A high-toughness welding electrode for marine engineering and its preparation method
By combining a specific coating powder with an H08G welding core, a high-toughness welding electrode for marine engineering was prepared, which solved the problem of insufficient low-temperature impact toughness of welding materials, and achieved stability of welding performance and improvement of low-temperature performance, thus meeting the needs of marine engineering.
Patent Information
- Application Number
- CN202611510684.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
The low-temperature impact toughness of existing F-grade steel plates paired with domestically produced welding materials cannot meet the requirements of engineering applications, thus limiting my country's ability to independently develop marine resources.
A high-toughness welding electrode for marine engineering is prepared by using a specific combination of coating and powder components, including carbonates, fluorides, rutile, silicon dioxide, electrolytic manganese, ferrosilicon, iron powder, soda ash, sodium alginate, graphite, and nickel powder, combined with an H08G welding core. The welding electrode is prepared using welding electrode production equipment.
The electrode arc is stable with virtually no spatter, exhibits good slag removal, produces aesthetically pleasing welds, and demonstrates proper control of alloying elements in the deposited metal. It also significantly improves low-temperature impact toughness, meeting the engineering application requirements of -60℃.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding materials technology, specifically to a high-toughness welding electrode for marine engineering and its preparation method. Background Technology
[0002] Steel, as a key structural material for marine engineering equipment, is widely used in drilling platforms, production platforms, and subsea pipelines. Due to their long service life and the need to withstand harsh wind and wave conditions, the steel plates used are increasingly developing towards higher strength, higher toughness, easier weldability, and larger thickness and larger specifications. The main grades of high-strength steel used in offshore platforms worldwide have yield strengths of 355, 420, 460, 500, 550, 620, and 690 MPa, and require low-temperature performance of at least -40℃, or even -60℃.
[0003] my country's offshore oil development started relatively late, with its own offshore oil platforms only being built in the 1980s. Currently, my country's offshore platforms mainly use D, E, and F grade steel plates with a yield strength of 355-460 MPa, which has basically achieved domestic production. The fixed structures of offshore jack-up platforms now use steel plates with a yield strength of over 500 MPa. However, the low-temperature impact toughness of domestically produced welding materials for F grade steel plates remains unstable. Most of the high-strength, high-toughness welding rods used in key parts of marine engineering still need to be imported, which limits my country's ability to independently develop marine resources. Summary of the Invention
[0004] This invention aims to address the technical problem that the low-temperature impact toughness of existing domestically produced welding materials for F-grade steel plates cannot meet the requirements of engineering applications. The purpose is to provide a high-toughness welding electrode for marine engineering and its preparation method. The electrode has a stable arc, minimal spatter, good slag removal, and aesthetically pleasing weld formation. The alloying elements in the deposited metal are properly controlled, resulting in good mechanical properties and significantly improved low-temperature impact toughness.
[0005] This invention is achieved through the following technical solution:
[0006] The first objective of this invention is to provide a high-toughness welding electrode for marine engineering, comprising a core and a coating powder covering the surface of the core, wherein the coating powder comprises, by weight, the following components:
[0007] Carbonates 26-32 parts, fluorides 18-24 parts, rutile 5-8 parts, silicon dioxide 4-7 parts, electrolytic manganese 3-6 parts, ferrosilicon 3-5 parts, iron powder 22-26 parts, soda ash 0.6-1.0 parts, sodium alginate 0.6-1.0 parts, graphite 0.10-0.30 parts, nickel powder 1.5-2.5 parts, ferromolybdenum 0.6-0.8 parts.
[0008] The main functions of each component of the herbal skin powder raw material in this invention are as follows:
[0009] Carbonates: Carbonates are used in welding electrodes. Under the action of electric arc heat, they decompose into CaO and CO2. They are commonly used slag-building and gas-generating materials in the manufacture of welding electrodes. They increase the basicity of slag, stabilize the electric arc, increase the interfacial tension and surface tension between slag and metal, improve slag removal, and have good desulfurization ability.
[0010] Fluorides: Adjusting the melting point and viscosity of slag, increasing the fluidity of the slag, and improving the physical properties of slag play a key role in weld formation and slag removal. They are also the main material for reducing the diffusion of hydrogen in the weld. However, the presence of fluorine can cause arc instability and produce toxic gases.
