A method for preparing polyester-based recycled composite chips from waste polyester blended textiles

By combining single-screw and twin-screw extruders, along with mechanical size reduction and a two-stage slag discharge structure, the problem of removing hard impurities from waste polyester blended textiles has been solved, enabling efficient and low-cost production of polyester-based recycled composite chips, suitable for chemical depolymerization and recycled polyester processing.

CN123103897APending Publication Date: 2026-11-17SHANGHAI SHANYI NETWORK TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611270880.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for processing waste polyester blended textiles suffer from problems such as high requirements for raw material purity, damage to equipment from hard impurities, high production costs, and low sorting efficiency. In particular, they are difficult to effectively remove hard impurities such as metal fasteners and zippers, resulting in uneven melt, high filtration load, and reduced product quality.

Method used

By employing a combination of single-screw and twin-screw extruders, hard and fine impurities are removed through mechanical size reduction, primary plasticization, and a two-stage slag discharge structure. Combined with appropriate temperature and speed control, the polyester component is semi-plasticized and uniformly dispersed to obtain polyester-based recycled composite chips.

Benefits of technology

It has enabled the stable and continuous production of waste polyester blended textiles, with high product purity and low impurity content. It is suitable for chemical depolymerization or recycled polyester processing, reducing production costs and improving product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103897A_ABST
    Figure CN123103897A_ABST
Patent Text Reader

Abstract

This application discloses a method for preparing polyester-based recycled composite chips from waste polyester blended textiles. The method includes: sorting and mechanically reducing the size of the waste polyester blended textiles; feeding the resulting material into a single-screw extruder to achieve a semi-plasticized state for the polyester component, wherein the screw speed is 25-35 rpm, the feeding speed is 450-550 kg / h, and at least one heating zone temperature is 280-290°C; after removing hard impurities through a first slag discharge structure, the material is fed into a twin-screw extruder for plasticizing, dispersing, mixing, and homogenizing, wherein the screw speed is 25-40 rpm, and at least one mixing temperature zone temperature is 280-290°C; after removing fine impurities through a second slag discharge structure, the material is extruded, cooled, and pelletized to obtain polyester-based recycled composite chips. This invention achieves continuous pretreatment through two-stage slag discharge and the coordinated operation of single and twin screws, resulting in chips with uniform composition and low impurity content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of waste textile resource utilization technology, specifically to a method for preparing polyester-based recycled composite chips from waste polyester blended textiles. Background Technology

[0002] Modern textiles contain a large number of blended systems such as polyester / cotton, polyester / wool, polyester / viscose, and polyester / spandex. If these materials are directly used in chemical depolymerization or remelting processes, they often suffer from problems such as equipment wear, melt pressure fluctuations, increased filtration load, and decreased product quality due to the presence of impurities such as metal fasteners, zippers, decorative pieces, dust, and unplasticized fiber agglomerates. On the other hand, relying entirely on traditional fine sorting and complete separation of fiber components results in lengthy pretreatment processes, high labor costs, and significant difficulties in industrial implementation.

[0003] Existing technologies for treating waste polyester materials mainly include direct melt granulation, pre-sorting followed by recycling, and chemical depolymerization. Direct melt granulation involves directly melting and extruding waste polyester textiles after sorting, washing, and drying. This route is simple, but requires high raw material purity. Non-polyester components and hard impurities in blended fabrics can lead to uneven melt, high filtration load, and decreased product quality, making stable continuous production difficult. In the pre-sorting followed by recycling route, different fiber components are separated using near-infrared spectroscopy and manual sorting. The polyester portion enters the recycling process, while the non-polyester components are processed separately. This route produces high-purity products, but has high sorting costs and low efficiency, and is ineffective for sorting dark-colored, small, or heavily mixed waste textiles. The chemical depolymerization route depolymerizes waste polyester into monomers through alcoholysis, hydrolysis, etc., which are then purified and repolymerized. This route can achieve closed-loop recycling of polyester, but it requires high purity and uniformity of the polyester component in the feed. Non-polyester fibers and impurities in blended fabrics increase the burden of depolymerization, reduce monomer yield, and affect product color value. It is evident that the above route generally suffers from problems such as high requirements for raw material purity, damage to equipment from hard impurities, impact on subsequent utilization from unplasticized particles, and high production costs when processing waste polyester blended textiles with high impurities, complex compositions, and irregular morphologies. Summary of the Invention

[0004] This application provides a method for preparing polyester-based recycled composite chips from waste polyester blended textiles, comprising the following steps: Waste polyester blended textiles are sorted and then mechanically reduced in size. The obtained material is continuously fed into a single-screw extruder for primary plasticization, so that the polyester component in the material reaches a semi-plasticized state. The screw speed of the single-screw extruder is 25–35 rpm, the feeding speed is 450–550 kg / h, and the temperature of at least one heating zone along the conveying direction of the single-screw extruder is 280–290℃. In the semi-plasticized state, the melt pressure fluctuation of the material at the discharge end of the single-screw extruder does not exceed ±0.10 MPa, and the output is continuous strip without any breakage. Hard impurities, including metal fasteners, zipper heads, rivets, and decorative pieces, are removed from the material through the first slag discharge structure of the single-screw extruder. The first slag discharge structure is located at the discharge end of the single-screw extruder. The material after removing hard impurities is conveyed to a twin-screw extruder for further plasticizing, dispersing, mixing and homogenizing. The screw speed of the twin-screw extruder is 25–40 rpm, and the temperature of at least one mixing temperature zone along the conveying direction of the twin-screw extruder is 280–290°C. Inorganic particles, dust, and unplasticized particles are removed by the second slag discharge structure of the twin-screw extruder to obtain the melt; the second slag discharge structure is set at the discharge end of the twin-screw extruder. The melt is extruded, cooled, and pelletized to obtain polyester-based recycled composite chips.

[0005] In some implementations, the single-screw extruder has a screw diameter of 130–180 mm, an aspect ratio of 24:1–32:1, and a motor power of 150–220 kW; the twin-screw extruder has a screw diameter of 140–190 mm, an aspect ratio of 28:1–52:1, and a motor power of 70–120 kW.

[0006] In some embodiments, the single-screw extruder is provided with a first heating zone, a second heating zone, a third heating zone, and a fourth heating zone in sequence along the material conveying direction; the temperature of the third heating zone is 280–290°C, the temperature of the fourth heating zone is 265–275°C, and the temperature of the third heating zone is higher than that of the fourth heating zone; the temperatures of the first and second heating zones are 240–250°C, and are not higher than that of the fourth heating zone. The twin-screw extruder is equipped with a fifth, sixth, seventh, and eighth heating zone sequentially along the material conveying direction. The temperature of the fifth and sixth heating zones is 255–265℃, the temperature of the seventh heating zone is 280–290℃, and the temperature of the eighth heating zone is 260–270℃. The temperature of the seventh heating zone is higher than that of the eighth heating zone, while the temperatures of the fifth and sixth heating zones are not higher than those of the eighth heating zone.

[0007] In some embodiments, the temperatures of the first to fourth heating zones are 245°C, 245°C, 285°C, and 270°C respectively, the screw speed of the single-screw extruder is 30 rpm, and the feeding speed is 500 kg / h; the temperatures of the fifth to eighth heating zones are 260°C, 260°C, 285°C, and 265°C respectively, and the screw speed of the twin-screw extruder is 30 rpm.

[0008] In some embodiments, conveying the material after removing hard impurities to the twin-screw extruder includes: conveying the material after removing hard impurities to the twin-screw extruder through a constant-temperature connecting section, wherein the constant-temperature connecting section is a conveying channel, connecting cavity or transfer device with heat preservation function, and the heat preservation temperature of the constant-temperature connecting section is 240–290°C.

[0009] In some embodiments, a single-screw extruder includes a feeding section, a compression section, and a metering section, while a twin-screw extruder includes a conveying section, a melting section, a mixing section, a reversing element section, and a venting section.

[0010] In some embodiments, the exhaust section of the twin-screw extruder is equipped with an atmospheric pressure exhaust port, a vacuum exhaust port, or a combination of both, for removing moisture, low-molecular-weight volatiles, and odor components.

[0011] In some embodiments, the first slag discharge structure is a continuous screen replacement structure, a filter head structure with a slag discharge channel, or a combination thereof, used to remove hard impurities with a particle size ≥ 1 mm; the second slag discharge structure is used to remove inorganic particles, dust, and insufficiently plasticized fiber agglomerates with a particle size < 1 mm.

[0012] In some embodiments, in the polyester-based recycled composite chips, polyester is the continuous phase, and at least one of the unmelted fiber component, the refractory fiber component, and the filler component is distributed as a dispersed phase in the continuous phase; the average particle size of the polyester-based recycled composite chips is 2–8 mm, the number of black spots is ≤15 / 500 g, and the impurity content is ≤0.5 wt%.

[0013] In some embodiments, the waste polyester blended textile is a blended textile containing polyester with cotton, wool, linen, viscose, lyocell, acetate, nylon, spandex or a combination thereof, wherein the mass fraction of polyester is 50%–95%. Attached Figure Description

[0014] Figure 1 This is a schematic flowchart illustrating a method for preparing polyester-based recycled composite chips from waste polyester blended textiles, as described in an embodiment of this application. Detailed Implementation

[0015] The preferred embodiments of this application are described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit this application.

[0016] like Figure 1 As shown, this application provides a method 10 for preparing polyester-based recycled composite chips from waste polyester blended textiles, the method including step 110.

[0017] Step 110: Sort the waste polyester blended textiles and perform mechanical size reduction treatment.

[0018] In this step, the waste polyester blended textiles are first sorted to remove foreign objects that are obviously not part of the target material. These foreign objects include, but are not limited to, large metal parts, stones, glass shards, and non-textile waste.

[0019] After removing obvious foreign objects, the material undergoes mechanical size reduction treatment, selected from one or more combinations of shearing, crushing, or opening. Shearing is suitable for fabrics with seams or joints, cutting the seams without damaging the main fabric structure. Crushing is suitable for industrial scraps, stiff fabrics, or materials containing large foreign objects, breaking large pieces into sizes suitable for subsequent screw conveying. Opening is suitable for loose, fibrous materials, untangling fibers, reducing material volume, and increasing bulk density for stable feeding. The size of the material after these treatments is typically controlled below 5 cm. Material within this size range can fall evenly into the feed port of the single-screw extruder, avoiding bridging or jamming caused by excessively large material sizes, and preventing excessive dust generation due to excessively small sizes. Excessive dust increases the filtration load of the subsequent slag discharge structure and may affect melt pressure stability.

[0020] For example, before and / or after mechanical size reduction of materials, some non-fibrous impurities may be removed by manual sorting, magnetic separation, air separation, sieving, dust removal or a combination thereof.

