A low-temperature impact-resistant polyvinyl chloride alloy material and its preparation method
By controlling the degree of pregelation and shear force in a twin-screw extruder, a rigid-flexible nested mesh topology is formed, which solves the problem of brittle fracture of polyvinyl chloride alloy materials at low temperatures and achieves high impact resistance and stiffness retention of the material.
Patent Information
- Application Number
- CN202610983972.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot maintain the rigidity-toughness balance of polyvinyl chloride alloys at low temperatures, leading to brittle fracture under low-temperature flexible loads and transient impacts. Furthermore, continuous extrusion processes can cause shear heat accumulation, resulting in the destruction of the resin matrix microcrystalline network.
By controlling the degree of pregelation and shear force in a twin-screw extruder, using unmelted primary particle cores as force transmission nodes, and combining low-melting-point lubricating composite additives and forced air cooling, a rigid-flexible nested network topology is formed, locking the dispersed phase structure and avoiding overheating and melting.
It achieves both rigidity and flexibility in materials at low temperatures, improves impact resistance and tensile strength, avoids stiffness decline and brittle fracture at room temperature, and maintains the morphological memory of resin particles.
Smart Images

Figure CN123104015A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a low-temperature impact-resistant polyvinyl chloride alloy material and its preparation method, belonging to the field of polyvinyl chloride composition blending technology. Background Technology
[0002] Currently, utilizing the rigidity, flame retardancy, and corrosion resistance of highly polar chlorine atoms on the molecular chain to construct multiphase alloys is a common approach. This typically involves introducing a chemically compatible, complementary rubber-elastomer polymer as an impact energy-absorbing phase to drive the elastomer components to fully disintegrate and spread within the melt rheological field. The mainstream industry approach generally relies on the strong heat input during continuous extrusion to allow resin particles to cross the melting inflection point and achieve a completely melted and homogenized matrix. This is then achieved by leveraging the interfacial shear force generated by the apparent viscosity of the melt to complete the blending and multiphase distribution of the elastomer. However, when modified alloy materials are used in low-temperature flexible applications… Under special working conditions where loads and transient impacts are intertwined, the inherent contradiction of this conventional path that relies on complete melting and homogenization begins to emerge. Although strong thermal shear input promotes elastomer dispersion, it also destroys the original hard microcrystalline core network inside the resin particles, causing the material to completely lose the morphological memory of the particles. In order to compensate for the shortcomings of notched impact toughness in ultra-low temperature environments, the industry usually adopts linear approaches such as increasing the proportion of elastomer or increasing the processing temperature. This often induces an imbalance in the two-phase rheological characteristics, which not only causes the room temperature tensile stiffness and Vicat softening temperature to deteriorate simultaneously due to the decrease in matrix yield strength, but also makes it easier to cause main chain degradation.
[0003] Besides the limitations imposed by hardware aspects such as the hardware shear configuration or basic processing temperature zone settings during continuous extrusion, continuous extrusion also suffers from shortcomings at the software level, such as dynamic process control methods for melt shear heat accumulation. For example, Chinese invention patent CN112571763B discloses a low-temperature extrusion molding method for unplasticized PVC or chlorinated PVC products, attempting to enhance mechanical energy by increasing screw speed or changing the conventional screw assembly configuration to complete plasticization at a lower barrel setting temperature. However, the existing technology implicitly... The underlying objective properties are based on the macroscopic parameter settings of a homogeneous and stable material system. When facing a multiphase blending modification system with rubber elastomers, high speed or strong shear configuration will inevitably generate extremely high and uncontrollable shear heat accumulation in the local screw. Since the existing technology lacks dynamic feedback adjustment of the transient thermal stress of the melt, this mismatch of boundary conditions is very likely to cause non-uniform local overheating and melting, thereby disintegrating the rigid microcrystalline skeleton of the primary particles of the resin matrix. As a result, the multiphase alloy will undergo brittle fracture in extreme low temperature environments because it cannot construct a rigid-flexible nested topological space network.
[0004] Therefore, in order to break through the bottleneck of rigidity and toughness mutual repulsion caused by phase homogenization, how to precisely control the thermodynamic morphological evolution of multiphase blend melt, while restricting the gelation process of the matrix to preserve the rigid microcrystalline core morphology of the primary resin particles, and enabling the elastomer phase to achieve nano-microscale ultrafine dispersion and spontaneously construct a rigid-flexible nested network topological space structure under a strong shear field, has become the technical problem to be solved by this invention. Summary of the Invention
[0005] To address the problems in the background art, the technical solution of the present invention is as follows: A method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material, comprising the following steps: Step S1: Mix 100 parts by weight of chlorinated polyvinyl chloride resin with 10 to 15 parts by weight of polymer elastomer in a mixer to obtain a premix. Step S2: The premixed material is fed into the feeding section of the twin-screw extruder; Step S3: In the pregelation section of the twin-screw extruder, the pregelation degree of the material is maintained in the range of 45% to 55% by adjusting the opening of the cold air valve and the heating power, so that the primary particle core of the chlorinated polyvinyl chloride resin maintains the crystal skeleton morphology, and the chain segment softening occurs on the periphery of the primary particles to form a free chain segment layer. Step S4: The pre-gelled material is transported to the high shear dispersion zone. At a temperature of 195°C to 205°C, the melt is subjected to axial stretching and radial deflection through the shear block assembly. The unmelted core of the primary particles is used as a force transmission node to transmit physical shear stress to the polymer elastomer. This causes the polymer elastomer to deform and peel off the phase interface in the gap between the primary particle cores, breaking into a dispersed phase structure with a particle size of 80nm to 150nm. Step S5: At the instant the material leaves the die outlet of the twin-screw extruder, an airflow or cold water spray is introduced for heat exchange, and the material temperature is reduced to below 80°C within 3 to 5 seconds, locking the spatial distribution of the dispersed phase structure and producing alloy material.
[0006] Preferably, the premix also contains a low-melting-point lubricating composite additive, wherein the low-melting-point lubricating composite additive is 1 to 3 parts by weight per 100 parts by weight of chlorinated polyvinyl chloride resin; the low-melting-point lubricating composite additive is formed by melt blending oxidized polyethylene wax and stearic acid in a mass ratio of 1:1 to 2:1, and the phase change temperature is 55°C to 65°C.
