A method for preparing ultracoarse-grained tungsten carbide powder

By employing a two-stage carbonization and carbonization process and a specific ball milling dispersion, combined with protective atmosphere cooling, the problems of grain uniformity and purity in the preparation of ultra-coarse tungsten carbide powder were solved, achieving efficient particle size control and high-purity powder production.

CN123102986APending Publication Date: 2026-11-17PENG TUNGSTEN ALLOY (SHANDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611594196.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing processes for preparing ultra-coarse tungsten carbide powder suffer from difficulties in controlling grain uniformity, low ball milling efficiency, easy particle agglomeration, incomplete carbonization reaction, easy powder oxidation and secondary grain growth during cooling, and low classification accuracy, resulting in insufficient raw material utilization.

Method used

A two-stage carbonization process is adopted, combining a ball milling dispersion with a specific formulation and cooling under a protective atmosphere. The transition phase tungsten carbide is generated through low-temperature pre-carbonization, and tungsten carbide grains are grown by high-temperature directional carbonization. Airflow classification screening is used to control the ball milling parameters and cooling process.

Benefits of technology

This method achieves improved particle size distribution and purity of ultra-coarse tungsten carbide powder, reduces oxygen and free carbon content, enhances raw material utilization and powder bulk density, and meets the application requirements of high hardness and high toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for preparing ultra-coarse-grained tungsten carbide powder, relating to the field of new powder metallurgy materials. The preparation method includes: ball milling and dispersing tungsten powder and cobalt powder, mixing them with a ball milling dispersion containing a specific complexing stabilizer, and obtaining a mixed raw material through vacuum filtration and drying; carbonizing the mixed raw material in two stages: low-temperature pre-carbonization to generate a transition phase tungsten carbide, and high-temperature directional carbonization to grow grains; after carbonization, cooling is first achieved through a protective atmosphere, then switching to an inert gas to cool to room temperature, and airflow classification to obtain the product. The powder prepared by this invention has uniform particle size, low oxygen and free carbon content, and suitable bulk density, making it suitable for high-end cemented carbide production. The process offers strong controllability and high raw material utilization, solving problems such as poor grain uniformity, easy particle agglomeration, incomplete carbonization, low cooling oxidation, and low classification accuracy associated with traditional processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new powder metallurgy materials, specifically to a method for preparing ultra-coarse-grained tungsten carbide powder. Background Technology

[0002] Ultra-coarse-grained tungsten carbide powder, due to its excellent wear resistance, impact resistance, and high-temperature stability, is a core raw material for preparing high-end cemented carbide (such as mining crushers, metallurgical rolls, and oil drilling tools). Its grain size and uniformity directly determine the mechanical properties of downstream products. Currently, the mainstream industrial process for preparing ultra-coarse-grained tungsten carbide powder is the "direct tungsten powder carbonization method," which involves mixing tungsten powder with a carbon source and then performing a carbonization reaction in a high-temperature furnace, followed by crushing and grading to obtain the target powder. However, this traditional process has significant limitations in practical applications, most notably the difficulty in controlling grain uniformity. Because the carbon source has poor dispersion in the tungsten powder, and local temperature fluctuations are common during carbonization, some areas experience excessive grain growth while others lack sufficient development. This results in a large particle size distribution in the final powder, making the subsequently pressed and sintered cemented carbide prone to structural defects, failing to meet the requirements of both high hardness and high toughness.

[0003] Existing technologies also have significant shortcomings in the raw material pretreatment and dispersion stages. The formulation design of existing ball milling dispersions lacks specificity, with most using only a single surfactant without the addition of a highly efficient complexing stabilizer. This fails to effectively inhibit the surface adsorption and agglomeration of tungsten and cobalt powder particles, and some dispersants have excessive residual amounts, which can easily decompose and generate impurity gases during subsequent carbonization. This results in excessive free carbon or oxygen content in the tungsten carbide powder, seriously affecting the purity of the powder and the compactness of the subsequent cemented carbide.

[0004] Furthermore, existing processes also have shortcomings in the cooling and grading stages. The cooling process after carbonization lacks scientific atmosphere control and mostly relies on natural air cooling. At high temperatures, tungsten carbide powder is prone to react with oxygen, leading to an increase in oxygen content. Moreover, the slow cooling rate can cause secondary grain growth, destroying grain uniformity.