[0021] For example, waste polyester blended textiles are textiles containing polyester blended with cotton, wool, linen, viscose, lyocell, acetate, nylon, spandex, or combinations thereof, wherein the mass fraction of polyester is 50%–95%, preferably 65%–95%. If the polyester content in the material is too low, the recycling value and economic viability are insufficient; if the polyester content is too high, the content of other fiber components in the blended system is too low, thus limiting the applicability of this method. Therefore, this method is suitable for waste polyester blended textiles with a polyester mass fraction of 50% to 95%. When the polyester mass fraction is within this range, polyester can form a sufficient continuous phase in the primary plasticizing stage, while the unmelted other fiber components are distributed as dispersed phases within the continuous polyester phase, forming a stable two-phase structure, which is beneficial for subsequent slag removal and homogenization treatment. The mechanical size reduction method used in this step can be flexibly selected according to the material morphology. Different materials can be treated with different methods, or multiple methods can be combined, all with the aim of bringing the material to a state suitable for continuous feeding in a single-screw extruder.

[0022] Step 120: The obtained material is continuously fed into a single-screw extruder for primary plasticization, so that the polyester component in the material reaches a semi-plasticized state. The screw speed of the single-screw extruder is 25–35 rpm, the feed rate is 450–550 kg / h, and the temperature of at least one heating zone along the conveying direction of the single-screw extruder is 280–290℃. In the semi-plasticized state, the melt pressure fluctuation at the discharge end of the single-screw extruder does not exceed ±0.10 MPa, and the discharged material is continuous and without breaks.

[0023] In the primary plasticizing step of a single-screw extruder, there are two objective indicators to measure whether polyester has reached a semi-plasticized state. The first indicator is that the melt pressure fluctuation at the discharge end of the single-screw extruder does not exceed ±0.10 MPa. Melt pressure fluctuation reflects the uniformity of plasticization and the stability of conveying the material in the screw. When the polyester component in the material achieves uniform semi-plasticization, the overall rheological properties of the material tend to be consistent, the back pressure formed during screw propulsion is stable, and the pressure gauge reading fluctuates within a small range. If plasticization is uneven, hard, unplasticized particles and semi-plasticized melt alternately pass through the screw, causing periodic and severe pressure fluctuations. The second indicator is that the discharged material is continuous and without breaks. When polyester reaches a uniform semi-plasticized state, the material extruded from the discharge end has sufficient melt strength and cohesion to form continuous strips. If the discharged material is discontinuous, lumpy, or powdery, it indicates insufficient plasticization. If the discharged material is flowing and cannot maintain a strip shape, it indicates that the material is too thin and may have undergone thermal degradation.

[0024] After mechanical dimensional reduction, the material is continuously fed into a single-screw extruder via a feeding device. In this step, the screw speed of the single-screw extruder needs to be controlled at 25–35 rpm, the feeding rate at 450–550 kg / h, and the temperature of at least one heating zone along the conveying direction of the single-screw extruder needs to be controlled at 280–290°C. The coordinated control of these three parameters—screw speed, feeding rate, and heating zone temperature—is crucial for achieving a semi-plasticized state for the polyester component.

[0025] The screw speed is set to 25 to 35 revolutions per minute. This speed range allows the material sufficient residence time in the screw to absorb heat, while avoiding excessive shear frictional heat caused by excessive speed. When the screw speed is below 25 revolutions per minute, the material's propulsion speed in the screw is too slow, resulting in low output and poor economic efficiency. Furthermore, the material's prolonged residence time in the high-temperature zone may lead to thermal degradation of the polyester. When the screw speed is above 35 revolutions per minute, the material residence time is shortened, and heat cannot be transferred from the material surface to the interior in time. This results in the material's central region not reaching the semi-plasticization temperature. Simultaneously, the frictional heat generated by the high speed can cause the local temperature of the material near the screw surface to exceed 300°C, triggering polyester molecular chain breakage and degradation, a decrease in melt viscosity, and unstable output.

[0026] The feeding speed is set to 450 to 550 kg per hour. This feeding speed, matched with the aforementioned screw speed, ensures that the screw channel of the single-screw extruder is at an appropriate filling rate. If the feeding speed is too low, the screw channel will not be fully filled, causing material to slip in the screw, reducing conveying efficiency and output. If the feeding speed is too high, the screw channel will be overloaded, causing material to accumulate and bridge at the feed port, preventing it from smoothly entering the screw. Excessive material will also increase the extruder torque, increase the motor load, and may even lead to overload shutdown. A feeding speed of 450 to 550 kg per hour, combined with a screw speed of 25 to 35 revolutions per minute, allows the material to form a stable plug in the screw, achieving continuous and uniform conveying.

[0027] The heating zone temperature of a single-screw extruder is the core factor determining whether polyester can reach a semi-plasticized state. Polyester has a melting point of approximately 255℃, but simply reaching this temperature is insufficient to achieve a stable, semi-plasticized state for transport. When the temperature is between 255 and 280℃, the crystalline structure of polyester is only partially destroyed. Although the surface softens, a large number of unmelted crystalline regions remain internally, resulting in a semi-cooked, paste-like consistency. In this state, the material's flowability and cohesion are unstable, easily carrying away unplasticized raw material during subsequent slag discharge. Simultaneously, the melt pressure fluctuates significantly, making continuous and stable operation difficult. When the heating zone temperature reaches 280 to 290℃, the crystalline structure of polyester is fully destroyed, and the molecular chains gain sufficient energy to overcome intermolecular forces and achieve relative sliding. The material then exhibits a uniform, high-viscosity fluid state, i.e., a semi-plasticized state. At this point, polyester has already acquired fluidity and deformability, allowing for continuous conveying under external force. Unmelted non-polyester fiber components, such as cotton, wool, and linen, remain in a solid fiber form within this temperature range due to their decomposition temperatures exceeding 300℃, and do not participate in plasticization. The heating zone temperature is set at 280-290℃ rather than higher because when the temperature exceeds 290℃, polyester undergoes thermal oxidation degradation in the presence of oxygen, causing molecular chain breakage and a sharp decrease in melt viscosity. This results in an excessively thin material that not only fails to effectively encapsulate unmelted fibers and hard impurities but also causes melt dripping through the mesh at the first slag discharge point, leading to slag discharge failure. Furthermore, excessively high temperatures increase energy consumption and equipment heat load, accelerating wear on the heating coil and screw. When the heating zone temperature is below 280℃, a uniform semi-plasticized state cannot be achieved, leaving a large amount of unsoftened polyester core in the material, resulting in insufficient plasticization during discharge and the presence of raw material during slag discharge. Therefore, 280-290℃ is the optimal temperature window, determined experimentally, for achieving uniform semi-plasticization while avoiding thermal degradation.

[0028] Step 130: Remove hard impurities from the material through the first slag discharge structure of the single screw extruder; the first slag discharge structure is set at the discharge end of the single screw extruder, and the hard impurities include metal fasteners, zipper heads, rivets, and decorative pieces.

[0029] A first slag discharge structure is set at the discharge end of the single screw extruder. This structure is used to remove hard impurities from the material. These hard impurities mainly include metal fasteners, zipper heads, rivets, and decorative pieces.

[0030] For example, the first slag discharge structure is set at the die head, i.e. the discharge end, of a single screw extruder, and its specific form is a continuous screen changing structure, a filter die head structure with a slag discharge channel, or a combination of the two.

[0031] For example, the filtration precision of the first slag discharge structure is set to remove hard impurities with a particle size greater than or equal to 1 mm. These hard impurities are trapped by the filter element under the pressure of the single-screw extruder and discharged from the system through the slag discharge channel. Meanwhile, the semi-plasticized polyester melt and material components with a particle size less than 1 mm pass through the filter element into the next process. The filtration particle size cutoff point of the first slag discharge structure is set to 1 mm because hard impurities such as metal parts, zipper teeth, and rivet fragments larger than or equal to 1 mm, if they enter the subsequent twin-screw extruder, will severely wear down the screw threads and the inner wall of the barrel, and may even cause the screw to jam or break. Furthermore, these large hard impurities may shatter into smaller metal fragments under the strong shearing action of the twin screw. If these fragments enter the final product, they will seriously affect the purity of the chips and the safety of subsequent use. Fine particles with a particle size less than 1 mm are processed in the subsequent second slag discharge structure, thus achieving graded impurity removal. When the first slag discharge structure adopts a continuous screen replacement structure, the filter elements can be replaced or cleaned without interrupting production, ensuring production continuity. When a filter die head structure with a slag discharge channel is used, the trapped impurities are automatically discharged from the slag discharge channel under pressure, eliminating the need for machine shutdown for cleaning. Both structures can achieve continuous automatic slag discharge, avoiding production capacity loss due to machine shutdown for cleaning.

[0032] Step 140 involves conveying the material, after removing hard impurities, to a twin-screw extruder for further plasticizing, dispersing, mixing, and homogenizing. The twin-screw extruder operates at a screw speed of 25 to 40 revolutions per minute, and the temperature of at least one mixing zone along the conveying direction is 280 to 290°C.

[0033] The function of a twin-screw extruder is to further process semi-plasticized materials from a single-screw extruder. While the single-screw extruder has completed primary plasticization and separation of large, hard impurities, the material's homogeneity is still not ideal; unmelted fiber components remain in agglomerate form, and the material also contains moisture, low-molecular-weight volatiles, and odorous components. The twin-screw extruder, utilizing its excellent mixing capabilities and adjustable modular screw assembly, applies high-intensity shearing and stretching forces to the semi-plasticized material, breaking up the fiber agglomerates and dispersing them uniformly within the continuous polyester phase. Simultaneously, the exhaust system removes volatiles and odorous components, ultimately yielding a homogeneous and clean melt. To achieve this, precise control of the twin-screw extruder's screw speed and mixing zone temperature is essential.

[0034] The screw speed of a twin-screw extruder is set at 25 to 40 revolutions per minute (rpm), with a lower upper limit than that of a single-screw extruder. This is because the material processed by a twin-screw extruder has already undergone a transformation from a solid to a semi-plasticized state. Unlike a single-screw extruder, it does not require the strong conveying and primary heating of solid materials. Its main task is mixing and homogenization, thus eliminating the need for excessively high speeds. A speed of 25 to 40 rpm provides sufficient residence time for the material, allowing it to undergo adequate shearing and dispersion in the mixing section, while avoiding excessive frictional heat from excessively high speeds that could lead to localized degradation. When the twin-screw speed is below 25 rpm, the residence time in the mixing section is too long, resulting in decreased production efficiency. Furthermore, the insufficient shear force is inadequate to break up unmelted fiber agglomerates, affecting the dispersion effect. When the twin-screw speed is above 40 rpm, the residence time is shortened, leading to insufficient mixing. Additionally, the frictional heat generated by high shear may cause the localized temperature of the material to exceed the safe limit.