[0007] Preferably, in step S3, the torque value of the torque sensor on the twin-screw extruder is acquired by the central control unit built into the twin-screw extruder, and the first derivative of the torque value with respect to time is calculated according to the following formula: ,in, The first derivative, This represents the current torque value collected during the current sampling period. This is the historical torque value collected in the previous sampling period. With a fixed sampling period, when the first derivative exceeds a set first threshold, the central control unit adjusts the cold air flow by controlling the opening of the cold air valve.
[0008] Preferably, the twin-screw extruder is equipped with a damping reverse shearing component at the tail end of the pregelation section. The damping reverse shearing component generates local pressure resistance, so that the actual melt temperature at the discharge point of the pregelation section is regulated and stabilized within the range of 175°C to 185°C.
[0009] Preferably, step S4, which applies axial tension and radial deflection to the melt through the shear block assembly, includes the following sub-steps: Step S41, controlling the axial extrusion frequency of the shear block assembly to be periodically adjusted within the range of 10Hz to 30Hz, so that the melt generates an axial velocity gradient; Step S42, guiding the melt to deflect its flow direction through the flow field deflection blades in the shear block assembly, and using the unmelted core of the primary particles as a force transmission node to introduce the tensile resistance and physical shear stress generated by the shear block assembly into the polymer elastomer.
[0010] Preferably, in step S4, by controlling the staggered angle and rotation speed of the shear block assembly in the strong shear dispersion zone, the shear rate of the strong shear dispersion zone is controlled within the range of 1500s⁻¹ to 2500s⁻¹, so that the chlorinated polyvinyl chloride resin and the polymer elastomer can be blended.
[0011] Preferably, the twin-screw extruder is a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1 to 48:1. The co-rotating twin-screw extruder is provided with a feeding section, a pre-gelling section, a high-shear dispersion zone, and an exhaust and vacuum zone in sequence along the material conveying direction. The temperature of the feeding section is controlled at 140°C to 160°C, the temperature of the exhaust and vacuum zone is controlled at 180°C to 190°C, and the vacuum degree of the exhaust and vacuum zone is maintained between -0.06MPa and -0.09MPa.
[0012] Preferably, in step S3, the twin-screw extruder is equipped with an external forced air cooling circuit, which includes a cooling air duct and a cold air valve surrounding the outer wall of the barrel. When the first derivative exceeds a set first threshold, the opening of the cold air valve is increased by 15% to 30% to control the melt temperature fluctuation at the pregelation section outlet within ±1℃.
[0013] Preferably, in step S1, the average particle size of the primary microparticles of chlorinated polyvinyl chloride resin is 60 μm to 120 μm, and the chlorine content is 65% to 69%; the polymer elastomer is selected from chlorinated polyethylene, acrylate copolymers and ethylene propylene diene monomer (EPDM) rubber, and its Mooney viscosity at 25°C is 60 to 80. The following subsequent steps are included: In step S6, the material output from the strong shear dispersion zone is introduced into a die head for drawing, cooled by a water cooling tank, and finally pelletized by a pelletizer to form granules.
[0014] A low-temperature impact-resistant polyvinyl chloride alloy material, which is prepared by the method described above.
[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. In the preparation of low-temperature impact resistant polyvinyl chloride alloy materials, the pregelation degree of the matrix is kept in the incomplete gelation range by controlling the thermal balance of the main melting zone. The rigid microcrystalline core of the primary particles is retained and the periphery of the particles is locally softened to form a layer of interfacial molecular chains with bonding activity. After the softened material enters the strong shear dispersion zone, the unmelted rigid core acts as a force transmission node, transferring the rheological shear force generated by the high apparent viscosity melt to the polymer elastomer phase, so that the nano-dispersed phase is formed. The nano-dispersed phase spontaneously entangles on the semi-softened periphery of the primary particles, forming a rigid-flexible nested network topology. With the end rapid cooling, this morphology is locked, avoiding the decline in room temperature stiffness caused by conventional toughening.
[0016] 2. The central control unit calculates the first-order time derivative based on the torque value returned by the torque sensor, and controls the forced air cooling circuit when the derivative exceeds the safety threshold, adjusting the cold air valve to increase the heat dissipation flux and eliminate non-uniform melting caused by local shear overheating. This thermal adaptive balance system, together with the local pressure hindrance generated by the damping reverse shear component, keeps the actual temperature of the melt constant during material flow, and stably controls the pregelation degree at the discharge point of the main melting zone within a specific range, providing stable rheological shear force for the deformation of the elastomer dispersed phase in the subsequent strong shear section, and preventing the melt from losing its shear conduction ability to the elastomer phase due to complete melting caused by overheating.
[0017] 3. A low-melting-point lubricating complementary factor composed of oxidized polyethylene wax and stearic acid is introduced into the dry mix. This factor melts and preferentially coats the surface of the primary resin particles, blocking direct friction between matrix particles in the main melting zone and delaying the gelation initiation time of the resin matrix. This allows the material to maintain a high apparent viscosity when entering the strong shear dispersion zone. The two-phase interface is thus stimulated with stronger mechanical shear stress, which promotes the evolution of the polymer elastomer phase towards a narrower distribution of ultrafine dispersed phase structure. This refines and hardens the network topology inside the multiphase alloy, improving the crack resistance of the composite material under typical low-temperature flexible load and sudden external impact service environments. Attached Figure Description
[0018] Fig. 1 This is a flowchart of the method for preparing polyvinyl chloride alloy materials according to the present invention; Fig. 2 This is a torque diagram illustrating the process of preparing polyvinyl chloride alloy materials according to the present invention. Fig. 3 This is a melt temperature diagram for the preparation process of polyvinyl chloride alloy material according to the present invention.
[0019] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0020] The technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application are within the scope of protection of this application.