[0011] Rutile: Its main functions in welding electrodes are slag building and arc stabilization. In this invention, the addition of the above-mentioned amount of rutile plays a key role in weld formation.
[0012] Silicon dioxide: Adjusting the Si content in the weld metal is beneficial to the welding process performance, but it deteriorates the mechanical properties. The amount added needs to be controlled. This invention strictly controls the amount of ferrosilicon added to balance the welding process and mechanical properties.
[0013] Iron powder: Adding it can improve the deposition efficiency of welding and also play a certain role in stabilizing the electric arc.
[0014] Electrolytic manganese: Its addition can play a role in desulfurization and deoxidation, and can also transfer manganese elements to the weld to improve the weld strength.
[0015] Soda ash and sodium alginate are added to ensure production and improve pressure coating performance.
[0016] The high-toughness marine welding electrode of the present invention utilizes the above-mentioned coating and powder, with the components of the coating and powder organically combined, resulting in excellent manufacturing process performance, stable arc, virtually no spatter, good slag removal, beautiful weld formation, proper control of alloying elements in the deposited metal, and good mechanical properties. Under the conditions of as-welded state and heat treatment at 620±15℃×6h, the low-temperature impact toughness at -60℃ is significantly improved, meeting the requirements of engineering applications.
[0017] In a preferred embodiment, the carbonate is marble.
[0018] In a preferred embodiment, the fluoride is fluorite.
[0019] In a preferred embodiment, the components of the medicated peel powder, by weight, include:
[0020] 26 parts carbonate, 24 parts fluoride, 8 parts rutile, 4 parts silicon dioxide, 5.5 parts electrolytic manganese, 4 parts ferrosilicon, 22 parts iron powder, 0.8 parts soda ash, 0.8 parts sodium alginate, 0.2 parts graphite, 2 parts nickel powder, and 0.7 parts ferromolybdenum.
[0021] In a preferred embodiment, the components of the medicated peel powder, by weight, include:
[0022] 29 parts carbonate, 22 parts fluoride, 6 parts rutile, 5 parts silicon dioxide, 4 parts electrolytic manganese, 5 parts ferrosilicon, 24 parts iron powder, 0.8 parts soda ash, 0.8 parts sodium alginate, 0.2 parts graphite, 2 parts nickel powder, and 0.7 parts ferromolybdenum.
[0023] In a preferred embodiment, the welding core is a low-sulfur, low-phosphorus welding core.
[0024] In a preferred embodiment, the welding core is an H08G welding core wire rod, the diameter deviation of which is ±0.4mm and the ellipticity of which is ≤0.5mm.
[0025] In a preferred embodiment, the H08G welding core comprises, by weight percentage:
[0026] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0027] The second objective of this invention is to provide a method for preparing high-toughness welding electrodes for marine engineering, comprising the following steps:
[0028] Mix the above-mentioned medicinal peel and powder evenly according to the component ratio;
[0029] Add water glass at a mass of 21-23 wt% of the drug coating powder for wet mixing;
[0030] Welding electrodes are prepared using a welding core on a hydraulic electrode production machine.
[0031] In a preferred embodiment, the potassium-sodium ratio of the water glass is 1:1, and the Baumé density is 41~42Be at 20°C.
[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0033] The high-toughness marine welding electrode of the present invention utilizes the above-mentioned coating and powder, with the components of the coating and powder organically combined, resulting in excellent manufacturing process performance, stable arc, virtually no spatter, good slag removal, beautiful weld formation, proper control of alloying elements in the deposited metal, and good mechanical properties. Under the conditions of as-welded state and heat treatment at 620±15℃×6h, the low-temperature impact toughness at -60℃ is significantly improved, demonstrating good low-temperature performance and meeting the requirements for engineering applications at low temperatures. Detailed Implementation
[0034] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the illustrative embodiments and descriptions of the present invention are only used to explain the present invention and are not intended to limit the present invention.
[0035] The embodiments of the present invention will be described in detail below. However, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art.
[0036] The "scope" disclosed in this invention is defined in the form of a lower limit and an upper limit. A given scope is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific scope. The scope defined in this way can include or exclude end values, and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a scope.