[0035] At least one mixing zone in a twin-screw extruder is set to a temperature of 285 to 290°C, the same range as the heating zone in a single-screw extruder. In a twin-screw extruder, the mixing zone corresponds to the area where high-shear elements are located, where the material is subjected to the greatest shear and tensile forces. Setting the mixing zone temperature to 280 to 290°C has the following advantages: First, at this temperature, the viscosity of the polyester melt is moderate—neither too high to flow nor too low to transmit shear forces. This moderate viscosity allows the mixing elements to effectively transfer shear energy to every phase of the material, breaking down unmelted cotton and linen fiber bundles into micron-sized dispersed particles. Second, this temperature is sufficient to further melt and plasticize any small amount of incompletely plasticized polyester core that may remain in the single-screw extruder under the combined effects of the high shear and temperature of the twin-screw extruder. Secondly, this temperature is lower than the decomposition temperature of non-polyester fiber components. Therefore, these fiber components remain in a solid state at this temperature, without melting or decomposition reactions, thus avoiding contamination of the melt by small molecules generated from fiber decomposition. When the temperature in the mixing zone is below 280℃, the polyester melt viscosity is too high. Fiber agglomerates are difficult to break up by shear force in a high-viscosity medium, resulting in poor dispersion. Ultimately, undispersed white spots or fiber clumps will appear on the surface of the chips. When the temperature in the mixing zone is above 290℃, the polyester melt viscosity is too low, making it unable to effectively transmit shear force. The mixing effect actually decreases, and the excessively high temperature increases the risk of polyester thermal degradation. Degradation products will cause the chips to darken in color and increase the number of black spots.

[0036] Step 150: Inorganic particles, dust and unplasticized particles are removed by the second slag discharge structure of the twin-screw extruder to obtain melt; the second slag discharge structure is set at the discharge end of the twin-screw extruder.

[0037] A second slag discharge structure is installed at the discharge end of the twin-screw extruder to remove inorganic particles, dust, and unplasticized particles. The filtration precision of the second slag discharge structure is set to remove inorganic particles, dust, and insufficiently plasticized fiber agglomerates with a particle size smaller than 1 mm. After passing through the first slag discharge structure, hard impurities with a particle size greater than or equal to 1 mm have been removed, but the material still contains fine inorganic particles such as dust and sand from waste textiles, as well as a small amount of fiber agglomerates that have not been fully dispersed by the twin-screw mixing section. If these fine impurities enter the final product, they will cause black spots, white spots, or excessive ash content in the chips, affecting the product's appearance quality and subsequent processing performance. The filtration precision of the second slag discharge structure is higher than that of the first slag discharge structure, enabling it to trap these fine impurities, thus achieving a two-stage slag discharge with distinct functions. The first slag discharge structure is responsible for coarse filtration, removing large, hard impurities and protecting the twin-screw extruder's threaded components and barrel from wear. The second slag discharge structure is responsible for fine filtration, removing fine impurities and ensuring the purity and uniformity of the final product. If only a single-stage slag discharge is set up, fine impurities will enter the product if the filtration precision is coarse, and large, hard impurities will directly impact the filter screen, causing rapid clogging and damage if it is fine. Therefore, a two-stage slag discharge structure is a necessary means to achieve continuous and stable production and ensure product quality.

[0038] Step 160: The melt is extruded, cooled and pelletized to obtain polyester-based recycled composite chips.

[0039] The clean melt, after being processed by the second slag discharge structure, is extruded from the discharge end of the twin-screw extruder and enters the cooling system for cooling. It is then pelletized by the pelletizing system to obtain polyester-based recycled composite chips. Extrusion can be performed using a water-cooled stranding method or underwater pelletizing.

[0040] In the water-cooled extrusion process, the melt is extruded from the die into multiple continuous strips, which are then cooled in a water tank and cut into cylindrical pellets by a pelletizer.

[0041] In underwater granulation, the melt is immediately cooled by circulating water after being extruded from the die and simultaneously cut into granules by rotating blades. The cooling temperature should be controlled within a range that allows the granules to fully solidify without sticking together.

[0042] In some embodiments, in the polyester-based recycled composite chips, polyester is the continuous phase, and at least one of the unmelted fiber component, the refractory fiber component, and the filler component is distributed as a dispersed phase in the continuous phase; the average particle size of the polyester-based recycled composite chips is 2–8 mm, the number of black spots is ≤15 / 500 g, and the impurity content is ≤0.5 wt%.

[0043] In the polyester-based recycled composite chips obtained in the embodiments of this application, polyester is the continuous phase, and at least one of the unmelted fiber components, refractory fiber components, and filler components is distributed as a dispersed phase within the continuous phase. The formation of this microstructure depends on the process conditions of this application. In the primary plasticizing step of the single-screw extruder, the polyester component reaches a semi-plasticized state under heating conditions of 280 to 290°C, becoming a high-viscosity fluid with fluidity. At the same time, natural fibers such as cotton, wool, and linen in the blended system do not melt under these conditions due to their decomposition temperatures being higher than 300°C, maintaining a solid fiber morphology. Regenerated fibers such as viscose and lyocell may partially decompose or carbonize at high temperatures and also do not participate in melting and plasticizing. Although nylon and spandex are thermoplastic synthetic fibers, their chemical compositions differ from polyester. At the processing temperatures of this application, they may have melted but are incompatible with polyester, or they may have undergone thermal degradation and do not exist as a continuous phase. Therefore, under the above process conditions, the semi-plasticized polyester melt, pushed and mixed by the screw, becomes a continuous matrix encapsulating all other components. Unmelted or refractory fiber components, as well as filler components from waste textiles, are sheared and dispersed into tiny particles, uniformly distributed within the continuous polyester phase. This structural characteristic of the continuous and dispersed phases gives the resulting chips an advantage in subsequent chemical depolymerization. In alcoholysis or hydrolysis, the solvent first contacts and penetrates the continuous polyester phase. The polyester molecular chains gradually depolymerize into monomers under the action of the solvent and catalyst. The solid fibers dispersed within do not participate in the depolymerization reaction and can be separated from the monomer solution by filtration after the reaction, without adding an additional separation burden. If the polyester in the chips is not a continuous phase but a dispersed phase, the solvent cannot fully contact all polyester components, and the depolymerization rate and monomer yield will decrease significantly. Therefore, the microstructure of polyester as a continuous phase is an important structural basis for the suitability of these chips as an intermediate raw material for chemical depolymerization.

[0044] The average particle size of the polyester-based recycled composite chips is 2-8 mm. During the pelletizing process, the length of the particles can be controlled by adjusting the rotation speed and traction speed of the pelletizer blades, ensuring they fall within the 2-8 mm range. Within this particle size range, the chips exhibit good flowability, making them suitable for pneumatic conveying, drying, and metering in subsequent processes. If the average particle size is less than 2 mm, dust is easily generated during conveying, increasing the risk of static electricity accumulation and blockage. Furthermore, fine particles may remain suspended on the liquid surface in the depolymerization reactor, reducing contact efficiency with the solvent. If the average particle size is greater than 8 mm, the temperature difference between the inside and outside of the particles is significant. During subsequent heating, the internal temperature of the particles lags behind the surface temperature, potentially leading to uneven depolymerization and prolonged reaction time. Therefore, an average particle size range of 2-8 mm balances ease of conveying with uniformity in subsequent processing.

[0045] The number of black spots in the polyester-based recycled composite chips does not exceed 15 per 500 grams. Black spots refer to dark or black particulate impurities visible to the naked eye in the chips. Their sources mainly include dust, dye residue, metal wear debris, and carbonized particles generated during the thermal degradation of polyester in the processing. The method for determining the number of black spots is as follows: 500 grams of chip sample is weighed, evenly spread on a white background illumination stage, and the number of all dark particles is counted one by one by the inspector using a magnifying glass or automatic optical detection equipment. The measurement is repeated three times, and the average value is taken. Controlling the number of black spots to no more than 15 per 500 grams is significant because black spots are non-meltable impurities that cannot be eliminated during subsequent melt spinning or granulation. Too many black spots will lead to increased yarn breakage in the spinning process and affect the appearance quality and mechanical properties of the granules in the granulation process. The two-stage slag removal structure of this application can effectively remove impurities from the material, and the removal of volatiles by the exhaust section of the twin-screw extruder ensures that the number of black spots in the final chips can be controlled to no more than 15 per 500 grams.

[0046] The impurity content of this polyester-based recycled composite chip does not exceed 0.5 wt.%. Impurity content refers to the total mass fraction of non-target components in the chip, excluding polyester and unmelted fiber components. It mainly includes ash, metal particles, sand, and incompletely removed carbides. The method for determining impurity content is as follows: the chip sample is ignited in a high-temperature furnace at 600℃ to constant weight; the ratio of the mass of the residue to the initial mass of the sample is the impurity content. Controlling the impurity content to no more than 0.5% by weight is significant because impurity content is a core indicator of chip purity, directly affecting the efficiency of subsequent depolymerization reactions and the quality of the final product. When the impurity content is too high, during the chemical depolymerization process, impurities will consume additional chemicals and catalysts, reducing monomer yield and purity, and introducing additional ash and color into the depolymerization products. The first slag removal structure of this application removes hard impurities with a particle size greater than or equal to 1 mm, while the second slag removal structure removes fine impurities with a particle size less than 1 mm and unplasticized fiber agglomerates. The combined effect of the two-stage slag removal allows the impurity content of the final slices to be controlled at no more than 0.5 wt.%. This impurity content level meets the basic requirements for feed purity in chemical depolymerization processes.

[0047] This polyester-based recycled composite chip can be directly used as a raw material for chemical depolymerization, depolymerizing into monomers such as diethyl terephthalate during alcoholysis or hydrolysis, which can then be purified and reused in polyester synthesis. The chip can also be used as a substrate for biological depolymerization, degrading polyester components into smaller molecules through enzymatic catalysis or microbial fermentation. Furthermore, the chip can be used for melt reprocessing of recycled polyester, producing recycled polyester fibers or products after drying and melt extrusion. In addition, the chip can serve as an intermediate for modification processing, preparing modified polyester materials with specific properties through blending, chain extension, or toughening modification. The chip can also be directly used for spinning, producing recycled polyester fibers through melt spinning. The feasibility of these various downstream applications stems from the chip's microstructure with polyester as the continuous phase, uniform composition, regular particle morphology, and low impurity content, which can meet the purity and uniformity requirements of different subsequent processing steps.

[0048] The above steps create a synergistic effect through matching process parameters, jointly achieving continuous pretreatment of waste polyester blended fabrics.

[0049] Single-screw extruders primarily handle the conveying and primary plasticizing of solid materials, leveraging their high torque to overcome the significant flow resistance of materials containing hard impurities during the initial stages of plasticization. Twin-screw extruders, on the other hand, utilize their superior mixing capabilities and adjustable modular screw assembly to perform deep mixing, dispersion and homogenization, and devolatilization. The two have clearly defined roles and complement each other. Using only a single-screw extruder results in insufficient mixing and uneven dispersion of fiber components; using only a twin-screw extruder struggles to handle coarse materials containing large amounts of hard impurities, leading to severe equipment wear. The tandem combination of the two achieves a balance between stable feeding, primary plasticizing, deep mixing, and homogenization.

[0050] The first and second slag discharge structures form a graded slag discharge combination. After the material reaches a semi-plasticized state in the single-screw extruder, large hard particles are removed by the first slag discharge structure at the discharge end of the single-screw extruder. After the removal of large hard particles, the semi-plasticized material enters the twin-screw extruder for deep mixing and homogenization. At the discharge end of the twin-screw extruder, fine impurities are removed by the second slag discharge structure. The fluidity and cohesiveness of the material in the semi-plasticized state allow large hard particles to be effectively trapped and discharged, preventing these hard impurities from entering the twin-screw extruder and damaging precision threaded components. The second slag discharge structure removes fine impurities after the material has undergone deep mixing and homogenization, ensuring the purity of the final product.

