temperature of 1395℃. After the cavity temperature drops to a suitable range, the mold is closed, and the remaining core steel is then poured using static casting at a temperature of 1365℃.

[0025] After casting, the roll blank is unpacked after 115 hours of cooling. The roll blank is then rough-machined, leaving a 35mm allowance at each end of the axial direction and a 9mm allowance in the radial diameter direction.

[0026] After rough machining, only the roll body is heat-treated: First, the entire roll is held at 650℃ for 15 hours. After the holding period, the roll body is heated to 1050℃ using differential temperature heat treatment and held for 185 minutes for high-temperature heating. Then, it is cooled by blowing air for 115 minutes and then air-cooled. When the roll body temperature drops to 400℃, it is put into the furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 40 hours, and the tempering is performed twice.

[0027] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained.

[0028] Metallographic observation was performed on samples of the outer layer of the prepared roll. The microstructure under a 500x microscope is shown below. Figure 1 As shown. By Figure 1 It can be seen that the carbides are in a diffuse and uniform distribution state, and the matrix structure consists of martensite, retained austenite and carbides. Example 2

[0029] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0030] The chemical composition of the outer layer of molten steel, by mass percentage, is: C 1.70%, Si 0.55%, Mn 0.95%, P 0.08%, S 0.08%, Cr 4.3%, Ni 0.3%, Mo 7.5%, V 2.9%, W 0.9%, Nb 0.5%, B 0.30%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 2.98%, Si 1.43%, Mn 0.55%, P 0.03%, S 0.16%, Cr 0.15%, Ni 0.35%, Mo 0.33%, W+V+Nb=0.05%, with the balance being Fe and unavoidable impurities.

[0031] The outer layer of molten steel is melted at 1555℃. After the composition meets the standards, the temperature is raised to 1676℃ before being centrifuged and cast. The core steel is melted at 1496℃. Before the core molten iron is tapped from the furnace, 3% spheroidizing agent is added to the bottom of the ladle. 1.3 minutes after the outer layer of molten steel is cast, 19% of the total mass of the core steel is first poured using centrifugal casting at a temperature of 1396℃. After the cavity temperature drops to a suitable range, the mold is closed, and the remaining core steel is then poured using static casting at a temperature of 1363℃.

[0032] After casting, the roll blank is unpacked after 113 hours of cooling. The roll blank is then rough-machined, leaving a 10mm allowance at each end of the axial direction and a 10mm allowance in the radial diameter direction.

[0033] After rough machining, only the roll body is heat-treated: First, the entire roll is heated to 600℃ and held for 30 hours. After the holding period, the roll body is heated to 1055℃ using differential heating and held for 189 minutes for high-temperature heating. Then, it is cooled by blowing air for 116 minutes and then air-cooled. When the roll body temperature drops to 410℃, it is placed in a furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 43 hours, and the tempering is performed twice.

[0034] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained. Example 3

[0035] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0036] The chemical composition of the outer layer of molten steel, by mass percentage, is as follows: C 1.00%, Si 0.56%, Mn 1.5%, P 0.05%, S 0.03%, Cr 4.5%, Ni 0.8%, Mo 0.6%, V 2.9%, W 1.5%, Nb 0.32%, B 0.4%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 2.30%, Si 3.50%, Mn 0.30%, P 0.18%, S 0.05%, Cr 0.18%, Ni 0.39%, Mo 0.37%, W+V+Nb=0.06%, with the balance being Fe and unavoidable impurities.

[0037] The outer layer of molten steel is melted at 1558℃. After the composition meets the standards, the temperature is raised to 1679℃ before being tapped out of the furnace and centrifugally cast. The core steel is melted at 1498℃. Before the core steel is tapped out of the furnace, 4% spheroidizing agent is added to the bottom of the ladle. 1.6 minutes after the outer layer of molten steel is poured, 18% of the total mass of the core steel is first poured using centrifugal casting at a temperature of 1398℃. After the cavity temperature drops to a suitable range, the mold is closed, and the remaining core steel is then poured using static casting at a temperature of 1361℃.

[0038] After casting, the roll blank is unpacked after 135 hours of cooling. The roll blank is then rough-machined, leaving a 39mm allowance at each end of the axial direction and an 11mm allowance in the radial diameter direction.

[0039] After rough machining, only the roll body is heat-treated: First, the entire roll is heated to 600℃ and held for 50 hours. After the holding period, the roll body is heated to 1059℃ using differential heating and held for 190 minutes for high-temperature heating. Then, it is cooled by blowing air for 135 minutes and then air-cooled. When the roll body temperature drops to 490℃, it is placed in a furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 50 hours, and the tempering is performed 3 times.

