A method for polishing low-warpage wafers for single-crystal thin-film bonding

By matching the specific relationship between the polishing motion direction and the low crystal density axis during the polishing process, combined with a three-stage gradient polishing process and modified graphene oxide, the problem of uneven polishing of anisotropic wafers is solved, achieving high-efficiency, low-warpage, and high-surface-finish wafer polishing, which is suitable for single-crystal thin-film bonding.

CN123103450APending Publication Date: 2026-11-17JINGXIN NEW MATERIALS (ZHUJI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611216169.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polishing processes cannot effectively adapt to anisotropic wafers, resulting in uneven polishing removal rates, excessive warpage, and difficulty in meeting surface roughness requirements, which fails to meet the requirements for single-crystal thin-film bonding, especially with extremely poor compatibility with X-axis lithium niobate wafers.

Method used

By matching the specific relationship between the polishing motion direction and the low crystal density axis, a three-stage gradient polishing process is adopted. Combined with customized polishing fluid and special fixtures, polishing parameters are monitored and dynamically adjusted in real time. Modified graphene oxide is used as a surfactant to achieve the synergistic effect of chemical corrosion and mechanical grinding, reduce clamping stress and local unevenness, and achieve closed-loop control.

Benefits of technology

It achieves wafer warpage ≤15μm, surface roughness 0.1-0.3nm, and removal rate deviation ≤5% after polishing, significantly improving the polishing pass rate to ≥98%, and is suitable for the industrial production of various wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103450A_ABST
    Figure CN123103450A_ABST
Patent Text Reader

Abstract

This invention discloses a method for polishing low-warpage wafers for single-crystal thin-film bonding, relating to the field of ultra-precision wafer processing technology. The polishing method employs an eccentric adaptive planetary wheel fixture, adjusting the polishing motion direction to form a specific angle with the low crystal density axis of the wafer, and using an alkaline composite polishing slurry containing modified graphene oxide. The polishing process consists of three stages: pre-polishing, stress relief, and fine polishing. An interferometer is used to collect data such as thickness and warpage in real time to dynamically adjust polishing parameters. Furthermore, the modified graphene oxide, obtained through two-step covalent grafting, optimizes the dispersion and lubrication effect of the polishing slurry. This invention can balance the material removal rate, significantly reduce residual stress and warpage deformation of the wafer, improve surface finish and thickness uniformity, achieve a high yield rate of polished finished products, and is suitable for processing various types of semiconductor crystal wafers, meeting the stringent process requirements of single-crystal thin-film bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wafer ultra-precision processing technology, specifically relating to a method for polishing low-warpage wafers for single-crystal thin-film bonding. Background Technology

[0002] Single-crystal thin-film bonding technology is one of the core processes for fabricating high-end semiconductor devices and optoelectronic devices. It has extremely high requirements for the surface finish, thickness uniformity, and warp of the wafer. The surface finish of the wafer must be ≤0.5nm, the warp must be ≤25μm, and the total thickness variation (TTV) must be ≤3μm. Otherwise, defects such as voids and peeling will appear at the bonding interface, which will seriously affect the reliability and service life of the device.

[0003] Currently, wafer polishing mainly employs conventional processes such as chemical mechanical polishing (CMP). However, for wafers with anisotropic crystal density (such as lithium niobate, gallium arsenide, sapphire, and silicon carbide), existing polishing processes have significant technical drawbacks: First, they do not consider the anisotropy of wafer crystal density and do not match the relationship between the polishing motion direction and the axis of low crystal density, resulting in uneven polishing removal rates (rate deviations typically exceeding 10%). This not only prolongs polishing time but also causes uneven wafer surface quality and excessive warpage. Second, the polishing slurry is not adapted to the specific requirements. Different wafer crystallization characteristics can easily lead to chemical corrosion imbalance, resulting in either insufficient surface roughness or excessive grinding damage, making it difficult to achieve low roughness, low stress, and high efficiency simultaneously. Third, unreasonable clamping methods and uneven clamping forces can cause edge stress concentration, exacerbating wafer warpage and exceeding TTV limits, making it unsuitable for the polishing requirements of anisotropic wafers. Fourth, the polishing process lacks targeted real-time monitoring and dynamic feedback mechanisms, and blind polishing makes it difficult to accurately control warpage and removal rate, resulting in a low polishing pass rate (usually below 90%).