[0037] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0038] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.
[0039] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other substances not listed may also be included, or that only the listed substances may be included.
[0040] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0041] The technical solution of the present invention will be further described in detail below with reference to the embodiments.
[0042] It should be noted that, unless otherwise specified, the experimental methods used in the embodiments are conventional methods. Unless otherwise specified, the materials, reagents, methods, and instruments used are all conventional materials, reagents, methods, and instruments in the art, and can be obtained commercially by those skilled in the art.
[0043] Example 1
[0044] A high-toughness welding electrode for marine engineering consists of a core and a coating of flux powder covering the surface of the core.
[0045] The welding core is a low-sulfur, low-phosphorus welding core, using H08G welding core wire rod. The diameter deviation of the H08G welding core wire rod is ±0.4mm, and the ellipticity of the wire rod is ≤0.5mm. The composition of the H08G welding core is as follows:
[0046] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0047] The components of the medicinal coating powder, by weight, include:
[0048] 26 parts by weight of carbonates, 24 parts by weight of fluorides, 8 parts by weight of rutile, 4 parts by weight of silicon dioxide, 5.5 parts by weight of electrolytic manganese, 4 parts by weight of ferrosilicon, 22 parts by weight of iron powder, 0.8 parts by weight of soda ash, 0.8 parts by weight of sodium alginate, 0.2 parts by weight of graphite, 2 parts by weight of nickel powder, and 0.7 parts by weight of ferromolybdenum.
[0049] The preparation method of the high-toughness welding electrode for marine engineering in this embodiment is as follows:
[0050] (1) Mix all the components of the above-mentioned medicinal peel and powder evenly;
[0051] (2) Add water glass accounting for 23 wt% of the drug coating powder for wet mixing. The potassium-sodium ratio of the water glass at 20°C is 1:1 and the Baumé density is 41~42Be.
[0052] (3) The H08G welding core is used to prepare the welding electrode on the hydraulic welding electrode production equipment.
[0053] Welding was performed using the high-toughness marine welding electrode of this invention. The welding current was 170A, the voltage was 22-26V, the welding speed was 15-20cm / min, and the interpass temperature was 180-200℃. The composition of the weld metal after welding is shown in Table 1, and the mechanical properties of the weld metal are shown in Table 2.
[0054] Table 1. Chemical composition of weld metal deposited by welding electrode in Example 1
[0055]
[0056] Table 2. Mechanical properties of weld metal deposited from welding electrodes in Example 1
[0057]
[0058] Example 2
[0059] A high-toughness welding electrode for marine engineering consists of a core and a coating of flux powder covering the surface of the core.
[0060] The welding core is a low-sulfur, low-phosphorus welding core, using H08G welding core wire rod. The diameter deviation of the H08G welding core wire rod is ±0.4mm, and the ellipticity of the wire rod is ≤0.5mm. The composition of the H08G welding core is as follows:
[0061] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0062] The components of the medicinal coating powder, by weight, include:
[0063] 29 parts by weight of carbonates, 22 parts by weight of fluorides, 6 parts by weight of rutile, 5 parts by weight of silicon dioxide, 4 parts by weight of electrolytic manganese, 5 parts by weight of ferrosilicon, 24 parts by weight of iron powder, 0.8 parts by weight of soda ash, 0.8 parts by weight of sodium alginate, 0.2 parts by weight of graphite, 2 parts by weight of nickel powder, and 0.7 parts by weight of ferromolybdenum.
[0064] The preparation method of the high-toughness welding electrode for marine engineering in this embodiment is as follows:
[0065] (1) Mix all the components of the above-mentioned medicinal peel and powder evenly;
[0066] (2) Add water glass accounting for 22 wt% of the drug coating powder for wet mixing. The potassium-sodium ratio of the water glass at 20°C is 1:1 and the Baumé density is 41~42Be.
[0067] (3) The H08G welding core is used to prepare the welding electrode on the hydraulic welding electrode production equipment.
[0068] Welding was performed using the high-toughness marine welding electrode of this invention. The welding current was 170A, the voltage was 22-26V, the welding speed was 15-20cm / min, and the interpass temperature was 180-200℃. The composition of the welded metal is shown in Table 3, the mechanical properties of the welded metal are shown in Table 4, and the performance data of the butt joint of the product are shown in Table 5.
