Molding methods for composite sandwich structures and composite sandwich structure products
By systematically drying the prepreg and foam core material, precisely controlling the cutting, and performing step-by-step vacuum compaction, the problem of excessive moisture content in the foam core material during the vacuum bag forming process is solved, ensuring high-quality molding and bonding strength of the sandwich structure, which is suitable for aerospace-grade composite material sandwich structures.
Patent Information
- Application Number
- CN202611135419.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
The lack of unified standards in the drying process of foam core materials in the existing vacuum bag molding process leads to excessively high moisture content in the core material, resulting in air bubbles and pore defects during the curing process, which affects the bonding quality of the sandwich structure.
By performing life checks and thawing treatments on the prepreg and foam core, drying the foam core, and laying the prepreg layer by layer on the mold, vacuum pre-compacting and final compaction are carried out to ensure strict control of the vacuum degree and the heating and curing process. Finally, the appearance quality is checked.
It improves the molding quality and bonding strength of sandwich structures, making it suitable for manufacturing aerospace-grade composite sandwich structure products.
Smart Images

Figure CN123104103A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of composite material molding technology, and in particular to a molding method for a composite material sandwich structure and a composite material sandwich structure product. Background Technology
[0002] Fiber-reinforced resin matrix composite sandwich structures have been widely used in aerospace, rail transportation, shipbuilding, and wind turbine blades due to their high specific strength, high specific stiffness, and excellent weight reduction effect. A typical composite sandwich structure consists of an outer skin, a foam core, and an inner skin, with the foam core serving to support the skin, transfer loads, and absorb energy.
[0003] Currently, the molding of composite sandwich structures mainly employs autoclave and oven curing processes. The autoclave process applies temperature and pressure to a prepreg blank sealed in a vacuum bag using heated circulating air or nitrogen, causing the resin to cross-link and cure. This process can precisely ensure the fiber orientation and geometric dimensions of the product, and the porosity can be controlled below 2%. However, autoclave systems are large, complex, and have extremely high investment costs. Each curing cycle requires a large amount of vacuum auxiliary materials, and thermal efficiency is low. Oven curing also suffers from long heating cycles and difficulty in ensuring temperature uniformity. Vacuum bag molding is widely used due to its simple operation and low cost, but it still has shortcomings: the drying treatment of the foam core material lacks unified standards, and excessive moisture content in the core material can lead to bubbles and pore defects during curing, affecting the bonding quality of the sandwich structure. Summary of the Invention
[0004] The purpose of this application is to provide a molding method for composite sandwich structures and composite sandwich structure products, in order to solve the technical problem that the lack of unified standards for the drying treatment of foam core materials in the existing vacuum bag molding process leads to excessive moisture content of the core material, resulting in air bubbles and pore defects during the curing process, which affects the bonding quality of the sandwich structure.
[0005] To address the aforementioned technical problems, this application provides a molding method for a composite sandwich structure, comprising: S1, performing a life check and thawing treatment on the prepreg, and drying the foam core material; S2, laying a release cloth on a clean mold surface; S3, checking and confirming the ambient temperature and humidity, measuring instruments, material life, and mold accessories before laying; S4, laying the prepreg layer by layer on the mold, removing air bubbles after each layer, and performing vacuum pre-compacting according to the layer sequence, followed by final compaction; S5, laying vacuum curing auxiliary material on the layer surface and making a vacuum bag, evacuating to the required level, and then testing the pressure holding capacity; S6, heating and curing the encapsulated mold, and then cooling and removing it from the oven after curing; S7, demolding and inspecting the appearance quality of the product.
[0006] This application also provides a composite material sandwich structure product, which is manufactured using the above-mentioned composite material sandwich structure molding method. The product includes an outer skin and an inner skin formed by prepreg layup, and a foam core material sandwiched between the two. An adhesive film layer is provided between the outer skin and the foam core material, and between the inner skin and the foam core material.
[0007] Optionally, the thawing time shall not be less than 8 hours, and the standard for completion of thawing is that no water droplets or moisture condense on the outer packaging after wiping it dry. The outer packaging shall not be opened or damaged during the thawing period.
[0008] Optionally, when cutting the prepreg, the fiber direction angle deviation of the unidirectional prepreg is controlled within ±2°, the fiber direction angle deviation of the fabric prepreg is controlled within ±3°, and the sheet size deviation is controlled within ±2.5mm.
[0009] Optionally, the drying process of the foam core material includes: for unprocessed foam, maintaining it at 135℃±5℃ for 4h±0.1h; for processed foam, drying it in stages at 60℃±5℃, 80℃±5℃, and 100℃±5℃; the dried foam core material is used in an environment with humidity below 70%RH, and the allowable external exposure time does not exceed 48h.
[0010] Optionally, after laying several layers, vacuum bags are made, with the vacuum level controlled between -100kPa and -80kPa, and the holding time not less than 15 minutes.
[0011] Optionally, after the last layer is laid, a vacuum bag is made. The vacuum bag has pleats evenly and symmetrically arranged, and the vacuum degree is controlled between -100kPa and -85kPa, and the holding time is not less than 1 hour.