[0021] A method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material includes the following steps: Step S1: Mix 100 parts by weight of chlorinated polyvinyl chloride resin with 10 to 15 parts by weight of polymer elastomer in a mixer to obtain a premix. Step S2: The premixed material is fed into the feeding section of the twin-screw extruder; Step S3: In the pregelation section of the twin-screw extruder, the pregelation degree of the material is maintained in the range of 45% to 55% by adjusting the opening of the cold air valve and the heating power, so that the primary particle core of the chlorinated polyvinyl chloride resin maintains the crystal skeleton morphology, and the chain segment softening occurs on the periphery of the primary particles to form a free chain segment layer. Step S4: The pre-gelled material is transported to the high shear dispersion zone. At a temperature of 195°C to 205°C, the melt is subjected to axial stretching and radial deflection through the shear block assembly. The unmelted core of the primary particles is used as a force transmission node to transmit physical shear stress to the polymer elastomer. This causes the polymer elastomer to deform and peel off the phase interface in the gap between the primary particle cores, breaking into a dispersed phase structure with a particle size of 80nm to 150nm. Step S5: At the instant the material leaves the die outlet of the twin-screw extruder, an airflow or cold water spray is introduced for heat exchange, and the material temperature is reduced to below 80°C within 3 to 5 seconds, locking the spatial distribution of the dispersed phase structure and producing alloy material.
[0022] Preferably, the premix also contains a low-melting-point lubricating composite additive, wherein the low-melting-point lubricating composite additive is 1 to 3 parts by weight per 100 parts by weight of chlorinated polyvinyl chloride resin; the low-melting-point lubricating composite additive is formed by melt blending oxidized polyethylene wax and stearic acid in a mass ratio of 1:1 to 2:1, and the phase change temperature is 55°C to 65°C.
[0023] Preferably, in step S3, the torque value of the torque sensor on the twin-screw extruder is acquired by the central control unit built into the twin-screw extruder, and the first derivative of the torque value with respect to time is calculated according to the following formula: ,in, The first derivative, This represents the current torque value collected during the current sampling period. This is the historical torque value collected in the previous sampling period. With a fixed sampling period, when the first derivative exceeds a set first threshold, the central control unit adjusts the cold air flow by controlling the opening of the cold air valve.
[0024] Preferably, the twin-screw extruder is equipped with a damping reverse shearing component at the tail end of the pregelation section. The damping reverse shearing component generates local pressure resistance, so that the actual melt temperature at the discharge point of the pregelation section is regulated and stabilized within the range of 175°C to 185°C.
[0025] Preferably, step S4, which applies axial tension and radial deflection to the melt through the shear block assembly, includes the following sub-steps: Step S41, controlling the axial extrusion frequency of the shear block assembly to be periodically adjusted within the range of 10Hz to 30Hz, so that the melt generates an axial velocity gradient; Step S42, guiding the melt to deflect its flow direction through the flow field deflection blades in the shear block assembly, and using the unmelted core of the primary particles as a force transmission node to introduce the tensile resistance and physical shear stress generated by the shear block assembly into the polymer elastomer.
[0026] Preferably, in step S4, by controlling the staggered angle and rotation speed of the shear block assembly in the strong shear dispersion zone, the shear rate of the strong shear dispersion zone is controlled within the range of 1500s⁻¹ to 2500s⁻¹, so that the chlorinated polyvinyl chloride resin and the polymer elastomer can be blended.
[0027] Preferably, the twin-screw extruder is a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1 to 48:1. The co-rotating twin-screw extruder is provided with a feeding section, a pre-gelling section, a high-shear dispersion zone, and an exhaust and vacuum zone in sequence along the material conveying direction. The temperature of the feeding section is controlled at 140°C to 160°C, the temperature of the exhaust and vacuum zone is controlled at 180°C to 190°C, and the vacuum degree of the exhaust and vacuum zone is maintained between -0.06MPa and -0.09MPa.
[0028] Preferably, in step S3, the twin-screw extruder is equipped with an external forced air cooling circuit, which includes a cooling air duct and a cold air valve surrounding the outer wall of the barrel. When the first derivative exceeds a set first threshold, the opening of the cold air valve is increased by 15% to 30% to control the melt temperature fluctuation at the pregelation section outlet within ±1℃.
[0029] Preferably, in step S1, the average particle size of the primary microparticles of chlorinated polyvinyl chloride resin is 60 μm to 120 μm, and the chlorine content is 65% to 69%; the polymer elastomer is selected from chlorinated polyethylene, acrylate copolymers and ethylene propylene diene monomer (EPDM) rubber, and its Mooney viscosity at 25°C is 60 to 80. The following subsequent steps are included: In step S6, the material output from the strong shear dispersion zone is introduced into a die head for drawing, cooled by a water cooling tank, and finally pelletized by a pelletizer to form granules.
[0030] A low-temperature impact-resistant polyvinyl chloride alloy material, which is prepared by the method described above.
[0031] Example 1: When the system faces low-temperature flexible loads and sudden external impacts, the PVC alloy material modified by polymer elastomer blends lacks control over the gelation process of the matrix during continuous extrusion processing. This leads to the complete melting of the chlorinated PVC resin matrix, thereby disintegrating the hard microcrystalline network and particle morphology memory composed of primary particles inside the resin matrix. Consequently, this causes a drop in the room temperature tensile strength and Vicat softening temperature of the alloy material. If the processing temperature is lowered to maintain the rigidity of the matrix, the added polymer elastomer phase cannot undergo nanoscale peeling and fragmentation due to the mass transfer resistance inside the melt and the lack of interfacial shear force. This results in the formation of agglomerates and phase separation morphology in the amorphous region of the resin matrix. As a result, local stress concentration occurs inside the material, and microcracks are induced at grain boundary defects, causing brittle fracture damage to the alloy material structure.