[0004] Among them, lithium niobate wafers with X-axis are widely used in high-end filters, optical modulators and other devices as crystal materials with excellent piezoelectric and optical properties. However, their crystal density is significantly anisotropic, with the low crystal density axis being

[100] crystal orientation. Existing polishing processes have extremely poor adaptability to them, and the warpage after polishing often exceeds 40μm, and the surface roughness is difficult to be lower than 0.5nm, which cannot meet the bonding requirements of single crystal thin films and has become a key bottleneck restricting the industrialization of lithium niobate devices. At the same time, silicon wafers (isotropic), gallium arsenide (anisotropic), sapphire (anisotropic), silicon carbide (anisotropic) and other wafers also face similar problems such as stress control, removal rate uniformity and surface quality optimization during the polishing process. Existing polishing methods lack universal guidance and cannot achieve efficient and high-quality polishing of different types of wafers.

[0005] Therefore, developing a polishing method that can be adapted to various wafers, takes into account the consistency of removal rate, low warpage and high surface finish, and has broad guiding significance has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] The purpose of this invention is to provide a method for polishing low-warpage wafers for single-crystal thin-film bonding. By matching the specific relationship between the polishing motion direction and the low crystal density axis, and by combining a customized polishing slurry, a special fixture, and a closed-loop control mechanism, the method achieves consistent polishing removal rate, shortens polishing time, and obtains ideal surface finish, removal amount, and low warpage value.

[0007] The technical solution adopted by the present invention to achieve the above objectives is as follows: A method for polishing low-warpage wafers for single-crystal thin-film bonding includes the following steps: Step 1: Wafer pretreatment and composite polishing solution preparation: Clean and dry the wafer to be polished to remove surface impurities and oil; prepare the composite polishing solution, adjust the pH value to 8.5-9.5, and ultrasonically mix evenly for later use. Step 2, Fixture Installation and Wafer Fixing: An eccentric adaptive planetary wheel fixture is used to adjust the wafer placement position so that the polishing motion direction forms an angle of 30°-45° with the low crystal density axis of the wafer; Step 3, Segmented Polishing: A three-stage process of pre-polishing, stress relief, and fine polishing is adopted. Data on wafer thickness, warpage, removal rate deviation, and axial angle deviation are collected in real time by an interferometer and fed back to the polishing equipment to dynamically adjust the polishing parameters. Step 4: Post-polishing treatment: Clean and dry the polished wafer to obtain a low-warpage wafer that meets the requirements for single-crystal thin-film bonding.

[0008] This invention leverages the low crystal density axial characteristics of anisotropic wafers, matching the polishing motion direction with the specific relationship between the low crystal density axis to achieve consistent polishing removal rates. Simultaneously, through customized polishing slurry, specialized fixtures, and a closed-loop control mechanism, it balances polishing efficiency, surface quality, and low warpage. Specific innovations include: 1. A three-stage gradient polishing process based on the crystallization characteristics of anisotropic wafers; 2. A customized composite polishing slurry system adapted to various wafer types. The slurry composition, pH value, and abrasive particle size are adjusted according to the crystallization characteristics and chemical activity of different wafers to achieve a synergistic effect of chemical etching and mechanical grinding, balancing low roughness, low stress, and high efficiency, thus solving the problem of poor compatibility in existing polishing slurries. Challenges: 3. Design an eccentric adaptive fixture that can adjust the wafer placement position, clamping pressure, and drainage hole layout according to the characteristics of different types of wafers (crystallization axis, brittleness, size), adapt to axial matching processes, reduce clamping stress and local polishing unevenness, improve polishing uniformity, and meet the polishing needs of 8-inch and larger wafers; 4. Adopt a real-time monitoring dynamic feedback closed-loop control mechanism, combined with the physical parameters of different wafers (refractive index, Young's modulus, Poisson's ratio), to monitor warpage, removal rate, and axial angle deviation in real time, dynamically adjust polishing parameters, achieve precise and controllable polishing process, significantly improve polishing yield (≥98%), and is suitable for the industrial production of various wafers.

