A wear-resistant and corrosion-resistant high-entropy alloy composite material, its preparation method and application

By intercalating FeCoCrNiMo layered powder with nanolayered materials and performing spark plasma sintering, a dense and stable layered structure is formed, which solves the problems of interfacial compatibility and uneven dispersion of high-entropy alloy composite materials in abrasive environments, achieving excellent wear and corrosion resistance, and is suitable for harsh working conditions such as marine and petrochemical industries.

CN123102983APending Publication Date: 2026-11-17XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611484320.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-entropy alloy composite materials exhibit poor interfacial compatibility under synergistic abrasion environments. The nanolayered materials are unevenly dispersed and cannot form a stable and regular stacked structure. Corrosive media can easily penetrate, and surface peeling is prone to occur during friction and wear, making it impossible to effectively block the synergistic damage path of corrosion and wear.

Method used

FeCoCrNiMo layered powder and various types of nano-layered materials are used to increase the intercalation contact area. Uniform dispersion is achieved by combining liquid phase mixing and vacuum filtration processes. A dense and stable stacked structure is formed by spark plasma sintering.

Benefits of technology

It achieves comprehensive performance enhancement of high-entropy alloy composite materials under wear and corrosion coupled conditions, significantly improving wear resistance and corrosion resistance, and is suitable for harsh working conditions such as marine and petrochemical industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102983A_ABST
    Figure CN123102983A_ABST
Patent Text Reader

Abstract

This application belongs to the technical field of high-entropy alloy composite materials, specifically a wear-resistant and corrosion-resistant high-entropy alloy composite material, its preparation method, and its application. The high-entropy alloy composite material comprises a FeCoCrNiMo high-entropy alloy lamellar matrix and a nanolayered functional phase. It uses FeCoCrNiMo high-entropy alloy lamellar powder and nanolayered powder as raw materials, and combines liquid-phase ultrasonic dispersion, vortex oscillation, filtration, and vacuum drying to uniformly mix the raw materials before spark plasma sintering. The high-entropy alloy composite material has a dense and uniform internal structure, exhibiting excellent wear resistance and corrosion resistance, achieving synergistic enhancement of comprehensive performance under corrosive and wear conditions. The preparation process is simple and standardized, enabling large-scale mass production of multilayered composite materials with different types and doping ratios, suitable for various harsh working conditions involving wear and corrosion, such as marine engineering, petrochemicals, and energy equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of high-entropy alloy composite material technology, specifically a wear-resistant and corrosion-resistant high-entropy alloy composite material, its preparation method, and its application. Background Technology

[0002] High-entropy alloys, as novel multi-component metallic materials, particularly FeCoCrNiMo series high-entropy alloys, possess fundamental application potential in wear-coupled conditions involving corrosive media due to the solid solution strengthening effect of Mo. To enhance the comprehensive wear and corrosion resistance of high-entropy alloys under synergistic abrasion environments, nano-layered materials such as MoS2, graphene, h-BN, black phosphorus, MXene, and layered silicates are often introduced for composite modification. However, in existing preparation techniques, the nano-layered materials exhibit poor interfacial compatibility and uneven dispersion with the spherical high-entropy alloy matrix, making it difficult to form a stable and regular stacked composite structure. Corrosive media easily penetrate rapidly along interfacial defects, leading to surface peeling and groove abrasion during friction and wear, failing to effectively block the synergistic destructive path of corrosion and wear.

[0003] Powder metallurgy is a common method for preparing high-entropy alloy composite modified materials. High-energy ball milling combined with spark plasma sintering can improve the bonding of powder interfaces. However, existing studies mostly focus on optimizing single corrosion resistance or single wear resistance properties, without designing a stacked structure matching system for wear and corrosion coupled conditions. Moreover, the intercalation mechanism of various types of nanolayered materials with lamellar high-entropy matrices is unclear, and the corrosion and wear transmission path cannot be modified through structural regulation, which limits the engineering application of such composite materials in harsh working conditions such as marine and petrochemical industries where wear and corrosion coexist. Summary of the Invention

[0004] To address the aforementioned issues, this application provides a wear-resistant and corrosion-resistant high-entropy alloy composite material, its preparation method, and its application. By employing FeCoCrNiMo layered powder, the intercalation and contact area between the powder and various types of nanolayered materials is increased. Combined with liquid-phase mixing and vacuum filtration processes, the nanolayered materials are uniformly dispersed. Then, a high-entropy alloy composite material with a dense and stable layered structure is constructed through sintering.

[0005] According to a first aspect of this application, this application provides a wear-resistant and corrosion-resistant high-entropy alloy composite material, the high-entropy alloy composite material comprising a FeCoCrNiMo high-entropy alloy sheet matrix and a nano-layered functional phase, the high-entropy alloy composite material comprising, by volume percentage, 85%~90% FCC phase, 2%~7% BCC phase and 3%~8% Laves phase.