[0005] Therefore, given the limitations of the aforementioned technologies, there is an urgent need to develop a method for preparing ultra-coarse crystalline tungsten carbide powder. Summary of the Invention

[0006] In view of this, the purpose of the present invention is to provide a method for preparing ultra-coarse crystalline tungsten carbide powder, which effectively solves the problems of difficulty in controlling grain uniformity, low ball milling efficiency and easy particle agglomeration, incomplete carbonization reaction or easy grain adhesion, easy oxidation of powder and secondary grain growth during cooling, and insufficient raw material utilization due to low classification accuracy during the preparation of ultra-coarse crystalline tungsten carbide powder.

[0007] The objective of this invention can be achieved through the following technical solutions: A method for preparing ultracoarse-grained tungsten carbide powder includes the following preparation steps: S1: Tungsten powder, cobalt powder and ball milling dispersion are ball milled and dispersed, and then vacuum filtered and dried to obtain mixed raw materials; S2: Carbon black is added to the mixed raw materials in two stages for carbonization and carbonization. The first stage is low-temperature pre-carbonization to generate transition phase tungsten carbide, and the second stage is high-temperature directional carbonization to grow tungsten carbide grains. The process involves pre-carbonization at a low temperature of 1000-1200℃ in a hydrogen atmosphere to generate a transition phase of tungsten carbide; and in the second stage, after adding carbon black, tungsten carbide grains are directionally carbonized at a high temperature of 1400-1600℃. S3: After carbonization, the tungsten carbide grains are first cooled by passing a protective atmosphere, and then cooled to room temperature by switching to an inert gas to obtain cooled ultra-coarse tungsten carbide. The ultra-coarse tungsten carbide is then screened by airflow classification to obtain ultra-coarse tungsten carbide powder.

[0008] Furthermore, in S1, the tungsten powder has a purity of ≥99.9% and an initial particle size of 5μm-10μm, the cobalt powder has a purity of ≥99.8% and a particle size of 1μm-3μm, and the mass ratio of the tungsten powder to the cobalt powder is 90:3-10.

[0009] Furthermore, the process parameters for ball milling in S1 are as follows: the grinding balls are zirconia ceramic grinding balls with a diameter of 5mm-8mm, the ball-to-material ratio is 12-15:1, the solid-liquid mass ratio of the ball milling dispersion to tungsten powder and cobalt powder is 1:2-4, the ball mill speed is 300rpm-500rpm, and the ball milling time is 4h-6h.

[0010] Furthermore, the preparation method of the ball-milled dispersion is as follows: Polyvinylpyrrolidone, sodium dodecylbenzenesulfonate, and deionized water were mixed, a complexing stabilizer was added, the mixture was heated and stirred, ethanol and glycerol were added, and the mixture was ultrasonically treated to obtain a ball-milled dispersion.

[0011] Furthermore, the polyvinylpyrrolidone is polyvinylpyrrolidone K30.

[0012] Furthermore, the complexing stabilizer is composed of disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate, with the mass ratio of disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate being 2:0.2-0.5:0.8-1.5.

[0013] Furthermore, the raw materials of the ball milling dispersion, by weight, are 2-5 parts of polyvinylpyrrolidone, 0.5-2 parts of sodium dodecylbenzenesulfonate, 70-85 parts of deionized water, 3-4 parts of complexing stabilizer, 5-12 parts of ethanol, and 2-6 parts of glycerol.

[0014] Furthermore, the specific process of the first stage of low-temperature pre-carbonization in S2 is as follows: the mixed raw materials and carbon black accounting for 4.8%-5.0% of the mass of the mixed raw materials are mixed at a speed of 200rpm-300rpm for 30min-45min, and then placed in a graphite crucible and placed in a high-temperature molybdenum wire furnace. Hydrogen gas is introduced at a flow rate of 50mL / min-80mL / min, and the temperature is raised to 1000℃-1200℃ at a rate of 5℃ / min-8℃ / min. The temperature is held for 2h-3h to generate the transition phase tungsten carbide. The purity of the carbon black is ≥99.5%, and the particle size is 20nm-50nm.

