A method for additive manufacturing of metal parts using SLM based on interlaminar stress regulation

By dividing the stress control unit during the SLM forming process, obtaining temperature information and determining the local shrinkage direction, and generating candidate scanning paths, the problem of thermal shrinkage superposition in SLM forming is solved, and a more stable forming process and higher forming quality are achieved.

CN123103016APending Publication Date: 2026-11-17ZHEJIANG JIAHENG INTELLIGENT EQUIP MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611496718.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing SLM forming methods are difficult to effectively coordinate the superposition of thermal shrinkage in different local areas during the scanning process, resulting in warping, deformation or residual stress concentration in the formed parts, and failing to accurately reflect the overall shrinkage imbalance.

Method used

By dividing the stress control unit, obtaining temperature change information, determining the local shrinkage direction and shrinkage weight, mapping it to the next forming layer, generating candidate scanning paths, and calculating the shrinkage resultant and torque resultant through vector synthesis, selecting scanning paths that meet the conditions, and correcting the scanning paths layer by layer.

Benefits of technology

It improves the stress control stability during the SLM forming process, reduces residual stress concentration and forming deformation caused by local thermal shrinkage accumulation, and improves the forming quality of metal parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103016A_ABST
    Figure CN123103016A_ABST
Patent Text Reader

Abstract

This application discloses an additive manufacturing method for SLM metal parts based on interlayer stress control, comprising: dividing stress control units according to the projection overlap relationship between the current forming layer and the adjacent formed layers and the free contour position; determining the local shrinkage direction, shrinkage weight, and constraint reference point according to the temperature change information and interlayer constraint degree of each stress control unit; mapping the local shrinkage direction and shrinkage weight to the next forming layer to generate multiple candidate scanning paths; determining the shrinkage sum and shrinkage torque sum according to the shrinkage increment of each scanning segment within the cooling interaction time window, and determining the path shrinkage imbalance accordingly; selecting candidate scanning paths that meet preset conditions for forming, and updating according to subsequent temperature change information. This application can coordinate the thermal shrinkage effect of different regions during the forming process, reducing the residual stress and deformation risk caused by the continuous accumulation of local shrinkage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal additive manufacturing technology, and in particular to a method for SLM metal part additive forming based on interlayer stress regulation. Background Technology

[0002] Selective Laser Melting (SLM) is a metal additive manufacturing technology that uses metal powder as raw material and melts and solidifies it layer by layer by a laser along a preset scanning path. During the SLM forming process, the laser heat source is characterized by localized concentration and rapid movement. The molten area undergoes rapid heating, melting, and cooling solidification in a short period of time. Large temperature gradients are easily formed between adjacent areas and adjacent forming layers, resulting in uneven thermal shrinkage during the subsequent cooling process.

[0003] Existing SLM forming methods typically reduce heat accumulation and residual stress by adjusting the scanning direction, scanning sequence, laser power, scanning speed, or by employing zonal scanning. For example, the scanning direction can be changed at a fixed angle between adjacent forming layers, or the scanning parameters of the next forming layer can be adjusted according to the temperature state of the forming region. These methods can improve the temperature distribution during the forming process to some extent, but different regions are constrained by adjacent formed layers, free contours, and local geometry to varying degrees. Even with similar temperature changes, their actual thermal shrinkage trends may differ.

[0004] Meanwhile, during continuous scanning of the same forming layer, the thermal shrinkage generated in different scanning areas is not independent, and the local shrinkage formed successively may still superimpose within a certain cooling time. When the shrinkage direction, location, and timing of multiple local areas are different, adjusting the scanning path based solely on the temperature, stress direction, or final scanning result of a single area is insufficient to reflect the overall shrinkage imbalance caused by the superposition of local thermal shrinkage during the forming process. This can easily lead to the continuous accumulation of shrinkage in the same direction or location in local areas, resulting in warping, deformation, or residual stress concentration in the formed part. Therefore, there is still room for improvement in how to coordinate the shrinkage of different local areas during the scanning process by combining the interlayer constraint state and the actual cooling process, and determine the scanning path of subsequent forming layers accordingly. Summary of the Invention

[0005] Therefore, it is necessary to propose an SLM metal part additive manufacturing method based on interlayer stress control to address the above problems.

[0006] A method for additive manufacturing of metal parts using SLM based on interlayer stress regulation, the method comprising: acquiring layer data of the metal part to be formed, and dividing the current forming layer into multiple stress regulation units according to the projection overlap relationship between the current forming layer and the adjacent formed layers and the free contour position; After completing the current forming layer scan, the temperature change information of each stress control unit is obtained in the preset cooling stage. The local shrinkage direction and shrinkage weight of each stress control unit are determined according to the temperature gradient direction, cooling attenuation characteristics and interlayer constraint degree. The constraint reference point is determined according to the interlayer constraint degree of each stress control unit. The local shrinkage direction and shrinkage weight are mapped to the next forming layer to generate multiple candidate scanning paths with different scanning orders and scanning directions. The shrinkage increment of each scanning segment in each candidate scanning path within a preset cooling interaction time window is calculated. The shrinkage increment is vector-synthesized to obtain the shrinkage resultant. The shrinkage torque resultant is determined according to the position of each shrinkage increment relative to the constraint reference point. The path shrinkage imbalance is determined according to the shrinkage resultant and the shrinkage torque resultant. Select a candidate scanning path whose path shrinkage imbalance meets the preset conditions to selectively laser melt the next forming layer, and update the local shrinkage direction and shrinkage weight according to the temperature change information after scanning the next forming layer, until the additive forming is completed.

[0007] In at least one embodiment of this application, determining the degree of interlayer constraint includes: Transform the contour data of the current forming layer and the adjacent formed layers into the same forming coordinate system, and divide the current forming layer into multiple local units; The projection overlap ratio between each local unit and the adjacent formed layer, the distance from each local unit to the nearest free contour boundary, and the amount of local contour change between adjacent formed layers are determined respectively. The projection overlap ratio, the distance, and the local contour change are normalized, and the interlayer constraint degree of each local unit is determined based on the normalization result. Local units that are spatially continuous and whose interlayer constraint degree is within the same preset range are merged into the stress control unit.

[0008] In at least one embodiment of this application, determining the constraint reference point includes: Obtain the geometric center coordinates and unit area of ​​each stress control unit. Use the product of the interlayer constraint degree of the corresponding stress control unit and the unit area as the coordinate weight, perform a weighted summation on the geometric center coordinates, and determine the constraint reference point by the ratio of the weighted summation result to the sum of the coordinate weights.

[0009] In at least one embodiment of this application, the temperature distribution of each stress control unit is acquired at at least three detection times after the laser scanning of the current forming layer stops, the cooling attenuation characteristics are determined based on the temperature changes between different detection times, and the temperature gradient direction is determined based on the temperature spatial changes inside the stress control unit at the same detection time. The free contraction direction of the stress control unit pointing to its corresponding free contour boundary is determined. The local contraction direction is obtained by vector synthesis based on the temperature gradient direction, the free contraction direction and the degree of interlayer constraint. The contraction weight is determined based on the cooling attenuation characteristics and the degree of interlayer constraint.

