A ceramic grinding wheel and its preparation method
By using titanate coupling agents to activate the surface of brown fused alumina and the low-temperature binder system in ceramic grinding wheels, the problem of mismatched thermal expansion coefficients in white fused alumina-brown fused alumina composites was solved, improving the flexural strength and grinding performance of the grinding wheels, extending their service life, and reducing the sintering temperature.
Patent Information
- Application Number
- CN202611303226.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ceramic grinding wheels with a mixture of white fused alumina and brown fused alumina suffer from mismatched coefficients of thermal expansion, resulting in interfacial tensile stress, insufficient bond strength, and high sintering temperature, leading to a decline in abrasive performance. Consequently, it is difficult to achieve both high grinding efficiency and long service life.
A low-expansion-coefficient Al2TiO5 shell is formed on the surface of brown fused alumina by activating it with a titanate coupling agent. A low-temperature binder system of β-spodumene and high borosilicate glass is combined with phosphate to form AlPO4 whiskers on the surface of the abrasive. Nano-zirconia is used to modify the interface to improve the flexural strength, and uniform pores are formed by mixing raw materials.
The thermal expansion coefficients of the white fused alumina and brown fused alumina composite abrasives were matched, reducing interfacial tensile stress, improving the flexural strength and grinding performance of the grinding wheel, extending its service life, and reducing sintering temperature and energy consumption.
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic grinding wheel technology, and in particular to a ceramic grinding wheel and its preparation method. Background Technology
[0002] Ceramic grinding wheels are mainly composed of three elements: abrasive, bonding agent, and porosity. Grinding wheels made with corundum-based materials as abrasives are widely used in high-speed grinding, precision grinding, and finishing of difficult-to-machine materials due to their advantages such as high grinding efficiency, good heat resistance, and strong shape retention.
[0003] The chemical essence of corundum-based materials is α-Al₂O₃. Among them, white corundum has high Al₂O₃ purity, a complete crystal structure, and relatively high brittleness, with a Mohs hardness of over 9.0. Ceramic grinding wheels made from it have strong self-sharpening properties, easily undergoing micro-fracture along grain boundaries during grinding, thus exposing new sharp cutting edges, and generating lower grinding heat. However, white corundum has poor toughness and relatively insufficient impact fracture resistance, making it prone to premature macroscopic fracture or even overall fragmentation. Brown corundum contains approximately 3% to 5% impurities such as TiO₂, SiO₂, and Fe₂O₃. The glassy coating formed by these impurity phases at the grain boundaries has a toughening effect, giving it better fracture toughness and bending strength compared to white corundum, enabling it to withstand greater grinding impact and resulting in higher grinding wheel durability. However, grinding wheels made from brown corundum have poor self-sharpening properties, and the dulled abrasive grains are difficult to actively detach and break, easily causing surface burns on the workpiece.
[0004] It is evident that neither white fused alumina nor brown fused alumina alone can simultaneously meet the combined requirements of high grinding efficiency and long service life. Currently, brown fused alumina and white fused alumina are often combined to address the issues of white fused alumina being sharp enough but not impact-resistant, and brown fused alumina being tough enough but not sharp enough, thereby improving the overall grinding performance of the grinding wheel.
[0005] However, the coefficient of thermal expansion of white fused alumina is approximately 7.0 × 10⁻⁶ / ℃, while that of brown fused alumina is approximately 7.8 × 10⁻⁶ / ℃, a significant difference. During the sintering and cooling process with ceramic binders, the binder bridge generates uneven radial tensile stress at the interface between the two abrasive grains with different expansion rates, inducing interfacial microcracks and reducing the bending strength and fracture toughness of the grinding wheel. This poses a risk of wheel breakage under high-speed grinding conditions. To address this issue, most methods involve adjusting the binder composition to suit a single abrasive, lacking a means to synergistically control the expansion of the two fused alumina composite systems.
[0006] In addition, to obtain sufficient glassy phase fluidity and densification, the sintering temperature of traditional binders typically needs to reach 1320℃~1350℃. Under this high temperature and long-term holding, the microcrystals on the surface of corundum abrasive grains will undergo secondary recrystallization and growth, and the internal residual thermal stress will increase sharply, causing the compressive strength of the abrasive grains themselves to decrease by about 15%~20%. Raising the sintering temperature to ensure the strength of the grinding wheel is essentially at the expense of the performance of the abrasive itself. Furthermore, during the sintering process, the impurities contained in brown corundum are prone to react with components such as SiO2 in the binder, causing the local composition of the binder bridge to deviate from the design value, weakening the strength of the binder bridge itself, and even producing abnormal crystalline phases with low expansion coefficients.
[0007] In summary, developing a ceramic grinding wheel preparation scheme that can adapt to white-brown fused alumina mixed abrasives, has low interfacial thermal stress, lower sintering temperature, and excellent mechanical properties has significant engineering application value. Summary of the Invention
[0008] The purpose of this invention is to provide a ceramic grinding wheel and its preparation method, which balances the thermal expansion coefficient of the white fused alumina and brown fused alumina composite abrasive, so that the grinding wheel made of the white fused alumina and brown fused alumina composite abrasive has good mechanical properties, and takes into account the dual requirements of high grinding efficiency and long service life.