[0051] There is a synergistic relationship between the screw speed, feed rate, and heating zone temperature of a single-screw extruder. A higher heating zone temperature, combined with a moderate screw speed and feed rate, ensures that the material has sufficient residence time in the screw to absorb heat, achieving uniform semi-plasticization. If the temperature is high but the speed is too high, the residence time is insufficient, and the material is ejected before it is fully heated, resulting in a less effective plasticization than under conditions of lower temperature but moderate speed. If the temperature meets the requirements but the feed rate is too high, the material accumulates too densely in the screw, making it difficult for heat to transfer from the barrel wall to the depth of the screw channel, also affecting the uniformity of plasticization. Therefore, all three parameters must be within the aforementioned ranges simultaneously to achieve stable semi-plasticized conveying.

[0052] There is also a synergistic relationship between the mixing zone temperature and the screw speed in a twin-screw extruder. When the mixing zone temperature reaches 280-290℃, the screw speed must be controlled within the range of 25-40 revolutions per minute (rpm) to ensure sufficient shear energy input to the material in the mixing section. When the mixing zone temperature is near the upper limit of this range, the polyester melt viscosity is low, and the shear force transmission efficiency is high; in this case, a lower speed is sufficient to effectively disperse the fiber agglomerates. When the mixing zone temperature is near the lower limit of this range, the polyester melt viscosity is relatively high, requiring a higher speed to provide sufficient shear energy to break up the fiber agglomerates. However, the speed should not exceed 40 rpm, because excessively high speeds will result in too short a residence time for the material in the mixing section, insufficient shearing time, and the frictional heat generated by excessively high speeds will cause the local temperature of the material to exceed the safe limit, leading to thermal degradation of the polyester. Therefore, the mixing zone temperature and screw speed must be coordinated within the specified range. If the temperature and speed are outside this range, for example, if the temperature is too low and the speed is too high, shear heat may cause local temperatures to exceed the safe value while the overall plasticizing temperature remains insufficient, resulting in a non-uniform state where local overheating and poor overall plasticization coexist. If the temperature is too high and the speed is too low, although the risk of overheating can be avoided, the shear energy input is insufficient, making it difficult to fully disperse fiber agglomerates and reducing the dispersion effect. Only by simultaneously controlling the mixing zone temperature and screw speed within the specified range and adapting their combination to the rheological properties of the material can the best dispersion and mixing effect be achieved while avoiding thermal degradation.

[0053] Through the synergistic effect of the above steps, this application achieves continuous pretreatment of waste polyester blended fabrics, obtaining polyester-based recycled composite chips that can stably enter the subsequent closed-loop recycling process. This method eliminates the need for fine fiber separation in the blended fabric. Instead, it utilizes the difference in properties—polyester can be semi-plasticized at 280-290℃ while other fiber components do not melt—to allow polyester to form a continuous phase, with other fiber components distributed as dispersed phases, directly obtaining composite chips. This shortens the process chain and reduces pretreatment costs. The two-stage slag removal structure removes hard impurities with a particle size greater than or equal to 1 mm at the single-screw discharge end to protect the twin-screw extruder components. The second slag removal structure removes fine impurities with a particle size less than 1 mm at the twin-screw discharge end to ensure product purity and appearance quality, thus simultaneously guaranteeing equipment operational stability and product quality. By combining a single-screw extruder and a twin-screw extruder in series, the single-screw extruder handles rough materials containing hard impurities and achieves primary semi-plasticization, while the twin-screw extruder further mixes, homogenizes, and removes volatiles from the semi-plasticized material. This division of labor and collaboration ensures stable feeding, primary plasticization, deep mixing, and homogenization. The resulting polyester-based recycled composite chips contain polyester as the continuous phase and unmelted fiber components as the dispersed phase. This structure allows the solvent to fully contact the continuous polyester phase during subsequent alcoholysis or hydrolysis, achieving efficient depolymerization. The dispersed solid fibers, not participating in the reaction, can be removed by filtration after depolymerization. The chips have an average particle size of 2 to 8 mm, no more than 15 black spots per 500 grams, and an impurity content of no more than 0.5% by weight. They can be directly used as intermediate raw materials for chemical depolymerization, biological depolymerization, recycled polyester preparation, or modification processing, ensuring the stability of subsequent processing steps and product quality.

[0054] In some specific embodiments, the screw diameter of the single-screw extruder is 130–180 mm, the length-to-diameter ratio is 24:1–32:1, and the motor power is 150–220 kW; the screw diameter of the twin-screw extruder is 140–190 mm, the length-to-diameter ratio is 28:1–52:1, and the motor power is 70–120 kW.

[0055] The screw diameter determines the extruder's capacity and torque capacity. Single-screw extruders typically have screw diameters of 130 to 180 mm, a range suitable for feed rates of 450 to 550 kg per hour. A diameter that is too small results in insufficient channel volume and mandrel torque, making it difficult to meet capacity and impact resistance requirements. Conversely, a diameter that is too large increases equipment investment and energy consumption. Furthermore, the increased channel depth increases the distance heat travels from the barrel wall to the screw core, negatively impacting temperature uniformity and potentially causing overheating and degradation of materials near the wall while resulting in insufficient plasticization of materials near the core. Twin-screw extruders have screw diameters of 140 to 190 mm, slightly larger than single-screw diameters. This is because twin-screw extruders need to provide a larger free volume at the same output to meet mixing and venting requirements. The larger diameter also provides higher torsional stiffness to withstand the higher torque loads generated by the strong shear elements in the mixing section, and allows for larger venting ports without affecting material conveying stability.

[0056] The aspect ratio (L / D ratio) determines the residence time of material in the extruder and the available processing length. Single-screw extruders have an L / D ratio of 24:1 to 32:1, a range that ensures sufficient heating length for semi-plasticization. A low L / D ratio results in insufficient residence time, leading to unplasticized raw material in the output; a high L / D ratio results in excessively long residence time, increasing the risk of thermal degradation and raising equipment footprint and manufacturing costs. Twin-screw extruders have an L / D ratio of 28:1 to 52:1, higher than single-screw extruders because their processing tasks are more complex, requiring sequential melting and plasticizing, fiber agglomeration dispersion, reverse pressure build-up, and venting and devolatilization, each functional stage requiring sufficient length. An L / D ratio below 28:1 compresses the length of each functional stage, resulting in insufficient mixing or venting; an L / D ratio above 52:1 makes the equipment too long, increasing investment costs and the risk of prolonged material heating.

[0057] The motor power determines the upper limit of the power input that the drive system can provide. Single-screw extruders use motors with power ranging from 150 to 220 kW. This power range provides sufficient torque for the screw to overcome the significant flow resistance of waste textile materials containing hard impurities during the initial plasticization stage. Insufficient power can easily lead to a sudden drop in speed or shutdown when encountering large impurities or feeding fluctuations; excessive power increases equipment investment and operating energy consumption, and may exceed the torque bearing limit of the screw mandrel. Twin-screw extruders use motors with power ranging from 70 to 120 kW, significantly lower than single-screw extruders. This is because the material entering a twin-screw extruder is already in a semi-plasticized state. The resistance the screw needs to overcome during propulsion and mixing is relatively small. Its main task is to apply shear force to the semi-plasticized material to disperse fiber agglomerates, rather than to forcefully convey solid materials.

[0058] The aforementioned equipment specifications and process parameters are mutually supportive. The combination of screw diameter and length-to-diameter ratio determines the residence time distribution and heat transfer area of ​​the material in the extruder, which in turn determines the temperature distribution in the heating zone and the feasibility of setting the screw speed; the motor power provides the power guarantee to achieve the aforementioned speed and heating power. When the equipment specifications are within the aforementioned range, process parameters such as temperature, speed, and feed rate can be stably reproduced in industrial production, ensuring the controllability of the semi-plasticized state and the consistency of product quality.

[0059] In some specific embodiments, the single-screw extruder is provided with a first heating zone, a second heating zone, a third heating zone, and a fourth heating zone sequentially along the material conveying direction; the temperature of the third heating zone is 280–290℃, the temperature of the fourth heating zone is 265–275℃, and the temperature of the third heating zone is higher than that of the fourth heating zone; the temperatures of the first and second heating zones are 240–250℃, and are not higher than that of the fourth heating zone. The twin-screw extruder is provided with a fifth heating zone, a sixth heating zone, a seventh heating zone, and an eighth heating zone sequentially along the material conveying direction; the temperatures of the fifth and sixth heating zones are 255–265℃, the temperature of the seventh heating zone is 280–290℃, and the temperature of the eighth heating zone is 260–270℃, and the temperature of the seventh heating zone is higher than that of the eighth heating zone; the temperatures of the fifth and sixth heating zones are not higher than that of the eighth heating zone.

[0060] The first and second heating zones of the single-screw extruder are each set to an independent temperature of 240 to 250°C. The first heating zone is located in the feed section of the single-screw extruder, specifically the area where the feed port is located. The temperature in this zone is set at 240 to 250°C, below the melting point of polyester. This temperature setting preheats the material entering the extruder, allowing the material temperature to rise gradually without premature melting at the feed port. If the temperature in the first heating zone is too high, exceeding 250°C, the material will begin to melt on the surface at the feed port. The melted material will adhere to the inner wall of the feed port and the screw surface, hindering the entry of subsequent material, causing poor feeding or even clogging the feed port. If the temperature in the first heating zone is too low, below 240°C, the material will receive almost no heat in this area, increasing the heating burden on the subsequent second and third heating zones, making it difficult for the material to reach a sufficiently semi-plasticized state within the limited heating length. The second heating zone is located after the feed section and at the beginning of the compression section, and its temperature is also set at 240 to 250°C. The second heating zone serves to continue the preheating effect of the first heating zone, further homogenizing the material temperature and preparing it for high-temperature plasticization in the third heating zone. The temperatures of the first and second heating zones are lower than those of the fourth heating zone. This relationship ensures that the material undergoes a gradual heating process along the conveying direction, avoiding uneven heating where the surface of the material degrades due to excessively rapid temperature rise while the interior remains underheated.

[0061] The temperature of the third heating zone in a single-screw extruder is 280 to 290°C. Located in the middle to rear of the compression section and the front of the metering section, this zone is the hottest area in the single-screw extruder. This zone is the core functional area where the material transforms from a solid to a semi-plasticized state. At this temperature, the polyester component gains sufficient heat energy to overcome intermolecular forces, its crystalline structure is fully disrupted, and it exhibits a uniform, high-viscosity fluid state—the semi-plasticized state. When the temperature of the third heating zone is below 280°C, the polyester component is not sufficiently plasticized, and a large number of unsoftened hard cores remain in the material. These hard cores easily clog filter elements or pass through the slag discharge structure with the semi-plasticized material during subsequent slag discharge, leading to decreased slag discharge efficiency and increased impurity content in the product. When the temperature in the third heating zone exceeds 290℃, polyester undergoes thermal oxidative degradation at high temperatures, resulting in molecular chain breakage and a significant decrease in melt viscosity. The material becomes too thin, failing to effectively encapsulate unmelted fiber components and hard impurities. Furthermore, it causes melt dripping at the filter element of the first slag discharge structure, preventing the effective retention of large, hard particles that pass through the filter element with the thin melt, leading to slag discharge failure. Therefore, 280 to 290℃ is the optimal semi-plasticization temperature range determined experimentally.