[0010] In at least one embodiment of this application, each candidate scan path is divided into multiple sequentially executed scan segments according to the boundary of the stress control unit; For any scan segment, the local contraction direction of the stress control unit where the scan segment is located is taken as the direction of the corresponding contraction increment, and the magnitude of the contraction increment is determined according to the contraction weight of the stress control unit, the effective scan length of the scan segment, and the time decay coefficient corresponding to the scan segment after execution.

[0011] In at least one embodiment of this application, the preset cooling interaction time window is determined based on the cooling attenuation characteristics of the stress control unit corresponding to the current forming layer; The initial temperature rise is taken as the temperature rise of the region at the end of the scan. When the temperature rise of the corresponding region drops to a preset ratio of the initial temperature rise, the time between the end of the scan and the arrival of the preset ratio is determined as the cooling interaction time of the corresponding stress control unit. The preset cooling interaction time window is determined according to the cooling interaction time of multiple stress control units. The time decay coefficient is determined based on the ratio of the remaining temperature rise after the scan segment is executed to the initial temperature rise.

[0012] In at least one embodiment of this application, when each scan segment of the candidate scan path is completed, each shrinkage increment that has not yet decayed within the preset cooling interaction time window is determined, and each shrinkage increment is vector-summed to obtain the current shrinkage sum. Determine the position vector of each contraction increment relative to the constraint reference point, and determine the current contraction torque resultant based on the vector product of the position vector and the corresponding contraction increment; The peak value of the magnitude of the current contraction sum and the peak value of the absolute value of the current contraction torque sum are obtained during the entire scanning process of the candidate scanning path, and the path contraction imbalance is determined based on the two peak values.

[0013] In at least one embodiment of this application, generating the candidate scan path includes: After determining the currently executed scan segment, calculate the current contraction sum and the current contraction torque sum corresponding to each unscanned segment after it is added to the current scan sequence; The unscanned segment that reduces at least one of the current contraction sum and the current contraction torque sum, and whose other does not exceed the corresponding preset growth range, is preferentially selected as the next scanned segment, and the execution order of the scanned segments is determined in the manner described above to form at least one candidate scanned path.

[0014] In at least one embodiment of this application, when none of the generated candidate scanning paths meet the preset condition for the path contraction imbalance, a target scanning segment is determined to make the absolute value of the current contraction torque reach the corresponding peak value for the first time, and the target scanning segment is divided into a first scanning sub-segment and a second scanning sub-segment. If there is an unscanned segment where the direction of the generated contraction torque is opposite to the direction of the current contraction torque sum corresponding to the peak value, the unscanned segment is inserted between the first scanned segment and the second scanned segment, and the path contraction imbalance is recalculated to obtain the adjusted candidate scanned path.

[0015] In at least one embodiment of this application, a first layer image is acquired at the first detection moment after the next forming layer is scanned, and a second layer image is acquired after a preset cooling. The actual shrinkage displacement of the corresponding stress control unit is determined based on the coordinate changes of the corresponding melting contour feature points in the first layer image and the second layer image. The direction of the actual contraction displacement is compared with the corresponding local contraction direction, and the relative magnitude of the actual contraction displacement is compared with the corresponding contraction weight. When the deviation of the comparison result exceeds the corresponding calibration threshold, the local shrinkage direction or shrinkage weight of the stress control unit in the subsequent forming layer is corrected. The SLM additive manufacturing method for metal parts based on interlaminar stress regulation, as described in this embodiment, will have at least the following beneficial effects: 1. By dividing stress control units according to the projection overlap relationship between the current forming layer and the adjacent formed layers and the free contour position, and combining the temperature gradient direction, cooling attenuation characteristics and interlayer constraint degree, the local shrinkage direction and shrinkage weight of each stress control unit are determined. This allows the judgment of the thermal shrinkage state of the forming area to consider both the actual thermal response and the interlayer structural constraint, and can more accurately reflect the shrinkage tendency of different local areas during the cooling process.

[0016] 2. By mapping the local shrinkage direction and shrinkage weight to the next forming layer, and calculating the shrinkage increment of each scanning segment in the candidate scanning path within the preset cooling interaction time window, the scanning path evaluation can take into account the thermal shrinkage effect of different scanning segments that has not yet completely decayed in time, and avoid ignoring the dynamic shrinkage superposition between different regions when determining the scanning path based solely on the temperature or final state of a single region.

[0017] 3. By vector synthesis of each shrinkage increment to obtain the total shrinkage amount, and the total shrinkage torque to be determined according to the position of each shrinkage increment relative to the constraint reference point, the path shrinkage imbalance to be determined according to the total shrinkage amount and the total shrinkage torque, so that the evaluation of the candidate scanning path reflects the overall imbalance of the shrinkage action in different regions in the direction and the deflection trend generated by different action positions. Based on this, the candidate scanning path that meets the preset conditions is selected, which is beneficial to reduce the residual stress concentration and forming deformation caused by the continuous accumulation of local thermal shrinkage in the same direction or the same position.

[0018] 4. By continuing to acquire temperature change information after the next forming layer is scanned, and updating the local shrinkage direction and shrinkage weight of the corresponding area, the scanning path of subsequent forming layers can be corrected layer by layer according to the actual forming state, thereby adapting to the changes in thermal state and constraint state at different heights and cross-sectional positions of the metal part, and improving the stress control stability in the SLM layer-by-layer forming process. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] in: Figure 1 This is a schematic flowchart of an SLM metal part additive manufacturing method based on interlaminar stress regulation, provided as an embodiment of this application.

[0021] Figure 2 This is a schematic diagram of the stress control unit division and constraint reference points in the current forming layer provided in the embodiments of this application.

[0022] Figure 3 This is a schematic diagram of the candidate scanning path, scanning segment, and scanning direction provided in the embodiments of this application.

[0023] 201. Current forming layer; 202. Projected outline of adjacent formed layers; 204-1~204-9, Stress control unit; 205. Constraint reference points.

[0024] 301. Candidate scan path; 303. Constraint reference point; 304. Candidate scan path. Detailed Implementation

[0025] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0026] This application provides a method for additive manufacturing of metal parts using SLM (Selective Laser Melting) based on interlayer stress regulation. This method can be applied to SLM additive manufacturing equipment that uses a metal powder bed and scanning laser for layer-by-layer selective melting, such as equipment that uses a fiber laser in conjunction with a galvanometer scanning mechanism to melt stainless steel powder, titanium alloy powder, aluminum alloy powder, nickel-based alloy powder, or other metal powders suitable for selective laser melting layer by layer. The metal part to be formed can be a structural part, a shell part, a mold part, a complex flow channel part, a lightweight component, or other three-dimensional part that can be formed by layer-by-layer melting of metal powder.

[0027] In one specific embodiment, the SLM device includes a forming chamber, a powder supply mechanism, a powder spreading mechanism, a forming platform, a laser, a galvanometer scanning assembly, a temperature detection assembly, and a controller. The powder supply mechanism provides metal powder to the forming area; the powder spreading mechanism forms a metal powder layer of a preset thickness on the forming platform or the surface of an existing formed layer; the laser generates a scanning laser capable of melting the corresponding metal powder; the galvanometer scanning assembly controls the laser beam to move within the current formed layer according to the scanning path generated by the controller; the temperature detection assembly acquires information on the temperature distribution and temperature change over time of the formed layer after laser scanning; and the controller performs tasks such as three-dimensional model layering, stress control unit division, determination of interlayer constraint degree, determination of local shrinkage direction and shrinkage weight, generation of candidate scanning paths, calculation of path shrinkage imbalance, and selection of scanning paths.