[0012] Optionally, during installation, the direction parallel to the edge of the mold is used as a reference, and the edges of the material in the 0° and 90° directions coincide with the installation reference baffle, respectively; the orientation tolerance of the prepreg fabric is ±3° of the fabric radial direction.
[0013] Optionally, the backing release paper and release film are retained during the installation process, and after installation, they are counted and checked to ensure that there is no release paper inclusion or foreign matter.
[0014] Optionally, the vacuum curing auxiliary material is laid in the following order: release cloth, non-porous release film, pressure equalizing plate, breathable felt and vacuum bag film. The pressure equalizing plate is smaller than the material sheet and is placed in the center, and is cured together with the product.
[0015] Optionally, the vacuum requirement is -100kPa to -85kPa, and the pressure holding test standard is that the vacuum degree decay is no more than 5kPa within 15 minutes. If the decay exceeds the standard, the leak point should be investigated and filled, and the test should be repeated.
[0016] Optionally, the curing curve for heat curing is as follows: heat treatment at 80°C for 2 hours, followed by heat treatment at 120°C for 2 hours; the product is removed from the oven after the temperature drops below 60°C.
[0017] Optionally, the appearance quality inspection includes: checking whether the product has one or more defects such as resin-poor areas, fiber wrinkles, creases, cracks, scratches, damaged release fabric, dry spots, surface pores, resin-rich areas, and fiber deformation and twisting areas, and marking the product surface if defects are found.
[0018] Optionally, it also includes steps of cutting, trimming, and sealing the product between demolding and appearance quality inspection.
[0019] Optionally, the prepreg layup is a carbon fiber fabric prepreg layup with a single layer thickness of 0.22 mm, and the layup structure of both the outer skin and the inner skin is [(45f°, 0f°)]. n , where n is the number of times the layer is repeated.
[0020] This application ensures the molding quality and bonding strength of the sandwich structure through systematic drying, precise cutting control, step-by-step vacuum compaction, and rigorous vacuum degree testing, making it suitable for manufacturing aerospace-grade composite material sandwich structure products. Attached Figure Description
[0021] Figure 1 The diagram shows a flow chart of a molding method for a composite material sandwich structure according to an embodiment of this application. Figure 2 This is a schematic diagram showing the position of the reference baffle used as a positioning reference in an embodiment of this application. Figure 3 The diagram shown is a schematic diagram of the sandwich structure according to an embodiment of this application. Detailed Implementation
[0022] The following embodiments further illustrate the technical solutions of this application. It should be understood that the specific embodiments described herein are merely for explaining this application. Furthermore, it should be noted that, for ease of description, only the parts relevant to this application are shown in the accompanying drawings, not all of them.
[0023] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to fixed connections or detachable connections; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.
[0024] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0025] The present application will be further described in detail below with reference to specific embodiments. This application uses a certain type of composite material sandwich structure test plate as an example to describe in detail the specific implementation process of the molding method for the composite material sandwich structure.
[0026] like Figure 1 As shown, the molding method of the composite material sandwich structure in this application includes the following steps: S1: Perform life check and thawing treatment on the prepreg, and dry the foam core material.
[0027] Specifically, first, the prepreg is removed from a -18°C freezing environment. In this embodiment, carbon fiber fabric prepreg is used, which is an epoxy resin system with a single-layer thickness of 0.22 mm and a resin content of 38% ± 2%. The operator needs to check the material label to confirm that the material batch number, production date, and expiration date information are complete.
[0028] The lifespan check specifically includes: checking the storage expiration date of the prepreg to confirm that the material has not exceeded its shelf life. Simultaneously, it checks the remaining operational life and remaining mechanical property life of the batch of material, ensuring both are greater than 0 hours, meeting usage requirements. Operational life refers to the time window during which the prepreg remains workable at room temperature after being removed from a frozen environment, while mechanical property life refers to the time window during which the prepreg maintains its cured mechanical properties at room temperature. If the remaining operational life is ≤0 hours, the prepreg will be difficult to handle during application due to insufficient flowability, making it difficult to remove air bubbles between layers and reducing interlayer bond strength. If the remaining mechanical property life is ≤0 hours, the mechanical strength of the cured product will not meet design requirements, affecting the product's load-bearing capacity and durability. Therefore, performing a lifespan check on the prepreg in step S1 is fundamental to ensuring subsequent molding quality and product mechanical properties.
[0029] The specific thawing procedure is as follows: Place the prepreg in a thawing area outside the installation room, maintaining an ambient temperature of 22℃±2℃ and a relative humidity of approximately 45%. The thawing time should be no less than 8 hours. During thawing, place the prepreg rolls horizontally on the thawing rack, ensuring a minimum spacing of 50mm between rolls to guarantee air circulation. Thawing is complete when the outer packaging is wiped dry and no water droplets or moisture condense. The outer packaging must not be opened or damaged during thawing. If the packaging bag is found to be damaged during handling, it must be immediately sealed with tape, and the start and end times of thawing must be recorded. Insufficient thawing time may result in uneven internal temperature of the prepreg, inadequate resin impregnation, and negatively impact subsequent installation quality and curing performance.
