A laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials
By employing a three-stage remelting energy matching method, a gradient energy incremental scanning mode, and a multi-scale verification process, the defects of laser selective melting technology in the forming of difficult-to-weld materials were solved, enabling the manufacturing of high-density and high-performance aerospace components, while reducing costs and time.
Patent Information
- Application Number
- CN202611410930.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing laser selective melting technology cannot effectively solve defects such as hot cracking, lack of fusion, porosity and spheroidization when manufacturing difficult-to-weld materials. Moreover, the process parameter adjustment depends on experience, resulting in high cost and low efficiency, and it cannot be adapted to many types of high-temperature alloys and intermetallic compound materials.
A three-stage remelting energy matching method is adopted, which uses a gradient energy increment mode of initial melting scan, first-stage remelting scan and second-stage remelting scan, combined with multi-scale progressive verification and directional iterative optimization process, to achieve crack-free, high-density precision forming of difficult-to-weld materials.
It significantly suppresses micro and macro hot cracks, improves component density and mechanical properties, shortens process development cycle, reduces costs, and is suitable for the rapid industrial application of various difficult-to-weld materials.
Smart Images

Figure CN123103015A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser selective melting precision forming process technology for metal additive manufacturing, specifically a three-stage remelting energy matching forming method for difficult-to-weld materials using laser selective melting. Background Technology
[0002] Laser selective melting technology, with its advantages of high precision, moldlessness, and rapid prototyping of complex and precision components, has become the mainstream manufacturing technology for core metal components of aero-engines, gas turbines, and high-end new energy equipment. Compared with traditional forging and casting processes, laser selective melting technology can achieve integrated molding of complex internal cavities, thin walls, and irregularly shaped components, significantly shortening the research and development and production cycle. Currently, high-end aerospace components extensively utilize high-performance materials such as precipitation-strengthened nickel-based superalloys, cobalt-based superalloys, and titanium-aluminum intermetallic compounds. These materials possess excellent properties such as high temperature resistance, high strength, corrosion resistance, and fatigue resistance. However, their metallurgical characteristics are poor, making them typical difficult-to-weld and highly crack-sensitive materials. They have a wide solid-liquid temperature range, a variety of alloying elements, severe solidification segregation, and enrichment of low-melting-point eutectic phases at grain boundaries. During the non-equilibrium metallurgical process of rapid laser melting and solidification, they are prone to defects such as intergranular thermal cracks, interlayer incomplete fusion, internal porosity, spheroidization, and residual stress concentration. These defects severely reduce the density, mechanical properties, and service reliability of components, greatly limiting the large-scale application of laser selective melting technology in the manufacturing of high-end difficult-to-weld material components.
[0003] Currently, the technical means to improve the quality of laser selective melting forming of difficult-to-weld materials are mainly divided into two categories, both of which have obvious technical shortcomings. One category is a single-parameter optimization single-pass melting process. This process optimizes basic parameters such as laser power, scanning speed, scanning spacing, and layer thickness in a single dimension through orthogonal experiments and response surface methodology. It can only slightly reduce porosity and cannot suppress hot cracking at its source. This process uses a fixed energy single scan. When increasing the energy input to eliminate porosity, it will cause severe heat accumulation and directly induce intergranular hot cracks. When reducing the energy input to avoid cracks, a large number of unfused defects will appear. There is a core contradiction between energy input and defect suppression, making it impossible to balance the integrity of the forming and metallurgical quality. Another type is the traditional single-layer single-remelting process. After the initial melting of the single-layer powder, a set of fixed parameters is used to perform an overall remelting scan of the cladding layer. Although this approach can improve surface smoothness to a certain extent, it does not distinguish the metallurgical functional differences between the initial melting and remelting. Using uniform energy parameters for scanning means that if the remelting energy is too low, it cannot eliminate the micro-pores and overlapping defects within the layer. If the remelting energy is too high, it will cause surface overheating, coarse grains, and a surge in thermal stress. This not only fails to suppress cracks but also expands the crack propagation range. At the same time, the existing remelting process lacks graded energy matching logic and standardized parameter screening procedures, relying entirely on the operator's experience and a large number of trial and error experiments.