[0009] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A ceramic grinding wheel comprises the following raw materials in parts by weight: 65-75 parts abrasive 16-22 parts of binder composite particles 1.5 to 2.5 parts phosphate 2-3 parts adhesive Organic polar wetting agent comprising 2-4 wt% of the total weight of the abrasive; The abrasive comprises, by weight: 40-50 parts of white fused alumina and 25-33 parts of activated brown fused alumina; The raw materials of the binder composite particles, by weight, include: 38-50 parts of β-spodumene, 17-26 parts of high borosilicate glass powder, 9-15 parts of active α-Al2O3 micro powder, 4-9 parts of surface-modified stabilized nano-zirconia, 2-6 parts of flux, 0.8-2.5 parts of rare earth oxides, and 7-12 parts of binder-binder aqueous solution; the activated brown fused alumina is obtained by modifying brown fused alumina with a titanate coupling agent; The surface-modified stabilized nano-zirconia is obtained by modifying nano-zirconia with a silane coupling agent.
[0010] Optionally, the titanate coupling agent comprises at least one of NDZ-311, KR-TTS, and KR-38S; The titanate coupling agent is used at an amount of 1.0~3.0 wt% of brown fused alumina. The silane coupling agent comprises at least one of KH-550, KH-560, KH-570, A-174, and HMDS; The stabilized nano-zirconia comprises at least one of 3Y-ZrO2, 2Y-ZrO2, Ce-TZP, and Mg-PSZ; The amount of the silane coupling agent used is 0.5~1.5wt% of the stabilized nano-zirconia.
[0011] Optionally, the organic polar wetting agent comprises at least one of ethylene glycol, glycerol, diethylene glycol, propylene glycol, and polyethylene glycol; The phosphate contains at least one of aluminum dihydrogen phosphate, aluminum monohydrogen phosphate, and silicon phosphate. The binder contains at least one of dextrin, methylcellulose, hydroxypropyl methylcellulose, corn starch, water glass, and paraffin.
[0012] Optionally, the flux comprises at least one of calcium fluoride, fluorite powder, cryolite, lithium fluoride, and sodium fluorosilicate; The rare earth oxides include at least one of ytterbium oxide, yttrium oxide, cerium oxide, lanthanum oxide, samarium oxide, and erbium oxide; The mass concentration of the binder aqueous solution is 7-15%; The binder comprises at least one of polyvinyl alcohol, dextrin, methylcellulose, hydroxypropyl methylcellulose, and polyethylene glycol.
[0013] Optionally, the method for preparing the binder composite particles includes mixing β-spodumene, borosilicate glass powder, active α-Al2O3 micro powder, surface-modified stabilized nano-zirconia, flux, rare earth oxides, and an aqueous solution of binder, followed by granulation and drying to obtain binder composite particles.
[0014] Optionally, the granulation process uses a 35-45 mesh sieve, and the drying temperature is 75-85℃ for 3-5 hours.
[0015] The present invention also provides a method for preparing a ceramic grinding wheel, comprising the following steps: 1) Mix white fused alumina and activated brown fused alumina, add an organic polar wetting agent, mix well, and then add phosphate to obtain an abrasive coated with phosphate. 2). Add the binder composite particles to the abrasive coated with phosphate obtained in step 1), and add the binder and water in sequence to obtain the grinding wheel forming material; 3) Press the grinding wheel forming material obtained in step 2) into shape, and sinter it to obtain the ceramic grinding wheel.
[0016] Optionally, the moisture content of the grinding wheel forming material in step 2) is 1.5~2.5wt%.
[0017] Optionally, step 3) of the compression molding specifically includes a first stage: pressurizing to 45~55MPa and holding for 3~8s, and a second stage: pressurizing to 110~130MPa and holding for 12~18s.
[0018] Optionally, the sintering in step 3) specifically includes a first stage: heating to 400-500℃ at a heating rate of 0.5-1.0℃ / min and holding at that temperature for 180-240min; Second stage: Heat to 900~1000℃ at a heating rate of 1.0~1.5℃ / min, and hold for 25~45min; The third stage: heat to 1150~1170℃ at a heating rate of 1.0~1.5℃ / min, and hold for 120~180min; Fourth stage: Cool down to 630~670℃ at a cooling rate of 1.5~2.0℃ / min, hold at that temperature for 60~120min, and then let it cool naturally to room temperature. The total cooling time shall not be less than 10h.
[0019] The ceramic grinding wheel provided by this invention comprises a composite of white and brown fused alumina abrasives. The brown fused alumina surface is activated using titanate ester to form a low-expansion-coefficient Al2TiO5 shell, reducing its apparent thermal expansion coefficient to match that of the white fused alumina. This reduces or even eliminates interfacial tensile stress, preventing microcrack formation. The binder system used in this invention is a low-temperature binder system of β-spodumene and high-borosilicate glass, lowering the sintering temperature and reducing high-temperature damage to the corundum abrasive grains while saving energy. The system contains framework materials (α-Al2O3, rare earth oxides), which are first mixed and granulated before being mixed with the abrasive. This ensures that the various binder materials form a microscopically close contact before contacting the abrasive grains, avoiding component segregation that may occur when the abrasive and binder raw materials are directly mixed.
