A system and method for preparing silver-coated copper alloy powder
By employing multi-stage activation, continuous silver salt feeding, and phased addition of reducing agent, combined with heat treatment and anti-oxidation treatment, the problems of bonding strength and oxidation resistance in the preparation of silver-coated copper alloy powder have been solved, achieving the preparation of high-performance, low-cost silver-coated copper alloy powder suitable for electronic components, conductive pastes, and electromagnetic shielding.
Patent Information
- Application Number
- CN202611446743.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silver-coated copper alloy powder preparation processes suffer from problems such as uneven copper powder surface activation, uneven silver layer coating thickness, poor interfacial bonding, uneven heat and mass transfer, poor batch repeatability, and insufficient antioxidant protection, making it difficult to meet the requirements of mid-to-high-end products.
A multi-stage activation unit is used for copper powder dispersion, etching and activation treatment. Combined with continuous silver salt feeding and phased addition of reducing agent, a silver-copper alloy transition layer is formed through heat treatment, and anti-oxidation post-treatment is performed, including passivation, drying and grading sieving.
It achieves metallurgical bonding between the silver layer and the copper core, improving bonding strength and oxidation resistance, reducing material costs, and is suitable for large-scale industrial applications in fields such as electronic components, conductive pastes, and electromagnetic shielding.
Smart Images

Figure CN123102989A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal powder material preparation technology, and in particular to a preparation system and method for silver-coated copper alloy powder. Background Technology
[0002] Pure silver powder possesses excellent conductivity and oxidation resistance, but silver resources are scarce and expensive, significantly increasing the manufacturing costs of downstream products and limiting its widespread application in low- to mid-range sectors. Pure copper powder is inexpensive, but its surface is highly susceptible to oxidation, its conductivity decreases significantly over storage time, and its stability under complex operating conditions is insufficient, making it difficult to meet the requirements of mid- to high-end products. Silver-coated copper alloy powder combines the low cost of copper with the high conductivity and oxidation resistance of silver, making it an ideal alternative to pure silver powder.
[0003] In existing technologies, the preparation of silver-coated copper powder mainly employs chemical reduction or electroless plating methods. However, existing processes generally suffer from the following shortcomings: uneven activation of the copper powder surface leads to uneven silver layer thickness, pinholes, or incomplete coating; the silver layer and copper core are only physically deposited, resulting in poor interfacial adhesion and easy detachment of the silver layer; traditional processes use a single stirred tank for intermittent reaction, leading to uneven heat and mass transfer, poor batch repeatability, and difficulty in large-scale continuous production; the reducing agent is added only once, making it difficult to control the reaction rate and easily causing silver particle agglomeration or localized over-reduction; insufficient antioxidant protection during post-processing results in the product still being prone to oxidation and discoloration during storage and transportation. These problems restrict the industrial application of silver-coated copper alloy powder in mid-to-high-end fields. Summary of the Invention
[0004] To solve the above-mentioned technical problems, the present invention provides a system and method for preparing silver-coated copper alloy powder.
[0005] To provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. This summary is not intended as a general commentary, nor is it intended to identify key / important components or to describe the scope of protection of these embodiments. Its sole purpose is to present some concepts in a simple form as a prelude to the detailed description that follows.
[0006] The present invention adopts the following technical solution: This invention provides a system for preparing silver-coated copper alloy powder, comprising: A multi-stage activation unit is used to sequentially disperse copper powder, perform weak acid etching, and activate it with a complexing agent. The deposition and coating unit is used to perform continuous feeding of silver salt and partial addition of reducing agent, so that silver ions are reduced and deposited on the surface of activated copper powder to form a silver layer. A heat treatment unit is used to heat treat the coating product output from the deposition coating unit so that a silver-copper alloy transition layer is formed at the interface between the silver layer and the copper core. An anti-oxidation post-treatment unit is used to perform anti-oxidation treatment, drying, and grading and sieving on the heat treatment products output from the heat treatment unit.