[0032] 100 parts by weight of chlorinated polyvinyl chloride resin and 12 parts by weight of polymer elastomer were mixed in a mixer to obtain a premix. The premix was then conveyed to the feeding section of a co-rotating twin-screw extruder with a length-to-diameter ratio of 42:1. As the material flowed through the pregelation section of the co-rotating twin-screw extruder, the temperature control circuit collected the torque value from the torque sensor on the co-rotating twin-screw extruder and calculated the first derivative of the torque value with respect to time according to the formula: ,in, The first derivative, This represents the current torque value collected during the current sampling period. This is the historical torque value collected in the previous sampling period. For a fixed sampling period, when the first derivative exceeds the first threshold, the central control unit adjusts the opening of the cold air valve to control the cold air flow. The cooling air duct on the outer wall of the barrel controls the actual melt temperature at the pre-gelling section outlet to be within the range of 175℃ to 185℃, controlling the pre-gelling degree of the material to 48%. The primary particle cores of the chlorinated polyvinyl chloride resin maintain the crystal skeleton morphology, while the outer chain segments soften to generate a free chain segment layer. The material is conveyed into a strong shear dispersion zone. At a processing temperature of 198℃, the shear block assembly in the screw applies... Axial tensile force and radial deflection force are applied to the melt. The unmelted core of the primary particles acts as a force transmission node, transmitting rheological shear force to the polymer elastomer. The polymer elastomer deforms and undergoes phase interface delamination within the gaps between the primary particle cores, breaking into a dispersed phase structure with a particle size of 80nm to 150nm. This structure spontaneously adsorbs and entangles in the semi-softened outer layer of the primary particles. Driven by surface energy, the two-phase macromolecular chains interpenetrate, encapsulating a flexible nanoshell around the rigid primary particles. As the material exits the die of the co-rotating twin-screw extruder... High-speed circulating airflow cools the material to 75°C within 4 seconds, locking the spatial distribution of the dispersed phase structure and creating a rigid-flexible nested network topological structure within the alloy material system. Specifically, this cross-scale rheological shear force transmission is achieved through a multi-stage material shearing and crushing chain. When unmelted crystal nuclei with an average particle size of 60 to 120 micrometers are densely distributed in the high-shear dispersion zone, the surrounding material channels narrow, causing the high-viscosity melt to generate negative pressure of up to 1500 seconds to 2500 seconds when passing through the narrow gaps between the crystal nuclei. A local high-intensity rheological velocity gradient occurs once. At this time, the polymer elastomer aggregates in the molten state are forcibly stretched and extended into films or filaments with a thickness of micrometers under the action of extremely high local shear stress and axial tensile force. As the material continues to generate chaotic flow between the deflection blades in the flow field, these micrometer-sized elastomer films undergo high-frequency viscoelastic instability, and then spontaneously break apart and peel off into ultrafine dispersed phase islands of 80 nanometers to 150 nanometers, thus completing the stepwise transfer and evolution of shear energy from micrometer-sized rigid core to nanometer-sized flexible dispersed phase.
[0033] A polyvinyl chloride (PVC) alloy supported by a rigid-flexible nested mesh topological space structure exhibits a notched impact strength of 48.5 kJ / m² at -40°C, a room temperature tensile strength of 54.2 MPa, and a Vicat softening temperature of 96.2°C. When the material is subjected to low-temperature flexible loads and alternating impact heavy loads, the forward-protruding brittle microcracks, upon encountering the nanoscale flexible coating shell, undergo physical entanglement of molecular chains at the phase interface, converting the impact kinetic energy into thermal energy from the displacement of macromolecular chain segments. This multi-level stress dispersion mechanism alters the energy threshold of the alloy system's load response. The material avoids localized stress concentration and continuous crack penetration at low temperatures, preserving the resin particle crystal memory core as a rigid base, maintaining the alloy's tensile stiffness and low-temperature flexibility. Under more than 100 cycles of alternating hot and cold temperatures, it suppresses phase interface debonding and delamination. Without introducing external functional groups or increasing the constraints of the hardware topology, high rigidity is eliminated through nonlinear sequence modulation of the processing time-series energy field. Regarding the technical issues that are mutually exclusive with high toughness, specifically, the aforementioned standardized quantitative test procedure for alternating hot and cold cycles is as follows: The prepared standard tensile specimen is placed in an alternating hot and cold test chamber and kept in a constant temperature environment of 80°C for 30 minutes. Within 2 minutes, the ambient temperature is rapidly reduced to -40°C and kept in this ultra-low temperature environment for another 30 minutes, which constitutes a complete test cycle. After 100 consecutive alternating cycles, the specimen is taken out and mechanical retests of room temperature tensile strength and ultra-low temperature notched impact strength are performed according to national standards. The test results show that after 100 hot and cold cycles, the room temperature tensile strength retention rate of the specimen is above 96%, and the ultra-low temperature simply supported beam notched impact strength has basically no decay. Furthermore, the critical peeling load at the fracture interface is measured digitally using a standard microhardness indentation peeling instrument, and the critical peeling force at the interface remains stable above 15 millinewtons. Thus, the macroscopic peeling or delamination phenomenon at the phase interface is quantitatively confirmed through repeatable mechanical decay indicators.
[0034] Example 2: To verify the impact resistance stability of the material under low-temperature conditions, the test platform uses a co-rotating twin-screw extruder with a length-to-diameter ratio of 42:1. It features a zoned temperature control jacket with a temperature control accuracy of ±0.5℃ and an online torque sensor with a resolution of 0.1 N·m. The simply supported beam notched impact tester used to test the material's mechanical properties conforms to GB / T1043.1-2008 standard, with a pendulum energy of 2.75 J. The power supply circuit of the co-rotating twin-screw extruder contains voltage harmonic disturbances with an amplitude of ±5%, and the feeding section contains periodic material flow shear disturbances with a material flow fluctuation range of ±3%. A fixed sampling period is used in the processing control flow. The value is determined by the central control unit based on the torque fluctuation characteristics transmitted from the online torque sensor. When the rate of change of melt torque transmitted from the online torque sensor increases, in order to meet the control loop's requirement for timely capture of transient crystal melting temperature rise fluctuations, the central control unit reduces the fixed sampling period. The value will be determined by the central control unit under this processing condition, with a fixed sampling period. The sampling period is set to 0.5s to provide a reference for parameter acquisition during the material flow process. In the specific step-by-step control logic, the aforementioned operation of reducing the fixed sampling period value adopts a segmented step adjustment mechanism. When the absolute value of the first derivative of the torque detected by the online torque sensor exceeds the preset first threshold for three consecutive sampling periods, it indicates that the material flow has entered the rapid softening stage of crystal particles. At this time, the central control unit switches the original 2.0s basic sampling period down to 0.5s and forces the constant sampling period step of 0.5s to be maintained within the time range of this processing condition or process block for continuous data acquisition until the first derivative of the torque falls back to the reference range. Then the sampling period step is adjusted back to 2.0s. This ensures that the time reference of the denominator of the differential operation is constant within each process segment, eliminating the risk of computational breakage caused by sudden changes in the time span of the discrete control algorithm.