[0028] The temperature detection component can be an infrared thermal imager, a coaxial infrared detection component, or a non-contact temperature detection device positioned above the forming chamber. Preferably, the detection area of ​​the temperature detection component covers the current forming layer and can continuously acquire the two-dimensional temperature distribution of the forming layer after laser scanning at preset time intervals.

[0029] In a further embodiment, the SLM device may also include a layer image acquisition component. The layer image acquisition component may be an industrial camera positioned above the forming chamber, a coaxial vision inspection component, or other imaging component capable of acquiring changes in the contour position of the forming area, used to calibrate the local shrinkage direction and shrinkage weight in subsequent embodiments.

[0030] It should be noted that this application does not simply determine whether there is large residual stress in the forming layer based on the highest or average temperature of the current forming layer, nor does it simply change the scanning direction of adjacent forming layers at a fixed angle. Instead, it considers the temperature change state of different local areas, the interlayer constraint state between the forming layer and the adjacent formed layers, and the positional relationship of the local area relative to the free contour. The above information is used to determine the local shrinkage direction and shrinkage weight of different local areas during the cooling process.

[0031] Furthermore, this application does not only independently determine the scanning direction for a single stress control unit, but also considers that the contraction effect generated by multiple scanning segments in the same candidate scanning path within a certain cooling time range may still be superimposed on each other. The contraction effect is vector-synthesized to obtain the contraction resultant, and the contraction torque resultant is determined according to the position of each contraction effect relative to the constraint reference point to evaluate different candidate scanning paths, thereby reducing the possibility that multiple local contraction effects will continue to accumulate in the same direction or at the same position during continuous scanning.

[0032] For ease of explanation, the following description uses SLM layer-by-layer forming with 316L stainless steel powder as an example. In an exemplary case, the metal powder layer thickness can be set to 0.03 mm to 0.05 mm, and the laser power and scanning speed are set according to a pre-determined stable melting process window based on the powder material and equipment. It should be noted that the above-mentioned material types and process parameter ranges are only used to illustrate one specific embodiment of the technical solution of this application and do not constitute a limitation on the scope of protection of this application.

[0033] like Figure 1 As shown, in one embodiment, an SLM metal part additive manufacturing method based on interlaminar stress regulation includes the following steps.

[0034] S101: Obtain the layer data of the metal part to be formed, and divide the current forming layer into multiple stress control units according to the projection overlap relationship between the current forming layer and the adjacent formed layers and the free contour position.

[0035] In this step, it should be noted that the 3D model of the metal part to be formed can be in STL, STEP, or other data formats that can describe the 3D contour of the metal part. The controller layers the 3D model along the forming direction of the metal part according to the preset forming layer thickness, thereby obtaining multiple 2D slice sections in sequence.

[0036] For any current forming layer 201, coordinate correspondence is established between the current forming layer 201 and the adjacent formed layer below it that has already been melted and formed, so that the contour data of the two forming layers are transformed to the same forming coordinate system.

[0037] like Figure 2 As shown, reference numeral 201 indicates the current forming layer, and reference numeral 202 indicates the projected contour of the adjacent formed layer. The controller divides the current forming layer 201 into multiple local units and determines the projection overlap ratio between each local unit and the adjacent formed layer, the distance from each local unit to the nearest free contour boundary, and the amount of local contour change between adjacent forming layers.

[0038] For the i-th local unit, its area in the current forming layer 201 can be denoted as Ai, and the area of ​​its projection overlapping with that of the adjacent formed layer can be denoted as Aoi. The corresponding projection overlap ratio Ri can then be expressed as: Ri=Aoi / Ai.

[0039] When Ri is closer to 1, it indicates that the current local unit has a large area of ​​formed metal below the forming direction; when Ri decreases, it indicates that the degree of overlap between the projection of the current local unit and the formed area below decreases.

[0040] Furthermore, the shortest distance di from the geometric center of the i-th local unit to the nearest free contour boundary can be determined. The free contour boundary can be understood as the boundary of one side of the current forming layer 201 that is not further constrained by other solid regions in the same layer.

[0041] Simultaneously, the local contour of the current forming layer 201 is compared with the corresponding local contour of the adjacent formed layer to determine the local contour change amount Ci. The local contour change amount Ci can be determined based on the non-overlapping area ratio of the corresponding regions of the two forming layers, the boundary offset distance, or a combination of the two.

[0042] In one embodiment, the projection overlap ratio Ri, the free contour distance di, and the local contour change Ci can be normalized to obtain R'i, d'i, and C'i.

[0043] Subsequently, the interlayer constraint degree Ki of the i-th local unit can be determined based on the normalized parameters.

[0044] For example, in one exemplary implementation, it can be represented as: Ki=a1×R'i+a2×d'i+a3×(1-C'i); Where a1, a2 and a3 represent the weighting coefficients corresponding to the projection overlap ratio, free contour distance and local contour change, respectively, and a1+a2+a3=1.

[0045] The above formula is mainly used to illustrate one way of determining the degree of interlayer constraint Ki based on multiple geometric parameters. In other embodiments, the degree of interlayer constraint can also be determined based on a pre-established geometric constraint calibration table, a piecewise function, or other calculation methods that can reflect the degree of constraint of the current local region on adjacent formed layers.

[0046] The controller further merges regions based on the interlayer constraint levels of multiple local units. When multiple adjacent local units are spatially continuous and their corresponding interlayer constraint levels are within the same preset range, they can be merged into a single stress control unit.

[0047] like Figure 2 As shown in the figure, reference numerals 204-1 to 204-9 respectively represent the multiple stress control units obtained by division.

[0048] It should be noted that each stress control unit is not required to have the same area or a regular rectangular shape, but is divided according to the actual contour of the current forming layer and the corresponding degree of interlayer constraint. Therefore, when the current forming layer has abrupt changes in cross-section, thin walls, overhanging connection areas, or significant changes in local contour, stress control units with different areas and shapes can be formed.

[0049] The technical solution of this embodiment, by simultaneously considering the projection overlap relationship between the current forming layer and the adjacent formed layers, the free contour position, and the local contour changes, enables subsequent stress control to no longer be based solely on the planar temperature state of the current forming layer, but to further reflect the differences in the constraints of the underlying formed structure on different regions.

[0050] S102: After completing the current forming layer scan, acquire the temperature change information of each stress control unit in the preset cooling stage, determine the local shrinkage direction and shrinkage weight of each stress control unit according to the temperature gradient direction, cooling attenuation characteristics and interlayer constraint degree, and determine the constraint reference point according to the interlayer constraint degree of each stress control unit.

[0051] In this step, it should be noted that after the current forming layer 201 completes selective laser melting, the temperature detection component continuously or intermittently acquires the temperature distribution of the current forming layer 201 within a preset cooling time period.