[0006] In the aforementioned high-entropy alloy composite material, a densely intercalated and stable layered structure is formed through the synergistic intercalation of nanolayered functional phases with the FeCoCrNiMo high-entropy alloy lamellar matrix. The microstructure is dominated by the FCC phase, containing small amounts of BCC and Laves phases. The formation mechanisms of each phase are as follows: FCC phase: The four main elements Fe, Co, Cr and Ni are all face-centered cubic structures with similar atomic radii. Under the action of high entropy effect, they can form infinitely miscible FCC-type substitutional solid solutions, which constitute the continuous matrix phase of the material and provide a good foundation for the material's plasticity and toughness. The spark plasma sintering method used in this application has the characteristics of rapid heating and short-time holding, which can effectively inhibit the growth of matrix grains and maintain the fine-grain strengthening effect of the FCC phase.

[0007] BCC phase: Mo has a significantly larger atomic radius than Fe, Co, Cr, and Ni, and its solid solubility in the FCC matrix is ​​limited. Through the mechanical alloying effect of high-energy ball milling and the atomic diffusion during sintering, a body-centered cubic solid solution phase will be formed in the locally Mo-rich region, which will improve the hardness and strength of the material through solid solution strengthening.

[0008] Laves phase: The atomic radius ratio of Mo to elements such as Fe and Co is about 1.2 to 1.3, which satisfies the size factor formation conditions of the Laves phase. During the sintering and holding process, Mo-rich Laves-type intermetallic compounds (mainly Fe2Mo and Co2Mo types) will precipitate and be dispersed in the matrix. They can further hinder dislocation movement, strengthen grain boundaries, and improve the corrosion resistance of the material.

[0009] The aforementioned multiphase synergistic structure can effectively modify the corrosion and wear path, and directionally improve the material's resistance to wear and corrosion synergy, making it suitable for harsh working conditions under the combined effects of wear and corrosion.

[0010] According to a second aspect of this application, this application provides a method for preparing a wear-resistant and corrosion-resistant high-entropy alloy composite material, comprising the following steps: S1. Obtain FeCoCrNiMo high-entropy alloy sheet-like powder and nano-layered powder, and ultrasonically disperse the nano-layered powder in a liquid medium to obtain a dispersion. S2. The dispersion is dropped into the FeCoCrNiMo high-entropy alloy sheet-like powder, and slurry is prepared by vortex oscillation. After filtration and vacuum drying, high-entropy alloy composite powder is obtained. S3. The high-entropy alloy composite powder is loaded into the mold in batches and layer by layer, and then subjected to spark plasma sintering to obtain the high-entropy alloy composite material.

[0011] In the above technical solution, the use of FeCoCrNiMo high-entropy alloy layered powder effectively increases the physical interlocking and interfacial contact area between the powder and the nanolayered powder. Combined with an integrated process of liquid-phase ultrasonic dispersion, vortex oscillation, filtration, and vacuum drying, compared to ordinary atmospheric pressure filtration which relies on gravity, has a slow filtration rate, and is prone to sedimentation and stratification due to particle density differences, vacuum filtration, driven by negative pressure, achieves rapid solid-liquid separation. This significantly shortens the filtration time, prevents sedimentation and segregation of the nanolayered powder and the high-entropy alloy layered powder due to density differences, and ensures uniform composition of the two phases in the filter cake. Furthermore, it simultaneously removes some solvent during filtration, reducing particle re-agglomeration caused by solvent migration in the subsequent drying stage and maintaining a uniform liquid-phase mixture. This integrated process enables the uniform dispersion of various types of nanolayered powders in the high-entropy alloy layered matrix. The resulting high-entropy alloy composite material has a dense and uniform internal structure, free from obvious interfacial defects, pores, and microcracks, and can construct a stable, densely layered composite structure with strong interfacial bonding. This layered structure relies on the interweaving of nano-layered functional phases and high-entropy alloy sheet matrix to effectively block the penetration and diffusion of corrosive media into the material interior along the interface channels, and significantly inhibit surface plowing, planing scratches, and surface material peeling failure during friction service. It precisely modifies and blocks the destructive path of the synergistic effect of corrosion and wear at the microstructural level, enabling the material to have both excellent wear resistance and corrosion resistance, and achieving comprehensive performance enhancement under corrosive and wear conditions. Finally, the high-entropy alloy composite powder is arranged in a regular manner along the mold axis by loading it in batches and layer by layer and pressing it lightly and leveling it step by step. This loading method allows the lamellar composite powder to form an approximately parallel orientation arrangement in the mold in advance. Combined with the axial pressure induction during the subsequent sintering process, it can promote the directional stacking and interfacial bonding of the lamellar powder along the direction perpendicular to the pressure direction, and finally form a continuous, dense, and regular alternating layered structure inside the block. This structure can significantly extend the penetration and diffusion path of corrosive media, while hindering the longitudinal propagation of cracks and surface peeling during friction and wear, blocking the synergistic failure path of corrosion and wear from the microstructural level.