[0015] Furthermore, the specific process of the second stage of high-temperature directional carbonization in S2 is as follows: 0.1%-0.3% of carbon black by mass of the transition phase tungsten carbide is added to the transition phase tungsten carbide, and after mixing for 15-20 minutes, it is put back into the graphite crucible and heated to 1400-1600℃ at a rate of 3℃ / min-5℃ / min, and held for 4-6 hours; during the heating process, the hydrogen flow rate is increased to 100mL / min-120mL / min.

[0016] Furthermore, after carbonization in step S3 is completed, the hydrogen atmosphere is maintained and the temperature is reduced at a rate of 5°C / min-8°C / min until it reaches 450°C-500°C. Then, the temperature is immediately switched to inert argon gas, and the argon gas flow rate is controlled at 60mL / min-80mL / min. The temperature is then reduced to room temperature at a rate of 12°C / min-15°C / min.

[0017] Furthermore, the step S3 of classifying and screening ultra-coarse tungsten carbide by airflow specifically includes: feeding ultra-coarse tungsten carbide into an airflow classifier, setting the wind speed to 12m / s-15m / s, and screening out ultra-coarse tungsten carbide powder with a particle size of 5μm-10μm.

[0018] The beneficial effects of this invention are: 1. This invention, by combining a ball milling dispersion with a specific formulation and a complexing stabilizer composed of disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate in precise proportions, can bind metal ions in tungsten and cobalt powders from different coordination angles, inhibiting adsorption and agglomeration on the particle surface. At the same time, polyvinylpyrrolidone and sodium dodecylbenzenesulfonate synergistically enhance the dispersion effect, making the material particles after ball milling uniformly dispersed. This lays a solid foundation for the uniformity of the subsequent carbonization reaction and completely improves the problem of large particle size distribution of powder and easy occurrence of structural defects in subsequent alloys caused by insufficient dispersion in traditional processes.

[0019] 2. The two-stage carbonization and carbonization process designed in this invention fully generates the transition phase tungsten carbide through low-temperature pre-carbonization, providing a foundation for the orderly grain growth in the high-temperature directional carbonization stage. This avoids the defects of incomplete carbonization or irregular and coarse grains in traditional single-stage carbonization. At the same time, after carbonization, a graded protective atmosphere cooling method of "high-purity hydrogen cooling to a specific temperature + inert argon rapid cooling" is adopted. This not only prevents the oxygen content from exceeding the standard due to the reaction of powder with oxygen at high temperature, but also avoids the secondary grain growth caused by the slow cooling rate. This ensures that the total carbon content of the final powder is accurately controlled, the free carbon content is low, and the grain size is uniform, meeting the stringent requirements of ultra-coarse tungsten carbide powder for purity and microstructure.

[0020] 3. The preparation process of this invention has strong overall controllability. The parameters of each link from raw material pretreatment to air classification are reasonably designed. The air classifier achieves stable screening of target particle size of 5μm-10μm by precisely controlling the wind speed, which greatly reduces the proportion of overly fine or overly coarse particles and improves the utilization rate of raw materials. The final product of ultra-coarse crystalline tungsten carbide powder not only has a suitable loose density and good flowability, but also facilitates the subsequent pressing and sintering of cemented carbide. Detailed Implementation

[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] Example 1 A method for preparing ultracoarse-grained tungsten carbide powder includes the following preparation steps: S1: Add 2 parts polyvinylpyrrolidone K30, 0.5 parts sodium dodecylbenzenesulfonate, and 70 parts deionized water to a mixing tank and stir at room temperature for 10 minutes until completely dissolved; then add 3 parts complexing stabilizer (prepared by disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate in a mass ratio of 2:0.2:0.8), heat to 50°C, and stir at 200 rpm for 20 minutes; next, add 5 parts ethanol and 2 parts glycerol, and continue stirring for 15 minutes; finally, transfer the mixture to an ultrasonic device and sonicate at 300W for 15 minutes to obtain a ball-milled dispersion; then add tungsten powder with a purity of 99.9% and an initial particle size of 5 μm... Cobalt powder with a purity of 99.8% and a particle size of 1 μm was added to a ball mill at a mass ratio of 90:3. Zirconia ceramic grinding balls with a diameter of 5 mm-8 mm were added, and the ball-to-material ratio was controlled at 12:1. The ball milling dispersion prepared above was added to the ball mill, so that the solid-liquid mass ratio of the ball milling dispersion to tungsten powder and cobalt powder was 1:2. The ball mill speed was set to 300 rpm, and the ball milling time was 4 h. After the ball milling was completed, the ball milled mixture was transferred to a vacuum filtration device and filtered for 30 min under a vacuum of -0.08 MPa to remove excess dispersion. Then the filter cake was placed in a vacuum drying oven and dried for 6 h at 80℃ and -0.09 MPa to obtain the mixed raw material.