[0030] After thawing, the prepreg is cut for later use. The prepreg is cut using an automatic fabric cutting machine. During cutting, the length edge of the roll coincides with the machine's 0° line to ensure accurate cutting angles. The fiber direction angle deviation for unidirectional prepreg is controlled within ±2°, for woven prepreg within ±3°, and the sheet size deviation within ±2.5mm. During cutting, operators use an angle gauge to measure the fiber direction deviation and vernier calipers to check the sheet size, ensuring cutting accuracy meets process requirements. The cut sheets are bagged according to the layup sequence, with labels indicating the part name, drawing number, and layup number. If laying is not planned to begin within 48 hours, the cut sheets are bagged and returned to the freezer, then thawed again before the laying process begins.
[0031] The foam core material needs to be dried before machining to remove adsorbed moisture and prevent moisture from evaporating and forming air bubbles during curing, which would affect the bonding strength of the sandwich structure. For unprocessed foam, the drying conditions are 135℃±5℃ for 4h±0.1h. For processed foam, due to changes in the surface structure and moisture adsorption characteristics during processing, the drying conditions are as follows: 60℃±5℃ for 6h±0.1h, 80℃±5℃ for 4h±0.1h, and 100℃±5℃ for 4h±0.1h. Segmented drying aims to prevent rapid temperature increases that could cause rapid vaporization of moisture inside the foam core, damaging the cell structure. After drying, the foam core material can be sealed in a sealed bag to maintain its dryness: if a polyethylene sealed bag is used, the seal is effective for 30 days; if an aluminum foil sealed bag is used, the seal is effective for 6 months. The dried foam core material must be used in an environment with a humidity level below 70%RH. Under this humidity condition, the material is allowed to be exposed to the outside for 48 hours. If the cumulative exposure time exceeds 48 hours, or the humidity of the usage site is above 70%, or the drying shelf life has expired, it must be dried again according to the above drying conditions.
[0032] S2: Lay a release cloth on the clean mold surface.
[0033] Specifically, glass molds are used for layering. Glass molds have the advantages of low thermal expansion coefficient and high surface smoothness, making them suitable for molding high-precision composite material parts. Ensure that the mold markings and engravings are complete and clear. The mold surface should be engraved with a 0° reference line for each layer and the outline of each layer, used to confirm the position and orientation of the layers during layering.
[0034] Use a white cotton cloth, cleaning agent, plastic scraper, and vacuum cleaner to clean dust and adhesive residue from the mold and tooling surfaces. The white cotton cloth makes it easier to observe whether any residue remains after cleaning. For any residual adhesive on the mold surface, gently scrape it off with a plastic scraper, avoiding the use of metal tools to prevent damage to the mold surface. After cleaning, the mold working surface should be visually clean, free of oil, and free of particulate matter.
[0035] Apply a fluorinated release liner with adhesive backing to the application area. The size of the release liner should be larger than the test panel size to ensure smooth demolding of the prepreg in the application area. When laying the release liner, use a soft scraper to adhere it to the mold surface, removing any air bubbles between the liner and the mold, and ensuring the release liner is flat and wrinkle-free. Wrinkles or air bubbles in the release liner will directly transfer to the product surface, affecting the product's appearance quality and dimensional accuracy.
[0036] In addition, auxiliary materials need to be prepared before and after step S2. The vacuum pre-compaction auxiliary material set is cut, including a porous release liner, release cloth, breathable felt, and vacuum bag film. The porous release liner has evenly distributed micropores, allowing gas to escape while preventing excessive resin loss, ensuring that air bubbles between layers can be smoothly discharged during pre-compaction. The vacuum pre-compaction auxiliary material is used for intermediate compaction during the laying process. Simultaneously, the vacuum curing auxiliary material set is cut, including a release cloth, non-porous release liner, breathable felt, and vacuum bag film. The non-porous release liner is a continuous non-porous film that acts as a barrier, preventing resin from penetrating into the breathable felt and vacuum bag film, avoiding contamination and adhesion of auxiliary materials. The vacuum curing auxiliary material is used in the final encapsulation and curing stage. The dimensions of the auxiliary materials are cut according to the area of the part to be laid. The vacuum bag film is cut to size according to the mold dimensions, ensuring complete coverage of the product and mold edges, with allowance for pleating. A medium-temperature vacuum sealing strip is used, 12mm wide, with a temperature resistance of not less than 150℃. The vacuum tubing uses nylon tubing with an inner diameter of 8mm to 12mm and is equipped with a vacuum quick-connect suction cup to ensure reliable tubing connection and good airtightness during the vacuuming process.
[0037] S3: Before installation, check and confirm the ambient temperature and humidity, measuring instruments, material lifespan, and mold components.
