A sound-reducing mask based on a four-layer sound-reducing structure and its preparation method

The nanofiber membrane, prepared by a four-layer structure design and electrospinning technology, combined with a voice acquisition module, solves the problems of bulky structure, poor air permeability and water vapor blockage in existing sound reduction equipment, and achieves efficient full-band sound reduction and real-time communication.

CN123104185APending Publication Date: 2026-11-17TIANJIN POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610685618.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sound-reducing equipment is bulky in structure, makes it difficult to balance sound reduction and breathability, and allows breathable moisture to easily clog the sound-absorbing pores, causing a decrease in sound reduction performance. Furthermore, physical sound insulation makes voice communication inconvenient.

Method used

It adopts a four-layer structure design, including a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound insulation layer. It is prepared by ultrasonic bonding and electrospinning technology to produce organic/inorganic nanofiber membranes. It achieves full-band sound reduction by utilizing the synergistic effect of multiple layers, and ensures real-time communication through a voice acquisition and communication module.

Benefits of technology

It achieves a reduction of ≥10dB in the human voice frequency range of 250Hz~4000Hz while maintaining breathability, solves the problem of moisture blockage, ensures the stability of sound reduction performance, and guarantees real-time communication through WebRTC technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104185A_ABST
    Figure CN123104185A_ABST
Patent Text Reader

Abstract

This invention provides a sound-reducing mask based on a four-layer sound-reducing structure and its preparation method. The mask comprises, from the inside out, a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer. The drying layer is made of hydrophilic ultrafine polypropylene meltblown nonwoven fabric; the high-frequency sound-absorbing layer is an organic / inorganic composite nanofiber membrane prepared by electrospinning technology; the low-frequency sound-absorbing layer is composed of three layers of polyester fibers with progressively increasing density; and the plastic sound-insulating layer uses ABS material as its outer shell. The mask incorporates a voice acquisition and communication interaction module, and, combined with WebRTC technology-assisted software, enables interference-free multi-person calls. This invention achieves efficient sound reduction through a multi-layer physical structure, while simultaneously solving the problems of water vapor clogging pores and remote information transmission, offering advantages such as good sound reduction effect, high breathability, and high privacy protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of acoustic noise reduction, nanomaterials and smart wearable devices, specifically to a noise-reducing mask based on electrospinning technology, featuring a four-layer composite noise reduction structure and real-time communication function. Background Technology

[0002] With the rapid development of information technology and the increasing frequency of social interactions, the protection of personal voice privacy and the acoustic safety of public environments have become a focus of social concern. In high-density social scenarios such as offices, schools, and public transportation, traditional voice communication methods present the following significant social pain points:

[0003] I. Social Pain Points of Existing Voice Communication Methods

[0004] First, there is the risk of voice privacy breaches. When handling sensitive information, conducting business negotiations, or making private calls, the sound waves generated by verbal communication are easily captured by those nearby or by eavesdropping devices. Especially in open-plan office environments or waiting rooms, the lack of effective physical acoustic isolation poses a significant challenge to personal information security.

[0005] Second, environmental noise interference. Conversations among users often create unnecessary noise disturbance to those nearby, disrupting the tranquility of public environments. This interference is particularly prevalent in university libraries, study rooms, or late-night office areas, often leading to social friction and limiting group activities such as discussions due to the difficulty in finding easily accessible private discussion spaces.

[0006] In summary, the root cause of these two types of social pain points lies in the lack of a practical product on the market that can balance efficient noise reduction, comfortable wear, and uninterrupted communication. Therefore, it is necessary to systematically review the current research status and technological limitations of existing noise reduction products both domestically and internationally.

[0007] II. Current Status of Product Research at Home and Abroad and Its Technological Limitations

[0008] Currently, a small number of noise reduction devices have appeared on the overseas market. Two representative products are known: Hushme, whose main function is to limit the propagation range of speech and reduce ambient noise; and PHASMAMask, targeting gamers and whose main selling point is eliminating player communication noise. Through research and analysis of the above-mentioned existing technologies, they generally suffer from the following technical limitations:

[0009] 1. Bulky structure: The device is large and heavy, which will cause serious burden on the head and neck if worn for a long time. In addition, the appearance is too obtrusive and does not meet the aesthetics of the general public or the needs of daily travel.