[0069] Table 3, Chemical composition of weld metal deposited by welding electrode in Example 2
[0070]
[0071] Table 4. Mechanical properties of weld metal deposited from welding electrodes in Example 2
[0072]
[0073] Table 5. Mechanical properties of the butt joint in Example 2
[0074]
[0075] As can be seen from the data in Tables 2, 4 and 5, the joints welded using the high-toughness welding rods of the present invention exhibit good mechanical properties. The deposited metal has a high impact energy at -60℃ under the conditions of being in the weld state and under heat treatment at 620±15℃×6h, and the low-temperature impact toughness is greatly improved, meeting the requirements for engineering applications at low temperatures.
[0076] Example 3
[0077] A high-toughness welding electrode for marine engineering consists of a core and a coating of flux powder covering the surface of the core.
[0078] The welding core is a low-sulfur, low-phosphorus welding core, using H08G welding core wire rod. The diameter deviation of the H08G welding core wire rod is ±0.4mm, and the ellipticity of the wire rod is ≤0.5mm. The composition of the H08G welding core is as follows:
[0079] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0080] The components of the medicinal coating powder, by weight, include:
[0081] 32 parts by weight of carbonates, 18 parts by weight of fluorides, 7 parts by weight of rutile, 7 parts by weight of silicon dioxide, 5 parts by weight of electrolytic manganese, 3 parts by weight of ferrosilicon, 26 parts by weight of iron powder, 0.6 parts by weight of soda ash, 0.6 parts by weight of sodium alginate, 0.1 parts by weight of graphite, 1.5 parts by weight of nickel powder, and 0.6 parts by weight of ferromolybdenum.
[0082] The preparation method of the high-toughness welding electrode for marine engineering in this embodiment is as follows:
[0083] (1) Mix all the components of the above-mentioned medicinal peel and powder evenly;
[0084] (2) Add water glass accounting for 22 wt% of the drug coating powder for wet mixing. The potassium-sodium ratio of the water glass at 20°C is 1:1 and the Baumé density is 41~42Be.
[0085] (3) The H08G welding core is used to prepare the welding electrode on the hydraulic welding electrode production equipment.
[0086] Example 4
[0087] A high-toughness welding electrode for marine engineering consists of a core and a coating of flux powder covering the surface of the core.
[0088] The welding core is a low-sulfur, low-phosphorus welding core, using H08G welding core wire rod. The diameter deviation of the H08G welding core wire rod is ±0.4mm, and the ellipticity of the wire rod is ≤0.5mm. The composition of the H08G welding core is as follows:
[0089] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0090] The components of the medicinal coating powder, by weight, include:
[0091] 29 parts by weight of carbonates, 20 parts by weight of fluorides, 7 parts by weight of rutile, 5 parts by weight of silicon dioxide, 5 parts by weight of electrolytic manganese, 3 parts by weight of ferrosilicon, 26 parts by weight of iron powder, 1.0 part by weight of soda ash, 1.0 part by weight of sodium alginate, 0.3 parts by weight of graphite, 2.5 parts by weight of nickel powder, and 0.8 parts by weight of ferromolybdenum.
[0092] The preparation method of the high-toughness welding electrode for marine engineering in this embodiment is as follows:
[0093] (1) Mix all the components of the above-mentioned medicinal peel and powder evenly;
[0094] (2) Add water glass accounting for 22 wt% of the drug coating powder for wet mixing. The potassium-sodium ratio of the water glass at 20°C is 1:1 and the Baumé density is 41~42Be.
[0095] (3) The H08G welding core is used to prepare the welding electrode on the hydraulic welding electrode production equipment.
[0096] Example 5
[0097] A high-toughness welding electrode for marine engineering consists of a core and a coating of flux powder covering the surface of the core.