[0038] Check and record the ambient temperature and humidity at the installation site, confirming that the ambient temperature is within the range of 22℃±4℃ and the ambient humidity is ≤60%. Excessive temperature at the installation site can lead to increased resin fluidity, layup slippage, and fiber orientation deviation from design requirements; excessively low temperature will increase resin viscosity, worsen wettability, and affect the bond strength between layups. Excessive humidity may cause the prepreg to absorb moisture, which will vaporize during curing, forming porosity defects.
[0039] Check whether the measuring instruments (including thermometers, hygrometers, vacuum gauges, and thermocouple thermometers) meet the usability requirements and confirm that all are within their calibration validity period. The accuracy of the measuring instruments is directly related to the accuracy of process parameter control. Instruments that have not been calibrated within their validity period may cause measurement deviations in key parameters such as temperature, humidity, and vacuum, thereby affecting product quality.
[0040] Check the remaining operating life and remaining mechanical property life of the prepreg to confirm that the remaining operating life and remaining mechanical property life are greater than 0 hours before laying begins. This second check of material life in this step is a secondary confirmation of the life check results in step S1, ensuring that the material life has not been exhausted during the time interval from S1 to S3.
[0041] Check if the mold information is correct, and if the bolts, movable parts and other accessories are complete. Confirm that the mold accessories have been installed in place.
[0042] S4: Lay the prepreg layer by layer on the mold, remove air bubbles after each layer, and vacuum pre-compact according to the layer sequence, and finally compact it.
[0043] The installation process is carried out in a clean installation room, and operators wear cleanroom suits, gloves, and anti-static shoes. A clean environment prevents dust, impurities, and other foreign matter from getting trapped between the layers and causing internal defects.
[0044] Cut the adhesive film in advance according to the dimensions of the core material sheet. The adhesive film is an epoxy resin film used to bond the skin and the foam core material. The dimensions of the adhesive film must be consistent with the dimensions of the core material. Prepare two pieces of adhesive film for each test board, one for bonding the outer skin to the foam core material and the other for bonding the inner skin to the foam core material.
[0045] Mark a coordinate system on the mold, with the 0° and 90° directions parallel to the mold edge. Using the mold edge parallel to the 0° and 90° directions as a reference, place a layup reference baffle parallel to the mold's layup area, and then lay the prepreg layer by layer according to the layup table at the layup locations. Figure 2 As shown, during the prepreg laying process, the edges of the prepreg at 0° and 90° must coincide with two laying reference baffles (A0, A90) respectively, ensuring that there is no overlap of prepregs at the bottom of the baffles. The function of laying reference baffle A is to provide a uniform positioning reference for each layup, ensuring consistency between each layup.
[0046] After each layer of prepreg is laid, visually inspect whether the fiber direction and the angle within the layup are consistent. The orientation tolerance of the prepreg should be ±3° of the fabric radial direction as specified in the engineering drawings. Use a scraper and a blower (hot air temperature approximately 50℃) to assist heating, pushing out air bubbles and smoothing wrinkles generated during the laying process from the center to the edge along the fiber direction. The purpose of heating is to reduce resin viscosity, improve the adhesion of the layup, and increase the efficiency of air bubble removal. Use scissors or a utility knife to remove excess prepreg outside the laying area.
[0047] During the application process, the backing release paper and release film should be retained. Their purpose is to protect the prepreg surface from contamination and prevent accidental adhesion between adjacent layers. After application, all release paper and release film should be counted and verified to match the quantity used, ensuring no release paper inclusions or foreign matter remain inside the layers.
[0048] Vacuum pre-compaction is performed according to the layer sequence required in the layup table. After every few layers (in this embodiment, it is performed every 4 layers), a vacuum bag is assembled using vacuum pre-compaction auxiliary materials. The specific steps for vacuum pre-compaction are as follows: a porous release film, a release cloth, a breathable felt, and a vacuum bag film are sequentially laid on the layup surface. The vacuum bag film is then adhered to the edge of the mold using sealing strips, and the vacuum pump is turned on to draw a vacuum. The vacuum level is controlled between -100 kPa and -80 kPa, and maintained for at least 15 minutes. The purpose of vacuum pre-compaction is to eliminate residual air bubbles between the layups, to initially compact each layup, and to prevent the formation of pore defects due to air bubble aggregation during final curing.
[0049] After the final layer is laid, remove the laying reference baffle and use vacuum pre-compaction auxiliary materials to assemble a vacuum bag for final compaction. The difference between final compaction and intermediate vacuum pre-compaction is that final compaction is a one-time, comprehensive compaction performed after all layers have been laid, with a longer holding time (no less than 1 hour) and a higher vacuum level requirement (-100kPa to -85kPa). The vacuum bag should have evenly and symmetrically arranged pleats, with a pleat spacing of approximately 150mm and a pleat depth of approximately 50mm. Evenly and symmetrically arranged pleats provide allowance for shrinkage of the vacuum bag during the vacuuming process, preventing uneven stress on the layers due to localized tightness of the vacuum bag film, and ensuring uniform pressure throughout the product.