[0020] This invention also provides a method for preparing the ceramic grinding wheel. During the raw material mixing process, phosphate is first coated onto the surface of the abrasive grains under the action of an organic polar wetting agent, and then a binder is added. Coating the abrasive grains with phosphate under the action of the organic polar wetting agent reduces direct contact between the phosphate and spodumene at a physical level, preventing a solid-phase displacement reaction that releases PH3 gas and causes blistering of the green body during the initial heating stage. During the sintering of the grinding wheel, phosphates generate AlPO4 whiskers in situ on the surface of the abrasive. These whiskers react with α-Al2O3 micro powder to form chemical bridges, changing the bonding method between the binder and the abrasive from the traditional mechanical interlocking to chemical bonding, thus improving the interfacial flexural strength. During the cooling process of the sintering step, holding at 630~670℃ provides sufficient phase transformation time for nano ZrO2. The volume expansion caused by the phase transformation introduces radial compressive stress into the binder-abrasive interface, which offsets the harmful tensile stress caused by the cooling shrinkage difference during the cooling process, avoids the generation of phase transformation cracks, improves the flexural strength of the grinding wheel, and can withstand higher grinding linear speeds.
[0021] This invention does not intentionally add pore-forming agents for the purpose of creating pores. Instead, pores are formed by the gas overflow caused by the oxidative decomposition of binders and wetting agents added during the raw material mixing process during the sintering step, as well as by the difference in particle size distribution between the abrasive and the binder. This method simplifies the formulation and results in a uniform distribution of pores, which is beneficial for industrial production. Detailed embodiments This invention provides a ceramic grinding wheel comprising the following raw materials in parts by weight: Abrasive material 65-75 parts; 16-22 parts of binder composite particles; 1.5 to 2.5 parts phosphate; 2-3 parts adhesive; Organic polar wetting agent comprising 2-4 wt% of the total weight of the abrasive; The abrasive comprises, by weight: 40-50 parts of white fused alumina and 25-33 parts of activated brown fused alumina; The raw materials of the binder composite particles, by weight, include: 38-50 parts of β-spodumene, 17-26 parts of high borosilicate glass powder, 9-15 parts of active α-Al2O3 micro powder, 4-9 parts of surface-modified stabilized nano-zirconia, 2-6 parts of flux, 0.8-2.5 parts of rare earth oxides, and 7-12 parts of binder-binder aqueous solution. The activated brown fused alumina was obtained by modifying brown fused alumina with a titanate coupling agent; The surface-modified stabilized nano-zirconia is obtained by modifying nano-zirconia with a silane coupling agent.
[0022] In this invention, the abrasive is preferably 68-74 parts, more preferably 69-73 parts, and even more preferably 70-72 parts. The preferred number of the binder composite particles is 17-21 parts, more preferably 18-20 parts, and even more preferably 19-20 parts; The preferred amount of phosphate is 1.6 to 2.3 parts, more preferably 1.8 to 2.2 parts, and even more preferably 2.0 to 2.1 parts; The adhesive is preferably in the amount of 2.1 to 2.8 parts, more preferably 2.3 to 2.6 parts, and even more preferably 2.4 to 2.5 parts. The organic polar wetting agent preferably accounts for 2.5 to 3.8 wt% of the total weight of the abrasive, more preferably 2.8 to 3.5 wt%, and even more preferably 3.0 to 3.2 wt%. In this invention, the preferred specification of the white corundum in the abrasive is F24~F120, and its weight is preferably 42~48 parts, more preferably 43~45 parts. The activated brown fused alumina is preferably 27-32 parts by weight, more preferably 28-30 parts by weight; The specific preparation method of the activated brown fused alumina includes mixing brown fused alumina (F16~F120) with an ethanol solution of a titanate coupling agent (anhydrous ethanol is selected), followed by drying and calcination to obtain activated brown fused alumina. The ratio of brown fused alumina to titanate coupling agent in ethanol solution is 1 kg: 1~1.5 L, preferably 1 kg: 1.2~1.4 L; In the ethanol solution of the titanate coupling agent, the mass concentration of the titanate coupling agent is 1.5-3%, preferably 1.8-2.8%, and more preferably 2.0-2.5%; The drying temperature is preferably 100~150℃, more preferably 120~130℃, and the drying time is preferably 1.5~3h, more preferably 2~2.5h; The preferred heating rate for calcination is 3~6℃ / min, more preferably 4~5℃ / min; the preferred temperature is 750~900℃, more preferably 800~850℃; and the preferred time is 1.5~3h, more preferably 2~2.5h. In this invention, the titanate coupling agent comprises at least one of NDZ-311, KR-TTS, and KR-38S; The amount of the titanate coupling agent is preferably 1.0 to 3.0 wt% of brown fused alumina, more preferably 1.5 to 2.8 wt%, and even more preferably 2.0 to 2.5 wt%.
[0023] The binder composite particles, by weight, contain the following components: β-spodumene preferably 40-48 parts, more preferably 42-46 parts; high borosilicate glass powder preferably 18-24 parts, more preferably 20-22 parts; active α-Al2O3 micro powder preferably 10-13 parts, more preferably 11-12 parts; and surface-modified stabilized nano-zirconia preferably 5-8 parts, more preferably 6-7 parts. The flux is preferably 3-6 parts, more preferably 4-5 parts; the rare earth oxide is preferably 1.0-2.2 parts, more preferably 1.2-2.0 parts, and even more preferably 1.5-1.8 parts; the binder aqueous solution is preferably 8-11 parts, more preferably 9-10 parts. The mass concentration of the binder aqueous solution is 7-15%, preferably 8-14%, more preferably 9-13%, and even more preferably 10-12%. The binder comprises at least one of polyvinyl alcohol, dextrin, methylcellulose, hydroxypropyl methylcellulose, and polyethylene glycol.