[0007] Furthermore, the multi-stage activation unit includes: an ultrasonic dispersion module, a weak acid etching module, and a complexing agent activation module connected sequentially along the material flow direction; the ultrasonic dispersion module is equipped with an ultrasonic generator, the weak acid etching module is equipped with a heating jacket, and the complexing agent activation module is equipped with a stirrer.
[0008] Furthermore, the deposition coating unit includes: a coating reactor, a continuous silver salt feeder, a reducing agent dosing device, and a parameter controller; the continuous silver salt feeder is connected to the inlet of the coating reactor via a flow meter, and the reducing agent dosing device is connected to the inlet of the coating reactor via a solenoid valve; the parameter controller is connected to the solenoid valve and is configured to open the solenoid valve at a set cycle, so that the reducing agent solution is injected into the coating reactor once per cycle with a fixed single dosing amount.
[0009] Furthermore, the heat treatment unit is a continuous heat treatment furnace, including a heating zone, a heat preservation zone and a cooling zone. Each zone is equipped with an independent temperature control device and the furnace chamber is filled with an inert protective atmosphere.
[0010] Furthermore, the anti-oxidation post-treatment unit includes: a passivation solution immersion tank, a deionized water cleaning tank, a vacuum drying oven, and an air classifier connected sequentially along the material flow direction.
[0011] Furthermore, the silver-coated copper alloy powder preparation system further includes a detection feedback unit; the detection feedback unit includes a particle size analyzer disposed at the outlet of the deposition coating unit and a resistivity tester disposed at the outlet of the heat treatment unit, and the detection feedback unit is connected to the parameter controller.
[0012] A method for preparing silver-coated copper alloy powder includes the following steps: S1: Copper powder is subjected to ultrasonic dispersion treatment, weak acid etching treatment and complexing agent activation treatment in sequence to obtain activated copper powder; S2: Silver salt solution is continuously fed into the suspension of activated copper powder, and reducing agent solution is injected in batches at a fixed amount per cycle, so that silver ions are reduced and deposited on the surface of activated copper powder to form a silver layer, and a coated product is obtained. S3: The coated product is heat-treated under an inert protective atmosphere to form a silver-copper alloy transition layer at the interface between the silver layer and the copper core, thereby obtaining the heat-treated product. S4: The heat-treated product is sequentially passivated, cleaned, dried and graded and sieved to obtain the finished silver-coated copper alloy powder.
[0013] Furthermore, in step S1, the solid content of the ultrasonic dispersion treatment is 10–30 wt%, the ultrasonic frequency is 20–60 kHz, and the treatment time is 5–30 min; the weak acid etching treatment uses an oxalic acid solution with a mass fraction of 0.5–3%, the treatment temperature is 25–60℃, and the treatment time is 5–20 min; the complexing agent activation treatment uses a 0.01–0.1 mol / L aminotriacetic acid solution as the complexing agent, the treatment temperature is 30–60℃, and the treatment time is 10–30 min.
[0014] Furthermore, in step S2, the concentration of the silver salt solution is 0.05–0.3 mol / L, and the continuous feed flow rate is 0.5–5 mL / min; the injection cycle of the reducing agent solution is 30–180 s, and the single addition amount per cycle is 0.5–5 g; the reaction temperature is 30–70℃, the pH value is 9–12, and the stirring speed is 200–600 r / min.
[0015] Furthermore, in step S3, the heating rate of the heat treatment is 2–10℃ / min, the holding temperature is 200–450℃, the holding time is 0.5–2h, and the cooling rate is 1–5℃ / min; in step S4, the passivation treatment uses an imidazole-based organic corrosion inhibitor solution with a passivation solution concentration of 0.1–1wt% and an immersion time of 1–5min; the drying temperature is 60–120℃, and the drying time is 2–6h.