[0052] In one embodiment, a two-dimensional temperature distribution can be obtained at at least three different detection times t1, t2, and t3 after the laser completes the scanning of the current forming layer, wherein t1 < t2 < t3.

[0053] For example, the three detection times can be set according to the forming speed of the SLM equipment, the thermal diffusion characteristics of the material, and the sampling frequency of the infrared detection component. When the metal powder cools quickly, the time interval between adjacent detection times can be set shorter; when the local area cools slowly, the detection time can be appropriately extended.

[0054] For any stress control unit 204-i, calculate the average temperature or characteristic temperature Ti(t1), Ti(t2) and Ti(t3) of the stress control unit at different detection times, and determine the corresponding cooling attenuation characteristics accordingly.

[0055] For example, the temperature drop per unit time can be used as a characterization parameter for cooling degradation. Vi = [Ti(t1) - Ti(t3)] / (t3 - t1).

[0056] The temperature rise attenuation ratio of the current stress control unit relative to the forming chamber reference temperature T0 can also be used as a cooling attenuation characteristic, for example: Qi = [Ti(t1) - Ti(t3)] / [Ti(t1) - T0].

[0057] The Vi and Qi mentioned above can be used individually or combined to form the cooling attenuation characteristics of the corresponding stress control unit.

[0058] Furthermore, the direction of the temperature gradient is determined based on the temperature distribution at different locations within the stress control unit at the same detection time.

[0059] For example, the stress control unit is divided into multiple temperature sampling positions, and the temperature value and planar coordinates of each sampling position are obtained. The temperature gradient is obtained based on the spatial variation of the temperature value in the X and Y directions. ∇Ti=(∂Ti / ∂x,∂Ti / ∂y).

[0060] The direction of the temperature gradient ∇Ti can be used as the direction of the temperature gradient corresponding to the stress control unit.

[0061] For situations where there are local fluctuations in temperature distribution, the dominant temperature gradient direction of the stress control unit can be obtained by using regional averaging, local fitting, or least squares methods, so as to reduce the impact of a single abnormal temperature pixel on the direction judgment.

[0062] Furthermore, the corresponding free shrinkage direction is determined based on the positional relationship between the stress control unit 204-i and the free contour of the current forming layer 201.

[0063] For example, the shortest distance line can be drawn from the geometric center of the stress control unit 204-i to the nearest free contour boundary, and the direction corresponding to the shortest distance line can be taken as the free contraction direction ufi of the stress control unit.

[0064] When a stress control unit is adjacent to multiple free profile boundaries, the weights of multiple candidate free contraction directions can be determined based on the corresponding distances and boundary lengths of each free profile boundary, and the final free contraction direction can be obtained through vector synthesis.

[0065] Subsequently, the local contraction direction ui is determined based on the temperature gradient direction, the free contraction direction, and the interlayer constraint degree Ki corresponding to the stress control unit.

[0066] For example, the temperature gradient direction and the free contraction direction can be converted into unit direction vectors uTi and ufi, respectively, and expressed as: ui = Norm(b1i × uTi + b2i × ufi); Where Norm represents normalization of the vector, and b1i and b2i are the corresponding direction weight coefficients.

[0067] In one embodiment, the directional weighting coefficient can be determined based on the degree of interlayer constraint Ki. For example, when the degree of interlayer constraint is high, the weight corresponding to the temperature gradient direction is increased; when the stress control unit is adjacent to the free profile and the degree of interlayer constraint is low, the weight corresponding to the free contraction direction is increased.

[0068] The aforementioned weighting relationships can be predetermined through preliminary sample calibration, numerical simulation, or empirical parameters of the equipment.

[0069] It should be noted that the local contraction direction ui in this application is used to characterize the main contraction trend of the corresponding stress control unit under the combined action of the current thermal state and structural constraints, and its value is not required to be directly equivalent to the actual residual stress direction.

[0070] Furthermore, the shrinkage weight Wi of the corresponding stress control unit is determined based on the cooling attenuation characteristics and the degree of interlayer constraint Ki.

[0071] For example, it can be represented as: Wi = c1 × V'i + c2 × Ki; Where V'i represents the normalized cooling decay characteristic, and c1 and c2 represent the corresponding weighting coefficients.

[0072] In another embodiment, the shrinkage weight can be determined by multiplying the cooling attenuation characteristics with the degree of interlayer constraint, so that regions with both a faster cooling process and a higher degree of structural constraint can obtain a larger shrinkage weight.

[0073] Therefore, each stress control unit corresponds to a local contraction direction ui and a contraction weight Wi.

[0074] Furthermore, constraint reference point 205 is determined based on the degree of interlayer constraint of each stress control unit.

[0075] like Figure 2 As shown in the figure, reference numeral 205 indicates the constraint reference point.

[0076] For the i-th stress control element, its geometric center coordinates are denoted as Pi=(xi,yi), the element area is denoted as Ai, and the product of the interlayer constraint degree Ki of the stress control element and the element area Ai is used as the coordinate weight.

[0077] Therefore, the constraint reference point P0 can be expressed as: P0=Σ(Ki×Ai×Pi) / Σ(Ki×Ai).

[0078] The summation range includes multiple stress control units within the current forming layer 201 used for stress control.

[0079] In the above manner, the stress control unit with a larger area and a higher degree of interlayer constraint has a greater influence on the position of the constraint reference point 205, so that the constraint reference point 205 can be used to characterize the position where the overall constraint effect is more concentrated in the current forming layer.

[0080] It should be noted that the constraint reference point 205 is mainly used to determine the torque effect formed by the shrinkage increment corresponding to different scanning segments relative to the overall constraint position of the current forming layer. It does not indicate that there are actual mechanical hinge points or fixed fulcrums inside the metal part.

[0081] The technical solution of this embodiment converts temperature changes, temperature gradients, and geometric constraint states into local shrinkage directions and shrinkage weights, and further determines the constraint reference points of the current forming layer, so that different local areas can be evaluated for subsequent shrinkage effects within a unified forming coordinate system.

[0082] S103: Map the local shrinkage direction and shrinkage weight to the next forming layer to generate multiple candidate scanning paths with different scanning orders and scanning directions. Calculate the shrinkage increment of each scanning segment in each candidate scanning path within a preset cooling interaction time window. Perform vector synthesis on each shrinkage increment to obtain the shrinkage resultant. Determine the shrinkage torque resultant based on the position of each shrinkage increment relative to the constraint reference point. Determine the path shrinkage imbalance based on the shrinkage resultant and the shrinkage torque resultant.

[0083] In this step, it should be noted that after determining the local shrinkage state of the current forming layer 201, the controller maps the local shrinkage direction ui and shrinkage weight Wi of each stress control unit to the corresponding position of the next forming layer according to the coordinate correspondence between the current forming layer 201 and the next forming layer.

[0084] For regions in the next forming layer that still have a projection correspondence with the current stress control unit, the corresponding local contraction direction and contraction weight can be inherited as the initial control parameters when generating the candidate scan path for the next layer.

[0085] For locations in the next forming layer where a corresponding region does not exist in the current forming layer, the initial local shrinkage direction and shrinkage weight can be determined based on the parameters of the adjacent stress control unit, the constraint state of the adjacent formed layer, or the preset basic parameters.