[0009] Specifically, the above-mentioned method for polishing low-warpage wafers for single-crystal thin-film bonding includes the following steps: Step 1: Wafer Pretreatment and Composite Polishing Fluid Preparation First, the wafer surface is rinsed with deionized water to remove surface dust and impurities. Then, the wafer is placed in an acetone solution and ultrasonically cleaned for 10-25 minutes to remove surface oil. Finally, it is dried with nitrogen to obtain a clean wafer to be polished. At the same time, abrasive, potassium hydroxide and surfactant are added to deionized water, and the pH value is adjusted to 8.5-9.5 with a pH adjuster. Then, the mixture is placed in an ultrasonic device and ultrasonically mixed at a power of 1500-2000W for 20-30 minutes to obtain a uniform and stable composite polishing solution. Step 2: Fixture Installation and Wafer Fixing An eccentric adaptive planetary wheel chuck is used, comprising a chuck body, an eccentric wafer placement slot, a flexible rubber ring, and drainage holes. The wafer to be polished is placed in the eccentric wafer placement slot, and the wafer position is adjusted so that the polishing motion direction (i.e., the tangential direction) forms a 30°-45° angle with the low crystal density axis of the wafer. The clamping pressure is 8-25 g / cm. 2 A flexible rubber ring (5mm wide) fits the edge of the wafer to avoid localized stress damage caused by hard contact; drainage holes are distributed around the fixture to ensure that the polishing slurry evenly covers the wafer surface; The eccentric adaptive fixture can adjust the wafer placement position, clamping pressure and drainage hole layout according to the characteristics of different types of wafers (crystallization axis, brittleness, size), adapt to the axis matching process, reduce clamping stress and local polishing unevenness, improve polishing uniformity, and adapt to the polishing needs of 8-inch and larger wafers.

[0010] Step 3: Segmented polishing: Place the wafer-mounted fixture onto the polishing equipment and employ a three-stage gradient polishing process, maintaining a 30°-45° angle between the polishing motion direction and the low crystal density axis of the wafer, as detailed below: (1) Pre-polishing stage: Set polishing pressure to 40-90 g / cm 2 The polishing speed is 70-100 r / min, the flow rate of the composite polishing fluid is 12-15 L / min, and the polishing time is 10-15 min. This method quickly removes macroscopic defects and damage layers from the wafer surface (removal amount 20-30 μm). At the same time, the surface height profile is acquired in real time by an interferometer to initially control the curvature. (2) Stress release stage: A variable pressure control mode is adopted, with a pressure change gradient of 5-10 g / cm. 2 The polishing speed is 30-50 r / min, the composite polishing fluid flow rate is 10-12 L / min, the polishing time is 8-12 min, and the polishing parameters are dynamically adjusted. By combining stress release characteristics, residual stress inside the wafer is gradually released to avoid warping deformation caused by stress concentration. In this stage, the polishing parameters are dynamically adjusted with reference to the stress calculation model of the damaged layer. Data is collected in real time by an interferometer to calculate the real-time thickness, curvature and warping. The real-time film thickness data is compared with the preset ideal removal rate curve. If the removal rate of the edge area is lower than the target value, a control command is generated to dynamically increase the pressure applied to the edge pressure area; otherwise, the pressure is reduced accordingly.

[0011] (3) Fine polishing stage: Set the polishing pressure to 15-30 g / cm 2 Polishing speed 50-60 r / min, composite polishing fluid flow rate 10-12 L / min, polishing time 15-25 min; Maintain the optimal angle between the polishing motion direction and the low crystal density axis to precisely control the material removal rate (total removal amount 40-60μm). Step 4: Post-polishing treatment: After polishing, the wafer is removed from the fixture and rinsed with deionized water to remove the remaining polishing liquid and abrasive. Then, it is ultrasonically cleaned in anhydrous ethanol for 8-12 minutes to remove residual impurities. Finally, it is dried with nitrogen to obtain a low warpage wafer that meets the requirements for single-crystal thin film bonding.

[0012] In this invention, during the entire polishing process in step 4 above, an interferometer is used to collect real-time profiles of the wafer surface height, interferograms, and removal rate data for each region. Simultaneously, the angular deviation between the polishing motion direction and the low crystal density axis, as well as the removal rate deviation for each region, are monitored in real-time. This data is fed back to the polishing equipment, and the polishing pressure is dynamically adjusted to ensure that the wafer warpage remains within a preset range (≤15μm) and the removal rate deviation is ≤5% throughout the entire polishing process. This achieves precise and controllable dual control over both low warpage and consistent removal rate.

[0013] In this invention, the interferometer collects the height changes of various points on the wafer surface in real time, and indirectly obtains the material removal rate of the region by calculating the height change, and uses this to characterize the thickness change.

[0014] For the purposes of this invention, the aforementioned curvature is calculated using a surface height profile, and the calculation formula is as follows: Where g1 and g2 are the average heights at both ends of the wafer, and g3 is the average height at the center.

[0015] For the purposes of this invention, the aforementioned wafer thickness is calculated based on the number of interference fringes, using the following formula: , where λ is the wavelength of the interference light, m ​​is the number of fringes, and n is the refractive index of the corresponding wafer; The formula for calculating warpage is: Where v is Poisson's ratio, σ is stress, d3 is the thickness of the damaged layer, d4 is the wafer diameter, d5 is the thickness of the bottom layer, and E is Young's elastic modulus.