[0098] The welding core is a low-sulfur, low-phosphorus welding core, using H08G welding core wire rod. The diameter deviation of the H08G welding core wire rod is ±0.4mm, and the ellipticity of the wire rod is ≤0.5mm. The composition of the H08G welding core is as follows:
[0099] C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
[0100] The components of the medicinal coating powder, by weight, include:
[0101] 26 parts by weight of carbonates, 20 parts by weight of fluorides, 7 parts by weight of rutile, 7 parts by weight of silicon dioxide, 5 parts by weight of electrolytic manganese, 5 parts by weight of ferrosilicon, 23 parts by weight of iron powder, 0.6 parts by weight of soda ash, 0.6 parts by weight of sodium alginate, 0.1 parts by weight of graphite, 1.5 parts by weight of nickel powder, and 0.7 parts by weight of ferromolybdenum.
[0102] The preparation method of the high-toughness welding electrode for marine engineering in this embodiment is as follows:
[0103] (1) Mix all the components of the above-mentioned medicinal peel and powder evenly;
[0104] (2) Add water glass accounting for 22 wt% of the drug coating powder for wet mixing. The potassium-sodium ratio of the water glass at 20°C is 1:1 and the Baumé density is 41~42Be.
[0105] (3) The H08G welding core is used to prepare the welding electrode on the hydraulic welding electrode production equipment.
[0106] Finally, it should be noted that the above specific embodiments are only used to describe the purpose, technical solution, and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation of the present invention and is not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the foregoing specific embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions or improvements can be made to some or all of the technical features. These modifications, equivalent substitutions, and improvements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.
Claims
1. A high toughness welding rod for marine use, characterized by, Composed of a welding core and a flux coating / powder covering the surface of the welding core, characterized in that the composition of the flux coating / powder, by weight, includes: Carbonates 26-32 parts, fluorides 18-24 parts, rutile 5-8 parts, silicon dioxide 4-7 parts, electrolytic manganese 3-6 parts, ferrosilicon 3-5 parts, iron powder 22-26 parts, soda ash 0.6-1.0 parts, sodium alginate 0.6-1.0 parts, graphite 0.10-0.30 parts, nickel powder 1.5-2.5 parts, ferromolybdenum 0.6-0.8 parts.
2. A high toughness welding rod for marine construction according to claim 1, wherein The carbonate is made from marble.
3. A high toughness welding rod for marine use according to claim 1, wherein The fluoride used is fluorite.
4. A high toughness welding rod for marine use according to claim 1, wherein The components of the medicinal coating powder, by weight, include: 26 parts carbonate, 24 parts fluoride, 8 parts rutile, 4 parts silicon dioxide, 5.5 parts electrolytic manganese, 4 parts ferrosilicon, 22 parts iron powder, 0.8 parts soda ash, 0.8 parts sodium alginate, 0.2 parts graphite, 2 parts nickel powder, and 0.7 parts ferromolybdenum.
5. A high toughness welding rod for marine use according to claim 1, wherein The components of the medicinal coating powder, by weight, include: 29 parts carbonate, 22 parts fluoride, 6 parts rutile, 5 parts silicon dioxide, 4 parts electrolytic manganese, 5 parts ferrosilicon, 24 parts iron powder, 0.8 parts soda ash, 0.8 parts sodium alginate, 0.2 parts graphite, 2 parts nickel powder, and 0.7 parts ferromolybdenum.
6. A high toughness welding rod for marine use according to claim 1, wherein The welding core is a low-sulfur phosphorus welding core.
7. A high toughness underwater welding electrode according to claim 6, wherein The welding core uses H08G welding core wire rod.
8. The high-toughness welding electrode for marine engineering according to claim 7, characterized in that, The composition of the H08G welding core, by weight percentage, is as follows: C≤0.10%, Mn: 0.30~0.55%, Si≤0.08%, S≤0.0045%, P≤0.008%, Ni≤0.30%, Cr≤0.10%, Cu≤0.20%, As≤0.007%, Al≤0.030%, with the balance being Fe and unavoidable impurities.
9. The method for preparing a high-toughness marine welding electrode as described in claim 1, characterized in that, Includes the following steps: Mix the above-mentioned medicinal peel and powder evenly according to the component ratio; Add water glass at a mass of 21-23 wt% of the drug coating powder for wet mixing; Welding electrodes are prepared using a welding core on a hydraulic electrode production machine.
10. A high-toughness welding electrode for marine engineering according to claim 9, characterized in that, The water glass has a potassium-sodium ratio of 1:1 and a Baumé density of 41~42Be at 20℃.