[0086] Subsequently, the controller generates multiple candidate scan paths for the next forming layer.

[0087] like Figure 3 As shown, reference numerals 301 and 304 represent candidate scan paths with different scan directions or scan sequences, respectively, and reference numeral 303 represents the corresponding constraint reference point.

[0088] Candidate scanning paths can adopt parallel reciprocating scanning, partitioned parallel scanning, or other scanning forms suitable for SLM forming, and multiple candidate schemes can be formed by changing the scanning direction, scanning start position, and execution order of each scanning area.

[0089] For example, for the same forming layer, a first candidate scanning path and a second candidate scanning path can be generated, wherein the main scanning direction of the first candidate scanning path is set along the X direction, and the main scanning direction of the second candidate scanning path is set along the Y direction.

[0090] In other embodiments, candidate scanning directions that form a preset angle with the X direction can also be set, such as 45°, 90°, 135°, or other scanning directions allowed by the device control system.

[0091] It should be noted that the number of candidate scanning directions is not limited to... Figure 3 The two shown in the image Figure 3 This is only used to illustrate the relationship between candidate scan paths corresponding to different scan directions.

[0092] Furthermore, each candidate scan path is divided into multiple scan segments to be executed sequentially according to the boundary of the stress control unit.

[0093] When a continuous scanning trajectory passes through different stress control units, it can be divided into two or more scanning segments at the boundary of the stress control unit, so that each scanning segment can correspond to a specific stress control unit.

[0094] For any scan segment j, the local contraction direction ui of the stress control unit where the scan segment is located is taken as the direction of the corresponding contraction increment ΔSj, and the magnitude of the contraction increment ΔSj is determined according to the contraction weight Wi corresponding to the stress control unit, the effective scan length Lj of the scan segment, and the time decay coefficient φj after the scan segment is executed.

[0095] For example, it can be represented as: ΔSj=k0×Wi×Lj×φj×ui; Where k0 represents the proportional coefficient that converts the scan length, shrinkage weight, and corresponding shrinkage effect into the same evaluation scale.

[0096] It should be noted that the shrinkage increment ΔSj is used to compare the relative shrinkage effects between different candidate scan paths, and is not required to be directly equivalent to the actual mechanical displacement or residual stress value generated in the metal part.

[0097] Furthermore, a preset cooling interaction time window is determined.

[0098] For any stress control unit, the temperature rise in the region at the end of the scan can be used as the initial temperature rise ΔTi0.

[0099] For example, if the characteristic temperature of the stress control unit is Ti0 after the scan is completed, and the reference temperature of the forming chamber or powder bed is Tb, then: ΔTi0 = Ti0 - Tb.

[0100] As cooling time increases, the temperature rise in the area gradually decreases.

[0101] A temperature rise ratio ρ can be preset, for example, ρ can be set between 0.1 and 0.3 according to the material's cooling characteristics.

[0102] When the remaining temperature rise of the stress control unit decreases to ρ times the initial temperature rise ΔTi0, the time from the end of the scan to reaching the temperature rise ratio is determined as the cooling interaction time τi corresponding to the stress control unit.

[0103] For multiple stress control units, the maximum value among multiple cooling interaction times τi can be selected as the preset cooling interaction time window τ corresponding to the current forming layer, so that the scanning segments that still have a significant residual temperature rise within the time window can participate in the subsequent shrinkage superposition evaluation.

[0104] In another embodiment, the corresponding cooling interaction time can be weighted according to the area or shrinkage weight of multiple stress control units to determine the preset cooling interaction time window.

[0105] The time decay coefficient φj can be determined based on the ratio of the remaining temperature rise to the initial temperature rise in the corresponding region after the execution of scan segment j.

[0106] For example: φj=ΔTj(t) / ΔTj0.

[0107] When the scan segment is just completed, φj is close to 1; as the cooling time increases, φj gradually decreases; when the corresponding scan segment exceeds the preset cooling interaction time window, it can be considered that its dynamic contraction interaction effect on subsequent scan segments has decayed to below the preset range and no longer participates in the dynamic contraction synthesis at the current moment.

[0108] Furthermore, when each scan segment in the candidate scan path is completed, all contraction increments that have not yet decayed within the preset cooling interaction time window are identified.

[0109] Assuming there are currently m scan segments still within the cooling interaction time window, with contraction increments of ΔS1, ΔS2, ..., ΔSm respectively, then the current contraction sum R can be expressed as: R=ΣΔSj.

[0110] The current contraction sum R is used to reflect the overall offset degree of the contraction effect generated by multiple local scan regions at the same time in the planar direction.

[0111] Furthermore, for each contraction increment ΔSj, the position vector rj of its effective position Pj relative to the constraint reference point P0 is determined.

[0112] The position vector rj can be represented as: rj = Pj - P0.

[0113] The action position Pj of the scanning segment can be selected as the geometric midpoint of the scanning segment, the energy input center, or the equivalent action point inside the stress control unit where the corresponding scanning segment is located.

[0114] The contraction torque formed by this scan segment relative to the constraint reference point 205 is determined by the vector product of the position vector rj and the corresponding contraction increment ΔSj. Mj = rj × ΔSj.

[0115] For a two-dimensional forming plane, the component of the above vector product along the forming direction can be taken as the signed evaluation value of the corresponding shrinkage torque.

[0116] The current resultant contraction torque M can be expressed as: M = ΣMj.

[0117] The sum of contraction torques M is used to reflect the degree of spatial imbalance of multiple local contraction effects relative to the constraint reference point 205. It should be noted that the sum of contraction torques is used to characterize the spatial offset of each contraction increment relative to the constraint reference point, and is an evaluation quantity of the candidate scan path, and does not represent the physical torque directly calculated from the actual mechanical force.

[0118] It should be noted that when two contraction increments are similar in magnitude and direction, but located on opposite sides of constraint reference point 205, their effects on the resultant contraction amount R may be superimposed, while their effects on the resultant contraction torque M may be partially canceled out; when two contraction increments are similar in magnitude but located on the same side of constraint reference point 205, a larger resultant torque may be formed.

[0119] Therefore, by simultaneously utilizing the resultant amount of contraction and the resultant amount of contraction torque, spatial positional differences that cannot be reflected by using only the resultant amount in a single direction can be further evaluated.

[0120] For each candidate scanning path, during the process of simulating the scanning segment by segment according to the corresponding scanning order, the contraction sum R and contraction torque sum M corresponding to each scanning stage are recorded respectively.

[0121] The peak value of the current contraction resultant magnitude that occurs during the entire scanning process of the candidate scanning path is denoted as Rmax, and the peak value of the absolute value of the current contraction torque resultant magnitude is denoted as Mmax.

[0122] Where Rmax = max‖R‖, Mmax = max|M|; then, the path contraction imbalance J is determined based on Rmax and Mmax.

[0123] For example, in one embodiment, it can be represented as: J=d1×Rmax / Rref+d2×Mmax / Mref; Where Rref and Mref represent the preset reference values ​​for total shrinkage and shrinkage torque, respectively, and d1 and d2 represent the corresponding evaluation weights.