[0016] The beneficial effects of this invention are as follows: By sequentially subjecting copper powder to ultrasonic dispersion, weak acid etching, and complexing agent activation treatment, the surface oxide layer is effectively removed and active sites are activated. Continuous feeding of silver salt combined with phased addition of the reducing agent precisely controls the silver ion reduction rate and nucleation density, avoiding uneven silver layer thickness and pinhole defects, achieving a dense and uniform coating. This forms a silver-copper alloy transition layer at the interface between the silver layer and the copper core, transforming the silver layer from physical adhesion to metallurgical bonding, significantly improving adhesion and oxidation resistance. Passivation, drying, and grading ensure product shelf life and particle size uniformity, guaranteeing controllable silver layer thickness and resistivity ≤3.0×10⁻⁶. -6 Under the premise of Ω·cm and oxidation resistance temperature ≥180℃, the material cost can be reduced by 40%–60% compared with pure silver powder, which has the advantages of high performance and low cost, and is suitable for large-scale industrial applications in electronic components, conductive pastes, electromagnetic shielding and other fields. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a schematic diagram of a silver-coated copper alloy powder preparation system according to the present invention. Detailed Implementation
[0019] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0020] like Figure 1 As shown in some illustrative embodiments, a system for preparing silver-coated copper alloy powder is provided. This system includes a multi-stage activation unit 100, a deposition and coating unit 200, a heat treatment unit 300, and an anti-oxidation post-treatment unit 400. Each unit is connected in series according to the material flow direction via a closed conveying pipeline, forming a continuous production line from raw copper powder input to finished silver-coated copper alloy powder output. The closed conveying pipeline effectively isolates external air, preventing oxidation of the copper powder during inter-process transfer and ensuring product quality stability.
[0021] The multi-stage activation unit 100 is located at the front end of the system and is used to pre-treat the raw copper powder. Specifically, the copper powder is subjected to dispersion treatment, weak acid etching treatment and complexing agent activation treatment in sequence to remove the oxide layer and contaminants on the surface of the copper powder, while generating a large number of active sites on the surface of the copper powder, creating favorable conditions for the uniform deposition of silver ions in the subsequent process.
[0022] The deposition and coating unit 200 is connected to the discharge end of the multi-stage activation unit 100, receiving the activated copper powder suspension. The deposition and coating unit 200 performs continuous feeding of silver salts and partial addition of reducing agent, causing silver ions to be reduced and deposited on the surface of the activated copper powder to form a silver layer. The silver salt solution is continuously fed into the reaction system at a constant flow rate to maintain a stable supply of silver ions, while the reducing agent is added in batches at set time intervals to avoid problems such as excessively rapid local reactions, uneven silver layer thickness, or the generation of free silver particles caused by a large-scale single addition, thereby achieving precise control over the silver layer growth process.
[0023] The heat treatment unit 300 receives the coating product from the deposition and coating unit 200 and performs heat treatment on the coating product to form a silver-copper alloy transition layer at the interface between the silver layer and the copper core. Specifically, through a controllable heat treatment process, limited interdiffusion occurs in the interface region between the silver layer and the copper core, forming a continuous silver-copper alloy transition layer. This transforms the physical deposition bond between the silver layer and the copper substrate into a metallurgical bond, thereby improving the adhesion and peel resistance of the silver layer, and also helping to further enhance the oxidation resistance of the powder.
[0024] The anti-oxidation post-treatment unit 400 is located at the end of the system and receives the heat-treated powder product. It is used to perform anti-oxidation treatment, drying and grading sieving on the heat-treated product output from the heat treatment unit 300. This includes anti-oxidation treatment, cleaning to remove residual impurities, drying to remove moisture and grading sieving to obtain the finished product within the target particle size range.
[0025] The multi-stage activation unit 100 includes an ultrasonic dispersion module 110, a weak acid etching module 120, and a complexing agent activation module 130 connected sequentially along the material flow direction.
[0026] Copper powder is prone to agglomeration during storage and transportation, and its surface is often contaminated with oil and organic pollutants. The ultrasonic dispersion module 110 is equipped with an ultrasonic generator. When copper powder and water form a suspension and enter this module, the ultrasonic generator produces high-frequency ultrasonic waves of 20–60 kHz. These waves can peel away organic pollutants and the adsorbed layer from the surface of the copper powder, while simultaneously using physical shear force to break up the agglomeration between copper powder particles, allowing the copper powder to suspend in a monodisperse state in the liquid phase. This module solves the problem of uneven initial dispersion of copper powder, preventing blind spots in the subsequent silver layer caused by particle agglomeration.