[0024] In this invention, the silane coupling agent comprises at least one of KH-550, KH-560, KH-570, A-174, and HMDS; The stabilized nano-zirconia comprises at least one of 3Y-ZrO2, 2Y-ZrO2, Ce-TZP, and Mg-PSZ; The amount of the silane coupling agent is 0.5 to 1.5 wt% of the stabilized nano-zirconia, preferably 0.8 to 1.3 wt%, and more preferably 1.0 to 1.2 wt%.
[0025] In this invention, the organic polar wetting agent comprises at least one of ethylene glycol, glycerol, diethylene glycol, propylene glycol, and polyethylene glycol; The phosphate contains at least one of aluminum dihydrogen phosphate, aluminum monohydrogen phosphate, and silicon phosphate. The binder comprises at least one of dextrin, polyvinyl alcohol, methylcellulose, hydroxypropyl methylcellulose, polyethylene glycol, corn starch, water glass, and paraffin.
[0026] In this invention, the flux contains at least one of calcium fluoride, fluorite powder, cryolite, lithium fluoride, and sodium fluorosilicate, which reduces the surface tension and viscosity of lithium-based glass melt, promotes solid-phase reaction ion diffusion, accelerates β-spodumene crystallization, and purifies the harmful effects of impurities on the surface of brown fused alumina. The rare earth oxide contains at least one of ytterbium oxide, yttrium oxide, cerium oxide, lanthanum oxide, samarium oxide, and erbium oxide. The rare earth ions in the rare earth oxide can segregate at the grain boundaries of β-lithium nepheline microcrystals, inhibiting excessive coarsening of β-lithium nepheline grains during high-temperature heat preservation and stabilizing the thermal expansion coefficient of the binder.
[0027] In this invention, the method for preparing the binder composite particles includes mixing β-spodumene, borosilicate glass powder, active α-Al2O3 micro powder, surface-modified stabilized nano-zirconia, flux, rare earth oxide, and binder aqueous solution, followed by granulation and drying to obtain binder composite particles. The β-spodumene is preferably β-spodumene powder with a D50 of 8~12μm. Specifically, commercially available spodumene concentrate (Li2O≥6.0%) is placed in a corundum crucible and calcined at 930~970℃ for 1.5~2.5h to completely convert α-spodumene into β-spodumene. After natural cooling, anhydrous ethanol is used as the medium, and zirconia balls are used as the grinding media at a ball-to-material ratio of (2~4):1. The mixture is then loaded into a planetary ball mill and ball-milled at 250~350rpm for 5~8h. After drying at 80~90℃, the powder is passed through a 325-mesh sieve to obtain β-spodumene powder with a D50 of 8~12μm, preferably 8~10μm. Spodumene under natural conditions is mostly α-spodumene. If used directly without calcination, an α→β phase transformation easily occurs during sintering, resulting in a volume expansion of about 30%, which causes tearing of the internal structure of the grinding wheel. The preferred method for obtaining high borosilicate glass powder is to clean and dry commercially available alkali-free high borosilicate glass waste (SiO2 content 78~82wt%, B2O3 content 12~15wt%), place it in a corundum crucible, melt it at 1380~1420℃ for 1~2h, then quickly pour it into cold deionized water for rapid cooling. After water quenching, the glass fragments are dried, and the water-quenched glass blocks are ball-milled at 300rpm with zirconia balls as the grinding medium at a ball-to-material ratio of 3~5:1 for 6~10h. The powder is then passed through a 400-mesh sieve to obtain high borosilicate glass powder with D50=5~8μm. This high borosilicate glass powder can form a continuous three-dimensional glass network skeleton during the sintering process. The B2O3 contained therein can effectively reduce the high-temperature viscosity of the glass phase and promote the uniform spreading of the liquid phase between the abrasive grains, thus forming a uniform and dense glass skeleton.
[0028] The active α-Al2O3 micro powder is preferably ≥99.0% pure and has a D50 of 1~3μm, preferably 1.5~2μm. During sintering, it reacts with free SiO2 decomposed from spodumene to generate mullite (3Al2O3·2SiO2) whiskers in situ, which are anchored in the glass phase and improve the room temperature flexural strength of the binder bridge.
[0029] The preparation of surface-modified stabilized nano-zirconia specifically includes taking commercially available stabilized nano-zirconia powder (particle size 20-80 nm, preferably 40-60 nm), adding 0.5-1.5% by mass of a silane coupling agent, and dry-treating at a speed of 1200-1800 rpm, preferably 1500-1600 rpm, for 4-8 minutes, preferably 5-6 minutes, to obtain surface-modified stabilized nano-zirconia. A small amount of the surface-modified stabilized nano-zirconia powder is sprinkled onto the surface of deionized water. If the powder floats or does not settle after standing for more than 30 minutes, it indicates that the powder surface has changed from hydrophilic to hydrophobic, and the modification effect is qualified. This step ensures that the silane coupling agent is uniformly coated on the surface of the nano-zirconia particles, changing them from hydrophilic to hydrophobic, preventing agglomeration when mixed with the binder dry powder, and allowing for uniform dispersion within the binder glass phase.
[0030] In this invention, the sieve used for granulation is 35-45 mesh, preferably 40 mesh; the drying temperature is 75-85℃, preferably 80℃, and the drying time is 3-5h, preferably 4h.