[0012] Furthermore, in step S1, the mass percentage of the FeCoCrNiMo high-entropy alloy sheet-like powder to the nano-layered powder is (85~95):(5~15).

[0013] Furthermore, in step S1, the FeCoCrNiMo high-entropy alloy sheet-like powder is prepared in the following manner: In an inert gas atmosphere, FeCoCrNiMo high-entropy alloy spherical powder is subjected to high-energy ball milling to prepare the FeCoCrNiMo high-entropy alloy layered powder. The FeCoCrNiMo high-entropy alloy spherical powder has a particle size of 5~100μm, and the ball-to-material ratio of the high-energy ball mill is (5~20):1, the rotation speed is 300~400rpm, and the time is 20~50h.

[0014] Furthermore, the high-energy ball mill is an intermittent ball mill, wherein the intermittent ball mill runs for 20-50 minutes and then stops for 5 minutes; Furthermore, the high-energy ball milling includes inert gas dry milling, anhydrous ethanol wet milling, or inert gas dry milling plus anhydrous ethanol wet milling; High-energy ball milling can modify FeCoCrNiMo high-entropy alloy spherical powder into powder with a layered structure, increasing the specific surface area to improve the physical interlocking and interfacial contact area with the nanolayered powder.

[0015] Furthermore, in step S1, the nanolayered powder includes MoS2 powder, graphene, h-BN (hexagonal boron nitride), black phosphorus, MXene (two-dimensional transition metal carbonitride), or layered silicate, and the particle size of the nanolayered powder is 1~20μm. MoS2 powder, graphene, h-BN, black phosphorus, MXene, or layered silicates are all powder materials with unique layered structures. These materials can be used for single doping or multiple compound doping, and the applicable filler categories are wide-ranging. The overall preparation process is highly versatile and adaptable.

[0016] Furthermore, in step S1, the liquid medium includes anhydrous ethanol, pure water, or an ethanol-water mixture, and the ultrasonic dispersion time is 0.5~2h. Ultrasonic dispersion can uniformly disperse nanolayered powder in a liquid medium to obtain a nanolayered powder dispersion.

[0017] Furthermore, in step S2, the mixing time of the vortex oscillation is 0.5~2h. Compared with ordinary paddle mechanical stirring, which relies only on the blades to drive local fluids and is prone to mixing dead zones and particle sedimentation and stratification due to density differences, vortex oscillation can form a three-dimensional global vortex flow field, realizing uniform mixing of nano-layered materials and sheet powder throughout the system. At the same time, this method relies on fluid shear force to complete the mixing, without direct mechanical collision between the stirring paddle and the powder, and will not destroy the large aspect ratio structure of FeCoCrNiMo sheet powder. It can promote the uniform adhesion and embedding of nano-layered materials on the surface of sheet matrix, providing a good interface foundation for subsequent sintering and construction of a regular stacked structure.

[0018] Furthermore, in step S2, a polytetrafluoroethylene filter membrane is used for the vacuum filtration, and the vacuum drying time is 12~60h.

[0019] Furthermore, in step S3, the discharge plasma sintering pressure is 20-40 MPa, the heating rate is 8-10 °C / min, the temperature is 850-1150 °C, and the holding time is 10-30 min. Compared to conventional sintering methods such as vacuum hot pressing and pressureless sintering, which rely on external heat conduction to gradually achieve powder densification, discharge plasma sintering relies on the instantaneous high temperature generated by interparticle pulse discharge to activate the particle surface. Combined with the synergistic effect of axial pressure, it can achieve high material densification at a lower sintering temperature and a shorter holding time. This process can effectively suppress the oxidation and decomposition of nanolayered functional phases such as MoS2 and graphene at high temperatures and the destruction of their crystal structure, thus preserving their layered lubrication and corrosion resistance functions. On the other hand, it can prevent the abnormal growth of high-entropy alloy matrix grains at high temperatures for a long time, maintaining the structural characteristics and fine grain strengthening effect of the lamellar matrix. At the same time, the discharge activation effect can strengthen the interfacial bonding between particles, reduce internal porosity and interfacial defects, and ultimately form a high-entropy alloy composite material with a regular stacked structure that is dense internally and has stable interfacial bonding.

[0020] The above sintering process can form a high-entropy alloy composite material block with a dense internal structure and stable interfacial interlocking.