[0027] The weak acid etching module 120 is equipped with a heating jacket for temperature control of the reaction system within the module. After ultrasonically dispersed copper powder suspension enters the module, a weak acid solution is added. The heating jacket provides a controlled temperature of 25–60°C. The weak acid undergoes a mild chemical reaction with the oxide layer on the copper powder surface, dissolving and removing the oxide layer to expose the active copper substrate. Compared to strong acid etching, the weak acid etching rate is gentle and controllable, effectively removing the oxide layer while avoiding damage to the copper powder morphology. The temperature control design of the heating jacket ensures a stable and uniform etching reaction rate.
[0028] The complexing agent activation module 130 is equipped with a stirrer. After the copper powder suspension, etched by a weak acid, enters this module, a complexing agent solution is added. The stirrer operates continuously to ensure thorough contact and uniform mixing between the copper powder and the complexing agent. The complexing agent molecules adsorb onto the active sites on the copper powder surface through coordination bonds, forming an ordered complex molecular film. This complex molecular film regulates the subsequent adsorption and reduction sites of silver ions, allowing silver atoms to preferentially and uniformly nucleate on the copper powder surface. Furthermore, the complexing agent can complex trace amounts of copper ions in the solution, preventing their reduction and precipitation during the coating process.
[0029] The multi-stage activation unit 100 solves the problems of copper powder agglomeration, surface oxide layer, and active site uniformity through physical dispersion, chemical etching, and surface complexation, making the activation more thorough than a single pretreatment method. The weak acid etching and complexing agent activation are both gentle processes, and the activation degree can be controlled by adjusting the parameters of the heating jacket and stirrer. The copper powder treated by this unit has a uniform distribution of active sites on the surface, which allows silver ions to nucleate uniformly on the surface of the copper powder. This avoids defects such as silver layer pinholes, peeling, and uneven thickness, and ultimately improves the conductivity and oxidation resistance of the silver-coated copper alloy powder.
[0030] The deposition and coating unit 200 is located between the multi-stage activation unit 100 and the heat treatment unit 300. Its feed end is connected to the discharge port of the multi-stage activation unit 100 through a closed conveying pipeline to receive the activated copper powder suspension; its discharge end is connected to the feed port of the heat treatment unit 300. The deposition and coating unit 200 includes: a coating reaction vessel 210, a silver salt continuous feeder 220, a reducing agent dosing device 230, and a parameter controller 240.
[0031] The encapsulated reaction vessel 210 is a vertical reaction container with a built-in stirring device. The vessel body is equipped with a temperature control jacket to maintain the required reaction temperature. The vessel lid has a silver salt inlet and a reducing agent inlet, and the vessel bottom has an outlet connected to the heat treatment unit 300 via a closed conveying pipeline. The activated copper powder suspension is fed into the vessel by the multi-stage activation unit 100 and is kept in a uniform suspension state under stirring, providing a reaction site for the reduction and deposition of silver ions.
[0032] The silver salt continuous feeder 220 is connected to the inlet of the coated reactor 210 via a flow meter 250. The silver salt continuous feeder 220 is used to store and stably supply silver salt solution to the reactor 210. The flow meter 250 measures the flow rate of the silver salt solution in real time. The continuous feeding method keeps the silver ion concentration in the reaction system at a relatively stable level, avoiding runaway silver layer growth rate due to drastic fluctuations in silver ion concentration.
[0033] The reducing agent dosing device 230 is connected to the feed port of the coated reactor 210 via a solenoid valve 260. The reducing agent dosing device 230 is used to store and quantitatively deliver the reducing agent solution to the reactor 210. The parameter controller 240 is connected to the solenoid valve 260 and is configured to open the solenoid valve 260 at a set cycle, so that the reducing agent solution is injected into the coated reactor 210 in a fixed manner once per cycle.