[0023] S2: Weigh the mixed raw material obtained in S1 above, and add it together with 4.8% of the mass of carbon black with a purity of 99.5% and a particle size of 20 nm into a twin-screw mixer. Set the speed to 200 rpm and mix for 30 min. Place the mixed material into a graphite crucible, put it into a high-temperature molybdenum wire furnace, and introduce hydrogen into the furnace. Control the hydrogen flow rate at 50 mL / min, and heat it to 1000℃ at a rate of 5℃ / min. Hold it at this temperature for 2 h to generate the transition phase tungsten carbide. Allow it to undergo low-temperature pre-carburization. After curing, the transition phase tungsten carbide was removed from the graphite crucible, and carbon black with a purity of 99.5% and a particle size of 20 nm, accounting for 0.1% of the mass of the transition phase tungsten carbide, was added directly to the transition phase tungsten carbide. The mixture was then placed in a mixer and mixed for 15 min. The mixed product was then put back into the graphite crucible and returned to the high-temperature molybdenum wire furnace. The temperature was increased to 1400 °C at a rate of 3 °C / min. During the heating process, the hydrogen flow rate was increased to 100 mL / min. After reaching the target temperature, the temperature was maintained for 4 h to complete the high-temperature directional carbonization.

[0024] S3: After carbonization, maintain a hydrogen atmosphere in the high-temperature molybdenum wire furnace and cool down at a rate of 5℃ / min. When the furnace temperature drops to 450℃, immediately switch the atmosphere to inert argon and control the argon flow rate to 60mL / min. Continue cooling down to room temperature at a rate of 12℃ / min. Take out the cooled ultra-coarse crystalline tungsten carbide and put it into an air classifier. Set the classifier wind speed to 12m / s and start the equipment to classify and screen the powder with a particle size of 5μm-10μm, which is the ultra-coarse crystalline tungsten carbide powder.

[0025] Example 2 A method for preparing ultracoarse-grained tungsten carbide powder includes the following preparation steps: S1: Add 3.5 parts of polyvinylpyrrolidone K30, 1.25 parts of sodium dodecylbenzenesulfonate, and 77.5 parts of deionized water to a mixing tank and stir at room temperature for 10 minutes until completely dissolved; then add 3.5 parts of complexing stabilizer (prepared from disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate in a mass ratio of 2:0.3:1.2), heat to 50°C, and stir at 200 rpm for 20 minutes; next, add 8.5 parts of ethanol and 4 parts of glycerol, and continue stirring for 15 minutes; finally, transfer the mixture to an ultrasonic device and sonicate at 300W for 15 minutes to obtain a ball-milled dispersion; 99.9% purity, initial particle size 7.5 μm Tungsten powder and cobalt powder with a purity of 99.8% and a particle size of 2 μm were added to a ball mill at a mass ratio of 90:6.5. Zirconia ceramic grinding balls with a diameter of 5 mm-8 mm were added, and the ball-to-material ratio was controlled at 13.5:1. The ball milling dispersion prepared above was added to the ball mill, so that the solid-liquid mass ratio of the ball milling dispersion to the tungsten powder and cobalt powder was 1:3. The ball mill speed was set to 400 rpm, and the ball milling time was 5 h. After the ball milling was completed, the ball milled mixture was transferred to a vacuum filtration device and filtered for 30 min under a vacuum of -0.08 MPa to remove excess dispersion. Then the filter cake was placed in a vacuum drying oven and dried at 80℃ and -0.09 MPa for 6 h to obtain the mixed raw material.