[0031] This invention also provides a method for preparing a ceramic grinding wheel, comprising the following steps: 1) Mix white fused alumina and activated brown fused alumina, add an organic polar wetting agent, mix well, and then add phosphate to obtain an abrasive coated with phosphate. 2). Add the binder composite particles to the abrasive coated with phosphate obtained in step 1), and add the binder and water in sequence to obtain the grinding wheel forming material; 3) Press the grinding wheel forming material obtained in step 2) into shape, and sinter it to obtain the ceramic grinding wheel.
[0032] In this invention, step 1) preferably further includes stirring at a speed of 250~350 rpm, more preferably 300~320 rpm, adding an organic polar wetting agent and adding phosphate and mixing for 3~6 min, more preferably 4~5 min respectively.
[0033] In this invention, before adding the binder and water sequentially in step 2), it is preferable to stir at a speed of 400-600 rpm, more preferably 450-500 rpm for 7-10 minutes, and more preferably 8-9 minutes. The sequential addition of binder and water preferably includes maintaining stirring at a certain speed for 2-5 minutes after adding the binder, more preferably for 3-4 minutes; the purpose of adding water is to maintain the moisture content of the molding material. The moisture content of the grinding wheel forming material is 1.5~2.5wt%, preferably 1.8~2.3wt%, and more preferably 2.0~2.2wt%. The obtained grinding wheel forming material also contains 18-22 mesh, preferably 19-20 mesh, sieve, and is placed in a sealed bag and aged for 10-15 hours, preferably 11-14 hours, and even more preferably 12-13 hours, so that the moisture can penetrate evenly.
[0034] In this invention, step 3) of the pressing molding specifically includes a first stage: pressurizing to 45~55MPa, preferably 50~52MPa, and holding for 3~8s, preferably 4~7s, and more preferably 5~6s. Under low pressure, air is allowed to escape slowly to prevent the air from being locked up by a one-time high pressure, which would cause delamination. At the same time, the particles are allowed to slide and rearrange to eliminate the "arch bridge effect" and make the bulk density initially uniform. Second stage: pressurize to 110~130MPa, preferably 115~125MPa, more preferably 115~120MPa; hold for 12~18s, preferably 13~16s, more preferably 14~15s; after the first stage of low-pressure exhaust, pressurize further to effectively transmit the pressure during the pressing process. The density of the grinding wheel molding material after pressing is preferably 2.10~2.15g / cm3.
[0035] In this invention, the sintering in step 3) specifically includes a first stage: heating to 400-500°C, preferably 420-480°C, more preferably 450-460°C, at a heating rate of 0.5-1.0°C / min, preferably 0.6-0.8°C / min, and holding at that temperature for 180-240 min, preferably 210-225 min; Second stage: Heat to 900-1000℃, preferably 950-970℃, at a heating rate of 1.0-1.5℃ / min, preferably 1.2-1.4℃ / min, and hold for 25-45 min, preferably 30-40 min; The third stage: the temperature is increased to 1150~1170℃, preferably 1155~1160℃, at a heating rate of 1.0~1.5℃ / min, preferably 1.2~1.4℃ / min, and held for 120~180min, preferably 150~175min. Fourth stage: Cool down to 630-670℃, preferably 640-650℃, at a cooling rate of 1.5-2.0℃ / min, preferably 1.6-1.8℃ / min, hold at that temperature for 60-120 minutes, and then allow to cool naturally to room temperature. The total cooling time shall be no less than 10 hours, preferably no less than 12 hours.
[0036] In this invention, the first sintering stage is preferably carried out in a strong oxidizing atmosphere, the second stage is preferably carried out in an oxidizing atmosphere, and the third stage is preferably carried out in a weak oxidizing atmosphere. The purpose of the first sintering stage is to remove organic matter (oxidized and decomposed into CO2 and H2O) and establish initial pores. A strong oxygen content should be maintained to ensure that the organic matter undergoes sufficient oxidation reaction and that the organic matter is fully burned off. In the second sintering stage, the binder composite particles and the phosphate wrapped around the abrasive soften and melt into a liquid phase, and AlPO4 whiskers begin to "take root" on the surface of the abrasive particles. The flux can reduce the surface tension and viscosity of the glass melt, promote the early crystallization of β-spodumene, and at the same time enable the binder liquid phase to have good fluidity before reaching the maximum temperature. In order to ensure that the phosphate reaction is sufficient and that low-valence phosphides are not generated due to lack of oxygen, an oxidizing atmosphere also needs to be maintained in the second stage.
[0037] In the third stage, the oxidizing atmosphere is maintained. In this stage, the glass phase is completely melted, spread evenly on the surface of the abrasive grains, and fills the gaps between the grains to form a dense binder bridge, completing the chemical bonding between the binder and the abrasive grains. β-Spodumene precipitates β-nepheline solid solution (Li2O·Al2O3·2SiO2) and mullite (3Al2O3·2SiO2) in the range of 1000~1150℃. β-Nepheline has low expansion characteristics, which can effectively adjust the thermal expansion coefficient of the binder to match the thermal expansion coefficient of the abrasive grains. Meanwhile, mullite whiskers (generated by the reaction of active α-Al2O3 + free SiO2) are pinned in the glass phase, which can improve the creep resistance and flexural strength of the binder bridge.