[0034] In the chemical reduction silver plating process, after the activated copper powder suspension enters the coating reaction vessel 210, the silver salt continuous feeding device 220 continuously feeds the silver salt solution into the vessel at a constant flow rate through the flow meter 250, maintaining a stable silver ion concentration in the reaction system. Simultaneously, the parameter controller 240 periodically triggers the opening of the solenoid valve 260 according to a pre-set cycle, and the reducing agent dosing device 230 injects a quantitative reducing agent solution into the vessel. Each injected reducing agent undergoes a local reduction reaction with the silver ions, and the generated silver atoms uniformly nucleate and grow into a continuous silver layer on the active sites already formed on the surface of the activated copper powder. Because the reducing agent is injected in stages, quantitatively, and periodically, rather than in large quantities all at once, the reducing agent is rapidly consumed after each injection, and the reaction system remains in a controlled state with a low reducing agent concentration. This precisely controls the reduction rate and nucleation density of silver ions, allowing the silver layer to grow densely layer by layer from the inside out.
[0035] The heat treatment unit 300 is a continuous heat treatment furnace, including a heating zone, a heat preservation zone and a cooling zone. Each section is equipped with an independent temperature control device, so that adjacent sections can be independently set and maintained at different target temperatures. An inert protective atmosphere is circulated in the furnace chamber, and laminar flow is formed by positive pressure gas supply to provide a uniform and stable protective atmosphere environment.
[0036] The heating zone, located at the front of the furnace, provides a gradient heating for the coating product fed by the deposition coating unit 200. This gradient heating design prevents the silver layer from cracking or peeling off due to thermal shock. The holding zone, located in the middle of the furnace, allows the silver-coated copper powder to undergo a holding period, enabling silver atoms to rearrange, diffuse, and fuse on the copper surface. Simultaneously, limited interdiffusion occurs at the interface between the silver layer and the copper core. The diffusion rate of copper atoms towards the silver layer is higher than that of silver atoms towards the copper substrate, forming a silver-copper alloy transition layer at the interface. The cooling zone, located at the rear of the furnace, provides controlled cooling for the powder leaving the hot zone after the holding treatment. Throughout the cooling process, an inert atmosphere is maintained within the furnace to prevent oxidation of the high-temperature powder upon contact with residual oxygen during the cooling phase. The powder is only removed from the furnace and proceeds to subsequent processes after reaching a safe temperature.
[0037] The anti-oxidation post-treatment unit 400 includes: a passivation solution immersion tank 410, a deionized water rinsing tank 420, a vacuum drying oven 430, and an air classifier 440 connected sequentially along the material flow direction.
[0038] The passivation solution immersion tank 410 is a corrosion-resistant container equipped with a stirring device. It contains the passivation solution. After heat treatment, the silver-coated copper powder is fed into the tank from the upstream unit and comes into contact with the passivation solution under stirring. The corrosion inhibitor molecules in the passivation solution form a protective film on the silver layer surface through chemical adsorption. This protective film can prevent oxygen and moisture in the air from contacting the silver layer and copper core, thereby enhancing the powder's oxidation resistance.
[0039] The deionized water cleaning tank 42 is a cleaning container equipped with an overflow outlet. Deionized water is circulated inside, and a spray device is provided. After passivation treatment, impurities may remain on the surface of the powder. These residues can affect the conductivity of the powder. The deionized water cleaning tank removes the soluble impurities remaining on the powder surface through multiple rinsing steps.
[0040] The vacuum drying oven 430 is a closed drying device with an internal heating plate and a vacuum pump system. After cleaning, the wet powder enters the drying oven and is dried at low temperature under negative pressure. The dried powder is in a loose and flowing state, which facilitates subsequent classification processing.
[0041] The air classifier 440 is a device that uses airflow power to separate particles by size. It typically consists of a cyclone separator, a classifying wheel, and a fine powder collector. The dried powder is carried into the classification chamber by the airflow, where coarse and fine particles are separated. Qualified powder that meets the target particle size range is collected as the finished product, while excessively coarse or excessively fine powder is returned to the previous process or processed separately.
[0042] The anti-oxidation post-treatment unit 400 sequentially completes the surface chemical protection, impurity removal, low-temperature dehydration, and particle size separation of the powder through passivation solution immersion, deionized water washing, vacuum drying, and airflow classification sieving. This results in a final silver-coated copper alloy powder product that possesses both antioxidant lifespan, high cleanliness, and narrow particle size distribution, directly meeting the stringent performance requirements of mid-to-high-end applications such as electronic components, conductive pastes, and electromagnetic shielding.