[0026] S2: Weigh the mixed raw material obtained in S1 above, and add it together with 4.9% of the mass of carbon black with a purity of 99.5% and a particle size of 35nm into a twin-screw mixer. Set the speed to 250 rpm and mix for 37.5 min. Place the mixed material into a graphite crucible, put it into a high-temperature molybdenum wire furnace, and introduce hydrogen into the furnace. Control the hydrogen flow rate at 65 mL / min, and heat it to 1100℃ at a rate of 6.5℃ / min. Hold the temperature for 2.5 h to generate the transition phase tungsten carbide. Allow it to undergo low-temperature pre-carbonization. After the carbonization process is complete, the transition phase tungsten carbide is removed from the graphite crucible, and carbon black with a purity of 99.6% and a particle size of 35 nm, accounting for 0.2% of the mass of the transition phase tungsten carbide, is added directly to the transition phase tungsten carbide. The mixture is then placed in a mixer and mixed for 17.5 min. The mixed product is then returned to the graphite crucible and placed back into the high-temperature molybdenum wire furnace. The temperature is increased to 1500℃ at a rate of 4℃ / min. During the heating process, the hydrogen flow rate is controlled to increase to 110 mL / min. After reaching the target temperature, the temperature is maintained for 5 h to complete the high-temperature directional carbonization.

[0027] S3: After carbonization, maintain a hydrogen atmosphere in the high-temperature molybdenum wire furnace and cool down at a rate of 6.5℃ / min. When the furnace temperature drops to 480℃, immediately switch the atmosphere to inert argon and control the argon flow rate to 70mL / min. Continue cooling to room temperature at a rate of 13.5℃ / min. Take out the cooled ultra-coarse crystalline tungsten carbide and put it into an air classifier. Set the classifier wind speed to 13.5m / s and start the equipment to classify and screen the particles. Collect powder with a particle size of 5μm-10μm, which is ultra-coarse crystalline tungsten carbide powder.

[0028] Example 3 A method for preparing ultracoarse-grained tungsten carbide powder includes the following preparation steps: S1: Add 5 parts of polyvinylpyrrolidone K30, 2 parts of sodium dodecylbenzenesulfonate, and 85 parts of deionized water to a mixing tank and stir at room temperature for 10 minutes until completely dissolved; then add 4 parts of complexing stabilizer (prepared by disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate in a mass ratio of 2:0.5:1.5), heat to 50°C, and stir at 200 rpm for 20 minutes; then add 12 parts of ethanol and 6 parts of glycerol, and continue stirring for 15 minutes; finally, transfer the mixture to an ultrasonic device and sonicate at 300W for 15 minutes to obtain a ball-milled dispersion; tungsten powder with a purity of 99.9% and an initial particle size of 10 μm is mixed with pure... Cobalt powder with a purity of 99.9% and a particle size of 3 μm was added to a ball mill at a mass ratio of 90:10. Zirconia ceramic grinding balls with a diameter of 5 mm-8 mm were added, and the ball-to-material ratio was controlled at 15:1. The ball milling dispersion prepared above was added to the ball mill, so that the solid-liquid mass ratio of the ball milling dispersion to tungsten powder and cobalt powder was 1:4. The ball mill speed was set to 500 rpm, and the ball milling time was 6 h. After the ball milling was completed, the ball milled mixture was transferred to a vacuum filtration device and filtered for 30 min under a vacuum of -0.08 MPa to remove excess dispersion. Then the filter cake was placed in a vacuum drying oven and dried at 80℃ and -0.09 MPa for 6 h to obtain the mixed raw material.

[0029] S2: Weigh the mixed raw material obtained in S1 above, and add it together with 5.0% of carbon black with a purity of 99.5% and a particle size of 50nm to a twin-screw mixer. Set the speed to 300 rpm and mix for 45 min. Place the mixed material into a graphite crucible, put it into a high-temperature molybdenum wire furnace, and introduce hydrogen into the furnace. Control the hydrogen flow rate at 80 mL / min, and raise the temperature to 1200℃ at a rate of 8℃ / min. Hold the temperature for 3 h to generate the transition phase tungsten carbide. Allow the material to undergo low-temperature pre-carburization. After curing, the transition phase tungsten carbide was removed from the graphite crucible, and carbon black with a purity of 99.8% and a particle size of 50 nm, accounting for 0.3% of the mass of the transition phase tungsten carbide, was added directly to the transition phase tungsten carbide. The mixture was then placed in a mixer and mixed for 20 min. The mixed product was then put back into the graphite crucible and returned to the high-temperature molybdenum wire furnace. The temperature was increased to 1600 °C at a rate of 5 °C / min. During the heating process, the hydrogen flow rate was increased to 120 mL / min. After reaching the target temperature, the temperature was maintained for 6 h to complete the high-temperature directional carbonization.