[0062] The temperature of the fourth heating zone in the single-screw extruder is 265 to 275°C. Located from the rear of the metering section to the discharge end, this fourth heating zone is the last heating zone the material passes through before leaving the extruder. The temperature of the fourth heating zone is lower than that of the third heating zone, and this temperature decrease is of significant process importance. After reaching a semi-plasticized state in the third heating zone, the material's temperature is approximately 280 to 290°C, resulting in a low melt viscosity. If the material directly enters the first slag discharge structure at this temperature, the excessively low melt viscosity will prevent large, hard impurities from forming an effective filter cake layer before the filter element. The impurities will pass through the filter screen with the diluted melt or accumulate on the screen surface, causing excessively high local pressure. The fourth heating zone lowers the material temperature to 265 to 275°C, appropriately increasing the viscosity of the polyester melt, thus improving the semi-plasticized material's ability to entrain hard impurities and its adaptability to the filter element. At 265-275℃, the material remains in a flowable, semi-plasticized state, preventing solidification and blockage of the slag discharge channel. Simultaneously, its high viscosity and cohesiveness allow large, hard particles to be effectively trapped by the filter element and discharged from the slag outlet. If the temperature of the fourth heating zone exceeds 275℃, the cooling effect is insignificant, and the slag discharge efficiency cannot be improved. If the temperature of the fourth heating zone is below 265℃, the material viscosity increases excessively, significantly raising flow resistance. This may lead to excessively high pressure at the first slag discharge structure, or even material solidification and breakage at the discharge end, preventing continuous conveying.

[0063] The fifth and sixth heating zones of the twin-screw extruder are each independently set to a temperature of 255 to 265°C. The fifth heating zone is located at the beginning of the melting section from the conveyor section, while the sixth heating zone is located in the middle to rear of the melting section. The purpose of setting the temperature of these two heating zones at 255 to 265°C is to maintain and appropriately supplement the heat of the semi-plasticized material from the single-screw extruder, ensuring that the material maintains a sufficient temperature level before entering the highest-temperature seventh heating zone. Since the material leaves the fourth heating zone at the discharge end of the single-screw extruder at approximately 265 to 275°C, and its temperature may drop slightly after being conveyed through the constant-temperature connecting section, the fifth and sixth heating zones maintain the temperature at 255 to 265°C to compensate for heat loss during conveying and prevent the material from cooling and solidifying. The temperatures of the fifth and sixth heating zones are lower than, but not higher than, the temperature of the eighth heating zone, ensuring a gradual transition of the material from the lower-temperature conveyor section to the higher-temperature mixing section, forming a reasonable temperature gradient.

[0064] The temperature of the seventh heating zone in the twin-screw extruder is 280 to 290°C. Located in the mixing section of the twin-screw extruder, this is the hottest area. The mixing section is equipped with high-shear mixing elements, where the material experiences the greatest shear and tensile forces. Setting the temperature of the seventh heating zone to 280 to 290°C, the same as the third heating zone in a single-screw extruder, is because at this temperature, the viscosity of the polyester melt is moderate—neither too high to hinder flow nor too low to effectively transmit shear force. This moderate viscosity allows the mixing elements to effectively transfer shear energy to every phase of the material, breaking up unmelted cotton and hemp fiber bundles into micron-sized dispersed particles. If the temperature of the seventh heating zone is below 280°C, the polyester melt viscosity is too high, reducing the efficiency of shear force transmission in the melt. Fiber agglomerates are difficult to break up in the high-viscosity medium, resulting in poor dispersion and ultimately undispersed white spots or fiber clumps on the surface of the chips. If the temperature of the seventh heating zone exceeds 290℃, the polyester melt viscosity will be too low, causing the melt to slip on the surface of the mixing elements. Shear force cannot be effectively applied to the fiber aggregates, resulting in a decreased mixing effect. Simultaneously, excessively high temperatures increase the risk of polyester thermal degradation, with degradation products causing the chips to darken in color and increase black spots. Therefore, the temperature of the seventh heating zone must be controlled within the range of 280 to 290℃, and this temperature must be higher than that of the eighth heating zone.

[0065] The temperature of the eighth heating zone in the twin-screw extruder is 260 to 270°C. This eighth heating zone is located between the reverse section and the venting section of the twin-screw extruder, representing the last heating zone the material passes through before leaving the discharge end. The temperature of the eighth heating zone is lower than that of the seventh heating zone; this temperature decrease is similar to the lower temperature of the fourth heating zone compared to the third heating zone in a single-screw extruder. After deep mixing in the seventh heating zone, the material's temperature is approximately 280 to 290°C, resulting in a low melt viscosity. If the material were to directly enter the second slag discharge structure at this temperature, the excessively low melt viscosity would cause fine impurities and unplasticized particles to penetrate or clog the filter screen, reducing slag discharge efficiency. The eighth heating zone lowers the material temperature to 260 to 270°C, appropriately increasing the viscosity of the polyester melt, thus improving the filtration efficiency of the second slag discharge structure. This allows fine impurities, dust, and unplasticized fiber agglomerates with a particle size less than 1 mm to be effectively trapped and discharged from the slag discharge port. Meanwhile, the temperature of 260 to 270°C is higher than the melting point of polyester, so the material remains in a flowable molten state, allowing it to pass smoothly through the second slag discharge structure and into the extrusion die without solidifying or clogging. If the temperature of the eighth heating zone is higher than 270°C, the cooling effect is not significant, the melt viscosity is too low, and fine impurities can easily pass through the filter screen. If the temperature of the eighth heating zone is lower than 260°C, the material viscosity is too high, resulting in excessive flow resistance when passing through the slag discharge structure and die, which may lead to unstable output or breakage.

[0066] The temperature settings of each heating zone in the single-screw and twin-screw extruders, together with the screw speed and feed rate settings, constitute a complete system of process parameters. The single-screw extruder sequentially undergoes preheating at 240-250°C, high-temperature semi-plasticization at 280-290°C, and discharge cooling at 265-275°C along the conveying direction, forming a temperature curve of initial heating followed by cooling. The twin-screw extruder sequentially undergoes heat preservation and replenishment at 255-265°C, high-temperature mixing at 280-290°C, and discharge cooling at 260-270°C along the conveying direction, similarly forming a temperature curve of initial heating followed by cooling. Both extruders exhibit a temperature distribution characterized by a high temperature in the middle and low temperatures at both ends. This temperature distribution ensures the highest temperatures required for semi-plasticization and mixing while appropriately cooling at the discharge end to improve slag removal and extrusion stability. The 280-290°C temperature in the third heating zone of the single-screw extruder is numerically the same as the 280-290°C temperature in the seventh heating zone of the twin-screw extruder, but their process purposes differ. The former serves the primary semi-plasticization of polyester, while the latter serves the deep dispersion and blending of fiber agglomerates. The specific numerical ranges for the aforementioned temperature, rotational speed, and feed rate have all been determined through experimental verification. These parameters have a synergistic relationship, and all parameters must be simultaneously satisfied within the specified ranges to achieve stable semi-plasticization conveying, efficient slag removal, and high-quality chip products.

[0067] In some specific embodiments, the temperatures of the first to fourth heating zones are 245°C, 245°C, 285°C, and 270°C respectively, the screw speed of the single-screw extruder is 30 rpm, and the feeding speed is 500 kg / h; the temperatures of the fifth to eighth heating zones are 260°C, 260°C, 285°C, and 265°C respectively, and the screw speed of the twin-screw extruder is 30 rpm.

[0068] The above parameter combination is the optimal process condition obtained through extensive experimental screening. Under these conditions, polyester-based recycled composite chips with excellent appearance can be stably obtained.

[0069] In a single-screw extruder, the temperature of both the first and second heating zones is 245℃. This preheating temperature ensures sufficient preheating of the material at the beginning of the feeding and compression sections without premature melting and sticking at the feed inlet. When the temperatures of the first and second heating zones are below 245℃, the material is insufficiently preheated, increasing the heating burden on the subsequent third heating zone and requiring a longer time to reach a semi-plasticized state. When the temperatures of the first and second heating zones are above 245℃, the material begins to melt on the surface in the feeding section, adhering to the inner wall of the feed inlet and the screw surface, affecting feeding stability.

[0070] The temperature of the third heating zone is 285℃, which was experimentally determined to achieve the optimal semi-plasticization effect. At 285℃, the crystalline structure of the polyester component is fully disrupted, the molecular chains gain sufficient energy to achieve relative sliding, and the material as a whole exhibits a uniform high-viscosity fluid state. When the temperature of the third heating zone is below 285℃, the polyester is not sufficiently plasticized, and the discharged material still contains unsoftened hard cores, resulting in raw material being carried along during slag removal. When the temperature of the third heating zone is above 285℃, the polyester begins to show signs of thermal degradation, the melt viscosity decreases, and the slag removal effect deteriorates. Therefore, 285℃ is the optimal balance point between semi-plasticization effect and thermal stability.

[0071] The temperature in the fourth heating zone is 270℃. The material enters the fourth heating zone after reaching 285℃ in the third zone, where the temperature drops from 285℃ to 270℃, a reduction of 15℃. This moderate temperature drop allows the viscosity of the polyester melt to rise appropriately without solidifying. At 270℃, the material maintains good fluidity and cohesion, and large, hard impurities can be effectively trapped by the first slag removal structure. If the temperature in the fourth heating zone deviates from 270℃, for example, approaching 275℃, the cooling effect is not significant, and the improvement in slag removal efficiency is limited. Approaching 265℃, the material viscosity becomes too high, increasing flow resistance.

[0072] The screw speed of the single-screw extruder is 30 revolutions per minute (rpm). This speed is preferred because it provides a longer residence time for the material, allowing it to fully absorb heat in each heating zone and achieve uniform semi-plasticization. At a feed rate of 500 kg / h, 30 rpm ensures sufficient residence time for the material in the third heating zone at 285°C, allowing heat to transfer from the surface to the interior, achieving uniform plasticization. Simultaneously, the lower speed generates less frictional heat, preventing localized overheating and degradation. If the speed is increased to 40 rpm or higher, even at the same 285°C temperature, the residence time shortens, and the uniformity of plasticization decreases. Therefore, 30 rpm is the optimal speed.

[0073] The feeding rate is 500 kg / h. This feeding rate strikes a balance between output and plasticizing quality. At a screw speed of 30 rpm, a feeding rate of 500 kg / h ensures a suitable filling rate in the screw channel of the single-screw extruder. The material forms a stable plug in the screw, preventing slippage due to underfilling or bridging due to overfilling. Experiments show that under temperature distributions of 245℃, 245℃, 285℃, and 270℃ and a speed of 30 rpm, a feeding rate of 500 kg / h enables the equipment to operate stably for extended periods with minimal melt pressure fluctuations.