[0124] The above expression is used to convert the combined shrinkage quantity and the combined shrinkage torque with different dimensions or evaluation scales into the same comprehensive evaluation index.

[0125] In other implementations, upper limits for the total amount of contraction and the total amount of contraction torque can be set separately. When both meet the corresponding preset conditions, the current candidate scanning path is determined to meet the path contraction imbalance requirement.

[0126] Furthermore, the controller can also generate candidate scan paths using a segment-by-segment construction method.

[0127] After the execution order of some scan segments has been determined, for the multiple scan segments that have not yet been executed, the current contraction sum and the current contraction torque sum after each unscanned segment is added to the current scan sequence are simulated respectively.

[0128] Prioritize selecting unscanned segments that reduce at least one of the current contraction sum and the current contraction torque sum, and whose other does not exceed the corresponding preset growth range, as the next scan segment.

[0129] For example, if the current contraction sum decreases after the first unscanned segment is added, and the current contraction torque sum only increases to within a preset allowable range, then the first unscanned segment can be added to the current scan sequence.

[0130] If the second unscanned segment can reduce the current contraction amount, but causes the current contraction torque to exceed the preset upper limit, then the second unscanned segment will not be selected first.

[0131] Repeating the above process sequentially will generate complete candidate scan paths.

[0132] The technical solution of this embodiment makes the determination of candidate scanning paths no longer based solely on a fixed scanning direction or the static temperature distribution after the final scan, but further considers the contraction effect of different scanning segments in the actual scanning sequence and their superposition relationship with cooling time.

[0133] S104: Select a candidate scanning path whose path shrinkage imbalance meets the preset conditions, perform selective laser melting on the next forming layer, and update the local shrinkage direction and shrinkage weight according to the temperature change information after scanning the next forming layer, until the additive forming is completed.

[0134] In this step, it should be noted that after multiple candidate scan paths have completed the calculation of the path shrinkage imbalance J, the final execution path can be determined according to preset conditions.

[0135] In one implementation, an upper limit Jlim for path shrinkage imbalance can be set, and candidate scan paths with J≤Jlim are determined as candidate scan paths that meet preset conditions.

[0136] When there are multiple candidate scanning paths that meet the preset conditions, they can be further sorted according to the magnitude of path shrinkage imbalance, total scan length, galvanometer jump distance, or total scan time, and the candidate scanning path with smaller path shrinkage imbalance should be selected first.

[0137] When none of the candidate scan paths meet the preset condition for path shrinkage imbalance, scan path correction can be further performed.

[0138] Specifically, during the current path simulation, the target scan segment is determined so that the absolute value of the current contraction torque reaches the corresponding peak value for the first time.

[0139] The target scan segment is divided into a first scan sub-segment and a second scan sub-segment, and the unscanned segment whose direction of the generated contraction torque is opposite to the direction of the current contraction torque resultant corresponding to the peak value is found from the currently unscanned scan segments.

[0140] The direction of the contraction torque can be determined by the sign of the vector product between the position vector corresponding to the unscanned segment and the contraction increment. When the direction of the contraction torque corresponding to the unscanned segment is opposite to the direction of the resultant current contraction torque corresponding to the peak value, it can be considered that the unscanned segment can cancel out the current peak force during subsequent scanning.

[0141] The unscanned segment is inserted between the first scanned segment and the second scanned segment, and the peak value of the current contraction magnitude modulus, the peak value of the current contraction torque absolute value, and the path contraction imbalance are recalculated for the adjusted candidate scan path.

[0142] If the adjusted path shrinkage imbalance meets the preset conditions, it will be used as an executable candidate scan path.

[0143] If the preset conditions are still not met, you can continue to select other unscanned segments with opposite torque directions or change the division position of the target scan segment.

[0144] It should be noted that the above-mentioned abnormal path correction method is mainly used to make targeted corrections to the local scanning position that causes the dynamic torque peak when the conventional candidate scanning direction and scanning sequence cannot reduce the path shrinkage imbalance to the preset range, rather than simply changing the fixed scanning direction of the entire forming layer.

[0145] After determining the final candidate scanning path, the controller controls the laser and galvanometer scanning assembly to selectively laser melt the next forming layer according to the candidate scanning path.

[0146] Laser power, scanning speed, scanning spacing, and powder layer thickness can be determined based on the pre-calibrated stable melting process window of the corresponding metal powder.

[0147] After completing the scanning of the next forming layer, the temperature detection component once again obtains the temperature change information of the corresponding forming layer in the preset cooling stage in accordance with the method in step S102, and redetermines the temperature gradient direction, cooling attenuation characteristics, local shrinkage direction and shrinkage weight of each stress control unit.

[0148] Therefore, the shrinkage control parameters used in the subsequent forming layer are not always based on the data of the first or initial layer, but are updated according to the changes in temperature and geometric constraints during the actual layer-by-layer forming process.

[0149] In a further embodiment, the local contraction direction and contraction weight can also be calibrated based on the layer image.

[0150] Specifically, at the first detection moment after the next forming layer is scanned, the corresponding first layer image is acquired using the layer image acquisition component, and the reference positioning mark in the forming platform or forming area is recorded to establish the correspondence between the image coordinates and the forming coordinates of the SLM device.

[0151] After a preset cooling process, the corresponding second-layer image is acquired again.

[0152] The corresponding melting contour feature points are extracted from the first-level image and the second-level image respectively, and the images are registered using the equipment coordinate reference.

[0153] For the same melting profile feature point, if its coordinates at the first detection time are denoted as Q1 and the corresponding coordinates at the second detection time are denoted as Q2, then the actual shrinkage displacement ΔQ can be expressed as: ΔQ = Q2 - Q1.

[0154] Based on the actual shrinkage displacement of multiple contour feature points, the actual shrinkage displacement direction and relative shrinkage magnitude of the corresponding stress control unit can be determined.

[0155] Subsequently, the actual contraction displacement direction is compared with the predicted local contraction direction corresponding to the stress control unit.

[0156] For example, the directional angle between the two can be denoted as θe. When θe exceeds a preset directional calibration threshold, the local shrinkage direction of the stress control unit corresponding to the subsequent forming layer can be corrected according to the actual shrinkage displacement direction.

[0157] At the same time, the relative magnitude of the actual contraction displacement can be compared with the corresponding contraction weight.

[0158] For example, when the predicted shrinkage weight is large but the actual shrinkage displacement of multiple consecutive forming layers is significantly smaller than that of similar regions, the shrinkage weight of subsequent forming layers can be appropriately reduced; when the actual shrinkage displacement is consistently greater than the relative level predicted based on the current shrinkage weight, the corresponding shrinkage weight can be increased.

[0159] It should be noted that the above image feedback is mainly used for relative calibration of local contraction direction and contraction weight, and does not require direct measurement of the actual residual stress inside the metal part through ordinary layer images.

[0160] After completing the scanning of the current forming layer, the powder spreading mechanism lays the next layer of metal powder on the surface of the current formed layer, reads the slice data of the next forming layer, and repeats the above-mentioned process of stress control unit division, temperature change analysis, local shrinkage parameter determination, candidate scanning path generation, and path shrinkage imbalance evaluation.