[0030] S3: After carbonization, maintain the hydrogen atmosphere in the high-temperature molybdenum wire furnace and cool down at a rate of 8℃ / min. When the furnace temperature drops to 500℃, immediately switch the atmosphere to inert argon and control the argon flow rate to 80mL / min. Continue cooling to room temperature at a rate of 15℃ / min. Take out the cooled ultra-coarse crystalline tungsten carbide and put it into an air classifier. Set the classifier wind speed to 15m / s and start the equipment to classify and screen the powder with a particle size of 5μm-10μm, which is the ultra-coarse crystalline tungsten carbide powder.

[0031] Comparative Example 1 Compared with Example 2, the "hydroxyethylidene diphosphonic acid" in the complexing stabilizer was replaced with an equal mass of "disodium ethylenediaminetetraacetate". All other steps and parameters were the same, and will not be repeated in this comparative example. Finally, ultra-coarse crystalline tungsten carbide powder was obtained.

[0032] Comparative Example 2 Compared with Example 2, the "ammonium citrate" in the complexing stabilizer in this comparative example is replaced with an equal mass of "disodium ethylenediaminetetraacetate". All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, ultra-coarse crystalline tungsten carbide powder is obtained.

[0033] Comparative Example 3 Compared with Example 2, the mass ratio of tungsten powder to cobalt powder in this comparative example is replaced with 90:2 instead of 90:6.5. All other steps and parameters are the same, and will not be repeated here. The final result is ultra-coarse crystalline tungsten carbide powder.

[0034] Comparative Example 4 Compared with Example 2, the mass ratio of tungsten powder to cobalt powder in this comparative example is replaced with 90:12 instead of 90:6.5. All other steps and parameters are the same, and will not be repeated here. The final result is ultra-coarse crystalline tungsten carbide powder.

[0035] Comparative Example 5 Compared with Example 2, this comparative example replaces the staged protective atmosphere cooling (first cooling to 500°C with high-purity hydrogen, then switching to inert argon to cool to room temperature) with natural air cooling. All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, ultra-coarse crystalline tungsten carbide powder is obtained.

[0036] Comparative Example 6 Compared with Example 2, this comparative example replaces the two-stage carbon preparation and carbonization (low-temperature pre-carbonization + high-temperature directional carbonization) with single-stage carbonization (adding the carbon black required for both stages at once and directly heating to 1500℃ at a rate of 4℃ / min and holding for 7.5h). The remaining steps and parameters are the same, and will not be repeated in this comparative example. Finally, ultra-coarse crystalline tungsten carbide powder is obtained.

[0037] The performance of the ultracoarse-grained tungsten carbide powders of Examples 1-3 and Comparative Examples 1-6 was tested, and the results are recorded in Table 1.

[0038] Table 1: Test Results

[0039] As shown in Table 1, the ultracoarse-grained tungsten carbide powders of Examples 1-3 exhibited a stable and optimized overall performance as the process parameters such as ball milling parameters, carbonization temperature, and carbon content were gradually adjusted within a reasonable range during the preparation process. The particle size was precisely matched with the target requirements, the particle size distribution was more concentrated and uniform, the carbon content was precisely controlled and the free carbon content was low, the oxygen content was maintained at a low level, the loose packing density gradually increased, and the porosity was reasonably reduced. Overall, the powders showed excellent consistency and stability, which fully demonstrates that the preparation process designed in this invention has good controllability and can stably produce products that meet the core performance requirements of ultracoarse-grained tungsten carbide powders.