[0043] The preparation system also includes a detection feedback unit; the detection feedback unit includes a particle size analyzer 510 installed at the outlet of the deposition coating unit 200 and a resistivity tester 520 installed at the outlet of the heat treatment unit 300, and the detection feedback unit is connected to the parameter controller 240.
[0044] The particle size analyzer 510 uses laser diffraction or dynamic light scattering principles to detect the particle size of the coating product flowing out of the deposition coating unit 200. Its purpose is to monitor the particle size distribution of the silver-coated copper powder after coating. If an abnormal increase in particle size is detected, it may indicate powder agglomeration or an excessively thick silver layer. If the particle size is abnormally decreased, it may indicate silver layer detachment or the formation of free silver particles. The particle size analyzer 510 transmits real-time detection data to the parameter controller 240. The resistivity tester 520 uses the eddy current method to perform online resistivity detection on the heat-treated powder. If the resistivity exceeds the set threshold, it indicates that the heat treatment process parameters, such as temperature and holding time, may be deviated and need to be adjusted promptly.
[0045] The parameter controller 240 compares the received real-time detection data with the internally stored target threshold to make a judgment: when the particle size data fed back by the particle size analyzer 510 deviates from the preset range, the parameter controller 240 determines that the coating process is abnormal, and then sends an adjustment command to the solenoid valve 260 to adjust the injection cycle or single addition amount of the reducing agent to restore the uniformity of the silver layer coating; when the resistivity data fed back by the resistivity tester 520 exceeds the set upper limit, the parameter controller 240 determines that the heat treatment effect is not as expected, and sends an adjustment command to the temperature control device of the heat treatment unit 300 to adjust the temperature or heat preservation time of the heat preservation zone to optimize the formation quality of the silver-copper alloy transition layer.
[0046] This application also provides a method for preparing silver-coated copper alloy powder, comprising the following steps: S1: Multi-stage activation treatment.
[0047] This step is used to remove the native oxide layer, organic contaminants and particle agglomeration on the surface of copper powder, while constructing uniform active sites on its surface. Specifically, the copper powder is subjected to ultrasonic dispersion treatment, weak acid etching treatment and complexing agent activation treatment in sequence to obtain activated copper powder.
[0048] The ultrasonic dispersion process involves preparing a suspension by mixing copper powder with deionized water at a solid content of 10–30 wt%, and then treating it in an ultrasonic field of 20–60 kHz for 5–30 min. The localized high-temperature and high-pressure microjets generated by the ultrasonic cavitation effect can effectively remove grease and impurities adsorbed on the surface of the copper powder, while simultaneously using physical shear force to break up soft agglomerates between particles, thus suspending the copper powder in a monodisperse state.
[0049] The weak acid etching process involves adding a 0.5–3% (w / w) oxalic acid solution to the dispersed suspension and stirring at 25–60°C for 5–20 minutes. Oxalic acid, as a weak organic acid, undergoes a mild complexation and dissolution reaction with the copper oxide on the copper powder surface, selectively removing the oxide layer. If the oxalic acid concentration is below 0.5%, the etching rate is too slow and the oxide layer cannot be completely removed; if it is above 3%, it may over-etch the copper powder surface, forming pits and affecting the smoothness of the subsequent silver layer. The reaction rate is controlled by the processing temperature and time, which can be flexibly adjusted within the 25–60°C range to accommodate different batches of copper powder with varying degrees of oxidation.
[0050] The complexing agent activation treatment includes adding a 0.01–0.1 mol / L solution of aminotriacetic acid to the etched suspension and stirring at 30–60 °C for 10–30 min.
[0051] S2: Depositional coating.
[0052] Silver salt solution is continuously fed into a suspension of activated copper powder, and reducing agent solution is injected in batches at a fixed amount per cycle, so that silver ions are reduced and deposited on the surface of activated copper powder to form a silver layer, thus obtaining a coated product.