[0021] According to a third aspect of this application, this application provides an application of the above-mentioned wear-resistant and corrosion-resistant high-entropy alloy composite material, which is used to manufacture structural components for marine engineering equipment, petrochemical pipelines, valves, pump bodies, and nuclear power plant cooling system parts. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate of the structural component is 1.2 × 10⁻⁶. -6 ~1.8×10 -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.0 × 10⁻⁶. -8 ~5.0×10 -8 A·cm -2 ; Compared to structural components made of pure FeCoCrNiMo high-entropy alloy, the layered high-entropy alloy composite material of this application effectively modifies the corrosion and wear transmission path through the interlocking of a layered matrix and nanolayered functions, exhibiting excellent wear and corrosion synergistic performance. It is limited to harsh working conditions where wear and corrosion coexist, and cannot be used alone as a corrosion-resistant or wear-resistant material. The prepared structural components are suitable for various erosion and wear coupling conditions containing chloride ions, acids, and alkalis, and the overall wear and corrosion synergistic failure rate can be reduced by about 60%.

[0022] This application proposes a wear-resistant and corrosion-resistant high-entropy alloy composite material, its preparation method, and its application, which yields the following beneficial effects: By uniformly dispersing nanolayered powder in FeCoCrNiMo high-entropy alloy sheet-layered powder, a high-entropy alloy composite material with a dense and uniform internal structure and excellent wear resistance and corrosion resistance is prepared, achieving synergistic enhancement of comprehensive performance under corrosive and wear conditions; the process is simple and standardized, easy to operate and controllable, and has low preparation cost, enabling large-scale mass production of multilayered composite materials with different types of nanolayered powder and different doping ratios. It can fully meet the customized material selection and key structural component preparation needs of various harsh working conditions with coexisting wear and corrosion, such as marine engineering, petrochemicals, and energy equipment, and has outstanding value for engineering promotion and application. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0024] Figure 1 SEM image of the FeCoCrNiMo high-entropy alloy spherical powder used in Example 1; Figure 2 SEM image of the FeCoCrNiMo high-entropy alloy lamellar powder obtained by high-energy ball milling in Example 1; Figure 3 Here is a SEM image of the high-entropy alloy composite powder prepared in Example 1; Figure 4 A bar chart showing the wear rate comparison of the high-entropy alloy composite materials prepared in Comparative Example 1, Example 1, and Example 2; Figure 5 Electrochemical potential polarization curves of the high-entropy alloy composite materials prepared in Comparative Example 1, Example 1, and Example 2 in 3.5 wt% NaCl solution.

[0025] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0026] The technical solutions in the embodiments will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0027] According to a first aspect of this application, this application provides a wear-resistant and corrosion-resistant high-entropy alloy composite material, the high-entropy alloy composite material comprising a FeCoCrNiMo high-entropy alloy sheet matrix and a nano-layered functional phase, the high-entropy alloy composite material comprising, by volume percentage, 85%~95% FCC phase, 2%~7% BCC phase and 3%~8% Laves phase.

[0028] The high-entropy alloy composite material is used to manufacture structural components for marine engineering equipment, petrochemical pipelines, valves, pump bodies, and nuclear power plant cooling system parts; Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate of the structural component is 1.2 × 10⁻⁶. -6 ~1.8×10 -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.0 × 10⁻⁶. -8 ~5.0×10 -8 A·cm -2 .

[0029] According to a second aspect of this application, this application provides a method for preparing a wear-resistant and corrosion-resistant high-entropy alloy composite material, comprising the following steps: S1. Obtain FeCoCrNiMo high-entropy alloy sheet-like powder and nano-layered powder, and ultrasonically disperse the nano-layered powder in a liquid medium to obtain a dispersion. Preferably, the mass percentage of FeCoCrNiMo high-entropy alloy sheet-like layered powder to nano-layered powder is (85~95):(5~15), the nano-layered powder includes MoS2 powder, graphene, h-BN, black phosphorus, MXene or layered silicate, and the particle size of the nano-layered powder is 1~20μm; the liquid medium includes anhydrous ethanol, pure water or ethanol-water mixture.