[0038] The fourth stage of the sintering process is cooling and phase transformation annealing. The rapid cooling first "freezes" the dense network structure formed at high temperature, inhibits the excessive growth of crystals such as β-spodumene, and allows the binder bridge to solidify smoothly, avoiding unnecessary excessive reaction between the abrasive surface and the binder. The heat preservation stage provides sufficient phase transformation time for nano-zirconia. The subsequent natural cooling to room temperature can ensure uniform grinding wheel temperature and prevent thermal shock cracking.
[0039] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention. Example
[0040] Activation treatment of brown fused alumina: Take 1 kg of brown fused alumina with a particle size of F60 (Al2O3≥95.0%), immerse it in 1.2 L of 2% (w / w) titanate coupling agent ethanol solution (the titanate coupling agent is NDZ-311, and anhydrous ethanol is used) for 15 min. After immersion, dry it at 120℃ for 2 h, then transfer it to a muffle furnace and heat it to 800℃ at a rate of 4℃ / min. Keep it at this temperature for 2 h in air atmosphere, and then cool it with the furnace to obtain activated brown fused alumina.
[0041] Preparation of β-spodumene powder Commercially available spodumene concentrate (Li₂O ≥ 6.0%) was placed in a corundum crucible and calcined at 950℃ for 2 hours. After natural cooling to room temperature in the furnace, it was removed. Using anhydrous ethanol as the medium and zirconia balls as the grinding media, the concentrate was ball-milled in a planetary ball mill at 300 rpm for 6 hours at a ball-to-material ratio of 3:1. The concentrate was then dried at 80℃ and passed through a 325-mesh sieve to obtain β-spodumene powder with a D50 of 8~10 μm.
[0042] Preparation of high borosilicate glass powder Commercially available alkali-free borosilicate glass waste (80% SiO2, 13% B2O3) was washed, dried, and placed in a corundum crucible. It was melted at 1400℃ for 1.5 hours, then quickly poured into cold deionized water for water quenching. After drying at 85℃ for 6 hours, water-quenched glass blocks were obtained. The water-quenched glass blocks were then ball-milled in a planetary ball mill at 300 rpm with zirconia balls as the grinding medium and a ball-to-material ratio of 3:1 for 8 hours to obtain borosilicate glass powder with D50 = 5~8μm.
[0043] Preparation of surface-modified stabilized nano-zirconia Nano-3Y-ZrO2 powder (particle size 40~60nm, Y2O3 content 3mol%) was taken and 1.0% of silane coupling agent KH-550 relative to the powder mass was added. The powder was dry-treated in a high-speed mixer at 1500rpm for 5min to obtain surface-modified nano-3Y-ZrO2. The treated powder was hydrophobic and did not settle when placed on the surface of deionized water for 30min, indicating that the modification effect was qualified.
[0044] Preparation of binder composite particles (all parts are parts by weight) Weigh out 48 parts of β-spodumene powder, 24 parts of high borosilicate glass powder, 7 parts of surface-modified nano-3Y-ZrO2, 13 parts of active α-Al2O3 micro powder (D50=1~2μm), 5 parts of calcium fluoride, and 2 parts of ytterbium oxide obtained by the above method, and put them into a V-type mixer. Dry mix for 30 min. Then, while stirring, 10 parts of a 10% polyvinyl alcohol aqueous solution were sprayed in. After mixing, the mixture was granulated by wet extrusion through a 40-mesh stainless steel screen. The resulting particles were spread evenly on a tray and dried in an 80°C forced-air drying oven for 4 hours to obtain binder composite particles.
[0045] Preparation of ceramic grinding wheels (all parts mentioned are parts by weight) (1) Take 42 parts of white fused alumina (particle size F60) and 30 parts of the activated brown fused alumina and put them into a mixer. Add 3.0 wt% of ethylene glycol of the total mass of the abrasive and mix at 300 rpm for 5 min to make the surface of the abrasive uniformly wetted. Then add 2.0 parts of aluminum dihydrogen phosphate powder and continue to stir at 300 rpm for 5 min to coat the surface of the fused alumina particles with phosphate to form abrasive with phosphate surface coating.
[0046] (2) Based on the abrasive coated with phosphate obtained in step (1), add 19 parts of the binder composite particles prepared by the above method while maintaining the rotation speed. The addition process takes 2 minutes. After the addition is completed, the rotation speed is increased to 500 rpm and stirred for 8 minutes. Then, add 2.5 parts of dextrin powder and stir for 3 minutes. Add deionized water to control the total moisture content of the grinding wheel forming material at 2.0%. Pass the grinding wheel forming material through a 20-mesh sieve and put it into a sealed bag to age for 12 hours.