[0053] The concentration of the silver salt solution is 0.05–0.3 mol / L, and the continuous feed flow rate is 0.5–5 mL / min. A silver salt solution with a concentration of 0.05–0.3 mol / L, such as silver nitrate, is fed into the coated reactor at a constant flow rate of 0.5–5 mL / min, ensuring a stable silver ion concentration in the reaction system. The silver salt concentration and flow rate must be matched: too low a concentration or too low a flow rate results in a slow deposition rate and low production efficiency; too high a concentration or too high a flow rate leads to an excess of silver ions, which easily undergoes homogeneous nucleation in the solution, forming free silver particles.
[0054] The reducing agent solution is injected in stages, with a cycle of 30–180 seconds and a single injection amount of 0.5–5 g per cycle. A parameter controller uses a solenoid valve to control the timing and dosage of each injection. Each injected reducing agent undergoes a localized reduction reaction with silver ions, and the resulting silver atoms preferentially nucleate and grow at activation sites on the copper powder surface. Because the reducing agent is added in small, staged injections, the reaction system remains at a low reducing agent concentration, thereby inhibiting homogeneous nucleation of silver atoms in the solution.
[0055] The reaction temperature is 30–70℃, the pH value is 9–12, and the stirring speed is 200–600 r / min. Increasing the temperature can accelerate the reduction reaction, but excessively high temperatures can easily lead to the decomposition of the reducing agent or a rough silver layer; an alkaline environment is conducive to the activity of the reducing agent, but a pH exceeding 12 may cause the decomposition and precipitation of the silver ammonia complex; the stirring speed needs to ensure uniform suspension of copper powder and sufficient mass transfer, but excessively high speeds may cause mechanical peeling of the silver layer.
[0056] S3: Heat treatment.
[0057] The coated product is heat-treated under an inert protective atmosphere to form a silver-copper alloy transition layer at the interface between the silver layer and the copper core, thus obtaining the heat-treated product.
[0058] The heating rate of the heat treatment is 2–10℃ / min, the holding temperature is 200–450℃, the holding time is 0.5–2h, and the cooling rate is 1–5℃ / min.
[0059] The coated product is heated from room temperature to the holding temperature at a rate of 2–10 °C / min. Slow heating avoids cracking or peeling of the silver layer due to differences in thermal expansion; too rapid a heating rate can cause thermal shock, while too slow a rate prolongs the processing time. Within the temperature range of 200–450 °C, silver atoms obtain sufficient diffusion driving force to form a continuously gradient silver-copper alloy transition layer. Holding temperatures below 200 °C result in too low a diffusion rate for effective alloy layer formation; temperatures above 450 °C may lead to excessive silver diffusion, compromising coating integrity. The holding time must be coordinated with the temperature.
[0060] S4: Anti-oxidation post-treatment.
[0061] The heat-treated product is sequentially passivated, cleaned, dried, and graded and sieved to obtain the finished silver-coated copper alloy powder. The passivation solution used is an imidazole-based organic corrosion inhibitor solution with a concentration of 0.1–1 wt%. Imidazole molecules form a hydrophobic organic protective film on the silver surface through chemical adsorption, effectively blocking oxygen and moisture corrosion. The immersion time is 1–5 minutes, followed by rinsing with deionized water to remove residual passivation solution and soluble impurities from the powder surface, ensuring product cleanliness. The drying temperature is 60–120℃, and the drying time is 2–6 hours.
[0062] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A system for preparing silver-coated copper alloy powder, characterized in that, include: A multi-stage activation unit is used to sequentially disperse copper powder, perform weak acid etching, and activate it with a complexing agent. The deposition and coating unit is used to perform continuous feeding of silver salt and partial addition of reducing agent, so that silver ions are reduced and deposited on the surface of activated copper powder to form a silver layer. A heat treatment unit is used to heat treat the coating product output from the deposition coating unit so that a silver-copper alloy transition layer is formed at the interface between the silver layer and the copper core. An anti-oxidation post-treatment unit is used to perform anti-oxidation treatment, drying, and grading and sieving on the heat treatment products output from the heat treatment unit.