[0016] For the purposes of this invention, the warpage is ≤15μm and the removal rate deviation is ≤5%.

[0017] For the purposes of this invention, the aforementioned curvature is <30μm.

[0018] For the purposes of this invention, the abrasive concentration in the above-mentioned composite polishing fluid is 15-20 wt%, the potassium hydroxide concentration is 1.2-1.8 wt%, and the surfactant concentration is 0.03-0.04 wt%.

[0019] For the purposes of this invention, the abrasive comprises silica sol and / or diamond.

[0020] For the purposes of this invention, the particle size of the silica abrasive in the silica sol is 15-40 nm.

[0021] For the purposes of this invention, the pH adjuster described above includes a phosphate-based pH adjuster.

[0022] For the purposes of this invention, the aforementioned wafer includes: an X-axis lithium niobate wafer, a silicon wafer, a gallium arsenide wafer, a sapphire wafer, or a silicon carbide wafer.

[0023] When the wafer is an X-axis lithium niobate wafer: In step one, a. the ultrasonic cleaning time is preferably 15-20 min; b. the silica abrasive particle size of the silica sol is preferably 20-40 nm; c. the pH value is preferably adjusted to 9.0-9.5 using a phosphoric acid-based pH adjuster. In step two, the clamping pressure is preferably 10-16 g / cm. 2 ; In step three, the pre-polishing stage: the preferred polishing pressure is 50-80 g / cm. 2 The preferred polishing speed is 80-100 r / min; during the fine polishing stage, the preferred polishing pressure is 20-30 g / cm. 2 The polishing time is preferably 15-20 minutes; When the wafer is a silicon wafer: In step one, a. hydrofluoric acid solution can be used to assist in cleaning; b. the silica abrasive particle size of the silica sol is preferably 20-40 nm; c. a phosphoric acid pH adjuster is preferably used to adjust the pH value to 8.5-9.0, which can reduce oxidation damage on the silicon wafer surface; In step two, the clamping pressure is preferably 8-18 g / cm. 2 ; In step three, the pre-polishing stage: the preferred polishing pressure is 40-70 g / cm. 2 The preferred polishing speed is 80-100 r / min; for the fine polishing stage, the preferred polishing pressure is 15-25 g / cm. 2 The polishing time is preferably 15-20 minutes; When the wafer is a gallium arsenide wafer: In step one, a. the silica abrasive particle size of the silica sol is preferably 20-40 nm; b. the pH value is preferably adjusted to 9.0-9.5 by a phosphoric acid pH adjuster; c. citric acid can also be added to the polishing solution, with the amount of citric acid in the polishing solution being 0.5-1.0 wt%, to enhance the synergistic effect of chemical corrosion and mechanical polishing. In step two, the clamping pressure is preferably 8-15 g / cm. 2 ; In step three, the pre-polishing stage: the preferred polishing pressure is 50-80 g / cm. 2 The preferred polishing speed is 70-90 r / min; during the fine polishing stage, the preferred polishing pressure is 20-30 g / cm. 2 The polishing time is preferably 15-20 minutes; When the wafer is a sapphire wafer: In step one, a. the silica abrasive particle size of the silica sol is preferably 15-30 nm to reduce mechanical damage to the crystal surface; b. the pH value is preferably adjusted to 9.0-9.5 by a phosphoric acid-based pH adjuster. In step three, the pre-polishing stage: the preferred polishing pressure is 50-80 g / cm. 2 The preferred polishing speed is 80-100 r / min; during the fine polishing stage, the preferred polishing pressure is 20-30 g / cm. 2 The polishing time is preferably 20-30 minutes; When the wafer is a silicon carbide wafer: In step one, a. the silica abrasive particle size of the silica sol is preferably 20-40 nm; b. the pH value is preferably adjusted to 9.0-9.5 by a phosphate-based pH adjuster; c. diamond abrasive may also be added to the polishing solution, and the amount of diamond abrasive in the polishing solution is 12-18 wt%.

[0024] In step two, the clamping pressure is preferably 15-25 g / cm. 2 ; In step three, the pre-polishing stage: the preferred polishing pressure is 70-90 g / cm. 2 The preferred polishing speed is 80-100 r / min; during the fine polishing stage, the preferred polishing pressure is 20-30 g / cm. 2 The polishing time is preferably 15-20 minutes; For the purposes of this invention, the surfactant is selected from at least one of graphene oxide or modified graphene oxide.