[0047] (3) Add the aged grinding wheel forming material from step (2) to the grinding wheel mold, and use a hydraulic press to first press up to 50MPa and hold for 5s, then slowly increase the pressure to 120MPa and hold for 15s. The density of the resulting pressed ceramic grinding wheel green is 2.12 g / cm3. Inspect the pressed ceramic grinding wheel blanks, and select those without cracks, with intact edges, flat end faces, and uniform color without delamination, to be sintered in a natural gas shuttle furnace. First stage: Heat to 450℃ at a heating rate of 0.8℃ / min and hold for 210min (maintain a strong oxidizing atmosphere, with the oxygen content of the flue gas >6 vol%, and the flame is light blue and transparent). Second stage: Heat to 950℃ at a heating rate of 1.2℃ / min and hold for 30min (maintain oxidizing atmosphere, oxygen content of flue gas is 4~6 vol%). The third stage: the temperature is increased to 1160℃ at a heating rate of 1.2℃ / min and held for 150min (maintaining a weak oxidizing atmosphere, with an oxygen content of 2~4 vol% in the flue gas). Fourth stage: The temperature is lowered to 650℃ at a rate of 1.8℃ / min, held at that temperature for 90 minutes, and then allowed to cool naturally to room temperature in the furnace. The total cooling time is no less than 12 hours. The ceramic grinding wheel is then produced. The firing pass rate is defined as the obtained grinding wheel having a complete appearance, flat end face, no cracks, no chipping, and no deformation. The firing pass rate is 98.9%. Example 2 Based on Example 1, the difference is as follows: Preparation of binder composite particles (all parts are parts by weight) Weigh out 45 parts of β-spodumene powder, 26 parts of high borosilicate glass powder, 8 parts of surface-modified nano-3Y-ZrO2, 14 parts of active α-Al2O3 micro powder, 5 parts of calcium fluoride, and 2.2 parts of ytterbium oxide obtained by the method described in Example 1, and put them into a V-type mixer. Dry mix for 30 min. Subsequently, while stirring, 11 parts of a 12% polyvinyl alcohol aqueous solution were sprayed in. After mixing, the mixture was granulated by wet extrusion through a 40-mesh stainless steel screen. The resulting granules were spread evenly on a tray and dried in an 80°C forced-air drying oven for 4 hours to obtain binder composite granules.
[0048] In the preparation of the ceramic grinding wheel, 48 parts of white fused alumina, 27 parts of activated brown fused alumina obtained by the method described in Example 1, and 18 parts of binder composite particles prepared in Example 2 were used. The remaining steps were the same as in Example 1, and the firing qualification rate was 99.1%.
[0049] Comparative Example 1 Based on Example 1, the difference is as follows: The activation treatment step of brown fused alumina was omitted, and brown fused alumina with a particle size of F60 (Al2O3≥95.0%) was used directly to prepare the ceramic grinding wheel. The remaining steps were the same as in Example 1, and the firing qualification rate was 67.4%.
[0050] Comparative Example 2 Based on Example 1, the difference is as follows: The calcination step in the preparation of β-spodumene powder was omitted. Instead, commercially available spodumene concentrate (Li2O≥6.0%) was directly used for the ball milling step in the preparation of β-spodumene powder in Example 1 to obtain spodumene powder with D50=8~10μm. This spodumene powder was used to replace the β-spodumene powder used in the preparation of binder composite particles in Example 1. The remaining steps were the same as in Example 1, and the calcination qualification rate was 4.3%.
[0051] Comparative Example 3 Based on Example 1, the difference is as follows: In step (1) of ceramic grinding wheel preparation, aluminum dihydrogen phosphate powder is not added, and the remaining steps are the same as in Example 1. The firing qualification rate is 96.4%.
[0052] Comparative Example 4 Based on Example 1, the difference is as follows: In the preparation of the binder composite particles, no nano 3Y-ZrO2 was added. In the preparation of the ceramic grinding wheel, the fourth stage was to allow the furnace to cool naturally to room temperature, with a total cooling time of not less than 12 hours. The remaining steps were the same as in Example 1, and the firing qualification rate was 95.2%.
[0053] Comparative Example 5 Based on Example 1, the difference is as follows: Without preparing the binder composite particles, the raw materials for the binder composite particles, white fused alumina, activated brown fused alumina, aluminum dihydrogen phosphate powder, dextrin powder, ethylene glycol and water were added to a mixer in one step and stirred at 500 rpm for 20 min. The amount of each raw material and the remaining steps were the same as in Example 1, and the firing qualification rate was 56.8%.
[0054] The ceramic grinding wheels prepared in Examples 1-2 and Comparative Examples 1-5 were subjected to performance testing. The total porosity was determined using the boiling method in GB / T 2997-2015 "Test Methods for Bulk Density, Apparent Porosity and True Porosity of Dense Shaped Refractory Products". The flexural strength was tested using the three-point bending method as specified in GB / T 4740-2024 "Test Methods for Strength of Ceramic Materials". The rotational strength was tested using the 70 m / s linear velocity overspeed test in GB / T 2493-2023 "Test Method for Rotational Strength of Abrasives"; The results are shown in Table 1: Table 1 Performance test results of various ceramic grinding wheels Testing items Total porosity (%) Flexural strength (MPa) 70m / s rotational strength Example 1 20 92 No cracks Example 2 19 94 No cracks Comparative Example 1 22 68 40% cracking Comparative Example 2 31 52 All cracked Comparative Example 3 24 62 60% cracking Comparative Example 4 22 68 50% cracking Comparative Example 5 32 47 80% cracking As can be seen from the above embodiments, the present invention provides a high-performance ceramic grinding wheel with a high yield and its preparation method. Using the raw materials and methods described in this invention, the yield of the ceramic grinding wheel is over 98%, and the resulting grinding wheel has a flexural strength of 92 MPa. It does not crack under high-speed rotation at 70 m / s, confirming that the grinding wheel obtained by this invention can withstand higher grinding linear speeds, indicating that it possesses excellent structural integrity and abrasive grain holding force, making it suitable for high-speed, heavy-duty grinding conditions. The ceramic grinding wheels prepared in Comparative Examples 1-5 have low firing pass rates, low flexural strength, and severe cracking during 70 m / s rotational strength testing. This shows that the pre-preparation of the binder composite particles, the activation treatment of brown corundum, the calcination and phase transformation of β-spodumene, the phosphate interface bonding, the toughening effect of nano-ZrO2 phase transformation, and the introduction of compressive stress during annealing at 650℃ all comprehensively affect the product performance. The raw material selection and mixing sequence of the preparation method in this invention have a synergistic effect.