[0050] The reference layup is a carbon fiber prepreg with a single layer thickness of 0.22 mm and a layup structure of [(45f°, 0f°)]. n / PMI / [(45f°, 0f°)] n That is, both the outer and inner skins are [(45f°, 0f°)]. nThe product consists of multiple layers, with a PMI foam core in the middle and an adhesive film layer at each interface. Here, n represents the number of layer repetitions, determined based on the product's load-bearing requirements, typically ranging from 4 to 8.
[0051] S5: Lay vacuum curing auxiliary material on the surface of the layer and make a vacuum bag. After evacuating to the required level, test the pressure retention.
[0052] A part label should be placed in the upper left corner of each test board. The label should include the part name, part number, placement date, and operator number. The label should be positioned so that the text is horizontal and upright for easy traceability and management.
[0053] Apply a layer of high-temperature tape (25mm wide, 180℃ resistant) to the bottom edge of the topmost sheet as a reference edge for the test plate, which will facilitate positioning during subsequent cutting and trimming.
[0054] Vacuum bags are constructed using a curing auxiliary material assembly for sealing. The auxiliary materials are laid out in the following order: release fabric, non-porous release film, pressure equalizing plate, breathable felt, and vacuum bag film. The release fabric is in direct contact with the laid-out surface, serving as an isolation and release agent, ensuring that the auxiliary materials can be easily peeled off from the product surface after curing. The non-porous release film covers the release fabric to prevent resin from penetrating into the breathable felt, thus preventing the breathable felt from losing its breathability due to resin contamination. The pressure equalizing plate, slightly smaller than the material sheet, is placed in the center. It cures together with the product inside the vacuum bag, and its function is to evenly distribute pressure during vacuuming, ensuring uniform pressure on the product surface and reducing localized stress concentration. The breathable felt covers the pressure equalizing plate, providing an escape channel for air and volatiles, ensuring smooth vacuuming. The vacuum bag film is the outermost layer, adhered to the mold edge by sealing strips, forming a sealed vacuum bag system.
[0055] During the encapsulation process, vacuum detection points, pre-arranged within the vacuum tube fabric, are placed at different locations within the vacuum bag membrane. A typical arrangement is one point at each of the four corners of the mold, used to independently monitor the vacuum level in each area. Thermocouples are embedded within the layup and at predetermined positions on the mold surface to monitor the temperature distribution during the curing process in real time.
[0056] Turn on the vacuum pump to remove air from the vacuum bag membrane. Stop vacuuming when the pressure at all test points reaches -100kPa to -85kPa. The vacuum decay at all test points should not exceed 5kPa within 15 minutes. If the decay exceeds 5kPa, check for leaks in the vacuum bag membrane, vacuum tubing, vacuum quick-connect suction cups, mold, etc. If leaks are found, use sealing strips to fill the leaks and repeat the vacuum test. Yellow sealing strips are highly visible and facilitate quick location of leaks on the vacuum bag membrane. All pressure holding test data are recorded in the sealing record sheet.
[0057] S6: Heat and solidify the packaged mold, then cool it down and remove it from the oven.
[0058] Pre-curing confirmation: Before turning on the heating equipment for curing, it must be ensured that the remaining mechanical property life of the material is >0 hours. Mechanical property life is a key parameter that determines whether the cured product can meet the design strength requirements, and it must be confirmed again before curing begins.
[0059] The mold, after completing the above operations, is then placed into the heating equipment. This embodiment uses an oven for curing; however, an autoclave or a self-heating mold can also be used depending on production conditions. For oven curing, the mold is placed stably on a rack inside the oven, ensuring sufficient space between the mold and the oven wall for air circulation to guarantee temperature uniformity.
[0060] Connect the vacuum tubing and thermocouple to the data acquisition and control system. Perform a vacuum test again: stop evacuating when the pressure at the vacuum test point reaches -100 kPa to -85 kPa. The vacuum level should decrease by no more than 5 kPa within 15 minutes. If the decrease exceeds 5 kPa, check for leaks in the vacuum bag membrane, vacuum tubing, vacuum quick-connect suction cups, mold, etc. If leaks are found, use sealing strips to fill the leaks and repeat the vacuum test.
[0061] Set the curing parameters: hold at 80℃ for 2 hours, then hold at 120℃ for 2 hours. The specific curing procedure is as follows: heat from room temperature to 80℃ at a rate of 2℃ / min, hold at 80℃ for 120 minutes; then heat from 80℃ to 120℃ at a rate of 1.5℃ / min, hold at 120℃ for 120 minutes. After the holding period, turn off the heating power. The purpose of the 80℃ holding stage is to allow the resin to initially cross-link and reduce the viscosity to its lowest point, which is conducive to further escape of air bubbles and full wetting of the fibers by the resin; the purpose of the 120℃ holding stage is to allow the resin to fully cross-link and cure, achieving the mechanical properties required by the design. During the curing process, the temperature control system displays the temperature values and time at each measuring point in real time, and the vacuum degree should remain stable within the required range throughout the process. All data of the curing process are automatically recorded by the control system, generating a curing curve report.