[0025] In this invention, the modified graphene oxide is obtained by a dehydration condensation reaction between graphene oxide and hydrolyzed γ-methacryloxypropyltrimethoxysilane, followed by a grafting reaction with phenylvinyl sulfone.

[0026] The modification process consists of two covalent grafting reactions. In the first step, within a weakly acidic ethanol system, the silane coupling agent undergoes hydrolysis to generate silanol groups, which then undergo dehydration condensation with the hydroxyl groups on the surface of graphene oxide. This covalent bond fixes the silane structure with unsaturated double bonds to the graphene sheets, and the silane branches can expand the stacked sheet structure, alleviating the problem of sheet aggregation. In the second step, using an azo initiator, the vinyl group of phenyl vinyl sulfone undergoes free radical polymerization with the terminal double bonds of the silane, and the sulfone functional group is stably grafted onto the sheet surface. The sulfone group is a strongly polar hydrophilic group, effectively improving the dispersion ability of graphene oxide in alkaline polishing fluid, preventing abrasive agglomeration and wafer surface scratches; it also improves the wetting effect at the polishing fluid-crystal interface, balancing the chemical corrosion rate of anisotropic crystals. Graphene sheets possess lubricating and friction-reducing properties, weakening the frictional shear stress at the polishing interface, reducing residual internal stress during wafer processing, and simultaneously optimizing wafer warpage, surface roughness, and material removal uniformity after polishing, thus adapting to the processing requirements of low-warpage wafers for single-crystal thin-film bonding.

[0027] Specifically, the preparation method of the above-mentioned modified graphene oxide includes: adding graphene oxide to an ethanol aqueous solution with a concentration of 93-95 wt%, ultrasonically dispersing for 1.5-2.5 h, adjusting the pH to 3.5-4, then adding an ethanol solution of γ-methacryloyloxypropyltrimethoxysilane with a concentration of 0.03-0.05 g / mL, heating to 55-60℃ and reacting for 20-28 h, washing 4-6 times with anhydrous ethanol, and vacuum drying at 75-85℃ for 10-12 h to obtain silane-modified graphene oxide; adding the silane-modified graphene oxide to N,N-dimethylformamide (silane-modified... A dispersion was prepared by mixing graphene oxide and N,N-dimethylformamide in a mass-to-volume ratio of 1 g: 50-80 mL. The mixture was ultrasonically dispersed for 25-35 min. Phenylvinyl sulfone was then added to N,N-dimethylformamide (in a mass-to-volume ratio of 1 g: 50-80 mL) and dissolved. Azobisisobutyronitrile was then added and stirred until homogeneous. The azobisisobutyronitrile was then slowly added to the dispersion at 75-85 °C. After the addition was complete, the reaction was continued for 10-15 h. The mixture was then ultrasonically treated for 35-40 min, centrifuged, washed, and dried to obtain modified graphene oxide.

[0028] The mass-to-volume ratio of graphene oxide to ethanol aqueous solution is 1 g: 100-150 mL; the mass ratio of graphene oxide to γ-methacryloyloxypropyltrimethoxysilane is 1: 2.5-3.5; the mass ratio of graphene oxide to phenyl vinyl sulfone is 1: 2.5-3.5; and the amount of azobisisobutyronitrile is 2-3 wt% of the amount of reactant monomers.

[0029] The beneficial effects of this invention include: 1. Excellent polishing effect: the wafer warpage after polishing is ≤15μm (far superior to the existing technology's Warp <40μm index), the surface roughness is 0.1-0.3nm, the total thickness variation (TTV) is ≤2μm, and the removal rate deviation is ≤5%, fully meeting the stringent requirements of single crystal thin film bonding for wafers.

[0030] 2. Polishing efficiency is significantly improved. Compared with existing polishing processes, this invention can shorten polishing time by 10%-20% through axial matching and closed-loop control, greatly reducing the time cost of industrial production.

[0031] 3. It has strong versatility and can be widely used in the polishing of various wafers without the need to design new polishing processes for different wafers, thus reducing R&D and production costs.