[0035] Material preparation included experimental groups, control groups, a partially missing control group, and an out-of-range control group. Each group used 100 parts by weight of chlorinated polyvinyl chloride resin with a chlorine content of 67% and an average particle size of 85 μm as the continuous matrix phase. All groups also contained 2 parts by weight of a low-melting-point lubricating composite additive composed of an equal mass of oxidized polyethylene wax and stearic acid. The content of polymeric elastomer in the experimental groups was set at 10 parts by weight, 12.5 parts by weight, and 15 parts by weight, respectively. The polymeric elastomer used was chlorinated polyvinyl chloride resin with a Mooney viscosity of 70 at 25°C. Ethylene, partially missing control groups include a missing feedback control group with a cut-off temperature control linkage circuit and a missing lubrication control group without low-melting-point lubricating composite additives. Out-of-range control groups include a low-addition control group with 8 parts by weight of polymer elastomer and a high-addition control group with 18 parts by weight of polymer elastomer. When the material flows through the pre-gelling section of the co-rotating twin-screw extruder, the central control unit collects the current torque value and historical torque value from the online torque sensor according to a fixed sampling period of 0.5 seconds, and calculates the first derivative of torque with respect to time using a formula. : ,in, The first derivative, This represents the current torque value collected during the current sampling period. This is the historical torque value collected in the previous sampling period. The sampling period is fixed, with subscript 1 indicating the current sampling period and subscript 2 indicating the previous sampling period. To eliminate the logical conflict between dynamic period adjustment and the fixed time base, the system adopts a phased time locking rule at the physical level. Specifically, the central control unit only initiates the reallocation of the sampling period value when it detects a large-scale switching of batch material flow resistance or a deviation from the steady-state trend for more than 5 consecutive periods. Once a new sampling period value, such as 0.5 seconds, is selected and issued, it will be rigidly locked as a constant within the current differential calculation interval and cooling damper adjustment cycle. This ensures that the time step term of the denominator remains absolutely fixed in the current real-time first derivative differential calculation network, guaranteeing the logical stability of the calculation formula and avoiding logical breaks caused by drastic periodic jumps within a single control loop. When the first derivative... When the preset first threshold is exceeded, the central control unit adjusts the opening of the cold air valve to control the cold air flow. Utilizing the cooling air ducts on the outer wall of the barrel, the actual melt temperature at the pre-gelling section outlet is adjusted to be within the range of 175℃ to 185℃, controlling the pre-gelling degree of the material to 48%. At this point, the primary particle cores of the chlorinated polyvinyl chloride resin maintain a crystalline skeleton morphology, while a free chain segment layer is generated around the particles. The softened material is input into a strong shear dispersion zone at a temperature of 200℃. At a shear rate of 2000s⁻¹, the unmelted primary particle cores act as physical shear force transmission nodes, transmitting rheological shear force to the polymer elastomer. The polymer elastomer deforms and peels off from the phase interface within the gaps between the primary particle cores, forming a dispersed phase structure. This dispersed phase structure spontaneously aggregates in the outer layer of the primary particles. When the blend melt exits the die head outlet of the co-rotating twin-screw extruder, the high-speed circulating airflow cools the material temperature to below 75℃ within 4 seconds, locking the spatial distribution of the dispersed phase structure. The impact fracture surface of the material was observed using a scanning electron microscope. The polymer elastomer phase formed a flexible nanoshell around the primary resin particles. The average particle size of the polymer elastomer phase was 142 nm in the 10 parts by weight test group, 115 nm in the 12.5 parts by weight test group, and 88 nm in the 15 parts by weight test group. In this adjustment and control chain, the opening of the cold air valve was increased by 15% to 30% based on the deviation of the first derivative. Specifically, when the first derivative calculated in real time exceeded the aforementioned first threshold by less than 10%, the stepper motor of the cold air valve in the control loop linearly increased the valve opening by 15%. When the deviation of the first derivative was greater than 20%, the valve opening was directly increased to the upper limit of 30%. By increasing the cold air convection heat dissipation flux, the frictional heat accumulation caused by strong shear inside the extrusion section was forcibly suppressed, ensuring that the pregelation process of the material was always in a stable and controllable state.
[0036] Mechanical properties were tested on the final alloy material specimens prepared in each group. At an ambient testing temperature of -40℃, the notched impact strength of the simply supported beam in the 10-part (parts by weight) group was 42.3 kJ / m², the room temperature tensile strength was 56.5 MPa, and the Vicat softening temperature was 97.4℃; the notched impact strength of the simply supported beam in the 12.5-part (parts by weight) group was 48.5 kJ / m², the room temperature tensile strength was 54.2 MPa, and the Vicat softening temperature was 96.2℃; the notched impact strength of the simply supported beam in the 15-part (parts by weight) group was 53.8 kJ / m², and the room temperature tensile strength was 5... The low-doped control group exhibited a notched impact strength of 15.4 kJ / m² at -40°C, a room temperature tensile strength of 57.1 MPa, and a Vicat softening temperature of 97.8°C. The low-doped control group had a notched impact strength of 54.1 kJ / m² at -40°C, a room temperature tensile strength of 38.6 MPa, and a Vicat softening temperature of 87.2°C. The low-doped control group had a polymer elastomer content below 10 parts by weight, resulting in insufficient stress interception source density within the material. The high-doped control group had a notched impact strength of 54.1 kJ / m² at -40°C, a room temperature tensile strength of 38.6 MPa, and a Vicat softening temperature of 87.2°C. The high-doped control group had a polymer elastomer content exceeding 15 parts by weight, resulting in insufficient stress interception source density within the material. The remaining rubber phase undergoes agglomeration and phase separation, reducing the rigidity of the continuous phase skeleton of chlorinated polyvinyl chloride. In the feedback control group, localized melt shear overheating to 196℃ during processing causes premature complete gelation of the primary resin particles and disintegration of the core network, resulting in an average particle size of 2.1 μm in the final dispersed phase and a notched impact strength of 12.6 kJ / m² at -40℃. In the lubrication control group, the lack of a low-melting-point lubricating composite additive to inhibit friction on the surface of the primary resin particles leads to premature gelation initiation of the resin matrix, causing the material to enter a state of high shear. The apparent viscosity decreased when the dispersion region was cut, and the average particle size of the polymer elastomer was measured to be 320 nm. The notched impact strength of the simply supported beam at -40℃ was 24.1 kJ / m². As the test environment temperature decreased regularly from -20℃ and -30℃ to -40℃, the notched impact strength of the simply supported beam in the test group remained above 40 kJ / m², while the notched impact strength of the simply supported beam in each control group decreased to below 25 kJ / m². The rigid-flexible nested mesh topological space structure constructed by each component under specific process parameters is used to intercept brittle microcracks and disperse load stress at extreme low temperatures.