2. The preparation system for silver-coated copper alloy powder according to claim 1, characterized in that, The multi-stage activation unit includes an ultrasonic dispersion module, a weak acid etching module, and a complexing agent activation module connected sequentially along the material flow direction; the ultrasonic dispersion module is equipped with an ultrasonic generator, the weak acid etching module is equipped with a heating jacket, and the complexing agent activation module is equipped with a stirrer.
3. The preparation system for silver-coated copper alloy powder according to claim 2, characterized in that, The deposition coating unit includes: a coating reactor, a continuous silver salt feeder, a reducing agent dosing device, and a parameter controller; the continuous silver salt feeder is connected to the inlet of the coating reactor via a flow meter, and the reducing agent dosing device is connected to the inlet of the coating reactor via a solenoid valve; the parameter controller is connected to the solenoid valve and is configured to open the solenoid valve at a set cycle, so that the reducing agent solution is injected into the coating reactor once per cycle with a fixed amount added each time.
4. The preparation system for silver-coated copper alloy powder according to claim 3, characterized in that, The heat treatment unit is a continuous heat treatment furnace, which includes a heating zone, a heat preservation zone and a cooling zone. Each zone is equipped with an independent temperature control device and the furnace chamber is filled with an inert protective atmosphere.
5. The preparation system for silver-coated copper alloy powder according to claim 4, characterized in that, The anti-oxidation post-treatment unit includes: a passivation solution immersion tank, a deionized water cleaning tank, a vacuum drying oven, and an air classifier connected in sequence along the material flow direction.
6. The preparation system for silver-coated copper alloy powder according to claim 5, characterized in that, Also includes: Detection feedback unit; The detection feedback unit includes a particle size analyzer located at the outlet of the deposition coating unit and a resistivity tester located at the outlet of the heat treatment unit. The detection feedback unit is connected to the parameter controller.
7. A method for preparing silver-coated copper alloy powder, characterized in that, Includes the following steps: S1: Copper powder is subjected to ultrasonic dispersion treatment, weak acid etching treatment and complexing agent activation treatment in sequence to obtain activated copper powder; S2: Silver salt solution is continuously fed into the suspension of activated copper powder, and reducing agent solution is injected in batches at a fixed amount per cycle, so that silver ions are reduced and deposited on the surface of activated copper powder to form a silver layer, and a coated product is obtained. S3: The coated product is heat-treated under an inert protective atmosphere to form a silver-copper alloy transition layer at the interface between the silver layer and the copper core, thereby obtaining the heat-treated product. S4: The heat-treated product is sequentially passivated, cleaned, dried and graded and sieved to obtain the finished silver-coated copper alloy powder.
8. The method for preparing silver-coated copper alloy powder according to claim 7, characterized in that, In step S1, the solid content of the ultrasonic dispersion treatment is 10–30 wt%, the ultrasonic frequency is 20–60 kHz, and the treatment time is 5–30 min. The weak acid etching process uses an oxalic acid solution with a mass fraction of 0.5–3%, a processing temperature of 25–60°C, and a processing time of 5–20 min. The complexing agent used in the activation treatment is a 0.01–0.1 mol / L nitric acid solution, the treatment temperature is 30–60℃, and the treatment time is 10–30 min.
9. The method for preparing silver-coated copper alloy powder according to claim 8, characterized in that, In step S2, the concentration of the silver salt solution is 0.05–0.3 mol / L, and the continuous feed flow rate is 0.5–5 mL / min; the injection cycle of the reducing agent solution is 30–180 s, and the single addition amount per cycle is 0.5–5 g; the reaction temperature is 30–70℃, the pH value is 9–12, and the stirring speed is 200–600 r / min.
10. The method for preparing silver-coated copper alloy powder according to claim 9, characterized in that, In step S3, the heating rate of the heat treatment is 2–10℃ / min, the holding temperature is 200–450℃, the holding time is 0.5–2h, and the cooling rate is 1–5℃ / min. In step S4, the passivation treatment uses an imidazole-based organic corrosion inhibitor solution with a concentration of 0.1–1 wt% and an immersion time of 1–5 min; the drying temperature is 60–120℃ and the drying time is 2–6 h.