[0030] In some preferred embodiments of this application, FeCoCrNiMo high-entropy alloy spherical powder with a particle size of 5-100 μm can be obtained by high-energy ball milling in an inert gas atmosphere. The ball-to-powder ratio of the high-energy ball milling is (5-20):1, the rotation speed is 300-400 rpm, and the time is 20-50 h. The steel balls used are stainless steel grinding balls with diameters of 5 mm and 10 mm, and the mass ratio of small steel balls to large steel balls is 13:7. The high-energy ball milling is carried out in an intermittent manner, with a 20-50 min run followed by a 5 min stop. The high-energy ball milling includes dry milling in inert gas, wet milling in anhydrous ethanol, or dry milling in inert gas combined with wet milling in anhydrous ethanol. In addition, in order to achieve sufficient and uniform dispersion of the nano-layered powder in the liquid medium, ultrasonication is required for 0.5-2 h, with an ultrasonic power of 100-300 W and a frequency of 20-40 kHz. S2. The dispersion is dropped into FeCoCrNiMo high-entropy alloy sheet-like powder, and slurry is prepared by vortex oscillation. After filtration and vacuum drying, high-entropy alloy composite powder is obtained. In some preferred embodiments of this application, in order to achieve uniform mixing of FeCoCrNiMo high-entropy alloy sheet-like powder and nano-layered powder, the slurry can be prepared by vortex oscillation for 0.5 to 2 hours; and after mixing, the mixture is rapidly filtered through a polytetrafluoroethylene filter membrane to obtain a filter cake, which is then vacuum dried at 60°C for 12 to 60 hours to obtain a uniformly dispersed high-entropy alloy composite powder.

[0031] S3. High-entropy alloy composite powder is loaded into the mold in batches and layer by layer, and then subjected to spark plasma sintering to obtain high-entropy alloy composite material. Preferably, the discharge plasma sintering pressure is 20~40MPa, the heating rate is 8~10℃ / min, the temperature is 850~1150℃, and the holding time is 10~30min.

[0032] In some preferred embodiments of this application, in order to obtain a dense, interfacially stable bulk high-entropy alloy composite material, a graphite mold with an inner diameter of 25 / 30 / 50 mm can be selected, graphite paper is laid on the inner wall of the mold, high-entropy alloy composite powder is loaded, and then the pressure sintering is carried out by spark plasma sintering.

[0033] The technical solution of this application will be further described below with reference to specific embodiments.

[0034] Example 1

[0035] A wear-resistant and corrosion-resistant high-entropy alloy composite material comprises 95% FeCoCrNiMo high-entropy alloy lamellar matrix and 5% MoS2 nanolayered functional phase. Its preparation method includes the following steps: S1. Obtain 95g of FeCoCrNiMo high-entropy alloy spherical powder with a particle size of 40μm and 5g of MoS2 nanolayered powder with a particle size of 5μm. FeCoCrNiMo high-entropy alloy spherical powder was subjected to high-energy ball milling to obtain FeCoCrNiMo high-entropy alloy lamellar powder. Anhydrous ethanol was used as the wet grinding medium. 5 mm and 10 mm stainless steel balls with a mass ratio of 13:7 and a ball-to-material ratio of 5:1 were selected. The ball milling was carried out intermittently at 360 rpm for 40 h, with a 5 min stop every 40 min. MoS2 nanolayered powder was ultrasonically dispersed in 50 mL of anhydrous ethanol for 1 h to obtain a dispersion. S2. The dispersion was dropped into FeCoCrNiMo high-entropy alloy sheet-like powder, and the slurry was adjusted by vortexing for 1 hour. The filter cake was obtained by filtration through a polytetrafluoroethylene filter membrane and then vacuum dried at 60°C for 48 hours to obtain high-entropy alloy composite powder. S3. Select a graphite mold with an inner diameter of 30 mm, line the inner wall of the mold with graphite paper, and load high-entropy alloy composite powder in batches and layers. Apply a pressure of 30 MPa in a sintering furnace, heat to 1000 °C at 10 °C / min and hold for 25 min for discharge plasma sintering. After cooling, obtain the high-entropy alloy composite material.

[0036] Testing showed that the high-entropy alloy composite material prepared in this embodiment exhibited a wear rate of 1.6 × 10⁻⁶ under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 4.5 × 10⁻⁶. -8 A·cm -2 .

[0037] Example 2

[0038] A wear-resistant and corrosion-resistant high-entropy alloy composite material comprises 95% FeCoCrNiMo high-entropy alloy sheet matrix and 5% graphene nanolayered functional phase, and its preparation method includes the following steps: S1. Obtain 95g of FeCoCrNiMo high-entropy alloy spherical powder with a particle size of 50μm and 5g of graphene nanolayer powder with a particle size of 8μm. FeCoCrNiMo high-entropy alloy spherical powder was subjected to high-energy ball milling to obtain FeCoCrNiMo high-entropy alloy lamellar powder. 1.9g of stearic acid was used as the ball milling medium. 5mm and 10mm stainless steel balls with a mass ratio of 13:7 and a ball-to-material ratio of 10:1 were selected. The ball milling was carried out intermittently at 400rpm for 30h, with a 5min stop after every 30min of operation. Graphene nanolayer powder was ultrasonically dispersed in 50 mL of anhydrous ethanol for 0.5 h to obtain a dispersion. S2. The dispersion was dropped into FeCoCrNiMo high-entropy alloy sheet-like powder, and the slurry was adjusted by vortexing for 1 hour. The filter cake was obtained by filtration through a polytetrafluoroethylene filter membrane and then vacuum dried at 60°C for 48 hours to obtain high-entropy alloy composite powder. S3. Select a graphite mold with an inner diameter of 30 mm, and line the inner wall of the mold with graphite paper. Load high-entropy alloy composite powder into the mold in batches and layers. Apply a pressure of 30 MPa in the sintering furnace, heat the mold to 1000 °C at 10 °C / min, and hold the temperature and pressure for 30 min for discharge plasma sintering. After cooling, the high-entropy alloy composite material is obtained.