[0040] A comparison of Example 2 and Comparative Example 1 reveals that in the original complexing stabilizer, disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid, and ammonium citrate exhibit a synergistic effect, binding tungsten / cobalt ions from different coordination angles, inhibiting particle agglomeration, and maintaining the stability of the ball milling dispersion. After replacement, this synergistic balance is disrupted, and the unique role of hydroxyethylidene diphosphonic acid in inhibiting hard agglomeration and assisting dispersion penetration disappears, leading to increased powder agglomeration during ball milling and the inability to form a uniform tungsten-cobalt mixture. This agglomeration is transmitted to the carbonization stage, causing uneven contact between the carbon source and tungsten powder, reducing carbonization uniformity, and ultimately deteriorating the particle size distribution, carbon content control, and oxygen content of the powder in Comparative Example 1. This confirms the crucial role of the selection and proportioning of the original complexing stabilizer components, and demonstrates that hydroxyethylidene diphosphonic acid is irreplaceable in maintaining system stability and improving powder performance.

[0041] As can be seen from the comparison between Example 2 and Comparative Example 2, ammonium citrate in the complexing stabilizer plays a key role in inhibiting the adsorption and agglomeration of tungsten powder and cobalt powder particles on the surface and assisting the subsequent carbonization reaction. After replacing it, not only does the dispersion effect of the powder decrease, but it also affects the uniform distribution and binding efficiency of carbon elements during the carbonization process, resulting in an increase in the free carbon content of the powder and a decrease in the control precision of the combined carbon content. At the same time, it also has an adverse effect on the porosity and loose packing density of the powder, which confirms the irreplaceable nature of ammonium citrate in the preparation process.

[0042] As can be seen from the comparison between Example 2 and Comparative Example 3, the mass ratio of tungsten powder to cobalt powder needs to be controlled within a reasonable range. If the proportion of cobalt powder is too low, it will weaken its auxiliary dispersion effect during the ball milling process and its subsequent support effect on the powder structure, resulting in insufficient powder adhesion, which in turn affects the improvement of loose packing density. At the same time, it will also have a certain impact on the bonding state between particles during carbonization, resulting in a slight increase in free carbon content. This shows that the cobalt powder ratio range defined by the present invention is an important prerequisite for ensuring the overall performance of the powder.

[0043] As can be seen from the comparison between Example 2 and Comparative Example 4, the mass ratio of tungsten powder to cobalt powder is not necessarily better the higher it is. If the proportion of cobalt powder is too high, it will cause excessive coating of tungsten powder particles during ball milling and carbonization. This may not only inhibit the normal directional growth of tungsten carbide grains, but also interfere with the full combination of carbon and tungsten elements, resulting in a decrease in the uniformity of powder particle size distribution. At the same time, it will also have an abnormal effect on the loose packing density. This shows that the upper limit of the cobalt powder ratio limited by the present invention is a reasonable design based on performance balance.

[0044] A comparison of Example 2 and Comparative Example 5 reveals that Comparative Example 5, using natural air cooling without a protective atmosphere to isolate oxygen, allows the tungsten carbide powder at high temperatures to react readily with oxygen in the air, resulting in a significant increase in oxygen content. Furthermore, the air cooling rate is much slower than staged protective atmosphere cooling, causing secondary growth of the carbonized grains during the cooling process, disrupting grain uniformity and increasing the particle size distribution range. In addition, natural air cooling affects the stable presence of carbon in the carbonization product, leading to increased free carbon content, decreased precision in controlling combined carbon content, reduced powder bulk density, increased porosity, and a significant deterioration in overall performance. In contrast, the staged protective atmosphere cooling in Example 2 effectively prevents high-temperature oxidation with hydrogen and accelerates cooling with argon to suppress secondary grain growth, while ensuring stable carbon content. The resulting powder exhibits low oxygen content, uniform particle size, and precise carbon content control, demonstrating that this cooling process is a crucial step in ensuring powder quality.

[0045] As can be seen from the comparison between Example 2 and Comparative Example 6, the single-stage carbonization process is significantly less controllable and thorough than the two-stage carbonization process of the present invention. It cannot lay a good foundation for subsequent high-temperature directional carbonization through low-temperature pre-carbonization, and it is easy to have local over-carbonization or incomplete carbonization. This results in poor uniformity of powder particle size distribution, large fluctuations in carbon content, and difficulty in achieving ideal levels of porosity and oxygen content. This further proves the necessity and superiority of the staged carbonization process of the present invention.