[0037] Example 3: This example combines Figs. 1 to 3 This document describes a low-temperature impact-resistant polyvinyl chloride alloy material and its preparation method, as follows: Fig. 1As shown, in step S1, 100 parts by weight of chlorinated polyvinyl chloride resin and 10 to 15 parts by weight of polymer elastomer are mixed in a mixer to obtain a premix. In step S2, the premix is conveyed to the feeding section of a twin-screw extruder. In step S3, the opening of the cold air valve and the heating power are adjusted to maintain the pregelation degree of the material within the range of 45% to 55%, so that the core of the primary resin particles maintains the crystalline skeleton morphology and the outer chain segments soften to form a free chain segment layer. In step S4, the melt is subjected to axial tension and radial deflection by a shear block assembly at 195°C to 205°C. The unmelted core is used to conduct physical shear stress, causing the polymer elastomer to peel and break into a dispersed phase structure with a particle size of 80nm to 150nm. In step S5, the material is introduced into the die outlet and cooled to below 80°C within 3s to 5s, locking the spatial distribution morphology of the dispersed phase structure and producing an alloy material.
[0038] like Fig. 2 As shown, the processing time on the horizontal axis ranges from 0 to 250 seconds, and the operating torque on the vertical axis ranges from 100 to 140 Newton-meters. The figure illustrates the changes in real-time monitored torque and process reference torque with processing time.
[0039] like Fig. 3 As shown, the horizontal axis ranges from 0 to 250, and the vertical axis represents the melt temperature, ranging from 170.0 to 190.0 in °C. The figure illustrates the variation characteristics between the actual temperature value adjusted by feedback and the target temperature value set by the system.
[0040] Example 4: When the system faces low-temperature flexible loads and sudden external impacts under the condition of low-temperature impact-resistant polyvinyl chloride alloy, the shear heat accumulation of the melt inside the co-rotating twin-screw extruder causes the local temperature of the material to rise. The interfacial mass transfer resistance between chlorinated polyvinyl chloride resin and polymer elastomer fluctuates with the blending stress field, causing the pregelation degree of the material at the discharge point of the pregelation section to deviate from the range of 45% to 55%. This destroys the rigid crystal skeleton morphology of the primary particles of chlorinated polyvinyl chloride resin and the surface morphology memory of the primary particles of resin. Subsequently, brittle microcracks are initiated at the micro-grain boundaries or amorphous defects of the continuous phase of the resin matrix, increasing the risk of brittle fracture damage to the material structure.
[0041] Under initial processing conditions with a feeding section set temperature of 150℃ and a main melting zone set temperature of 185℃, a co-rotating twin-screw extruder with a length-to-diameter ratio of 42:1 operates in a steady-state rheological environment. The central control unit collects the reference torque value returned by the online torque sensor under steady-state processing, and calculates the first threshold for air cooling based on the reference torque value and the inherent time constant of the transmission system according to the following formula: ,in, The first threshold is determined for air cooling. This is the fluctuation correction factor, with a value of 0.05; The reference torque value is 120 N·m; The inherent time constant of the transmission system is 2s, and its transmission inertia through the exhaust vacuum zone is determined to be 2s, with the subscript... The first threshold is indicated by the subscript 0, which represents the baseline. In the parameter configuration of the process system, the general selection range of the fluctuation correction coefficient is controlled between 0.03 and 0.08. It is selected based on the magnitude of the periodic shear fluctuation caused by the screw machining tolerance, and is used to filter and correct the disturbance of the baseline torque value. The inherent time constant of the transmission system is generally controlled between 1 second and 3 seconds. It is determined and calibrated offline by applying a step speed signal to the screw drive motor under no-load conditions and measuring the physical delay time experienced when the output response of the online torque sensor reaches 63.2% of the steady-state value. This reflects the rotational inertia hysteresis characteristics of the long-distance melt material flow in the exhaust vacuum zone of the whole machine transmission chain.