[0032] 4. The process is stable and reliable. Through the synergistic effect of closed-loop control mechanism, special fixtures and customized polishing fluid, the polishing qualification rate is increased to ≥98%, avoiding the problem of high scrap rate caused by blind polishing in existing polishing processes. It is suitable for large-scale industrial production, significantly improves wafer bonding performance and device reliability, and has important engineering application value. Attached Figure Description

[0033] Figure 1 This is a real-time curvature diagram of wafer polishing during the stress relief stage of Example 1; Figure 2 This is a real-time total thickness deviation diagram of wafer polishing during the stress relief stage of Example 1; Figure 3 The results are shown in the infrared spectrum test of the modified graphene oxide prepared in Example 6 and the graphene oxide. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be further described in detail below with reference to specific embodiments: Example 1:

[0035] A method for polishing low-warpage wafers for single-crystal thin-film bonding includes the following steps: Step 1: Wafer pretreatment and composite polishing slurry preparation. An 8-inch diameter lithium niobate wafer with an initial thickness of 500 μm was selected. The surface was rinsed with deionized water, ultrasonically cleaned in acetone solution for 18 min, and dried with nitrogen to obtain a clean wafer to be polished. Based on the total mass fraction of solute, 18 wt% silica sol (silica abrasive particle size 30 nm), 1.5 wt% potassium hydroxide, and 0.035 wt% graphene oxide surfactant were added. Sodium dihydrogen phosphate buffer solution was used as the pH adjuster to 9.2, and deionized water was used as the solvent. The ultrasonic mixing power was 2000 W for 30 min to obtain the composite polishing slurry. Step 2: Fixture installation. An eccentric adaptive planetary wheel fixture is used to place the wafer in the wafer placement slot. The position is adjusted so that the polishing motion direction forms a 38° angle with the

[100] low crystal density axis. The clamping pressure is 13 g / cm. 2 The flexible rubber ring fits the edge of the wafer to ensure that the drainage holes are unobstructed; Step 3: Segmented polishing, pre-polishing stage: pressure 65g / cm 2Rotation speed 90 r / min, composite polishing fluid flow rate 13 L / min, time 12 min, removal amount 25 μm; Stress release stage: Data is collected in real time using an interferometer to calculate real-time thickness, curvature, and warpage. The real-time film thickness data is compared with the preset ideal removal rate curve. If the removal rate in the edge region is lower than the target value, a control command is generated to dynamically increase the pressure applied to the edge pressure zone; conversely, the pressure is reduced accordingly. During the adjustment process, the pressure change gradient is 8 g / cm. 2 / min, rotation speed 40r / min, composite polishing fluid flow rate 11L / min, time 10min; fine polishing stage: pressure 25g / cm 2 Rotation speed 55 r / min, composite polishing fluid flow rate 11 L / min, time 18 min, total removal amount 50 μm; ensure removal rate deviation ≤5%, warpage ≤15 μm, and curvature <30 μm; Step 4: Post-processing, rinse with deionized water, ultrasonically clean with anhydrous ethanol for 10 minutes, and dry with nitrogen to obtain the finished wafer.

[0036] Finished product inspection: wafer warpage 12μm, surface roughness 0.2nm, TTV 1.8μm, removal rate deviation 4.2%, polishing pass rate 99%, fully meeting the requirements for single crystal thin film bonding. Furthermore, the warpage before polishing was >40μm, and the warpage after polishing was 12μm, demonstrating a significant improvement.

[0037] Example 2:

[0038] A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that an 8-inch silicon wafer is used instead of the X-axis lithium niobate wafer, and the pH of the polishing slurry is adjusted to 8.8, with a clamping pressure of 12 g / cm. 2 Finished product inspection: warpage 11μm, surface roughness 0.25nm, TTV 1.7μm, polishing pass rate 98.5%.

[0039] Example 3:

[0040] A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that a 6-inch gallium arsenide wafer is used instead of the X-axis lithium niobate wafer, and the

[110] crystal orientation is adjusted to a 35° angle. 0.8 wt% citric acid is added to the polishing solution. Finished product inspection: warpage 13 μm, surface roughness 0.22 nm, TTV 1.9 μm, polishing pass rate 98.2%.

[0041] Example 4:

[0042] A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that an 8-inch sapphire wafer is used instead of the lithium niobate wafer along the X-axis, and a 40° c-axis angle is matched. A 20nm silica sol abrasive is used. Finished product testing results: warpage 14μm, surface roughness 0.18nm, TTV 1.8μm, polishing pass rate 98.8%.

[0043] Example 5:

[0044] A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that an 8-inch silicon carbide wafer is used instead of the X-axis lithium niobate wafer, and a 42° angle is matched to the

[100] crystal orientation. Diamond abrasive is added to the polishing slurry at a concentration of 15 wt%. Finished product testing: warpage 13 μm, surface roughness 0.21 nm, TTV 1.9 μm, polishing pass rate 98.1%.