[0004] Overall, existing technologies lack a graded energy matching mechanism, and the energy ratio of the initial melting and remelting processes is not theoretically constrained. Fixed-parameter remelting cannot meet the multi-stage metallurgical forming requirements of difficult-to-weld materials. Process debugging costs are high, and parameter determination relies entirely on blind trial and error, resulting in numerous test iterations, large powder consumption, long R&D cycles, and high labor costs. Defect suppression is incomplete, and it is impossible to simultaneously solve multiple defects such as hot cracking, lack of fusion, porosity, and spheroidization, making it difficult to achieve the required density and mechanical properties of formed components. The process has poor versatility, lacks a standardized parameter determination system, and requires re-exploration of parameters for different difficult-to-weld materials, making it impossible to batch adapt to various crack-sensitive materials such as high-temperature alloys and intermetallic compounds.
[0005] Therefore, in view of the above situation, there is an urgent need to develop a laser selective melting method for three-stage remelting energy matching to overcome the shortcomings in current practical applications. Summary of the Invention
[0006] The purpose of this invention is to provide a laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A laser selective melting method for three-stage remelting energy matching of refractory materials involves performing a three-stage scanning process—initial melting scan, first-stage remelting scan, and second-stage remelting scan—once for the powder layer to be formed in the same powder spreading process. The volumetric energy density of the three-stage scanning process satisfies the gradient increasing constraint: the volumetric energy density of the initial melting scan is less than that of the first-stage remelting scan, the volumetric energy density of the first-stage remelting scan is less than that of the second-stage remelting scan, and the volumetric energy density of the second-stage remelting scan is less than or equal to the critical crack energy threshold of the difficult-to-weld material to be formed.
[0008] As a further aspect of the present invention: the volumetric energy density of the initial melting scan is 20 J / mm². 3 ~40J / mm 3 It is used to achieve initial melting of powder to form a continuous, unbroken melt channel; The volumetric energy density of the first-stage remelting scan is 35 J / mm². 3 ~60J / mm 3 It is used to eliminate the defects of incomplete fusion at the junction of the micro-pores and melt channels caused by the initial melting process; The volumetric energy density of the secondary remelting scan is 50 J / mm². 3 ~80J / mm 3 It is used to reconstruct the metallurgical interface of the molten pool, refine the solidified grains, and release interlayer residual stress.
[0009] As a further aspect of the present invention: the process parameters of the three-level scanning process are determined through a multi-scale progressive process, which sequentially includes a single-pass molten pool initial screening step, a single-layer overlap verification step, and a block iterative optimization step.
[0010] As a further aspect of the present invention: the single-stage molten pool initial screening step specifically comprises: With fixed preset powder layer thickness, laser spot diameter, and forming environment parameters, single-pass scanning experiments were conducted for initial melting scan, first-level remelting scan, and second-level remelting scan, respectively. The morphology of the single-pass melt channel and the size of the melt pool were observed. Parameter combinations with spheroidization and agglomeration, severe spattering, overheating and oxidation, and melt channel fracture were eliminated. The candidate parameter range for each level of scanning was obtained with the melt pool depth being 1.0 to 1.5 times the powder layer thickness as the screening criterion.
[0011] As a further aspect of the present invention: the single-layer overlap verification step specifically comprises: Based on the combination of candidate intervals of parameters from each scanning level, multiple sets of three-level remelting parameter schemes are formed. The three-level scanning molding of single-layer powder is completed in sequence. The surface quality of single-layer molding and the overlap state of the melt channel are observed. The qualified three-level remelting parameter combinations are selected based on the criteria of melt channel overlap rate of 30% to 60%, smooth and continuous surface, no macroscopic pores and no overlap cracks.