[0039] Testing showed that the high-entropy alloy composite material prepared in this embodiment exhibited a wear rate of 1.8 × 10⁻⁶ under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.2 × 10⁻⁶. -8 A·cm -2 .

[0040] Example 3

[0041] A wear-resistant and corrosion-resistant high-entropy alloy composite material comprises 85% FeCoCrNiMo high-entropy alloy lamellar matrix and 15% h-BN / MoS2 composite nanolayered functional phase. Its preparation method includes the following steps: S1. Obtain 85g of FeCoCrNiMo high-entropy alloy spherical powder with a particle size of 50μm, 7g of h-BN nanolayered powder with a particle size of 5μm, and 8g of MoS2 nanolayered powder with a particle size of 5μm. FeCoCrNiMo high-entropy alloy spherical powder was subjected to high-energy ball milling to obtain FeCoCrNiMo high-entropy alloy lamellar powder. 0.85g stearic acid and 0.85g anhydrous ethanol were used as the ball milling media. 5mm and 10mm stainless steel balls with a mass ratio of 13:7 and a ball-to-material ratio of 8:1 were selected. The ball milling was carried out intermittently at 400rpm for 30h, with a 5min stop after every 30min of operation. h-BN nanolayered powder and MoS2 nanolayered powder were ultrasonically dispersed in 50 mL of anhydrous ethanol for 1 h to obtain a dispersion. S2. The dispersion was dropped into FeCoCrNiMo high-entropy alloy sheet-like powder, and the slurry was adjusted by vortexing for 1 hour. The filter cake was obtained by filtration through a polytetrafluoroethylene filter membrane and then vacuum dried at 60°C for 48 hours to obtain high-entropy alloy composite powder. S3. Select a graphite mold with an inner diameter of 30 mm, and line the inner wall of the mold with graphite paper. Add high-entropy alloy composite powder in batches and layers. Apply a pressure of 30 MPa in a sintering furnace, heat to 950 °C at 10 °C / min and hold for 30 min for discharge plasma sintering. After cooling, obtain the high-entropy alloy composite material.

[0042] Testing showed that the high-entropy alloy composite material prepared in this embodiment exhibited a wear rate of 1.3 × 10⁻⁶ under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.8 × 10⁻⁶. -8 A·cm -2 .

[0043] Comparative Example 1 A pure FeCoCrNiMo high-entropy alloy composite material without nanolayered materials, without lamellarization, and without stacked structures is prepared in a manner that differs from that in Example 1 in that: 100g of FeCoCrNiMo high-entropy alloy spherical powder with a particle size of 40μm was obtained. Without high-energy ball milling or adding nano-layered powder, the FeCoCrNiMo high-entropy alloy spherical powder was directly sintered using the method in step S3 of Example 1.

[0044] Testing revealed that the high-entropy alloy composite material prepared in this comparative example lacked a lamellar matrix, nanolayered fillers, and a regular stacked structure, possessing only basic intrinsic wear and corrosion resistance. Its performance significantly degraded under synergistic abrasion conditions. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate was 9.2 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 6.8 × 10⁻⁶. -7 A·cm -2 .

[0045] Comparative Example 2 A high-entropy alloy composite material without nanolayered materials, without lamellar structures, and without stacked structures is prepared in a manner that differs from that in Example 1 in that: The FeCoCrNiMo high-entropy alloy spherical powder was not subjected to high-energy ball milling, and the MoS2 nanolayered powder was not subjected to liquid phase dispersion; the FeCoCrNiMo high-entropy alloy spherical powder and MoS2 nanolayered powder were directly mixed by dry mechanical stirring for 30 min; and then sintered using the method in step S3 of Example 1.

[0046] Testing revealed that the high-entropy alloy composite material prepared in this comparative example exhibited severe agglomeration of nanolayered materials, loose bonding at the interface with the spherical matrix, and lacked an internal interlocking layered structure. Corrosive media easily penetrated rapidly along the interface, leading to large-area peeling during the wear process. Its wear-corrosion synergy performance was significantly worse than the high-entropy alloy composite material with a layered structure in Example 1. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate was 5.1 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 4.2 × 10⁻⁶. -7 A·cm -2 .