[0045] Example 6:

[0046] A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that modified graphene oxide is used instead of graphene oxide. Finished product testing showed a wafer warpage of 10 μm, surface roughness of 0.17 nm, TTV of 1.4 μm, removal rate deviation of 3.3%, and a polishing pass rate of 99.6%, fully meeting the requirements for single-crystal thin-film bonding. The modified graphene oxide incorporates sulfone groups, improving the dispersion stability within the alkaline polishing solution and preventing abrasive agglomeration that scratches the wafer; it also enhances the wettability of the polished liquid crystal, balancing anisotropic corrosion; and provides stronger lubrication, reducing interfacial friction and residual wafer stress, thus optimizing warpage, roughness, and removal uniformity.

[0047] A method for preparing modified graphene oxide includes: adding graphene oxide to a 94 wt% ethanol aqueous solution, ultrasonically dispersing for 2 h, adjusting the pH to 3.5, then adding an ethanol solution of 0.04 g / mL γ-methacryloyloxypropyltrimethoxysilane, heating to 58 °C and reacting for 24 h, washing five times with anhydrous ethanol, and vacuum drying at 80 °C for 11 h to obtain silane-modified graphene oxide; adding the silane-modified graphene oxide to N,N-dimethylformamide (silane-modified graphene oxide and N, A dispersion was prepared by mixing N,N-dimethylformamide (mass-volume ratio of 1 g: 60 mL) and ultrasonically dispersing for 30 min. Phenyl vinyl sulfone was then added to N,N-dimethylformamide (mass-volume ratio of phenyl vinyl sulfone to N,N-dimethylformamide was 1 g: 70 mL) and dissolved. Azobisisobutyronitrile was then added and stirred until homogeneous. The mixture was then slowly added to the above dispersion at 82 °C. After the addition was complete, the reaction was continued for 14 h. The mixture was then ultrasonically treated for 38 min, centrifuged, washed, and dried to obtain modified graphene oxide.

[0048] The mass-to-volume ratio of graphene oxide to ethanol aqueous solution was 1 g: 120 mL; the mass ratio of graphene oxide to γ-methacryloyloxypropyltrimethoxysilane was 1:3; the mass ratio of graphene oxide to phenylvinyl sulfone was 1:3; and the amount of azobisisobutyronitrile was 2.5 wt% of the amount of reactant monomers.

[0049] The above tests were performed on modified graphene oxide and graphene oxide, and the results are as follows: Figure 3 As shown, by Figure 3 It can be seen that, compared with the infrared spectrum of graphene oxide, the infrared spectrum of modified graphene oxide is at 1257 cm⁻¹. -1 1135cm -1 The presence of a sulfone-based infrared absorption peak at the α-position indicates that phenyl vinyl sulfone participated in the formation reaction of modified graphene oxide.

[0050] Comparative Example 1: A method for polishing low-warpage wafers for single-crystal thin-film bonding differs from Example 1 in that the pH value is adjusted to 10 in step two. Finished product testing: wafer warpage 28 μm, surface roughness 0.65 nm, TTV 3.7 μm, removal rate deviation 11.6%, polishing pass rate 78%. Excessively high pH, ​​with its strong alkaline KOH, exacerbates the anisotropic chemical corrosion of lithium niobate crystals, amplifying the difference in corrosion rates between different crystal orientations; the internal corrosion stress of the wafer surges, resulting in severely uneven removal rates between the edges and the center, causing warpage, TTV, and roughness to all exceed standards, rendering the wafer unsuitable for single-crystal thin-film bonding.

[0051] Comparative Example 2: The difference between a method for polishing low-warpage wafers for single-crystal thin-film bonding and Example 1 is as follows: In step three, the position is adjusted so that the polishing motion direction forms a 50° angle with the

[100] low crystal density axis. Finished product inspection: wafer warpage 24μm, surface roughness 0.55nm, TTV 3.2μm, removal rate deviation 9.8%, polishing pass rate 84%. The angle deviates from the optimal range of 30°-45°, which cannot offset the difference in removal rate caused by the anisotropy of the crystal density of lithium niobate crystals; the low crystal density crystal orientation grinding removal efficiency is low, the radial material removal of the wafer is uneven, the residual mechanical stress is concentrated, and the warpage and thickness uniformity do not meet the standards.

[0052] The conventional techniques described in the above embodiments are existing technologies known to those skilled in the art, and therefore will not be described in detail here.