[0012] As a further aspect of the present invention: the block iterative optimization step specifically comprises: Block samples were prepared using the qualified parameter combination obtained through screening. The defect state and density of the samples were tested. The process parameters were adjusted in a targeted manner according to the test results until the samples had no macroscopic or microscopic intergranular thermal cracks and the density was greater than or equal to 99.2%. At this point, the parameter combination was locked as the optimal process parameters.
[0013] As a further aspect of the present invention: the rules for the directional adjustment of process parameters include: If macroscopic or microscopic thermal cracks appear in the sample, the volumetric energy density of the first-level remelting scan and the second-level remelting scan should be reduced simultaneously. If the sample has micropores or incomplete fusion defects, increase the volumetric energy density of the first-stage remelting scan; If the sample exhibits spheroidization, overheating, or coarse grains, reduce the laser power of the secondary remelting scan or increase the scanning speed.
[0014] As a further aspect of the present invention: the three-stage scanning process uses the same scanning trajectory, or adopts a scanning strategy of 67° rotation between layers.
[0015] As a further aspect of the present invention: the powder layer thickness during the molding process is 30μm to 60μm, the laser spot diameter is 50μm to 120μm, the molding chamber is protected by inert gas with an oxygen content of less than or equal to 100ppm, and the preheating temperature of the molding substrate is 80℃ to 120℃.
[0016] As a further aspect of the present invention: the difficult-to-weld material is a precipitation-strengthened nickel-based superalloy, cobalt-based superalloy, or titanium-aluminum intermetallic compound with a powder particle size of 15μm to 53μm.
[0017] Compared with the prior art, the beneficial effects of the present invention are: The defect suppression effect is significant, which can eliminate micro and macro thermal cracks in laser selective melting of difficult-to-weld materials, effectively solve common defects such as interlayer lack of fusion, micropores, and spheroidization, and greatly improve the quality of component forming. With excellent molding precision and performance, the component density is stable at over 99.2%, the grain structure is uniform, the residual stress is low, and the mechanical properties, fatigue resistance and high temperature resistance are significantly improved, which can meet the service standards of high-end aerospace components. It has significant advantages in cost reduction and efficiency improvement. The standardized iterative process can reduce blind trials by more than 80%, greatly save metal powder, equipment energy consumption, manpower and time costs, and shorten the process development cycle by more than 60%. It has strong engineering versatility and can be adapted to various difficult-to-weld materials such as nickel-based high-temperature alloys, cobalt-based high-temperature alloys, and intermetallic compounds. It can also be adapted to the forming of various precision and complex structural components, and can be quickly industrialized and applied. Attached Figure Description
[0018] Figure 1 This is a process flow diagram of the three-stage remelting energy matching forming method for laser selective melting of difficult-to-weld materials in an embodiment of the present invention.
[0019] Figure 2 The images shown are metallographic defect diagrams formed using conventional processes and metallographic diagrams formed using step-by-step remelting, as described in this embodiment of the invention. Among them, (a) is the metallographic structure of the conventional melting strategy, and (b) is the metallographic structure of the step-by-step remelting strategy.
[0020] Figure 3 The density results of CT detection for the three-stage remelting process in this embodiment of the invention are shown.
[0021] Figure 4 This is a comparative experimental curve of component density and crack rate under different energy ratios in an embodiment of the present invention. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.
[0024] Please see Figures 1-4 This invention provides a three-stage remelting energy matching forming method for laser selective melting of refractory materials. Addressing the challenges of simultaneously managing hot cracks and porosity defects during laser selective melting of crack-sensitive refractory metals, and the reliance on trial-and-error for process parameter adjustments, this method employs a three-stage gradient energy-increasing scanning mode consisting of initial melting scan, first-stage remelting scan, and second-stage remelting scan. Combined with multi-scale progressive verification and directional iterative optimization processes, this achieves crack-free, high-density precision forming of refractory materials.
[0025] Step S1: Material property acquisition and presetting of basic molding parameters The core thermal properties and critical performance parameters of the difficult-to-weld material to be formed are obtained in advance, including the solid-liquid phase temperature range, thermal conductivity at room temperature and high temperature, specific heat capacity, latent heat of fusion, solidification shrinkage rate, and critical crack energy threshold of the material; wherein, the critical crack energy threshold of the material is the maximum volumetric energy density of the material without generating micro-thermal cracks.