[0046] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing ultracoarse-grained tungsten carbide powder, characterized in that, The preparation steps include the following: S1: Tungsten powder, cobalt powder and ball milling dispersion are ball milled and dispersed, and then vacuum filtered and dried to obtain mixed raw materials; S2: Carbon black is added to the mixed raw materials in two stages for carbonization and carbonization. The first stage is low-temperature pre-carbonization to generate transition phase tungsten carbide, and the second stage is high-temperature directional carbonization to grow tungsten carbide grains. The process involves pre-carbonization at a low temperature of 1000-1200℃ in a hydrogen atmosphere to generate a transition phase of tungsten carbide; and in the second stage, after adding carbon black, tungsten carbide grains are directionally carbonized at a high temperature of 1400-1600℃. S3: After carbonization, the tungsten carbide grains are first cooled by passing a protective atmosphere, and then cooled to room temperature by switching to an inert gas to obtain cooled ultra-coarse tungsten carbide. The ultra-coarse tungsten carbide is then screened by airflow classification to obtain ultra-coarse tungsten carbide powder.

2. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The tungsten powder in S1 has a purity of ≥99.9% and an initial particle size of 5μm-10μm, the cobalt powder has a purity of ≥99.8% and a particle size of 1μm-3μm, and the mass ratio of the tungsten powder to the cobalt powder is 90:3-10.

3. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The process parameters for ball milling in S1 are as follows: the grinding balls are zirconia ceramic grinding balls with a diameter of 5mm-8mm, the ball-to-material ratio is 12-15:1, the solid-liquid mass ratio of the ball milling dispersion to tungsten powder and cobalt powder is 1:2-4, the ball mill speed is 300rpm-500rpm, and the ball milling time is 4h-6h.

4. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The preparation method of the ball-milled dispersion is as follows: Polyvinylpyrrolidone, sodium dodecylbenzenesulfonate, and deionized water were mixed, a complexing stabilizer was added, the mixture was heated and stirred, ethanol and glycerol were added, and the mixture was ultrasonically treated to obtain a ball-milled dispersion.

5. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 4, characterized in that, The complexing stabilizer is composed of disodium ethylenediaminetetraacetate, hydroxyethylidene diphosphonic acid and ammonium citrate, with a mass ratio of 2:0.2-0.5:0.8-1.

5.

6. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 4, characterized in that, The raw materials of the ball milling dispersion, by weight, are 2-5 parts polyvinylpyrrolidone, 0.5-2 parts sodium dodecylbenzenesulfonate, 70-85 parts deionized water, 3-4 parts complexing stabilizer, 5-12 parts ethanol and 2-6 parts glycerol.

7. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The specific process of the first stage of low-temperature pre-carbonization in S2 is as follows: the mixed raw materials and carbon black accounting for 4.8%-5.0% of the mass of the mixed raw materials are mixed at a speed of 200rpm-300rpm for 30min-45min, and then placed in a graphite crucible and placed in a high-temperature molybdenum wire furnace. Hydrogen gas is introduced at a flow rate of 50mL / min-80mL / min, and the temperature is raised to 1000℃-1200℃ at a rate of 5℃ / min-8℃ / min. The temperature is held for 2h-3h to generate the transition phase tungsten carbide; the purity of the carbon black is ≥99.5%, and the particle size is 20nm-50nm.

8. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The specific process of the second stage of high-temperature directional carbonization in S2 is as follows: 0.1%-0.3% carbon black of the mass of the transition phase tungsten carbide is added to the transition phase tungsten carbide, and after mixing for 15-20 minutes, it is put back into the graphite crucible and heated to 1400-1600℃ at a rate of 3℃ / min-5℃ / min, and held for 4-6 hours; during the heating process, the hydrogen flow rate is increased to 100mL / min-120mL / min.

9. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, After carbonization in step S3 is completed, maintain the hydrogen atmosphere and cool down at a rate of 5℃ / min-8℃ / min until the temperature reaches 450℃-500℃. Immediately switch to inert argon gas and control the argon gas flow rate to 60mL / min-80mL / min. Continue cooling down to room temperature at a rate of 12℃ / min-15℃ / min.

10. The method for preparing ultracoarse-grained tungsten carbide powder according to claim 1, characterized in that, The process of classifying and screening ultra-coarse tungsten carbide using airflow classification in step S3 specifically includes: feeding ultra-coarse tungsten carbide into an airflow classifier, setting the wind speed to 12m / s-15m / s, and screening out ultra-coarse tungsten carbide powder with a particle size of 5μm-10μm.