[0161] After completing all the slicing layers one by one, the SLM metal part is obtained.

[0162] Implementing the technical solution of this embodiment can form a control process of "geometric constraint analysis of forming layer - division of stress control unit - detection of actual temperature change - determination of local shrinkage direction and shrinkage weight - determination of constraint reference point - generation of candidate scanning path - calculation of dynamic shrinkage increment of scanning segment - evaluation of shrinkage sum and shrinkage torque sum - selection of candidate path - subsequent forming layer feedback update", so that the dynamic shrinkage effect formed in different local areas during continuous scanning and cooling can participate in the determination of scanning path.

[0163] It should be further explained that, in this application, the local shrinkage direction and shrinkage weight are not used to directly give the actual residual stress value, but are used to characterize the relative shrinkage trend of different stress control units under the current temperature and geometric constraint conditions.

[0164] For example, in a current forming layer, the first stress control unit is adjacent to the free contour and has a low projection overlap ratio with the adjacent formed layer, so its corresponding interlayer constraint degree can be relatively small; the second stress control unit is located inside the current forming layer and has a large projection overlap area with the adjacent formed layer, so its corresponding interlayer constraint degree can be relatively high.

[0165] Even if the two stress control units mentioned above have similar average temperatures during the cooling stage, they can still obtain different local contraction directions and contraction weights due to the different degrees of interlayer constraint.

[0166] This reduces the bias caused by judging the residual stress state solely based on the temperature of the region.

[0167] In another embodiment, for different metal powders, corresponding parametric relationships between cooling attenuation characteristics, interlayer constraint degree and shrinkage weight can be established respectively.

[0168] For example, for metal materials with low thermal conductivity and large temperature gradients during cooling, the influence of temperature gradient factors on the determination of local shrinkage direction and shrinkage weight can be increased; for metal parts with large cross-sectional changes or many thin-walled areas, the influence of interlayer constraint degree and free contour position can be increased.

[0169] In another embodiment, the division of stress control units is not limited to a regular mesh. The current forming layer can be initially discretized according to a fixed mesh, and then regions can be merged based on the interlayer constraint degree of adjacent basic meshes. Alternatively, irregular regions can be divided directly based on the contour change position, self-supporting region, free contour boundary, and abrupt cross-sectional changes between the current forming layer and adjacent formed layers.

[0170] In another embodiment, the constraint reference point 205 can also be set separately for different local areas of the current forming layer. When the current forming layer includes multiple independent solid areas that are far apart from each other, a constraint reference point can be determined for each independent solid area, and the shrinkage resultant and shrinkage torque resultant formed by the scan segment in the corresponding area can be calculated separately to avoid unnecessary path coupling evaluation between different independent solid areas.

[0171] In another embodiment, the path contraction imbalance is not limited to the weighted sum of the peak value of the contraction sum and the peak value of the contraction torque. A first threshold Rlim and a second threshold Mlim can be set respectively, and the corresponding candidate scan path is determined to meet the preset conditions only when Rmax≤Rlim and Mmax≤Mlim are satisfied throughout the entire execution process of the candidate scan path.

[0172] In another embodiment, the total scanning time of the candidate scanning paths can also be used as an auxiliary constraint. When the path shrinkage imbalance corresponding to two candidate scanning paths is similar, the candidate scanning path with a shorter total scanning time or a shorter galvanometer jump distance can be preferentially selected to balance the interlayer stress control effect and forming efficiency.

[0173] It should be noted that the temperature gradient direction, cooling attenuation characteristics, interlayer constraint degree, local contraction direction, contraction weight, cooling interaction time window, contraction increment, contraction sum, contraction torque sum, and path contraction imbalance in this application can all be calculated by the SLM device controller or a host computer that is communicatively connected to the SLM device.

[0174] For the candidate scanning path generation process, which involves a large amount of computation, the candidate path calculation for the next forming layer can also be completed in parallel during the cooling and powder spreading process of the current forming layer, so as to reduce additional waiting time.

[0175] To facilitate understanding of the labels and steps in the attached drawings, further explanations are provided below.

[0176] Figure 1S101 represents the step of acquiring the layered data of the metal part to be formed, and dividing the stress control unit according to the projection overlap relationship between the current forming layer and the adjacent formed layer and the free contour position; S102 represents the step of acquiring temperature change information in the preset cooling stage after scanning the current forming layer, and determining the local shrinkage direction, shrinkage weight and constraint reference point; S103 represents the step of mapping the local shrinkage direction and shrinkage weight to the next forming layer, generating multiple candidate scanning paths and determining the path shrinkage imbalance; S104 represents the step of selecting the candidate scanning path that meets the preset conditions to perform selective laser melting of the next forming layer and updating the local shrinkage direction and shrinkage weight according to the subsequent temperature change information.

[0177] Figure 2 In the figure, reference numeral 201 indicates the current forming layer; reference numeral 202 indicates the projected outline of the adjacent formed layer; reference numerals 204-1, 204-2, 204-3, 204-4, 204-5, 204-6, 204-7, 204-8 and 204-9 respectively indicate the multiple stress control units formed by division; reference numeral 205 indicates the constraint reference point determined according to the interlayer constraint degree and unit area of ​​each stress control unit.

[0178] Figure 3 In the figure, reference numerals 301 and 304 represent candidate scan paths with different scan directions or scan sequences, respectively; reference numeral 303 represents the corresponding constraint reference point; each linear scan part in the figure represents a scan segment that makes up a candidate scan path, and each arrow represents the scan direction of the corresponding scan segment.

[0179] It should be noted that the above-mentioned projection overlap ratio Ri, free contour distance di, local contour change Ci, interlayer constraint degree Ki, cooling attenuation characteristic Vi, local shrinkage direction ui, shrinkage weight Wi, cooling interaction time τ, time attenuation coefficient φj, shrinkage increment ΔSj, shrinkage sum R, shrinkage torque sum M, and path shrinkage imbalance J are all used to illustrate the specific implementation of the technical solution of this application. Their specific value range and weight coefficients can be adaptively calibrated according to the type of metal powder, laser power, scanning speed, powder layer thickness, scanning spacing, forming part size, and SLM equipment thermal management conditions.

[0180] It should be noted that the temperature change information in this application is not limited to being obtained through an infrared thermal imager. Where the temperature changes during the cooling process in different local areas of the current forming layer can be obtained, coaxial temperature detection, point infrared detection combined with scanning position reconstruction, or other methods suitable for temperature field detection in the SLM process can also be used.

[0181] It should be noted that the local shrinkage direction and shrinkage weight in this application are not limited to being determined using fixed analytical formulas. For specific metallic materials and SLM equipment, the correspondence between the temperature gradient direction, cooling attenuation characteristics, interlayer constraint degree and actual shrinkage displacement can be established using pre-prepared calibration samples, and the corresponding local shrinkage direction and shrinkage weight can be obtained by looking up tables, interpolation or function fitting.