[0026] Commercial slicing software was used to slice the 3D model of the part to be molded into layers to obtain the scanning trajectory data of each layer cross section. Based on the material properties and component accuracy requirements, the thickness t of the base powder layer was preset. At the same time, the laser spot diameter and molding chamber environmental parameters were fixed, with the oxygen content in the molding chamber ≤100ppm and the preheating temperature of the molding substrate 80℃~120℃, to eliminate the interference of environmental variables on the molding process and test results.
[0027] This step is applicable to difficult-to-weld materials such as precipitation-strengthened nickel-based superalloys, cobalt-based superalloys, and titanium-aluminum intermetallic compounds with a powder particle size of 15μm to 53μm, which are crack-sensitive difficult-to-weld metal powders.
[0028] By presetting the parameters in this step, the basic experimental conditions can be standardized, the interference of environmental and basic process variables on subsequent parameter selection can be eliminated, and the accuracy and reproducibility of the optimization of the three-stage remelting process parameters can be guaranteed.
[0029] Step S2: Construct a mathematical model for energy matching in three-stage remelting. A three-layer progressive scanning process is set up, namely, the initial melting scanning process, the first-level remelting scanning process, and the second-level remelting scanning process. The volumetric energy density calculation formula for each scanning process is defined as follows: Ev(i)=P(i) / (v(i)×h(i)×t); In the formula: Ev(i) is the volumetric energy density of the i-th scanning process, in J / mm². 3 P(i) is the laser power of the i-th scanning process, in W; v(i) is the scanning speed of the i-th scanning process, in mm / s; h(i) is the scanning spacing of the i-th scanning process, in mm; t is the fixed powder layer thickness, in mm.
[0030] The core energy constraint relationship of the three-level process is established: the volumetric energy density of the initial melting scan < the volumetric energy density of the first-level remelting scan < the volumetric energy density of the second-level remelting scan, and the volumetric energy density of the second-level remelting scan ≤ the critical crack energy threshold of the material. While achieving the incremental energy gradient, the upper limit of heat input is controlled throughout the process to avoid the risk of hot crack initiation.
[0031] The energy ranges and corresponding functions for each scanning process are as follows: (1) The initial melting scanning volumetric energy density is 20 J / mm². 3 ~40J / mm 3 It is used to achieve initial melting of powder and form a continuous and unbroken melt channel, avoiding initial thermal cracks induced by high-energy heat accumulation through low energy input; (2) The volumetric energy density of the first-stage remelting scan is 35 J / mm². 3 ~60J / mm 3 It is used to perform secondary melting on the melt channel formed by the initial melting, and to eliminate the micro-pores in the layer and the defects of incomplete fusion at the overlap of the melt channel generated during the initial melting process. (3) The volumetric energy density of the secondary remelting scan is 50 J / mm². 3 ~80J / mm 3 It is used to reconstruct the metallurgical interface of the molten pool, refine the solidified grains, release interlayer residual stress, and at the same time avoid molten pool overheating and secondary crack initiation through energy upper limit constraints.
[0032] In this system, the energy level gradually increases, and cannot be less than or equal to the energy level of the previous level.
[0033] The three-stage scanning process uses the same scanning trajectory or a scanning strategy with 67° rotation between layers to ensure uniform overlap of the molten pool and avoid anisotropic defects in the formed structure.
[0034] The quantitative energy matching model established in this step can clarify the energy boundaries and functional positioning of each process level, break the traditional mode of irregular parameter adjustment, and resolve the inherent contradiction between hot cracks and porosity defects from the metallurgical mechanism level.
[0035] Step S3: Single-channel molten pool test to screen preliminary candidate intervals for each parameter level With fixed powder layer thickness, spot diameter and environmental parameters in step S1, single-pass scanning tests were carried out independently for the three-level processes of initial melting scan, first-level remelting scan and second-level remelting scan. By adjusting the laser power, scanning speed and scanning spacing parameters in a gradient manner, the morphology of the single-pass melt channel under different parameter combinations was obtained.