[0053] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for polishing low-warpage wafers for single-crystal thin-film bonding, characterized in that, Includes the following steps: Step 1: Wafer pretreatment and composite polishing solution preparation: Clean and dry the wafer to be polished to remove surface impurities and oil; prepare the composite polishing solution, adjust the pH value to 8.5-9.5, and ultrasonically mix evenly for later use. Step 2, Fixture Installation and Wafer Fixing: An eccentric adaptive planetary wheel fixture is used to adjust the wafer placement position so that the polishing motion direction forms an angle of 30°-45° with the low crystal density axis of the wafer; Step 3, Segmented Polishing: A three-stage process of pre-polishing, stress relief, and fine polishing is adopted. Data on wafer thickness, warpage, removal rate deviation, and axial angle deviation are collected in real time by an interferometer and fed back to the polishing equipment to dynamically adjust the polishing parameters. Step 4: Post-polishing treatment: Clean and dry the polished wafer to obtain a low-warpage wafer that meets the requirements for single-crystal thin-film bonding.

2. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 1, characterized in that, The wafer includes any one of the following: an X-axis lithium niobate wafer, a silicon wafer, a gallium arsenide wafer, a sapphire wafer, or a silicon carbide wafer.

3. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 1, characterized in that, The preparation method of the composite polishing fluid includes: adding abrasive, potassium hydroxide and surfactant to deionized water, adjusting the pH value to 8.5-9.5 with a pH adjuster, and then placing it in an ultrasonic device for ultrasonic mixing at a power of 1500-2000W for 20-30 minutes to obtain a uniform and stable composite polishing fluid.

4. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 3, characterized in that, The composite polishing fluid contains 15-20 wt% abrasive, 1.2-1.8 wt% potassium hydroxide, and 0.03-0.04 wt% surfactant.

5. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 3, characterized in that, The abrasive comprises silica sol and / or diamond; The surfactant is selected from at least one of graphene oxide or modified graphene oxide. The pH adjuster includes a phosphate-based pH adjuster.

6. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 5, characterized in that, The method for preparing the modified graphene oxide includes: adding graphene oxide to an ethanol aqueous solution with a concentration of 93-95 wt%, ultrasonically dispersing for 1.5-2.5 h, adjusting the pH to 3.5-4, then adding an ethanol solution of γ-methacryloyloxypropyltrimethoxysilane with a concentration of 0.03-0.05 g / mL, heating to 55-60℃ and reacting for 20-28 h, washing 4-6 times with anhydrous ethanol, and vacuum drying at 75-85℃ for 10-12 h to obtain the modified silane. Modified graphene oxide: Silane-modified graphene oxide was added to N,N-dimethylformamide to prepare a dispersion. The dispersion was ultrasonically dispersed for 25-35 min. Phenylvinyl sulfone was added to N,N-dimethylformamide and dissolved. Azobisisobutyronitrile was then added and stirred until homogeneous. The mixture was then slowly added to the dispersion at 75-85℃. After the addition was complete, the reaction was continued for 10-15 h. The mixture was then ultrasonically treated for 35-40 min, centrifuged, washed, and dried to obtain modified graphene oxide.

7. The method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 1, characterized in that, The three-stage process includes: Pre-polishing stage: Set polishing pressure to 40-90 g / cm 2 The polishing speed is 70-100 r / min, the flow rate of the composite polishing fluid is 12-15 L / min, and the polishing time is 10-15 min. This method quickly removes macroscopic defects and damage layers from the wafer surface and simultaneously acquires surface height profiles in real time using an interferometer to initially control the curvature. The stress release phase includes: employing a variable pressure control mode with a pressure gradient of 5-10 g / cm³. 2 / min, polishing speed 30-50r / min, composite polishing fluid flow rate 10-12L / min, polishing time 8-12min; The fine polishing stage includes setting the polishing pressure to 15-30 g / cm. 2 Polishing speed 50-60 r / min, composite polishing fluid flow rate 10-12 L / min, polishing time 15-25 min.

8. A method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 7, characterized in that, The curvature is calculated based on the surface height profile, and the calculation formula is as follows: Where g1 and g2 are the average heights at both ends of the wafer, and g3 is the average height at the center.

9. A method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 1, characterized in that, The wafer thickness is calculated based on the number of interference fringes, using the following formula: , where λ is the wavelength of the interference light, m ​​is the number of fringes, and n is the refractive index of the corresponding wafer; The warpage is calculated using the following formula: Where v is Poisson's ratio, σ is stress, d3 is the thickness of the damaged layer, d4 is the wafer diameter, d5 is the thickness of the bottom layer, and E is Young's elastic modulus.

10. A method for polishing low-warpage wafers for single-crystal thin-film bonding according to claim 1, characterized in that, The warpage is ≤15μm, and the removal rate deviation is ≤5%.