[0074] In the twin-screw extruder, the temperature in both the fifth and sixth heating zones is 260°C. This temperature is set in the middle of the range of 255 to 265°C. The material from the single-screw extruder leaves the fourth heating zone at approximately 270°C, and its temperature drops slightly after being conveyed through the thermostatic connecting section into the fifth heating zone of the twin-screw extruder. The 260°C holding temperature compensates for heat loss during conveying, ensuring the material maintains a sufficient temperature level before entering the seventh heating zone. Simultaneously, 260°C is lower than the 265°C of the eighth heating zone, meeting the requirement for a gradual temperature gradient along the conveying direction, from the highest temperature to a moderate cooling.

[0075] The temperature of the seventh heating zone is 285℃. This temperature is the same as that of the third heating zone in a single-screw extruder, both at 285℃. In a twin-screw extruder, the seventh heating zone corresponds to the mixing section, where the material is subjected to high-shear mixing elements. The temperature of 285℃ provides the polyester melt with a suitable viscosity, effectively transmitting shear force without becoming too viscous and difficult to flow. At this temperature, the mixing elements can effectively transfer shear energy to each phase of the material, breaking down unmelted cotton and hemp fiber bundles into micron-sized dispersed particles. Experiments show that at 285℃ in the seventh heating zone, the resulting chips exhibit the best fiber dispersion, with smooth surfaces free of undispersed white spots or fiber clumps. If the temperature of the seventh heating zone is below 285℃, the fiber agglomerates are insufficiently dispersed, resulting in white spots on the chip surface. If the temperature of the seventh heating zone is above 285℃, the melt viscosity is too low, the shear force transmission efficiency decreases, and the risk of degradation increases.

[0076] The temperature in the eighth heating zone is 265℃. The material enters the eighth heating zone after reaching 285℃ in the seventh zone, where the temperature drops from 285℃ to 265℃, a decrease of 20℃. This temperature drop is slightly greater than that in the fourth heating zone of a single-screw extruder. This is because the second slag discharge structure after the eighth heating zone in a twin-screw extruder requires higher filtration precision, demanding a higher melt viscosity to trap fine impurities with a particle size less than 1mm. The discharge temperature of 265℃ significantly increases the viscosity of the polyester melt compared to 285℃, but the material still maintains good flowability, allowing it to pass smoothly through the second slag discharge structure and the extrusion die. At this temperature, fine impurities, dust, and unplasticized fiber agglomerates with a particle size less than 1mm can be effectively trapped by the second slag discharge structure, resulting in chips with fewer black spots and lower impurity content.

[0077] The twin-screw extruder operates at a screw speed of 30 revolutions per minute (rpm). This speed is the same as that of a single-screw extruder. This speed is preferred because the material entering the twin-screw extruder is already semi-plasticized, eliminating the need for high speeds to overcome solid transport resistance. The lower speed provides sufficient shear energy for mixing while allowing adequate residence time in the mixing section for thorough dispersion. Experiments show that under temperature distributions of 260°C, 260°C, 285°C, and 265°C, and a speed of 30 rpm, the material residence time in the mixing section is moderate, fiber agglomerates are effectively broken up, and the venting section provides sufficient time to remove moisture and volatiles, resulting in stable output and excellent slice appearance.

[0078] Under the above optimal parameter combination, the synergistic relationship between the parameters is fully demonstrated. The single-screw extruder's 245℃ preheating, 285℃ high-temperature semi-plasticization, and 270℃ discharge cooling, combined with a rotation speed of 30 rpm and a feeding rate of 500 kg / h, ensures stable semi-plasticized material conveying within the single-screw extruder. The melt pressure fluctuation at the single-screw discharge end does not exceed ±0.05 MPa, and the output is a continuous, uniform strip without any breaks. The twin-screw extruder's 260℃ heat preservation, 285℃ high-temperature mixing, and 265℃ discharge cooling, combined with a rotation speed of 30 rpm, ensures thorough dispersion, mixing, and efficient degassing and devolatilization of the material within the twin-screw extruder, resulting in a uniform, clean, and bubble-free melt composition. Both stages of the slag discharge structure operate stably under the above temperature conditions. The first slag discharge structure effectively removes large, hard impurities, while the second slag discharge structure effectively removes fine impurities and unplasticized particles. The resulting polyester-based recycled composite chips have a smooth appearance, uniform composition, few black spots, and low impurity content, and can be directly used as intermediate raw materials for chemical depolymerization, recycled polyester preparation, or modification processing.

[0079] In some specific embodiments, conveying the material after removing hard impurities to a twin-screw extruder for further plasticizing, dispersing, mixing and homogenizing includes: conveying the material after removing hard impurities to a twin-screw extruder via a constant-temperature connecting section for further plasticizing, dispersing, mixing and homogenizing; the constant-temperature connecting section is a conveying channel, connecting cavity or transfer device with heat preservation function, and the heat preservation temperature of the constant-temperature connecting section is 240–290℃.

[0080] The thermostatic connection section plays a crucial role in maintaining temperature and state throughout the entire process. After primary plasticization in the single-screw extruder, the material leaves the extruder at approximately 265-275°C, in a semi-plasticized state. If this semi-plasticized material lacks effective insulation during transfer, its temperature will drop rapidly due to heat dissipation from the environment. When the material temperature drops below 240°C, the viscosity of the polyester component increases sharply, its fluidity decreases significantly, and it may even partially solidify. This solidified or semi-solidified material, upon entering the feed port of the twin-screw extruder, cannot be effectively gripped and conveyed forward by the screws, leading to material accumulation and blockage at the feed port, abnormally high screw torque, and even triggering overload protection shutdown. Therefore, the thermostatic connection section must provide sufficient insulation to maintain a stable material temperature during transfer, ensuring smooth entry into the twin-screw extruder.

[0081] The insulation temperature of the constant-temperature connecting section is set between 240 and 290°C. The lower limit of this temperature range, 240°C, is slightly lower than the melting point of polyester. However, considering the heat carried by the material when exiting the single-screw extruder and the short residence time in the constant-temperature connecting section, 240°C is sufficient to maintain the material in a semi-plasticized state, preventing solidification within the connecting section. When the insulation temperature is below 240°C, the material temperature continues to drop during conveying, and may partially solidify by the time it reaches the feed port of the twin-screw extruder, affecting the feeding stability of the twin-screw extruder. The upper limit of the insulation temperature of the constant-temperature connecting section is set at 290°C. This temperature does not exceed the highest temperature of the third heating zone of the single-screw extruder and the seventh heating zone of the twin-screw extruder. When the insulation temperature is above 290°C, the material may undergo thermal degradation in the constant-temperature connecting section due to excessive temperature. Simultaneously, excessively high temperatures may cause the material viscosity to become too low, potentially leading to backflow and overflow from the feed port when entering the twin-screw extruder. Therefore, a heat preservation temperature range of 240 to 290°C can ensure that the material remains in a semi-plasticized state during the transfer process, and will not affect the stability of subsequent processes due to excessively high or low temperatures.

[0082] The specific structural form of the constant-temperature connection section can be flexibly selected according to equipment layout and space conditions. When the constant-temperature connection section adopts the form of a conveying channel with heat preservation function, the channel is round or square, with an insulation jacket or covering of insulation material on the pipe wall. The insulation material is generally rock wool, aluminum silicate fiber, or other heat-resistant insulation materials. Electric heating elements or heat transfer oil heating jackets are installed on the outside or inside of the pipe wall to achieve active heating and temperature maintenance. When using the conveying channel form, the length of the channel should be as short as possible to reduce the residence time of the material in it and the risk of temperature drop. When the constant-temperature connection section adopts the form of a connecting cavity, the cavity is an insulated container with a large internal cavity. Its upper opening connects to the discharge end of the single-screw extruder, and its lower outlet connects to the feed port of the twin-screw extruder. The cavity is equipped with an insulation layer and heating elements. After the material accumulates briefly in the cavity, it enters the twin-screw extruder by gravity or the pushing force of the single-screw extruder. The connecting cavity type is suitable for situations where there is a height difference or a large horizontal distance between the discharge end of a single-screw extruder and the feed inlet of a twin-screw extruder. When the constant temperature connecting section uses an adapter, this device is a specially designed transition joint whose internal cavity shape and size match the discharge end interface of the single-screw extruder and the feed end interface of the twin-screw extruder. The adapter itself integrates heating and insulation functions, enabling a sealed transition connection between two interfaces of different specifications. The adapter type is suitable for situations where the single-screw extruder and twin-screw extruder models are different and their interface sizes do not match.

[0083] In actual operation, the insulation temperature of the constant-temperature connecting section can be adjusted appropriately based on the actual temperature of the material at the discharge end of the single-screw extruder and the temperature setting of the twin-screw extruder. When the temperature of the fourth heating zone of the single-screw extruder is set within the range of 265 to 275℃, the insulation temperature of the constant-temperature connecting section can be set in the lower part of this range, i.e., 250 to 260℃, because the heat carried by the material itself is sufficient to maintain its semi-plasticized state, and the constant-temperature connecting section only needs to compensate for a small amount of heat loss during the conveying process. When the temperature of the fourth heating zone of the single-screw extruder is set near the lower limit of the 265 to 275℃ range, the insulation temperature of the constant-temperature connecting section should be increased accordingly to close to 270℃ to prevent the material temperature from dropping further below the semi-plasticized temperature window. When the ambient temperature is low or the length of the constant-temperature connecting section is long, the insulation temperature should be set at the upper part of the range to compensate for a larger amount of heat loss. The constant-temperature connecting section can also be equipped with a temperature sensor and a heating power adjustment device to automatically adjust the heating power based on real-time temperature feedback, so that the insulation temperature is stabilized within the set range.

[0084] Another important function of the thermostatic connecting section is to serve as a buffer and transition zone for material flow. The semi-plasticized material exiting the single-screw extruder exits the die head in a continuous strip or block shape, and its flow pattern is affected by the screw rotation and pushing action of the single-screw extruder, exhibiting a certain degree of pulsation. The internal space of the thermostatic connecting section can buffer this pulsation to a certain extent, allowing the material to enter the twin-screw extruder with a more uniform flow rate and a more stable state. Simultaneously, the thermostatic connecting section remains sealed during material transfer, preventing external air from entering the material system and preventing thermal oxidative degradation caused by contact with oxygen at high temperatures.

[0085] If the material remains in the thermostatic connecting section for too long, degradation may occur even at the insulation temperature due to prolonged heating. Therefore, in actual production, the matching relationship between the discharge rate of the single-screw extruder and the feed rate of the twin-screw extruder should be reasonably controlled to ensure that the average residence time of the material in the thermostatic connecting section does not exceed the allowable value. The internal volume of the thermostatic connecting section should be as small as possible, and a compact design should be adopted while meeting the connection and sealing requirements to reduce the amount of material retained within it.

[0086] A sealing structure should be installed at the connection between the constant-temperature connecting section and the discharge end of the single-screw extruder and the feed end of the twin-screw extruder to prevent melt leakage. The sealing structure generally uses high-temperature resistant flexible sealing rings or metal gaskets, capable of long-term stable operation within a temperature range of 240 to 290°C. The inner wall transition at the connection should be smooth, without steps or dead corners, to avoid material accumulation at the connection. Accumulated material may degrade and form gel particles under prolonged high temperatures. If these gel particles are carried into the subsequent melt, they will become the source of black spots in the final slices.