[0040] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained. Example 4

[0041] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0042] The chemical composition of the outer layer of molten steel, by mass percentage, is: C 1.36%, Si 0.35%, Mn 0.82%, P 0.09%, S 0.05%, Cr 5.1%, Ni 0.7%, Mo 3.1%, V 3.4%, W 0.5%, Nb 1.00%, B 0.6%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 3.13%, Si 1.69%, Mn 0.88%, P 0.09%, S 0.09%, Cr 0.21%, Ni 0.59%, Mo 0.50%, W+V+Nb=0.08%, with the balance being Fe and unavoidable impurities.

[0043] The outer layer of molten steel was melted at 1653℃. After the composition met the standards, the temperature was raised to 1449℃ before being tapped out of the furnace and centrifugally cast. The core steel was melted at 1563℃. Before the core steel was tapped out of the furnace, 3.5% spheroidizing agent was added to the bottom of the ladle. 1.9 minutes after the outer layer of molten steel was poured, 19% of the total mass of the core steel was first poured using centrifugal casting at a temperature of 1399℃. After the cavity temperature dropped to a suitable range, the mold was closed, and the remaining core steel was then poured using static casting at a temperature of 1365℃.

[0044] After casting, the roll blank is unpacked after 139 hours of cooling. The roll blank is then rough-machined, leaving a 45mm allowance at each end of the axial direction and an 8mm allowance in the radial diameter direction.

[0045] After rough machining, only the roll body is heat-treated: First, the entire roll is heated to 650℃ and held for 40 hours. After the holding period, the roll body is heated to 1080℃ using differential heating and held for 210 minutes for high-temperature heating. Then, it is cooled by blowing air for 145 minutes and then air-cooled. When the roll body temperature drops to 510℃, it is placed in a furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 40 hours, and the tempering is performed 4 times.

[0046] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained. Example 5

[0047] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0048] The chemical composition of the outer layer of molten steel, by mass percentage, is: C 1.55%, Si 0.65%, Mn 0.76%, P 0.03%, S 0.03%, Cr 3.9%, Ni 1.1%, Mo 4.5%, V 3.0%, W 0.9%, Nb 0.36%, B 0.4%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 3.20%, Si 1.58%, Mn 0.79%, P 0.07%, S 0.07%, Cr 0.31%, Ni 0.91%, Mo 0.30%, W+V+Nb=0.06%, with the balance being Fe and unavoidable impurities.

[0049] The outer layer of molten steel is melted at 1658℃. After the composition meets the standards, the temperature is raised to 1659℃ before being removed from the furnace and centrifugally cast. The core steel is melted at 1579℃. 1.8 minutes after the outer layer of molten steel is cast, 20% of the total mass of the core steel is first centrifugally cast at a temperature of 1385℃. After the cavity temperature drops to a suitable range, the mold is closed, and the remaining core steel is then statically cast at a temperature of 1370℃.

[0050] After casting, the roll blank is unpacked after 140 hours of cooling. The roll blank is then rough-machined, leaving a 41mm allowance at each end of the axial direction and a 9mm allowance in the radial diameter direction.

[0051] After rough machining, only the roll body is heat-treated: First, the entire roll is heated to 650℃ and held for 35 hours. After the holding period, the roll body is heated to 1070℃ using differential heating and held for 220 minutes for high-temperature heating. Then, it is cooled by blowing air for 146 minutes and then air-cooled. When the roll body temperature drops to 500℃, it is put into the furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 35 hours, and the tempering is performed 3 times.

[0052] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained. Example 6

[0053] A method for preparing a high-surface-quality high-speed steel composite roll includes the following steps: Using scrap steel chips, forged steel scrap, ferromolybdenum, ferrovanadium, ferrotungsten, fercobalt, and electrode powder as raw materials, the outer layer of molten steel and the core of molten steel are smelted separately in a medium-frequency furnace.

[0054] The chemical composition of the outer layer of molten steel, by mass percentage, is: C 2.5%, Si 1.5%, Mn 0.86%, P 0.15%, S 0.04%, Cr 17.0%, Ni 1.5%, Mo 0.5%, V 0.5%, W 0.8%, Nb 0.25%, B 0.3%, with the balance being Fe and unavoidable impurities; The chemical composition of the molten iron in the core, by mass percentage, is: C 3.80%, Si 1.20%, Mn 0.89%, P 0.08%, S 0.08%, Cr 0.50%, Ni 2.0%, Mo 0.40%, W+V+Nb=0.05%, with the balance being Fe and unavoidable impurities.