[0036] After the single-channel scanning test was completed, the observation sample was prepared using the standard metallographic sample preparation process of resin cold mounting, sandpaper step-by-step grinding and diamond suspension polishing. The morphology of the single-channel melt channel, the width of the melt pool and the depth of the melt pool were observed using an ultra-depth-of-field microscope and a laser confocal microscope. Unqualified parameter combinations with spheroidization and agglomeration, severe splashing, overheating oxidation and melt channel fracture were eliminated.
[0037] The parameter selection criteria are: the depth of the molten pool is 1.0 to 1.5 times the thickness of the powder layer to ensure effective metallurgical bonding between layers; finally, the parameter candidate ranges for each of the three processes are obtained, narrowing the parameter optimization range for subsequent single-layer forming tests.
[0038] By conducting preliminary screening on a single scale, obviously unqualified parameter combinations can be quickly eliminated, significantly reducing the workload of subsequent molding tests and improving the efficiency of parameter determination.
[0039] Step S4: Verification and screening of qualified parameter combinations for single-layer overlap molding Based on the candidate range of the three-level process parameters obtained in step S3, multiple sets of three-level remelting parameter schemes are combined to complete the complete single-layer step-by-step scanning forming of initial melting scan, first-level remelting scan, and second-level remelting scan in sequence.
[0040] The surface quality, melt channel overlap, surface porosity and cracks of single-layer molding are observed. The core judgment criteria are melt channel overlap rate of 30%~60%, smooth and continuous surface, no macroscopic porosity and no overlap cracks. Multiple qualified three-level remelting parameter combinations are screened out and enter the subsequent block iterative optimization stage.
[0041] By verifying the overlap at a single-layer scale, the in-layer forming quality and overlap matching of parameter combinations can be further checked, overlapping defects that cannot be detected by single-pass tests can be eliminated, and the basic quality of block forming can be guaranteed.
[0042] Step S5: Iterative molding of bulk specimens and locking of optimal parameters Using the qualified parameter combination obtained in step S4, standard block samples are printed. The preferred standard block samples are cubic samples of 10mm × 10mm × 10mm. After molding, samples are cut from the substrate using wire cutting. After grinding, polishing, and chemical etching, metallographic observation samples are prepared. Simultaneously, the Archimedes method is used to test the component density.
[0043] Anhydrous kerosene was used as the test medium, and the bulk density and relative density of the sample were calculated according to the standard test procedure of Archimedes' water displacement method.
[0044] Establish iterative optimization rules corresponding to defects, and adjust process parameters in a targeted manner based on sample test results: (1) If micro or macro hot cracks appear in the sample: simultaneously reduce the volumetric energy density of the first-level remelting scan and the second-level remelting scan to reduce heat accumulation and suppress crack propagation; (2) If the sample has a large number of micropores and incomplete fusion defects: prioritize increasing the volumetric energy density of the first-level remelting scan to enhance the fusion effect within the layer and eliminate pores and incomplete fusion defects; (3) If the sample exhibits spheroidization, overheating, or coarse grains: reduce the laser power of the secondary remelting scan or increase the scanning speed to reduce the peak heat input and avoid overheating of the molten pool.
[0045] When the sample meets the criteria of having no macroscopic or microscopic intergranular hot cracks and a component density ≥ 99.2%, this parameter combination is locked as the optimal three-stage remelting process parameter.
[0046] Through iterative optimization at the block scale and directional parameter tuning rules, parameters can be precisely adjusted for molding defects of different materials, eliminating the need for blind trial and error and quickly obtaining the optimal combination of process parameters that meets quality requirements.
[0047] Step S6: Batch of components are formally formed Using the optimal three-stage remelting process parameters locked in step S5, laser selective melting batch forming of the target parts is carried out; each layer of powder is scanned step by step in strict accordance with the order of initial melting scan, first-stage remelting scan, and second-stage remelting scan, and finally the integrated forming of the entire component is achieved.