[0087] It is evident that although the thermostatic connecting section does not directly participate in the plasticization or mixing of materials, it is a crucial link connecting the single-screw extruder and the twin-screw extruder, ensuring process continuity. The insulation temperature of the thermostatic connecting section must match the discharge temperature of the single-screw extruder and the feed temperature of the twin-screw extruder, and its structural form must be rationally selected based on equipment layout and process requirements. At an insulation temperature of 240 to 290°C, the material can be continuously transferred from the single-screw extruder to the twin-screw extruder in a stable semi-plasticized state, providing temperature assurance for subsequent deep mixing and homogenization.

[0088] In some specific embodiments, a single-screw extruder includes a feeding section, a compression section, and a metering section, while a twin-screw extruder includes a conveying section, a melting section, a mixing section, a reversing element section, and a venting section.

[0089] A single-screw extruder is sequentially configured with a feeding section, a compression section, and a metering section along the material conveying direction. The feeding section is located at the beginning of the screw, from below the feed port to before the compression section. Its function is to receive material from the feeding device and convey it forward. The screw channel depth in the feeding section is relatively large, and the material is propelled by the screw in a loose state without significant compression. The compression section is located after the feeding section, and its screw channel depth gradually decreases along the conveying direction, causing the material to experience gradually increasing compressive force during forward conveying. The voids between materials are squeezed out, increasing the material density. Simultaneously, due to compression and heat transfer from the barrel wall, the material temperature begins to rise. The metering section is located after the compression section, and its screw channel depth is shallow and constant. In this section, the material is subjected to the combined effects of barrel wall heating and screw shearing, and the polyester component reaches a semi-plasticized state.

[0090] The feeding section, compression section, and metering section of the single-screw extruder correspond to the aforementioned four heating zones. The first heating zone is located in the barrel area corresponding to the feeding section, with a temperature of 240 to 250°C. This temperature is below the melting point of polyester, keeping the material solid in the feeding section to facilitate screw engagement and propulsion, while preventing premature melting and adhesion of the material at the feed inlet. The second heating zone is located in the barrel area from the end of the feeding section to the beginning of the compression section, also with a temperature of 240 to 250°C. Its function is to extend the preheating effect, ensuring the material's temperature is initially raised before entering the compression section. The third heating zone is located in the barrel area from the middle to the rear of the compression section to the front of the metering section, with a temperature of 280 to 290°C, making it the hottest area in the entire single-screw extruder. This region is the core functional area for the semi-plasticization of the polyester component. The gradually shallowing screw channel structure of the compression section subjects the material to compression and shearing as it propels forward. The high temperature provided by the third heating zone allows the polyester to reach a uniform semi-plasticized state under the synergistic effect of compression and shearing. The fourth heating zone is located in the barrel area corresponding to the rear of the metering section to the discharge end, with a temperature of 265 to 275°C. This zone appropriately cools the semi-plasticized material before it leaves the single-screw extruder, causing the viscosity of the polyester melt to rise again, thereby improving the slag removal efficiency of the first slag removal structure. Therefore, the four heating zones of the single-screw extruder are not evenly distributed across the three functional sections, but rather different heating temperatures are set according to the process requirements of each functional section. The highest temperature zone of the third heating zone covers the rear of the compression section and the front of the metering section, forming the core temperature region for this semi-plasticization; the fourth heating zone covers the rear of the metering section and serves as the cooling function at the discharge end.

[0091] A twin-screw extruder is configured sequentially along the material conveying direction as a conveying section, melting section, mixing section, reversing element section, and venting section. The conveying section, located after the feed port and before the melting section, stably conveys the semi-plasticized material from the constant-temperature connecting section, preventing material accumulation or backflow at the feed port. The melting section, located after the conveying section and before the mixing section, further heats the semi-plasticized material from the conveying section, allowing any remaining small amount of incompletely plasticized polyester components to melt. The mixing section, located after the melting section and before the reversing element section, is equipped with high-shear mixing elements that use strong shear force to break up unmelted fiber agglomerates and evenly disperse them within the continuous polyester phase. The reversing element section, located after the mixing section and before the venting section, is equipped with reverse threaded elements or reverse kneading blocks to establish back pressure at the end of the mixing section, extending the material's residence time and improving the mixing effect. The exhaust section is located in the area from the reverse element section to the discharge end. It has an exhaust port on its barrel to remove moisture, low molecular weight volatiles and odor components from the material.

[0092] The conveying section, melting section, mixing section, reversing element section, and venting section of the twin-screw extruder correspond to the aforementioned four heating zones. The fifth heating zone is located in the barrel area corresponding to the beginning of the melting section from the conveying section, with a temperature of 255 to 265°C. The material entering the twin-screw extruder may experience a slight temperature drop in the constant-temperature connecting section; the fifth heating zone provides insulation and reheating to this section, ensuring that the material's temperature does not fall below a reasonable range before entering the subsequent high-temperature zone. The sixth heating zone is located in the barrel area corresponding to the middle and rear of the melting section, with a temperature of 255 to 265°C, similar to the fifth heating zone. Its function is to further heat the material, allowing any remaining, incompletely plasticized polyester core to completely melt before entering the mixing section. The seventh heating zone is located in the barrel area corresponding to the mixing section, with a temperature of 280 to 290°C, making it the hottest area in the entire twin-screw extruder. The mixing section is equipped with high-shear mixing elements. Under these high-temperature conditions, the polyester melt has a moderate viscosity, which effectively transmits shear force without hindering fiber dispersion due to excessive viscosity. This allows the mixing elements to effectively transfer shear energy to each phase of the material, breaking down unmelted cotton and linen fiber bundles into micron-sized dispersed particles. The eighth heating zone is located in the barrel area corresponding to the reverse element section and the exhaust section, with a temperature of 260 to 270°C. The reverse element section and the exhaust section share the same heating zone because the main function of this section is to establish back pressure and remove volatiles, and it does not need to maintain extremely high temperatures like the mixing section. On the contrary, appropriately lowering the temperature is beneficial to increasing the melt viscosity, which enhances the pressure-building effect of the reverse element and also facilitates the retention of fine impurities by the second slag discharge structure. At the same time, the exhaust section can still effectively remove volatiles at this temperature. It can be seen that the four heating zones of the twin-screw extruder correspond to the barrel areas where each functional section is located. The seventh heating zone, which has the highest temperature, covers the mixing section and is the core temperature area for this deep dispersion. The eighth heating zone covers both the reverse element section and the venting section, and undertakes the comprehensive functions of pressure building, venting, and material cooling.

[0093] In this embodiment, the heating zone is configured with different temperatures according to the process requirements of each functional section. Both single-screw extruders and twin-screw extruders adopt a temperature distribution pattern with a high temperature in the middle and low temperatures at both ends. That is, the preheating section has a lower temperature, the core functional section has the highest temperature, and the discharge end temperature is moderately reduced. This temperature distribution pattern matches the process tasks undertaken by each functional section. The functional section determines where the material undergoes what kind of processing task, and the heating zone provides the required temperature conditions for that processing task. Together, they constitute the basis of the equipment operation of this method.

[0094] In some specific embodiments, the exhaust section of the twin-screw extruder is equipped with an exhaust port for removing moisture, low-molecular-weight volatiles, and odor components from the material. The exhaust port is located in the exhaust section corresponding to the barrel position, and can be an atmospheric pressure exhaust port, a vacuum exhaust port, or a combination of both. The atmospheric pressure exhaust port is open to the atmosphere; when the material is depressurized in the exhaust section, the entrained water vapor and air escape from the melt and are discharged through the atmospheric pressure exhaust port. The vacuum exhaust port uses a vacuum pump system to create a negative pressure environment at the exhaust port, which reduces the partial pressure required for volatiles to escape from the melt, more effectively extracting gases and volatiles from deeper layers of the melt. Its vacuum level is typically controlled between -0.06 MPa and -0.095 MPa. When the moisture and low-molecular-weight volatile content in the material is high, a vacuum exhaust port or a combination of an atmospheric pressure exhaust port and a vacuum exhaust port is preferred. When the moisture and volatile content in the material is low, an atmospheric pressure exhaust port alone is sufficient. The temperature of the heating zone corresponding to the venting section is typically set to 260℃ to 270℃. This temperature maintains sufficient material fluidity to facilitate gas escape while preventing material from escaping from the vent due to excessive temperature. The location and size of the vent should be designed based on the material's filling rate in the screw, ensuring that the screw channel is not completely filled when the material passes through the vent, thus providing a larger free surface area for gas diffusion. After treatment in the venting section, the melt exhibits significantly reduced moisture content, and low-molecular-weight volatiles and odor components are effectively removed, ensuring the production of clean polyester-based recycled composite chips.

[0095] The specific embodiments are described below.

[0096] Example 1 Waste polyester blended textiles with a polyester mass fraction of 85% were selected as raw materials. These raw materials originated from post-consumer clothing, and other components included 14% spandex and 1% viscose. The raw materials were manually sorted to remove obvious non-target foreign objects, and then crushed. The size of the crushed material was controlled to be less than 5 cm.

[0097] Pretreatment is performed using a combination of a single-screw extruder and a twin-screw extruder connected in series. The single-screw extruder has a screw diameter of 150 mm, a length-to-diameter ratio of 28:1, and a main motor power of 188 kW. The twin-screw extruder has a screw diameter of 165 mm and a slave motor power of 90 kW. Both the single-screw and twin-screw extruders have four independently temperature-controlled heating zones along the conveying direction.

[0098] To determine the appropriate process window, four sets of experiments were conducted, comparing different combinations of temperature and screw speed, denoted as A1, A2, A3, and A4. The parameter settings for each set of experiments are as follows.

[0099] Group A1: The temperatures of the four heating zones of the single-screw extruder are 245℃, 245℃, 255℃, and 260℃ respectively, and the screw speed is 30 rpm; the temperatures of the four heating zones of the twin-screw extruder are 260℃, 260℃, 285℃, and 265℃ respectively, and the screw speed is 30 rpm; the feeding speed is 500 kg / h.

[0100] Group A2: The temperatures of the four heating zones of the single-screw extruder are 245℃, 245℃, 285℃, and 270℃ respectively, and the screw speed is 30 rpm; the temperatures of the four heating zones of the twin-screw extruder are 260℃, 260℃, 285℃, and 265℃ respectively, and the screw speed is 30 rpm; the feeding speed is 500 kg / h.

[0101] Group A3: The temperatures of the four heating zones of the single-screw extruder are 245℃, 245℃, 255℃, and 260℃ respectively, and the screw speed is 45 rpm; the temperatures of the four heating zones of the twin-screw extruder are 260℃, 260℃, 275℃, and 265℃ respectively, and the screw speed is 40 rpm; the feeding speed is 600 kg / h.