[0182] The technical solution implemented in this embodiment can form an interlayer stress control link by considering the spatial geometric constraint state of the forming layer, the actual cooling temperature change, the local thermal shrinkage trend, and the temporal and spatial positions of the scanning path. By evaluating the dynamic shrinkage sum and shrinkage torque sum of different candidate scanning paths during the scanning process, a scanning path with relatively balanced local shrinkage effect is selected. The corresponding control parameters are continuously updated using the actual temperature change of the subsequent forming layer, thereby reducing the risk of residual stress concentration and forming deformation caused by the continuous accumulation of local shrinkage during the layer-by-layer forming process of SLM metal parts.

[0183] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of this patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for additive forming of SLM metal parts based on interlayer stress regulation, characterized in that, include: Obtain the layer data of the metal part to be formed, and divide the current forming layer into multiple stress control units based on the projection overlap relationship between the current forming layer and the adjacent formed layers and the free contour position. After completing the current forming layer scan, the temperature change information of each stress control unit is obtained in the preset cooling stage. The local shrinkage direction and shrinkage weight of each stress control unit are determined according to the temperature gradient direction, cooling attenuation characteristics and interlayer constraint degree. The constraint reference point is determined according to the interlayer constraint degree of each stress control unit. The local shrinkage direction and shrinkage weight are mapped to the next forming layer to generate multiple candidate scanning paths with different scanning orders and scanning directions. The shrinkage increment of each scanning segment in each candidate scanning path within a preset cooling interaction time window is calculated. The shrinkage increment is vector-synthesized to obtain the shrinkage resultant. The shrinkage torque resultant is determined according to the position of each shrinkage increment relative to the constraint reference point. The path shrinkage imbalance is determined according to the shrinkage resultant and the shrinkage torque resultant. Select a candidate scanning path whose path shrinkage imbalance meets the preset conditions to selectively laser melt the next forming layer, and update the local shrinkage direction and shrinkage weight according to the temperature change information after scanning the next forming layer, until the additive forming is completed.

2. The SLM metal part additive forming method based on interlayer stress regulation according to claim 1, characterized in that, Determining the degree of interlayer constraint includes: Transform the contour data of the current forming layer and the adjacent formed layers into the same forming coordinate system, and divide the current forming layer into multiple local units; The projection overlap ratio between each local unit and the adjacent formed layer, the distance from each local unit to the nearest free contour boundary, and the amount of local contour change between adjacent formed layers are determined respectively. The projection overlap ratio, the distance, and the local contour change are normalized, and the interlayer constraint degree of each local unit is determined based on the normalization result. Local units that are spatially continuous and whose interlayer constraint degree is within the same preset range are merged into the stress control unit.

3. The SLM metal part additive forming method based on interlayer stress regulation according to claim 2, characterized in that, Determining the constraint reference point includes: Obtain the geometric center coordinates and unit area of ​​each stress control unit. Use the product of the interlayer constraint degree of the corresponding stress control unit and the unit area as the coordinate weight, perform a weighted summation on the geometric center coordinates, and determine the constraint reference point by the ratio of the weighted summation result to the sum of the coordinate weights.

4. The SLM metal part additive forming method based on interlayer stress regulation according to claim 1, characterized in that, At least three detection times after the laser scanning of the current forming layer stops, the temperature distribution of each stress control unit is obtained, the cooling attenuation characteristics are determined according to the temperature changes between different detection times, and the temperature gradient direction is determined according to the temperature spatial changes inside the stress control unit at the same detection time. The free contraction direction of the stress control unit pointing to its corresponding free contour boundary is determined. The local contraction direction is obtained by vector synthesis based on the temperature gradient direction, the free contraction direction and the degree of interlayer constraint. The contraction weight is determined based on the cooling attenuation characteristics and the degree of interlayer constraint.

5. The SLM metal part additive forming method based on interlayer stress regulation according to claim 4, characterized in that, Each candidate scan path is divided into multiple scan segments to be executed sequentially according to the boundary of the stress control unit; For any scan segment, the local contraction direction of the stress control unit where the scan segment is located is taken as the direction of the corresponding contraction increment, and the magnitude of the contraction increment is determined according to the contraction weight of the stress control unit, the effective scan length of the scan segment, and the time decay coefficient corresponding to the scan segment after execution.

6. The SLM metal part additive forming method based on interlayer stress regulation according to claim 5, characterized in that, The preset cooling interaction time window is determined based on the cooling attenuation characteristics of the stress control unit corresponding to the current forming layer; The initial temperature rise is taken as the temperature rise of the region at the end of the scan. When the temperature rise of the corresponding region drops to a preset ratio of the initial temperature rise, the time between the end of the scan and the arrival of the preset ratio is determined as the cooling interaction time of the corresponding stress control unit. The preset cooling interaction time window is determined according to the cooling interaction time of multiple stress control units. The time decay coefficient is determined based on the ratio of the remaining temperature rise after the scan segment is executed to the initial temperature rise.

7. The SLM metal part additive forming method based on interlayer stress regulation according to claim 1, characterized in that, When each scan segment of the candidate scan path is completed, determine each shrinkage increment that has not yet decayed within the preset cooling interaction time window, and perform vector summation on each shrinkage increment to obtain the current shrinkage sum. Determine the position vector of each contraction increment relative to the constraint reference point, and determine the current contraction torque resultant based on the vector product of the position vector and the corresponding contraction increment; The peak value of the magnitude of the current contraction sum and the peak value of the absolute value of the current contraction torque sum are obtained during the entire scanning process of the candidate scanning path, and the path contraction imbalance is determined based on the two peak values.

8. The SLM metal part additive forming method based on interlayer stress regulation according to claim 7, characterized in that, Generating the candidate scan path includes: After determining the currently executed scan segment, calculate the current contraction sum and the current contraction torque sum corresponding to each unscanned segment after it is added to the current scan sequence; The unscanned segment that reduces at least one of the current contraction sum and the current contraction torque sum, and whose other does not exceed the corresponding preset growth range, is preferentially selected as the next scanned segment, and the execution order of the scanned segments is determined in the manner described above to form at least one candidate scanned path.

9. The SLM metal part additive forming method based on interlayer stress regulation according to claim 8, characterized in that, When none of the generated candidate scanning paths meet the preset condition for the path contraction imbalance, a target scanning segment is determined that makes the absolute value of the current contraction torque reach the corresponding peak value for the first time, and the target scanning segment is divided into a first scanning sub-segment and a second scanning sub-segment. If there is an unscanned segment where the direction of the generated contraction torque is opposite to the direction of the current contraction torque sum corresponding to the peak value, the unscanned segment is inserted between the first scanned segment and the second scanned segment, and the path contraction imbalance is recalculated to obtain the adjusted candidate scanned path.

10. The SLM metal part additive forming method based on interlayer stress regulation of claim 4, wherein, At the first detection moment after the next forming layer is scanned, the corresponding first layer image is acquired, and after a preset cooling, the corresponding second layer image is acquired. The actual shrinkage displacement of the corresponding stress control unit is determined based on the coordinate changes of the corresponding melting contour feature points in the first layer image and the second layer image. The direction of the actual contraction displacement is compared with the corresponding local contraction direction, and the relative magnitude of the actual contraction displacement is compared with the corresponding contraction weight. When the deviation of the comparison result exceeds the corresponding calibration threshold, the local shrinkage direction or shrinkage weight of the stress control unit in the subsequent forming layer is corrected.