[0048] In this method, the laser spot diameter remains consistent throughout the three-stage scanning process, ranging from 50μm to 120μm, ensuring uniformity in the molten pool size. The powder layer thickness ranges from 30μm to 60μm, adapting to the fine-grain forming requirements of difficult-to-weld materials. Argon gas protection is used during the forming process, with an oxygen content ≤100ppm in the forming chamber to prevent oxidation between the powder and the molten pool. The overlap rate of the weld channel is controlled between 30% and 60%, balancing forming efficiency and overlap integrity to avoid overlap defects.
[0049] Example 1: Three-stage remelting forming of cobalt-based superalloy K6509 This embodiment uses cobalt-based superalloy K6509 as the molding material, and the specific implementation process is as follows: (1) Preset basic parameters: K6509 cobalt-based alloy powder with a particle size of 15μm to 53μm was used, and the critical crack energy threshold of the material was pre-determined to be 82J / mm. 3 The preset powder layer thickness is 30μm, the laser spot diameter is 75μm, the oxygen content in the molding chamber is controlled at 80ppm, and the preheating temperature of the molding substrate is 100℃.
[0050] (2) Step-by-step energy matching setting: The volumetric energy density of the initial melting scan is 33 J / mm. 3 The volumetric energy density of the first-stage remelting scan is 46.6 J / mm². 3 The volumetric energy density of the secondary remelting scan is 66.6 J / mm². 3 It satisfies the increasing energy gradient relationship, and the secondary remelting energy is lower than the critical crack energy threshold of the material.
[0051] (3) Specific process parameters: Initial melting scan: laser power 120W, scanning speed 1200mm / s, scanning spacing 100μm; First-stage remelting scanning: laser power 140W, scanning speed 1000mm / s, scanning spacing 100μm; Secondary remelting scanning: laser power 180W, scanning speed 900mm / s, scanning interval 100μm.
[0052] (4) Molding effect: The depth of the single-pass melt pool is 35μm~42μm, which meets the requirement of 1.0 times to 1.5 times the thickness of the powder layer; the overlap rate of the single-layer molding melt channel is 45%, and the surface is flat without macroscopic defects; the block sample has no microscopic intergranular thermal cracks as observed by metallography, and the density measured by CT is 99.92%, and the molding quality is significantly better than the traditional single-melting process.
[0053] Example 2: Three-stage remelting of nickel-based superalloy GH5188 This embodiment uses nickel-based superalloy GH5188 as the molding material, and the specific implementation process is as follows: (1) Preset basic parameters: GH5188 nickel-based alloy powder with a particle size of 15μm to 53μm was used, and the critical crack energy threshold of the material was pre-determined to be 75J / mm. 3 The preset powder layer thickness is 30μm, the laser spot diameter is 70μm, the oxygen content in the molding chamber is controlled to be ≤100ppm, and the preheating temperature of the molding substrate is 100℃.
[0054] (2) Step-by-step energy matching setting: The volumetric energy density of the initial melting scan is 28 J / mm². 3 The volumetric energy density of the first-stage remelting scan is 42 J / mm². 3 The volumetric energy density of the secondary remelting scan is 58 J / mm². 3 It satisfies the increasing energy gradient relationship, and the secondary remelting energy is lower than the critical crack energy threshold of the material.
[0055] (3) Molding effect: The block component has no thermal cracks or pore defects, and the density can reach 99.99%. The uniformity of mechanical properties of the molded component is significantly improved.
[0056] It should be noted that the above embodiments are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited thereto. For those skilled in the art, within the scope of the technical principles disclosed in the present invention, any technical solution obtained by measuring the critical crack energy threshold of the corresponding material and making conventional adjustments according to the three-level energy matching rules and parameter iteration process of the present invention for different types of difficult-to-weld materials should be covered within the scope of protection of the present invention.