[0042] When the absolute value of the first derivative calculated by the central control unit within five consecutive sampling cycles is greater than the first threshold for air cooling, the central control unit outputs a control level to the forced air cooling circuit, adjusting the opening of the cold air valve to increase convective heat dissipation. The damping reverse shear assembly generates local pressure retardation to compensate for the time delay in axial material transport. Within the strong shear dispersion zone of the twin-screw extruder, the shear block assembly applies axial tension and radial deflection. The central control unit superimposes a sinusoidal speed disturbance with an amplitude of 3% of the reference speed and a frequency of 10 Hz to 30 Hz onto the reference speed of 300 rpm. Utilizing the viscoelastic response of the melt under high-frequency shear, an axial pressure pulse is induced in situ between the windward and leeward sides of the shear block. Axial velocity gradient is generated along the material propulsion direction under rigid constraint of axial displacement. To eliminate high-frequency mechanical vibration noise caused by feeding fluctuations, the raw torque data collected by the online torque sensor is first filtered by a moving average window waveform before being input into the differential calculation unit. The average torque value within 5 consecutive sampling periods is selected as the reference torque value. The first derivative of torque with respect to time calculated from the reference torque value is input to the air-cooling judgment unit to control the opening of the cold air valve at the pre-gelling section outlet point. This controls the pre-gelling degree of the material at the pre-gelling section outlet point to be maintained within the range of 48%, ensuring that the core of the primary chlorinated polyvinyl chloride resin particles maintains a rigid crystal skeleton morphology. Combined with the free chain segment layer generated by the deentanglement and softening of the primary particles, the material pre-gels. The degree of gelation is controlled within the range of 45% to 55% through a pre-established digital control lookup table. Before production, the actual melt temperature is gradient by fine-tuning the heating power of the pre-gelation section. Samples are then rapidly cooled at the discharge point, and the actual degree of gelation is tested using a differential scanning calorimeter. The mapping data of the actual degree of gelation with the actual discharge point temperature and the reference torque value is calibrated and implanted into the central control unit. When the pre-gelation degree is below 45%, the softening of the outer molecular chains of the primary resin particles is insufficient, reducing the binding activity of the polymer elastomer on the periphery. This leads to the formation of micron-sized aggregates and phase separation morphology under subsequent operating conditions, reducing the low-temperature impact strength of the alloy material. When the pre-gelation degree is above 55%, the primary resin particles form hard microcrystalline nuclei. Excessive melting of the core causes the complete loss of particle morphological memory, which serves as a rigid base. Under low-temperature flexible loads and transient impacts, it is unable to construct a rigid-flexible nested topological spatial network, causing the room-temperature tensile stiffness and Vicat softening temperature to deteriorate simultaneously. The softened equilibrium material is transported to a strong shear dispersion zone with a set temperature of 200°C by the material conveying flow. At a shear rate of 2000 s⁻¹, the shear block assembly in a specific section of the screw applies axial tensile force and radial deflection force to the melt. The damping reverse shear assembly consists of two sets of counter-rotating left-handed shear block assemblies. The axial length of a single assembly is equal to 0.6 times the screw diameter and the thread lead is 20 mm. They are staggered at the end of the pregelation section to create a locally completely filled section, forming a 1.5 MPa to 3 MPa range.A 0 MPa axial reverse pressure damping wall enhances local heat transfer efficiency within the region, maintaining the actual temperature of the material within the range of 175°C to 185°C before it enters the high-shear dispersion zone.
[0043] Because unmelted chlorinated polyvinyl chloride (PVC) primary particles exhibit erosive abrasion in their incompletely plasticized state, an integral powder metallurgy tungsten carbide alloy layer is applied to the outer surface of the screw assembly and the inner wall of the barrel within the high-shear dispersion zone. This layer has a surface hardness of at least 65 HRC and a thickness of at least 1.5 mm. It resists the physical erosion of the unmelted hard core within the high-density distribution channel, maintaining the stability of the screw shear gap size. This allows the polymer elastomer to be pulverized into a dispersed phase structure of 80 to 150 nanometers under a localized high-intensity rheological velocity gradient at the two-phase interface. The unmelted primary particle core acts as a force transmission node, axially... Tensile force and radial deflection force are introduced into the polymer elastomer. The elastomer deforms and peels off at the phase interface within the gaps between the primary particle cores, breaking into a dispersed phase structure with particle sizes ranging from 80 nm to 150 nm. This dispersed phase structure spontaneously adsorbs and entangles in the semi-softened outer layer of the primary particles. Driven by local surface energy, the two-phase macromolecular chains generate microscopic lattice interpenetration, encapsulating a seamless, flexible nanoshell around the rigid primary particles. The instant the material exits the die of the co-rotating twin-screw extruder, the cooling system regulates the high-speed circulating airflow to reduce the material temperature to below 75°C within 4 seconds, locking in the dispersed phase. The spatial distribution of the dispersed phase structure forms a rigid-flexible nested network topological space structure within the continuous phase of the resin matrix. In the aforementioned thermodynamic evolution of the two-phase interface, the physical essence of micro-lattice interpenetration refers to the thermal diffusion of amorphous polymer elastomer macromolecular segments into the locally softened layer that is unentangled on the surface of chlorinated polyvinyl chloride resin primary particles. Because the rigid core of the resin particles still maintains a short-range ordered crystal framework structure, the macromolecular segments of its surface softened layer exhibit a specific regular arrangement trend, forming a pseudo-lattice morphology at the microscopic level. The active free segments of the polymer elastomer penetrate and, driven by surface energy,... Entangled within the regularly arranged softened boundary layer, the surface segments of the continuous phase of the resin matrix undergo deep topological slip entanglement, resulting in a highly physically entangled, interpenetrating compatibility state at the microscopic interface. This enhances the shear strength of the phase interface. The rigid-flexible nested mesh topological space structure blocks the propagation path of low-temperature transient impact forces, enabling the PVC alloy material supported by the rigid-flexible nested mesh topological space structure to exhibit a notched impact strength of 53.8 kJ / m² at -40℃, a room-temperature tensile strength of 54.2 MPa, and a stable Vicat softening temperature of 96℃.At 2℃, when polyvinyl chloride (PVC) alloys are subjected to low-temperature flexible loads and alternating impact loads, the forward-protruding brittle microcracks, upon encountering a nanoscale flexible coating shell, undergo deep molecular chain slippage and physical entanglement at the phase interface. This converts the concentrated impact kinetic energy into thermal energy from the microscopic slippage of large molecular chain segments. A multi-level stress dispersion mechanism alters the energy threshold of the PVC alloy's load response. Under low-temperature conditions, the material avoids localized stress concentration and continuous crack penetration, preserving the resin particle crystal memory core as a rigid base to maintain tensile stiffness and low-temperature flexibility. After more than 100 cycles of alternating heating and cooling, it suppresses phase interface debonding and delamination. Without introducing external functional groups or increasing hardware topology constraints, the technical problem of the mutual exclusion between high rigidity and high toughness is eliminated through nonlinear sequence modulation of the processing time-series energy field.
[0044] Example 5: When the system faces flow resistance fluctuations caused by different batches of chlorinated polyvinyl chloride resin and rubber phases of different viscosities entering the feeding section, the co-rotating twin-screw extruder performs no-load measurement of the screws before processing to eliminate zero-point bias of the sensor. Under the calibration state of the feeding section and preheating section set at 140°C, the central control unit collects 300 cycles of no-load torque signals and calculates the average value to establish the zero-point correction. A reference material is introduced into the main melting zone, the original measured torque is obtained, and the reference torque value is calibrated according to the formula based on the zero-point correction. : ,in, This is the calibrated reference torque value. The original measured torque value was collected. The zero-point correction is determined by the no-load average value, and the subscript... For measured values, subscripts This is a correction amount.