[0102] Group A4: The temperatures of the four heating zones of the single-screw extruder are 245℃, 245℃, 285℃, and 270℃ respectively, and the screw speed is 45 rpm; the temperatures of the four heating zones of the twin-screw extruder are 260℃, 260℃, 275℃, and 265℃ respectively, and the screw speed is 40 rpm; the feeding speed is 600 kg / h.

[0103] The evaluation indicators for each group of experiments included single screw discharge status, melt pressure fluctuation, slag discharge operation, and slice appearance evaluation.

[0104] In group A1, the single-screw extruder's discharge end was under-plasticized, with melt pressure fluctuations of 0.30 MPa. The first slag discharge structure carried out a large amount of unplasticized raw material during operation, resulting in unstable slag discharge and ultimately poor surface quality of the slices.

[0105] In group A2, the single-screw extruder exhibits a stable semi-plasticized conveying state at the discharge end, with melt pressure fluctuations of only 0.05 MPa. The first slag discharge structure effectively discharges large, hard impurities, resulting in smooth operation. After deep mixing in a twin-screw extruder and treatment by the second slag discharge structure, the resulting slices have a smooth appearance, uniform composition, and an excellent appearance rating. The process conditions corresponding to group A2 can be considered as the optimal process window.

[0106] In group A3, the single-screw extruder's discharge end was under-plasticized, with melt pressure fluctuations of 0.20 MPa. The first slag discharge structure carried out some unplasticized raw material during operation, resulting in unstable slag discharge and ultimately poor surface quality of the slices.

[0107] In group A4, the single-screw extruder's discharge end was under-plasticized, the melt pressure fluctuated by 0.25 MPa, the first slag discharge structure was frequently blocked, the operating stability was poor, and the surface quality of the final slices was good.

[0108] The comparative results of the four sets of experiments above indicate that whether the temperature of the third heating zone of the single-screw extruder reaches 285℃ and whether the screw speed is controlled at around 30 rpm are key factors determining whether stable semi-plasticized material conveying can be achieved. In groups A1 and A3, the temperature of the third heating zone was only 260℃, failing to fully semi-plasticize the polyester component, resulting in under-plasticized output. In group A2, the temperature of the third heating zone reached 285℃, and with a lower speed of 30 rpm, stable semi-plasticized conveying and high-quality slicing products were achieved. In group A4, although the temperature of the third heating zone reached 285℃, the higher speed of 45 rpm shortened the residence time of the material in the screw and increased frictional heat, also failing to achieve stable semi-plasticized conveying.

[0109] Example 2 To verify the effectiveness of the two-stage slag discharge structure in this application, four different slag discharge configurations were set up for comparative experiments under the same feeding conditions as in Example 1 A2 group.

[0110] Group B1: No first slag discharge structure or second slag discharge structure is set.

[0111] Group B2: Only the first slag discharge structure is set, and the second slag discharge structure is not set.

[0112] Group B3: Only the second slag discharge structure is set, and the first slag discharge structure is not set.

[0113] Group B4: Simultaneously set up the first slag discharge structure and the second slag discharge structure.

[0114] To ensure the comparability of experimental results, the raw material source, pretreatment size, feed rate, and main temperature parameters were kept consistent across all groups, with only the configuration of the slag discharge structure being changed. The evaluation indicators included equipment operational stability, residual metal impurities, filtration pressure difference, number of black spots on slices, impurity content in slices, and frequency of shutdown for cleaning.

[0115] Experimental results show that group B4 outperformed the other three groups in terms of downtime frequency, metal residue, number of black spots, and impurity content. Group B1, lacking any slag discharge structure, allowed a large amount of hard and fine impurities to enter subsequent processes, resulting in severe equipment wear, high impurity content in the slices, and extremely high downtime for cleaning. Group B2, with only a first slag discharge structure, could remove hard impurities with a particle size greater than or equal to 1 mm, but fine impurities smaller than 1 mm, dust, and unplasticized fiber agglomerates were not effectively removed, resulting in a still high number of black spots and impurity content in the final slices. Group B3, with only a second slag discharge structure, could remove fine impurities, but large hard particles entered the twin-screw extruder, causing wear on the screw elements and a rapid increase in filtration pressure differential, resulting in poor equipment stability and high downtime for cleaning. Group B4 incorporates both a first and a second slag removal structure. The first structure removes large, hard impurities at the single-screw extruder's discharge end, protecting the twin-screw extruder's threaded components from damage. The second structure removes fine impurities at the twin-screw extruder's discharge end, ensuring the purity and appearance quality of the final slices. This two-stage slag removal system enables the equipment to operate continuously and stably for extended periods, significantly reducing the frequency of shutdowns for cleaning. The resulting slices exhibit a black spot count and impurity content that meet the requirements for subsequent processing.

[0116] Example 3 To verify the applicability of the polyester-based recycled composite chips obtained from group B4 in the subsequent depolymerization process, the chips obtained from group B4 were selected as the experimental group, and the control material without two-stage slag discharge treatment, namely group B1, was used as the control group. The comparative experiments were carried out under the same chemical depolymerization conditions.

[0117] The specific method for chemical depolymerization is as follows: 100g of pretreated PET substrate is added to 1L of ethylene glycol, and 5g of zinc acetate is added as a catalyst. The mixture is heated to 196℃ under a stirring speed of 400rpm and reacted at a constant temperature for 4 hours for alcoholysis. After the reaction is completed, the mixture is cooled, and the depolymerization product, diethyl terephthalate, is obtained through steps such as filtration, crystallization, and drying.

[0118] Experimental results show that, due to its lower impurity load and more uniform composition, the chips obtained in group B4, under the same depolymerization conditions, experienced a lower filtration load, a more stable reaction process, higher monomer yield, and better product color. The control group material, containing more impurities and insufficiently dispersed fiber aggregates, experienced a high filtration load during the depolymerization reaction, significant pressure fluctuations, a lower monomer yield than the experimental group, and a darker product color. These comparative results indicate that the polyester-based recycled composite chips obtained in this application are more suitable as intermediate raw materials for subsequent closed-loop recycling.

[0119] Principles and steps not explicitly described in this application are all obtainable by those skilled in the art through conventional technical means, and therefore will not be elaborated upon. Obviously, those skilled in the art can make various modifications and variations to this application without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this application and their equivalents, this application also intends to include these modifications and variations.

Claims

1. A method for preparing polyester-based recycled composite chips from waste polyester blended textiles, characterized in that, Includes the following steps: Waste polyester blended textiles are sorted and then mechanically reduced in size. The obtained material is continuously fed into a single-screw extruder for primary plasticization, so that the polyester component in the material reaches a semi-plasticized state. The screw speed of the single-screw extruder is 25–35 rpm, the feeding speed is 450–550 kg / h, and the temperature of at least one heating zone along the conveying direction of the single-screw extruder is 280–290℃. In the semi-plasticized state, the melt pressure fluctuation of the material at the discharge end of the single-screw extruder does not exceed ±0.10 MPa, and the output is continuous strip without breakage. The first slag removal structure of the single-screw extruder removes hard impurities from the material, including metal fasteners, zipper heads, rivets, and decorative pieces; the first slag removal structure is located at the discharge end of the single-screw extruder. The material after removing hard impurities is conveyed to a twin-screw extruder for further plasticizing, dispersing, mixing and homogenizing, wherein the screw speed of the twin-screw extruder is 25–40 rpm, and the temperature of at least one mixing temperature zone of the twin-screw extruder along the conveying direction is 280–290°C. Inorganic particles, dust, and unplasticized particles are removed by the second slag discharge structure of the twin-screw extruder to obtain a melt; the second slag discharge structure is located at the discharge end of the twin-screw extruder. The melt is extruded, cooled, and pelletized to obtain polyester-based recycled composite chips.

2. The method according to claim 1, characterized in that, The single-screw extruder has a screw diameter of 130–180 mm, an aspect ratio of 24:1–32:1, and a motor power of 150–220 kW; the twin-screw extruder has a screw diameter of 140–190 mm, an aspect ratio of 28:1–52:1, and a motor power of 70–120 kW.

3. The method according to claim 1, characterized in that, The single-screw extruder is provided with a first heating zone, a second heating zone, a third heating zone, and a fourth heating zone in sequence along the material conveying direction; the temperature of the third heating zone is 280–290℃, the temperature of the fourth heating zone is 265–275℃, and the temperature of the third heating zone is higher than that of the fourth heating zone; the temperatures of the first heating zone and the second heating zone are 240–250℃, and are not higher than that of the fourth heating zone. The twin-screw extruder is provided with a fifth heating zone, a sixth heating zone, a seventh heating zone, and an eighth heating zone in sequence along the material conveying direction; the temperature of the fifth heating zone and the sixth heating zone is 255–265℃, the temperature of the seventh heating zone is 280–290℃, and the temperature of the eighth heating zone is 260–270℃, and the temperature of the seventh heating zone is higher than the temperature of the eighth heating zone, while the temperatures of the fifth heating zone and the sixth heating zone are not higher than the temperature of the eighth heating zone.

4. The method according to claim 3, characterized in that, The temperatures of the first heating zone to the fourth heating zone are 245℃, 245℃, 285℃, and 270℃ respectively, the screw speed of the single-screw extruder is 30 rpm, and the feeding speed is 500 kg / h; the temperatures of the fifth heating zone to the eighth heating zone are 260℃, 260℃, 285℃, and 265℃ respectively, and the screw speed of the twin-screw extruder is 30 rpm.

5. The method according to claim 1, characterized in that, The process of conveying the material after removing hard impurities to the twin-screw extruder includes: conveying the material after removing hard impurities to the twin-screw extruder through a constant temperature connecting section, wherein the constant temperature connecting section is a conveying channel, connecting cavity or transfer device with heat preservation function, and the heat preservation temperature of the constant temperature connecting section is 240–290℃.

6. The method according to claim 1, characterized in that, A single-screw extruder includes a feeding section, a compression section, and a metering section, while a twin-screw extruder includes a conveying section, a melting section, a mixing section, a reversing element section, and a venting section.

7. The method according to claim 6, characterized in that, The exhaust section of the twin-screw extruder is equipped with an atmospheric pressure exhaust port, a vacuum exhaust port, or a combination of both, for removing moisture, low-molecular-weight volatiles, and odor components.

8. The method according to claim 1, characterized in that, The first slag discharge structure is a continuous screen replacement structure, a filter head structure with a slag discharge channel, or a combination thereof, used to remove hard impurities with a particle size ≥ 1 mm; the second slag discharge structure is used to remove inorganic particles, dust, and insufficiently plasticized fiber agglomerates with a particle size < 1 mm.

9. The method according to claim 1, characterized in that, In the polyester-based recycled composite chips, polyester is the continuous phase, and at least one of the unmelted fiber component, the refractory fiber component, and the filler component is distributed as a dispersed phase in the continuous phase; the average particle size of the polyester-based recycled composite chips is 2–8 mm, the number of black spots is ≤15 / 500 g, and the impurity content is ≤0.5 wt%.

10. The method according to claim 1, characterized in that, The waste polyester blended textiles are blended textiles containing polyester with cotton, wool, linen, viscose, lyocell, acetate, nylon, spandex or combinations thereof, wherein the mass fraction of polyester is 50%–95%.