[0047] Comparative Example 3 A high-entropy alloy composite material with an irregular dense laminated structure, the preparation method of which differs from that of Example 1, is as follows: In step S3, the composite powder is randomly and loosely packed into a graphite mold with an inner diameter of 30 mm without any layered and orderly arrangement control, and the sintering process is not oriented and stacked induction.

[0048] Testing revealed that the matrix of the high-entropy alloy composite material prepared in this comparative example had a layered structure, but the nanolayered materials were uniformly dispersed, lacking a continuous and dense regular stacked arrangement. The interlayer interfaces were disordered and contained voids and defects, failing to effectively modify the corrosion and wear conduction paths. Therefore, its wear synergy performance was far inferior to the high-entropy alloy composite material with a stacked structure in Example 1. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate was 2.4 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 1.8 × 10⁻⁶. -7 A·cm -2 .

[0049] Comparative Example 4 The only difference between this comparative example and Example 1 is that in step S1, mechanical stirring was used to disperse the MoS2 nanolayered powder in anhydrous ethanol, and the high-entropy alloy composite material was finally prepared.

[0050] Testing revealed microscopic agglomeration of MoS2 in the high-entropy alloy composite material prepared in this comparative example. This resulted in decreased uniformity of the load on the lamellar matrix surface and increased interfacial defects. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate was 2.7 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 2.1 × 10⁻⁶. -7 A·cm -2 .

[0051] Comparative Example 5 The only difference between this comparative example and Example 1 is that in step S2, only mechanical stirring is used to prepare the slurry, and the high-entropy alloy composite material is finally obtained.

[0052] Testing revealed that the high-entropy alloy composite material prepared in this comparative example exhibited decreased two-phase mixing homogeneity, localized segregation of the lubricating phase, and a small amount of fragmentation in the lamellar powder. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, its wear rate was 2.6 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 2.0 × 10⁻⁶. -7 A·cm -2 .

[0053] Comparative Example 6 The only difference between this comparative example and Example 1 is that vacuum hot pressing sintering is used instead of spark plasma sintering in step S3, and a high-entropy alloy composite material is finally prepared.

[0054] Testing revealed that the MoS2 nanolayered functional phase in the high-entropy alloy composite material prepared in this comparative example underwent partial oxidation and decomposition due to prolonged high-temperature sintering, resulting in damage to the original layered crystal structure and a decrease in lubrication function. Simultaneously, the high-entropy alloy matrix exhibited abnormal grain growth, weakened lamellar structure characteristics, loose interlayer bonding, and numerous micropore defects. Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, its wear rate was 4.3 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.1 × 10⁻⁶. -7 A·cm -2 .

[0055] Results Analysis Figure 1The figure shows the microstructure of FeCoCrNiMo high-entropy alloy spherical powder. As can be seen from the figure, the alloy powder before ball milling has a regular spherical morphology and uniform particle size distribution, which is a typical characteristic of commercial spherical high-entropy alloy powder. It has no lamellar structure and serves as the original morphology control group for the high-energy ball milling lamellar modification in this application.

[0056] Figure 2 The image shows the microstructure of FeCoCrNiMo high-entropy alloy lamellar powder obtained after intermittent high-energy ball milling. As can be seen from the figure, the spherical powder is completely transformed into a large-diameter-to-thickness lamellar structure after high-energy ball milling and cold welding. The specific surface area of ​​the powder is greatly increased, providing sufficient interfacial interlocking sites and effectively increasing the contact area with nanolayered materials such as MoS2 and graphene. This solves the problems of poor interfacial bonding and uneven dispersion between traditional spherical matrices and nanolayered fillers.

[0057] Figure 3 The image shows the SEM morphology of the MoS2-FeCoCrNiMo high-entropy alloy composite powder prepared in Example 1. As can be seen from the figure, after liquid-phase ultrasonic dispersion and vortex oscillation mixing, the nano-layered MoS2 particles are uniformly dispersed and adhered to the surface of the lamellar high-entropy alloy powder, without obvious agglomeration or segregation. The interface bonding is tight, which verifies that the liquid-phase composite process of this application can achieve uniform loading of nano-layered materials in the lamellar matrix, laying the foundation for subsequent sintering to build a dense stacked structure.

[0058] Figure 4 A bar chart comparing the wear rates of the pure FeCoCrNiMo high-entropy alloy (Comparative Example 1), the high-entropy alloy composite material modified with 5% MoS2 (Example 1), and the high-entropy alloy composite material modified with 5% graphene under 3.5 wt% NaCl corrosion and wear conditions. The results show that the pure FeCoCrNiMo high-entropy alloy, lacking a solid lubricating phase, exhibits the highest wear rate under the coupled corrosion and wear effect. The introduction of nanolayered MoS2 and graphene modification significantly reduces the wear rate of the composite material. The layered structure formed by the interlocking of the sheet matrix and the nanolayered functional components effectively suppresses plowing, planing, and surface peeling behaviors during friction, significantly improving the wear resistance of the composite material.