[0062] The product should be removed from the oven after the temperature drops below 60℃. The cooling rate should not be too fast, otherwise thermal stress may cause the product to deform or crack.
[0063] S7: Demold and perform an appearance quality inspection on the product.
[0064] Allow the product to cool to room temperature naturally. The cooling rate should not be too rapid to avoid deformation or cracking due to thermal stress. Natural cooling to room temperature typically takes 4–6 hours, depending on the product's thickness and size.
[0065] Remove auxiliary materials such as vacuum bag film, breathable felt, non-porous isolation film, release cloth, and sealing strips from the surface of the parts. Remove the thermocouples and vacuum connectors and clean them thoroughly, placing them in designated locations. Auxiliary materials are generally for single use only and should be disposed of or recycled according to regulations after cleaning.
[0066] Using nylon release wedges (approximately HRC55 hardness, 2mm thickness), gradually insert them along the seam between the part and the mold, placing one wedge approximately every 200mm. Gently pry to separate the part from the mold. The nylon material has moderate hardness, preventing damage to the mold surface and scratches to the product surface. Due to the effective release cloth and release agent, the adhesion between the product and the mold is relatively weak, and demolding can be completed in approximately 15-30 minutes. Remove the intact product and place it on a dedicated tray.
[0067] Clean the small amount of residual glue on the mold surface using a plastic scraper and cleaning agent to remove it, preparing for the next product.
[0068] The appearance quality inspection is conducted under a standard light source with an illuminance of not less than 1000 lux. The product surface quality is comprehensively inspected visually, including the following items: Check for areas of resin deficiency on the product – ensure that the resin is evenly distributed across the entire surface of the product, with no exposed fibers. Areas of resin deficiency will reduce the product's environmental resistance and surface quality, and in severe cases, may lead to fiber shedding.
[0069] Inspect the product for defects such as fiber wrinkles, creases, cracks, or scratches that damage the fibers. The product surface should be smooth and flat, with a clear and continuous fiber texture. Any defects should be circled on the product surface with a white paint pen. Fiber wrinkles will severely reduce the product's compressive strength and fatigue resistance.
[0070] Check the integrity of the release fabric – ensure that the release fabric has been completely and completely removed without any residue or damage. Damaged or residual release fabric will affect the surface quality of the product and subsequent coating processes.
[0071] Check for dry spots or surface pores – observe under strong transmitted light to confirm that the product is free of dry spots and surface pores, and that the surface is dense with no visible air bubbles. Dry spots refer to dry areas formed when the resin fails to fully wet the fibers, severely reducing the product's mechanical properties.
[0072] Check for areas rich in resin – ensure there are no areas of resin buildup on the product surface and that the resin is evenly distributed. While areas rich in resin will not significantly reduce strength, they can lead to increased product weight and uneven thickness.
[0073] Check the product for areas of fiber deformation or twisting—confirm that the fiber orientation of all layers conforms to design requirements and that there is no fiber twisting or deformation. Fiber twisting alters the load-bearing path of the product, leading to localized stress concentration and reduced strength.
[0074] After all inspection items are qualified, the apparent quality of the product is determined to be qualified.
[0075] It should be noted that, in actual production, the present application further includes the steps of subjecting the product to cutting trimming and edge sealing treatment between demolding and apparent quality inspection. In the cutting trimming process, according to the product design edge line, a numerical control water cutting device or a mechanical processing method is adopted for cutting to remove the allowance outside the laying area. Water cutting has the advantages of no heat-affected zone and good cut surface quality, and is suitable for cutting and processing composite material parts. After the cutting is completed, compressed air is used to blow off dust and cutting residues on the product surface, and then tweezers and a soft scraper are used to carefully remove the remaining demolding cloth fibers on the product surface. The edge sealing treatment is used to protect the cut edge, prevent moisture intrusion and edge delamination, and improve the environmental durability of the product. A dust-free cloth dipped in industrial alcohol with a purity of not less than 99.5% is used to clean the cut edge area to be sealed, with a wiping width of about 20mm, and then a dry dust-free cloth is used to wipe off the alcohol. A protective tape with a width of 12mm and a temperature resistance of 80°C is used to protect the surface fibers within a range of 5mm on each side of the area to be sealed. A two-component epoxy edge sealing adhesive is prepared, wherein the weight ratio of component A to component B is 100:30, and after being weighed by an electronic scale, the mixture is fully stirred in a mixing cup until the color is uniform and consistent. A fine brush is dipped in the edge sealing adhesive, and the adhesive is evenly brushed along the cut edge, with a brushing width of about 3mm, and the adhesive layer thickness is controlled to 0.3 to 0.5mm. After brushing, the mixture is cured at room temperature for 24 hours, and after curing, the edge sealing surface is gently polished with 800-mesh fine sandpaper to remove excess adhesive burrs.