[0055] The outer layer of molten steel is melted at 1668℃. After the composition meets the standards, the temperature is raised to 1456℃ before being tapped out of the furnace and centrifugally cast. The core steel is melted at 1589℃. Before the core steel is tapped out of the furnace, 3.9% spheroidizing agent is added to the bottom of the ladle. 1.7 minutes after the outer layer of molten steel is poured, 15% of the total mass of the core steel is first poured using centrifugal casting at a temperature of 1395℃. After the cavity temperature drops to a suitable range, the mold is closed, and the remaining core steel is then poured using static casting at a temperature of 1380℃.

[0056] After casting, the roll blank is unpacked after 130 hours of cooling. The roll blank is then rough-machined, leaving a 40mm allowance at each end of the axial direction and an 8mm allowance in the radial diameter direction.

[0057] After rough machining, only the roll body is heat-treated: First, the entire roll is heated to 680℃ and held for 25 hours. After the holding period, the roll body is heated to 1050℃ using differential heating and held for 200 minutes for high-temperature heating. Then, it is cooled by blowing air for 130 minutes and then air-cooled. When the roll body temperature drops to 480℃, it is placed in a furnace for tempering treatment. The tempering temperature is 500-550℃, the holding time is 36 hours, and the tempering is performed 4 times.

[0058] After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained.

[0059] Compare with Example 1 The conventional high-speed steel roll preparation method was adopted, meaning that Nb and B elements were not added to the chemical composition of the outer layer of molten steel. The amounts of other elements added, as well as the process steps and parameters, were the same as in Example 1. Metallographic observation was performed on samples of the outer layer of the prepared roll. The microstructure under a 500x microscope is shown below. Figure 2 As shown.

[0060] Compare with Example 2 Based on Example 1, the Cr content was further increased to 5.0 and the Mo content to 2.0, so that the Cr equivalent (Cr+1.05×Mo+3.33×V+0.55×W+2.17×Nb)=31.4%. The amount of each other element added and the process steps and parameters of the preparation method were the same as those in Example 1.

[0061] The finished roll products obtained from Examples 1 to 6 and the control example were subjected to tensile mechanical property testing. The performance testing was carried out in accordance with the national standard GB / T 228.1-2021 "Metallic materials, tensile testing - Part 1: Test method at room temperature". The test results are shown in Table 1.

[0062] Table 1. Product performance test results of Examples 1-6 and control examples

[0063] As shown in Table 1, the roll products prepared in Examples 1-6 of this invention are significantly superior to the control examples in many key performance indicators. Regarding thermal shock resistance, the impact crack depth of Examples 1-6 is 200-220 μm, while that of Control Examples 1 and 2 is as high as 1005 μm and 563 μm, respectively. This indicates that the present invention effectively strengthens the matrix structure by adding element B, significantly improving the thermal shock resistance of the high-speed steel composite roll, and exhibiting a significant crack suppression effect. Regarding oxidation resistance, the oxidation weight gain of Examples 1-6 is only 0.0122-0.0131 mg, while that of Control Examples 1 and 2 is 0.0555 mg and 0.0296 mg, respectively. This demonstrates that the high-temperature oxidation resistance of the present invention is significantly superior to that of conventional high-speed steel materials, reducing oxidation weight gain by approximately 50%-75%. Regarding the size of inclusions in the working layer, the inclusion sizes in Examples 1-6 were 13-16 μm, with a uniform size distribution and narrow fluctuation range. In contrast, the inclusion sizes in Control Examples 1 and 2 were 19 μm and 158 μm, respectively. The inclusion size in Control Example 2, in particular, far exceeded that of the examples, indicating that the present invention, by rationally controlling the Cr equivalent value of each alloying element in the high-speed steel, ensures good fluidity of the molten steel, which is conducive to the full floating of fine inclusions in the working layer, thereby significantly improving the cleanliness of the working layer and ensuring that the high-speed steel working layer has excellent high surface quality retention capabilities. Considering the above three performance indicators, when practically applied to high-surface rolling, the present invention can form a dense and stable oxide film on the roll surface, while also possessing excellent resistance to hot cracking and structural purity, thereby effectively extending the service life of the rolls and improving the surface quality of the strip steel, fully meeting the requirements of high-intensity continuous rolling conditions.