[0059] Figure 5 The electrochemical potentiodynamic polarization curves of the high-entropy alloy composites prepared in Comparative Examples 1, 1, and 2 are shown. Compared to the pure FeCoCrNiMo high-entropy alloy, the corrosion potential of the high-entropy alloy composites modified with MoS2 and graphene nanolayers is shifted positively, and the self-corrosion current density is significantly reduced. The densely interlocked layered structure can effectively block the penetration of corrosive media such as chloride ions into the material interior along interface defects, modify the corrosion conduction path, and enable the composite material to have excellent wear resistance and corrosion resistance synergistic properties, making it suitable for harsh service conditions involving wear and corrosion coupling in marine engineering, petrochemicals, and other fields.

[0060] The above description is only a preferred embodiment of this application and does not limit the patent scope of this application. All equivalent structural transformations made using the content of this application's specification under the inventive concept of this application, or direct / indirect applications in other related technical fields, are included within the patent protection scope of this application.

Claims

1. A wear and corrosion resistant high-entropy alloy composite material, characterized in that, The high-entropy alloy composite material comprises a FeCoCrNiMo high-entropy alloy sheet matrix and a nano-layered functional phase. The high-entropy alloy composite material comprises, by volume percentage, 85%~90% FCC phase, 2%~7% BCC phase and 3%~8% Laves phase.

2. A method for preparing a wear and corrosion resistant high-entropy alloy composite material, characterized in that, The method for preparing the wear-resistant and corrosion-resistant high-entropy alloy composite material according to claim 1 includes the following steps: S1. Obtain FeCoCrNiMo high-entropy alloy sheet-like powder and nano-layered powder, and ultrasonically disperse the nano-layered powder in a liquid medium to obtain a dispersion. S2. The dispersion is dropped into the FeCoCrNiMo high-entropy alloy sheet-like powder, and slurry is prepared by vortex oscillation. After filtration and vacuum drying, high-entropy alloy composite powder is obtained. S3. The high-entropy alloy composite powder is loaded into the mold in batches and layer by layer, and then subjected to spark plasma sintering to obtain the high-entropy alloy composite material.

3. The method of claim 2, wherein the method further comprises the step of: In step S1, the mass percentage of the FeCoCrNiMo high-entropy alloy sheet-like powder to the nano-layered powder is (85~95):(5~15). ​ 4. The method of claim 2, wherein the method further comprises the step of: In step S1, the FeCoCrNiMo high-entropy alloy sheet-like powder is prepared in the following manner: FeCoCrNiMo high-entropy alloy spherical powder was ball-milled in an inert gas atmosphere to prepare the FeCoCrNiMo high-entropy alloy sheet-like powder. The FeCoCrNiMo high-entropy alloy spherical powder has a particle size of 5~100μm, and the ball-to-material ratio of the high-energy ball mill is (5~20):1, the rotation speed is 300~400rpm, and the time is 20~50h.

5. The method of claim 2, wherein the method further comprises the step of: In step S1, the nanolayered powder includes MoS2 powder, graphene, h-BN, black phosphorus, MXene, or layered silicate, and the particle size of the nanolayered powder is 1~20μm.

6. The method of claim 2, wherein the method further comprises: In step S1, the liquid medium includes anhydrous ethanol, pure water, or an ethanol-water mixture, and the ultrasonic dispersion time is 0.5~2h.

7. The method of claim 2, wherein the method further comprises the step of: In step S2, the mixing time of the vortex oscillation is 0.5~2h. ​ 8. The method of claim 2, wherein the method further comprises the step of: In step S2, a polytetrafluoroethylene filter membrane is used for vacuum filtration, and the vacuum drying time is 12-60 hours.

9. The method of claim 2, wherein the method further comprises the step of: In step S3, the pressure of the discharge plasma sintering is 20~40MPa, the heating rate is 8~10℃ / min, the temperature is 850~1150℃, and the holding time is 10~30min. ​ 10. Use of the wear and corrosion resistant high-entropy alloy composite material of claim 1, characterized in that, The high-entropy alloy composite material is used to manufacture structural components for marine engineering equipment, petrochemical pipelines, valves, pump bodies, and nuclear power plant cooling system parts; Under conditions of 3.5 wt% NaCl solution, a load of 50 N, and a sliding speed of 0.2 m / s, the wear rate of the structural component is 1.2 × 10⁻⁶. -6 ~1.8×10 -6 mm 3 ·N -1 ·m -1 The self-corrosion current density is 3.0 × 10⁻⁶. -8 ~5.0×10 -8 A·cm -2 .