[0055] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A ceramic grinding wheel, characterized in that, It contains the following ingredients in parts by weight: 65-75 parts abrasive 16-22 parts of binder composite particles 1.5 to 2.5 parts phosphate 2-3 parts adhesive Organic polar wetting agent comprising 2-4 wt% of the total weight of the abrasive; The abrasive comprises, by weight: 40-50 parts of white fused alumina and 25-33 parts of activated brown fused alumina; The raw materials of the binder composite particles, by weight, include: 38-50 parts of β-spodumene, 17-26 parts of high borosilicate glass powder, 9-15 parts of active α-Al2O3 micro powder, 4-9 parts of surface-modified stabilized nano-zirconia, 2-6 parts of flux, 0.8-2.5 parts of rare earth oxides, and 7-12 parts of binder-binder aqueous solution. The activated brown fused alumina was obtained by modifying brown fused alumina with a titanate coupling agent; The surface-modified stabilized nano-zirconia is obtained by modifying nano-zirconia with a silane coupling agent.
2. The ceramic grinding wheel according to claim 1, characterized in that, The titanate coupling agent comprises at least one of NDZ-311, KR-TTS, and KR-38S; The titanate coupling agent is used at an amount of 1.0~3.0 wt% of brown fused alumina. The silane coupling agent comprises at least one of KH-550, KH-560, KH-570, A-174, and HMDS; The stabilized nano-zirconia comprises at least one of 3Y-ZrO2, 2Y-ZrO2, Ce-TZP, and Mg-PSZ; The amount of the silane coupling agent is 0.5~1.5wt% of the stabilized nano-zirconia.
3. A ceramic grinding wheel according to claim 1 or 2, characterized in that, The organic polar wetting agent comprises at least one of ethylene glycol, glycerol, diethylene glycol, propylene glycol, and polyethylene glycol; The phosphate contains at least one of aluminum dihydrogen phosphate, aluminum monohydrogen phosphate, and silicon phosphate. The binder comprises at least one of dextrin, polyvinyl alcohol, methylcellulose, hydroxypropyl methylcellulose, polyethylene glycol, corn starch, water glass, and paraffin.
4. A ceramic grinding wheel according to claim 1 or 2, characterized in that, The flux contains at least one of calcium fluoride, fluorite powder, cryolite, lithium fluoride, and sodium fluorosilicate. The rare earth oxides include at least one of ytterbium oxide, yttrium oxide, cerium oxide, lanthanum oxide, samarium oxide, and erbium oxide; The mass concentration of the binder aqueous solution is 7-15%; The binder comprises at least one of polyvinyl alcohol, dextrin, methylcellulose, hydroxypropyl methylcellulose, and polyethylene glycol.
5. A ceramic grinding wheel according to claim 4, characterized in that, The method for preparing the binder composite particles includes mixing β-spodumene, borosilicate glass powder, active α-Al2O3 micro powder, surface-modified stabilized nano-zirconia, flux, rare earth oxides, and an aqueous solution of binder, followed by granulation and drying to obtain binder composite particles.
6. A ceramic grinding wheel according to claim 5, characterized in that, The granulation process uses a 35-45 mesh sieve, and the drying temperature is 75-85℃ for 3-5 hours.
7. A method for preparing a ceramic grinding wheel according to any one of claims 1 to 6, characterized in that, Includes the following steps: 1) Mix white fused alumina and activated brown fused alumina, add an organic polar wetting agent, mix well, and then add phosphate to obtain an abrasive coated with phosphate. 2). Add the binder composite particles to the abrasive coated with phosphate obtained in step 1), and add the binder and water in sequence to obtain the grinding wheel forming material; 3) Press the grinding wheel forming material obtained in step 2) into shape, and sinter it to obtain the ceramic grinding wheel.
8. The method for preparing a ceramic grinding wheel according to claim 7, characterized in that, Step 2) The moisture content of the grinding wheel forming material is 1.5~2.5wt%.
9. A method for preparing a ceramic grinding wheel according to claim 7 or 8, characterized in that, Step 3) The pressing molding specifically includes the following stages: first stage: pressurize to 45~55MPa and hold for 3~8s; second stage: pressurize to 110~130MPa and hold for 12~18s.
10. A method for preparing a ceramic grinding wheel according to claim 7 or 8, characterized in that, Step 3) The sintering specifically includes the first stage: heating to 400~500℃ at a heating rate of 0.5~1.0℃ / min and holding at that temperature for 180~240min; Second stage: Heat to 900~1000℃ at a heating rate of 1.0~1.5℃ / min, and hold for 25~45min; The third stage: heat to 1150~1170℃ at a heating rate of 1.0~1.5℃ / min, and hold for 120~180min; Fourth stage: Cool down to 630~670℃ at a cooling rate of 1.5~2.0℃ / min, hold at that temperature for 60~120min, and then let it cool naturally to room temperature. The total cooling time shall not be less than 10h.