[0064] In summary, the high-surface-quality high-speed steel composite roll developed in this invention has significantly better oxidation resistance and thermal shock resistance than conventional high-speed steel rolls, and its roll surface has outstanding anti-roughening ability, effectively solving the technical problem of easy roughening of the roll surface of conventional high-nickel-chromium infinite chilled cast iron rolls when rolling high-surface-quality plates.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a high-surface-quality high-speed steel composite roll, characterized in that, Includes the following steps: Step A: Use an intermediate frequency furnace to smelt the outer layer of molten steel and the core steel separately. Control the smelting temperature of the outer layer of molten steel to be 1500-1650℃ and the smelting temperature of the core steel to be 1400-1580℃. After the chemical composition of the outer layer of molten steel and the core steel reaches the design target value, tap them out separately for later use. Step B: Continue heating the outer layer molten steel obtained in Step A to 1600-1750℃, hold for 30-50 minutes, and then remove it from the furnace. When the temperature of the outer layer molten steel drops to 1350-1450℃, pour it using a ladle with a turning ladle. Continue heating the core molten steel obtained in Step A to 1500-1650℃, hold for 10-20 minutes, and then remove it from the furnace. When removing it from the furnace, add 2%-4% of the total mass of the core molten steel to the bottom of the core ladle, and then pour the core. Step C: After casting is completed, the roll blank is opened after cooling for 120-240 hours. The roll blank is then rough-machined. During rough machining, a radial allowance of 6-15mm is left on one side of the roll body, and a axial allowance of ≥10mm is left on both ends. Step D: The rough-machined rolls undergo heat treatment, which involves high-temperature quenching followed by high-temperature tempering. Step E: After heat treatment, the rolls are precision machined and, after passing inspection, the finished rolls are obtained.

2. The method for preparing a high surface quality high-speed steel composite roll according to claim 1, characterized in that, In steps A and B, the chemical composition of the outer layer of molten steel, by mass percentage, is as follows: C 1.0–2.5%, Si 0.3–1.5%, Mn 0.3–1.5%, P≤0.15%, S≤0.1%, Cr 3.0–17.0%, Ni 0.3–4.5%, Mo 0.5–7.5%, V 0.5–7.5%, W 0.5–1.5%, Nb≤1.0%, B 0.3–0.6%, with the balance being Fe and unavoidable impurities; The chemical composition of the core steel, by mass percentage, is: C 2.3-3.8%, Si 1.2-3.5%, Mn 0.3-1.2%, P≤0.18%, S≤0.16%, Cr≤0.5%, Ni≤2.0%, Mo 0.1-0.5%, and the total amount of W+V+Nb ≤0.8%, with the balance being Fe and unavoidable impurities.

3. The method for preparing a high surface quality high-speed steel composite roll according to claim 2, characterized in that: The chemical composition of the outer layer of molten steel also satisfies the following relationship: (Cr+1.05×Mo+3.33×V+0.55×W+2.17×Nb)≤30%, where each element symbol represents its mass percentage value in the outer layer of molten steel.

4. The method for preparing a high surface quality high-speed steel composite roll according to claim 1, characterized in that, In step A, the amount of scrap steel added to the furnace charge used for smelting the outer layer of molten steel shall not exceed 30% of the total mass of the outer layer furnace charge by mass percentage; the furnace charge used for smelting the core molten steel and the remaining part of the outer layer furnace charge other than the scrap steel may be made of alloy material or recycled scrap.

5. The method for preparing a high surface quality high-speed steel composite roll according to claim 1, characterized in that, In step B, the core molten steel is poured using a combination of centrifugal pouring and static pouring. Specifically, within 1 to 2 minutes after the outer layer of molten steel is poured, 15% to 25% of the total mass of the core molten steel is poured using centrifugal pouring. After the cavity temperature drops to 960 to 1090°C after pouring, the mold is closed, and then the remaining core molten steel is poured using static pouring.

6. The method for preparing a high surface quality high-speed steel composite roll according to claim 1, characterized in that, In step C, the axial allowance is adjusted according to the total length of the roll blank and the effective furnace chamber size of the heat treatment furnace. The allowance at both ends of the axial direction is ≥30mm, and is increased accordingly according to the furnace chamber length.

7. The method for preparing a high surface quality high-speed steel composite roll according to claim 1, characterized in that, The heat treatment process described in step D, which involves high-temperature quenching followed by high-temperature tempering, specifically includes the following steps: (1) Temperature uniform treatment: Heat the rough-machined roll to 600-700℃ and keep it at that temperature for 15-50 hours to make the overall temperature of the roll uniform. (2) High temperature heating: The temperature of the uniformly heated roll is raised to the furnace temperature of 1000-1180℃, and the holding time after the furnace temperature is reached is 150-240 min; (3) Quenching and cooling: The air cooling method is adopted, the air pressure is controlled at 0.2-0.45MPa, the air cooling time is 80-200min, and then the roll body is air cooled until the temperature drops to 300-500℃; (4) Tempering treatment: Temper the cooled rolls at a temperature of 500-550℃ and a holding time of 30-50h.

8. A high-surface-quality high-speed steel composite roll, characterized in that, The roll is composed of an outer layer and a core, wherein the outer layer is made of high-speed steel and the core is made of ductile iron. The chemical composition of the outer layer and the core is as defined in claim 2. The roll is prepared by the preparation method as described in any one of claims 1 to 7.