[0076] After the apparent quality inspection is qualified, the quality department is requested to conduct quality inspection. The quality inspection generally includes: dimension detection (using a coordinate measuring machine to detect the overall dimension and the position of key hole positions), and ultrasonic non-destructive testing (using water-immersion ultrasonic C-scan to detect the internal quality to confirm that there are no delamination and pore defects). After all inspections are qualified, the quality department issues a qualification certificate, accompanied by quality documents such as laying records, curing curves, and inspection reports, and transfers the qualified product to subsequent processes or hands it over to the customer.
[0077] Through the above steps, the present application realizes systematic control of the molding process of the composite material sandwich structure, effectively improves the molding quality and adhesive bonding strength of the sandwich structure, and is suitable for the manufacture of aviation-grade composite material sandwich structure products.
[0078] An embodiment of the present application provides a composite material sandwich structure product manufactured by the above molding method.
[0079] As Figure 3As shown, the composite sandwich structure product is a flat test plate used for the verification and testing of aerospace-grade composite structures. The product includes an outer skin 100 and an inner skin 200 formed by carbon fiber prepreg layups, and a foam core material 300 sandwiched between the outer skin 100 and the inner skin 200. A first adhesive layer 400 and a second adhesive layer 500 are respectively provided between the outer skin 100 and the foam core material 300, and between the inner skin 200 and the foam core material 300. The thickness of the outer skin 100 and the inner skin 200 is determined according to the number of layup repetitions.
[0080] Regarding the structure of the outer skin 100, it is composed of layers of carbon fiber fabric prepreg, with a single layer thickness of 0.22 mm. The layup structure alternates between 45° and 0° directions, specifically in the following sequence: 45°, 0°, 45°, 0°, 45°, 0°, 45°, 0°, for a total of 8 layers, i.e., the number of layup repetitions n=4. The total thickness of the outer skin 100 is 8 × 0.22 mm = 1.76 mm. The fiber volume content of the outer skin 100 is 58% ± 2%, the resin content is 38% ± 2%, and the porosity is no greater than 2%.
[0081] The inner skin 200 uses the same material and layup structure as the outer skin 100, also employing carbon fiber prepreg with a single-layer thickness of 0.22 mm. The layup structure is also the same, alternating between 45° and 0° four times, with a total thickness of 1.76 mm. The inner skin 200 has a fiber volume content of 58%±2%, a resin content of 38%±2%, and a porosity of no more than 2%. The layup structures of the outer skin 100 and inner skin 200 are symmetrically arranged with the foam core material 300 as the center of symmetry, ensuring balanced stress on the inner and outer skins when the product is bent, fully utilizing the mechanical advantages of the composite sandwich structure.
[0082] The foam core material 300 sandwiched between the outer skin 100 and the inner skin 200 is made of polymethacrylamide foam. This material is lightweight, high-strength, heat-resistant, and has excellent compatibility with epoxy resin systems, making it an ideal core material for aerospace-grade composite sandwich structures.
[0083] In this embodiment, the thickness of the foam core material 300 is 10 mm and the density is 75 kg / m³. 3The compressive strength should be no less than 2.0 MPa, and the shear strength no less than 1.5 MPa. The foam core material 300 should be used after drying, with a moisture content of no more than 0.5%. The drying process conditions are as follows: unprocessed foam is kept at 135℃±5℃ for 4 h±0.1 h; after processing and molding, it is kept at 100℃±5℃ for 4 h±0.1 h. The dried foam core material 300 should be sealed in an aluminum foil bag for storage, with a shelf life of 6 months. Before installation, the foam core material 300 should be cut to a length of 580 mm and a width of 380 mm, with a 10 mm cutting allowance.
[0084] The first adhesive layer 400 between the outer skin 100 and the foam core material 300 and the second adhesive layer 500 between the inner skin 200 and the foam core material 300 are both made of epoxy resin film with a surface density of 150 g / m². 2 The thickness is 0.15 mm. The function of the first adhesive layer 400 and the second adhesive layer 500 is to firmly bond the outer skin 100 and the inner skin 200 to the surface of the foam core material 300, so as to achieve effective load transfer between the skin and the core material. The adhesive strength of the first adhesive layer 400 and the second adhesive layer 500 is not less than 25 MPa, ensuring that the sandwich structure will not debond at the interface when subjected to bending and shear loads.
[0085] This composite sandwich structure can be widely used in various aerospace structural components, including aircraft flaps, ailerons, rudders and other control surface structures; aircraft doors, fairings, access hatches and other secondary load-bearing structures; UAV fuselage panels and wing skins; and fuselage panels and doors of vertical takeoff and landing aircraft. By adjusting the number of ply repetitions, n, the product thickness and mechanical properties can be flexibly adjusted according to different load requirements, meeting a wide range of needs from secondary load-bearing structures to primary load-bearing structures. When the number of ply repetitions, n, increases, the skin thickness increases, and the bending stiffness and load-bearing capacity of the product increase accordingly, but the weight also increases. Those skilled in the art can select an appropriate number of ply repetitions, n, according to specific operating conditions and load requirements; generally, the value of n ranges from 4 to 8.