[0045] After achieving the benchmark torque value After calibration, the formula flow is input into the co-rotating twin-screw extruder. The central control unit activates temperature monitoring when the material temperature reaches 185°C. When faced with voltage disturbances, the central control unit utilizes the reference torque value. The zero-point drift of the real-time torque is corrected, the first derivative of the real-time torque is calculated, and the opening of the cold air valve is adjusted according to the first threshold of air cooling. The pre-gelation degree of the material at the discharge point is controlled to be kept within the range of 48%. Unmelted primary particle skeleton is provided as a force transmission node, causing the polymer elastomer to break and generate dispersed phase islands with an average particle size of 115nm. Thus, after the material undergoes convective quenching, the rigid-flexible nested network topological space structure composed of flexible nanoshell and continuous phase skeleton intercepts low-temperature impact cracks, and the polymer alloy matrix exhibits a stable state that resists the propagation of impact stress.
[0046] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the present invention.
[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material, characterized in that, Includes the following steps: Step S1: Mix 100 parts by weight of chlorinated polyvinyl chloride resin with 10 to 15 parts by weight of polymer elastomer in a mixer to obtain a premix. Step S2: The premixed material is fed into the feeding section of the twin-screw extruder; Step S3: In the pregelation section of the twin-screw extruder, the pregelation degree of the material is maintained in the range of 45% to 55% by adjusting the opening of the cold air valve and the heating power, so that the primary particle core of the chlorinated polyvinyl chloride resin maintains the crystal skeleton morphology, and the chain segment softening occurs on the periphery of the primary particles to form a free chain segment layer. Step S4: The pre-gelled material is transported to the high shear dispersion zone. At a temperature of 195°C to 205°C, the melt is subjected to axial stretching and radial deflection through the shear block assembly. The unmelted core of the primary particles is used as a force transmission node to transmit physical shear stress to the polymer elastomer. This causes the polymer elastomer to deform and peel off the phase interface in the gap between the primary particle cores, breaking into a dispersed phase structure with a particle size of 80nm to 150nm. Step S5: At the instant the material leaves the die outlet of the twin-screw extruder, an airflow or cold water spray is introduced for heat exchange, and the material temperature is reduced to below 80°C within 3 to 5 seconds, locking the spatial distribution of the dispersed phase structure and producing alloy material.
2. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, The premix also contains a low-melting-point lubricating composite additive. Based on 100 parts by weight of chlorinated polyvinyl chloride resin, the low-melting-point lubricating composite additive is 1 to 3 parts by weight. The low-melting-point lubricating composite additive is made by melt blending oxidized polyethylene wax and stearic acid in a mass ratio of 1:1 to 2:1, with a phase change temperature of 55°C to 65°C.
3. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, In step S3, the torque value of the torque sensor on the twin-screw extruder is acquired by the central control unit built into the twin-screw extruder, and the first derivative of the torque value with respect to time is calculated according to the following formula: ,in, The first derivative, This represents the current torque value collected during the current sampling period. This is the historical torque value collected in the previous sampling period. With a fixed sampling period, when the first derivative exceeds a set first threshold, the central control unit adjusts the cold air flow by controlling the opening of the cold air valve.
4. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, The twin-screw extruder is equipped with a damping reverse shearing component at the end of the pregelation section. The damping reverse shearing component generates local pressure resistance, so that the actual melt temperature at the discharge point of the pregelation section is regulated and stabilized within the range of 175℃ to 185℃.
5. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, Step S4, which applies axial tension and radial deflection to the melt through the shear block assembly, includes the following sub-steps: Step S41, controlling the axial extrusion frequency of the shear block assembly to be periodically adjusted within the range of 10Hz to 30Hz, so that the melt generates an axial velocity gradient; Step S42, guiding the melt to deflect its flow direction through the flow field deflection blades in the shear block assembly, and using the unmelted core of the primary particles as a force transmission node to introduce the tensile resistance and physical shear stress generated by the shear block assembly into the polymer elastomer.
6. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, In step S4, by controlling the staggered angle and rotation speed of the shear block assembly in the strong shear dispersion zone, the shear rate in the strong shear dispersion zone is controlled within the range of 1500s⁻¹ to 2500s⁻¹, so that the chlorinated polyvinyl chloride resin and the polymer elastomer can be blended.
7. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, The twin-screw extruder is a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1 to 48:
1. The co-rotating twin-screw extruder is equipped with a feeding section, a pre-gelling section, a high-shear dispersion zone, and an exhaust and vacuum zone in sequence along the material conveying direction. The temperature of the feeding section is controlled at 140℃ to 160℃, the temperature of the exhaust and vacuum zone is controlled at 180℃ to 190℃, and the vacuum degree of the exhaust and vacuum zone is maintained between -0.06MPa and -0.09MPa.
8. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 3, characterized in that, In step S3, the twin-screw extruder is equipped with an external forced air cooling circuit, which includes a cooling air duct and a cold air valve surrounding the outer wall of the barrel. When the first derivative exceeds the set first threshold, the opening of the cold air valve is increased by 15% to 30% to control the melt temperature fluctuation at the pregelation section outlet within ±1℃.
9. The method for preparing a low-temperature impact-resistant polyvinyl chloride alloy material according to claim 1, characterized in that, In step S1, the average particle size of the primary microparticles of chlorinated polyvinyl chloride resin is 60 μm to 120 μm, and the chlorine content is 65% to 69%; the polymer elastomer is selected from chlorinated polyethylene, acrylate copolymers and EPDM rubber, and its Mooney viscosity at 25°C is 60 to 80. The following subsequent steps are included: In step S6, the material output from the strong shear dispersion zone is introduced into the die head for drawing, cooled by a water cooling tank, and finally pelletized by a pelletizer to form granules.
10. A polyvinyl chloride alloy material resistant to low-temperature impact, characterized in that, The polyvinyl chloride alloy material is prepared by the method described in claim 1.
Citation Information
Patent Citations
A method for low-temperature extrusion molding of unplasticized polyvinyl chloride or chlorinated polyvinyl chloride products