Claims
1. A method for three-stage remelting energy-matching forming of difficult-to-weld materials using laser selective melting, characterized in that, For the powder layer to be formed in the same powder spreading process, a three-level scanning process is performed in sequence: initial melting scan, first-level remelting scan, and second-level remelting scan. The volumetric energy density of the three-stage scanning process satisfies the gradient increasing constraint: the volumetric energy density of the initial melting scan is less than that of the first-stage remelting scan, the volumetric energy density of the first-stage remelting scan is less than that of the second-stage remelting scan, and the volumetric energy density of the second-stage remelting scan is less than or equal to the critical crack energy threshold of the difficult-to-weld material to be formed.
2. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 1, characterized in that, The volumetric energy density of the initial melting scan is 20 J / mm². 3 ~40J / mm 3 It is used to achieve initial melting of powder to form a continuous, unbroken melt channel; The volumetric energy density of the first-stage remelting scan is 35 J / mm². 3 ~60J / mm 3 It is used to eliminate the defects of incomplete fusion at the junction of the micro-pores and melt channels caused by the initial melting process; The volumetric energy density of the secondary remelting scan is 50 J / mm². 3 ~80J / mm 3 It is used to reconstruct the metallurgical interface of the molten pool, refine the solidified grains, and release interlayer residual stress.
3. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 1, characterized in that, The process parameters of the three-level scanning process are determined through a multi-scale progressive process, which includes a single-pass molten pool initial screening step, a single-layer overlap verification step, and a block iterative optimization step.
4. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 3, characterized in that, The specific steps of the single-stage molten pool initial screening are as follows: With fixed preset powder layer thickness, laser spot diameter, and forming environment parameters, single-pass scanning experiments were conducted for initial melting scan, first-level remelting scan, and second-level remelting scan, respectively. The morphology of the single-pass melt channel and the size of the melt pool were observed. Parameter combinations with spheroidization and agglomeration, severe spattering, overheating and oxidation, and melt channel fracture were eliminated. The candidate parameter range for each level of scanning was obtained with the melt pool depth being 1.0 to 1.5 times the powder layer thickness as the screening criterion.
5. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 3, characterized in that, The specific steps for verifying single-layer overlap are as follows: Based on the combination of candidate intervals of parameters from each scanning level, multiple sets of three-level remelting parameter schemes are formed. The three-level scanning molding of single-layer powder is completed in sequence. The surface quality of single-layer molding and the overlap state of the melt channel are observed. The qualified three-level remelting parameter combinations are selected based on the criteria of melt channel overlap rate of 30% to 60%, smooth and continuous surface, no macroscopic pores and no overlap cracks.
6. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 3, characterized in that, The block iterative optimization steps are as follows: Block samples were prepared using the qualified parameter combination obtained through screening. The defect state and density of the samples were tested. The process parameters were adjusted in a targeted manner according to the test results until the samples had no macroscopic or microscopic intergranular thermal cracks and the density was greater than or equal to 99.2%. At this point, the parameter combination was locked as the optimal process parameters.
7. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 6, characterized in that, The rules for directional adjustment of process parameters include: If macroscopic or microscopic thermal cracks appear in the sample, the volumetric energy density of the first-level remelting scan and the second-level remelting scan should be reduced simultaneously. If the sample has micropores or incomplete fusion defects, increase the volumetric energy density of the first-stage remelting scan; If the sample exhibits spheroidization, overheating, or coarse grains, reduce the laser power of the secondary remelting scan or increase the scanning speed.
8. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 1, characterized in that, The three-stage scanning process uses the same scanning trajectory, or adopts a scanning strategy of 67° rotation between layers.
9. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 1, characterized in that, During the molding process, the powder layer thickness is 30μm~60μm, the laser spot diameter is 50μm~120μm, the molding chamber is protected by inert gas with an oxygen content of less than or equal to 100ppm, and the preheating temperature of the molding substrate is 80℃~120℃.
10. The laser selective melting method for three-stage remelting energy matching of difficult-to-weld materials according to claim 1, characterized in that, The difficult-to-weld material is a precipitation-strengthened nickel-based superalloy, cobalt-based superalloy, or titanium-aluminum intermetallic compound with a powder particle size of 15μm to 53μm.