[0086] The above embodiments are merely illustrative of the principles and effects of this application. Any person skilled in the art can modify or alter the above embodiments without departing from the purpose of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the purpose disclosed in this application should still be covered by the claims of this application.
Claims
1. A method of forming a composite sandwich structure, characterized by include: S1, perform life check and thawing treatment on the prepreg, and dry the foam core material; S2, Lay a release cloth on the clean mold surface; S3, Before laying, check and confirm the ambient temperature and humidity, measuring instruments, material lifespan, and mold accessories; S4, Lay prepreg layer by layer on the mold, remove air bubbles after each layer, and vacuum pre-compact according to the layer sequence, and finally perform final compaction; S5, Lay vacuum curing auxiliary material on the layer surface and make vacuum bags, evacuate to the required level, and test the pressure holding capacity; S6, Heat and cure the sealed mold, and cool it down after curing before removing it from the oven; S7, Demold and inspect the appearance quality of the product.
2. The molding method for the composite material sandwich structure according to claim 1, characterized in that, The thawing time shall not be less than 8 hours. The standard for completion of thawing is that no water droplets or moisture condense on the outer packaging after wiping it dry. The outer packaging shall not be opened or damaged during the thawing period.
3. The molding method for the composite material sandwich structure according to claim 1, characterized in that, When cutting the prepreg, the fiber direction angle deviation of the unidirectional prepreg is controlled within ±2°, the fiber direction angle deviation of the fabric prepreg is controlled within ±3°, and the sheet size deviation is controlled within ±2.5mm.
4. The molding method for the composite material sandwich structure according to claim 1, characterized in that, The drying process of the foam core material includes: for unprocessed foam, maintaining it at 135℃±5℃ for 4h±0.1h; for processed foam, drying it in stages at 60℃±5℃, 80℃±5℃, and 100℃±5℃; the dried foam core material can be used in an environment with humidity below 70%RH, and the allowable external exposure time shall not exceed 48h.
5. The molding method for the composite material sandwich structure according to claim 1, characterized in that, After laying several layers, vacuum bags are made, and the vacuum degree is controlled between -100kPa and -80kPa, and the time is not less than 15 minutes.
6. The molding method for the composite material sandwich structure according to claim 1, characterized in that, After the final layer is laid, vacuum bags are made. The vacuum bags are evenly and symmetrically pleated, and the vacuum degree is controlled between -100kPa and -85kPa, and the time is not less than 1 hour.
7. The molding method for the composite material sandwich structure according to claim 1, characterized in that, When laying the fabric, the direction parallel to the edge of the mold is used as the reference. The edges of the fabric pieces in the 0° and 90° directions coincide with the laying reference baffle, respectively. The orientation tolerance of the prepreg fabric is ±3° of the fabric radial direction.
8. The molding method of the composite material sandwich structure according to claim 1, characterized in that, During the installation process, retain the backing release paper and release film. After installation, count and check to ensure that there is no release paper residue or foreign matter.
9. The molding method of the composite material sandwich structure according to claim 1, characterized in that, The vacuum curing auxiliary materials are laid out in the following order: release cloth, non-porous release film, pressure equalizing plate, breathable felt and vacuum bag film. The pressure equalizing plate is smaller than the material sheet and is placed in the center, and is cured together with the product.
10. The molding method of the composite material sandwich structure according to claim 1, characterized in that, The vacuum requirement is -100kPa to -85kPa. The pressure holding test standard is that the vacuum degree decreases by no more than 5kPa within 15 minutes. If the decrease exceeds the standard, the leak point should be checked and filled, and the test should be repeated.
11. The molding method of the composite material sandwich structure according to claim 1, characterized in that, The curing curve for heat curing is as follows: hold at 80℃ for 2 hours, then hold at 120℃ for 2 hours; remove the product from the oven after the temperature drops below 60℃.
12. The molding method of the composite material sandwich structure according to claim 1, characterized in that, The appearance quality inspection includes checking whether the product has one or more defects such as resin-poor areas, fiber wrinkles, creases, cracks, scratches, damaged release fabric, dry spots, surface pores, resin-rich areas, and fiber deformation and twisting areas. If defects are found, they are marked on the product surface.
13. The molding method for the composite material sandwich structure according to claim 1, characterized in that, It also includes the steps of cutting, trimming, and sealing the product between demolding and appearance quality inspection.
14. A composite material sandwich structure product, characterized in that, The product is manufactured using the molding method of the composite sandwich structure according to any one of claims 1-13. The product includes an outer skin and an inner skin formed by prepreg layup, and a foam core material sandwiched between the two. An adhesive film layer is provided between the outer skin and the foam core material, and between the inner skin and the foam core material.
15. The composite material sandwich structure product according to claim 14, characterized in that, The prepreg plies are carbon fibre fabric prepreg plies, with a single ply thickness of 0.22mm, and the lay-up structure of both the outer skin and the inner skin is [(45f°, 0f°)] n where n is the number of lay-up repetitions.