[0010] 2. Difficulty in balancing acoustic performance: Existing physical sound insulation materials often struggle to balance noise reduction and breathability. If high noise reduction is prioritized, poor airflow inside the mask can cause breathing difficulties for the wearer; if breathability is prioritized, the noise reduction coefficient decreases significantly, especially in the absorption of mid-to-high frequency human voices.

[0011] 3. Poor environmental adaptability: Existing products ignore the impact of water vapor produced by human respiration on sound-absorbing materials. The aggregation of water molecules fills the gaps between sound-absorbing fibers, changing the acoustic impedance of the material, causing the noise reduction performance to rapidly decrease with prolonged wear.

[0012] Third, there is a gap in the domestic market. Research has found that the domestic noise-reducing mask industry is still in its infancy. There is a lack of mature integrated products that combine efficient noise reduction, comfortable wearing, breathability, and electronic communication, which cannot meet the huge privacy protection and social needs of office workers and college students.

[0013] In conclusion, developing a new type of noise-reducing mask that can achieve efficient full-band noise reduction, solve the problem of water vapor clogging the pores and maintain a good breathing feel, and compensate for communication barriers caused by physical sound insulation through electronic means is of great practical significance and technical value. Summary of the Invention

[0014] The purpose of this invention is to overcome the problems of existing sound-reducing devices, such as bulky structure, difficulty in balancing sound reduction and breathability, easy clogging of sound-absorbing pores by breathable moisture leading to reduced sound reduction performance, and inconvenience in voice communication after physical sound insulation. This invention provides a sound-reducing mask based on a four-layer sound-reducing structure and its preparation method. Through the layered synergy of a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer, this invention integrates moisture management, full-frequency sound absorption, sound wave blocking, and voice communication functions into a single mask structure. This allows the mask to maintain breathability while achieving stable sound reduction in the human voice frequency range. Furthermore, through a voice acquisition and communication interaction module combined with WebRTC technology, it ensures the wearer's real-time communication needs.

[0015] The technical solution adopted by this invention to solve the above-mentioned technical problems is as follows: a sound-reducing mask based on a four-layer sound-reducing structure, comprising a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer stacked sequentially from the inside to the outside. The four layers are bonded together by ultrasonic waves, and the synergistic sound reduction enables the sound-reducing mask to reduce the sound volume of the human voice frequency band from 250Hz to 4000Hz by ≥10dB. Through the sequential arrangement of the above four layers, the humid airflow exhaled by the wearer first passes through the drying layer for moisture absorption and interception. Subsequently, the sound waves enter the high-frequency and low-frequency sound-absorbing layers, where multi-scale friction, scattering, reflection, and energy dissipation occur. The remaining sound energy that is not absorbed is further blocked by the outer plastic sound-insulating layer, thereby forming a composite sound-reducing path from the inside to the outside: "dehumidification protection - high-frequency absorption - low-frequency absorption - outer shell sound insulation".

[0016] Preferably, the drying layer is the innermost layer of the face mask, made of hydrophilic ultrafine polypropylene meltblown nonwoven fabric with a surface density of 25-35 g / m². 2 The thickness is 0.3–0.8 mm. This drying layer faces the wearer's mouth and nose area directly, and its high specific surface area effectively traps water molecules produced by breathing, reducing the probability of liquid water or condensation entering the subsequent sound-absorbing layer, and preventing the pores of the high-frequency and low-frequency sound-absorbing layers from being blocked by water vapor.

[0017] Preferably, the high-frequency sound-absorbing layer is closely attached to the outer side of the drying layer and is composed of an organic / inorganic composite nanofiber membrane with a thickness of 5-15 mm and a porosity >80%. This organic / inorganic composite nanofiber membrane has nanoscale fiber diameters and high porosity, which can significantly increase the contact area between high-frequency sound waves in human voices and the fiber surface. This causes viscous frictional loss, heat dissipation, and interface scattering of sound waves within the nanofiber network, thereby primarily enhancing the mid-to-high frequency sound absorption capability in the 500Hz–4000Hz range. Controlling the thickness of the high-frequency sound-absorbing layer to 5-15 mm ensures the sound absorption path length while maintaining the overall thickness of the mask and wearing comfort.

[0018] Preferably, the low-frequency sound-absorbing layer is closely attached to the outer side of the high-frequency sound-absorbing layer and is composed of three layers of polyester fibers with a thickness of 10-20 mm and a density that increases in a stepped manner. The average diameter of the polyester fibers is 1-2 μm, and the areal density of the three layers from the inside to the outside is 100-150 g / m³. 2 200~250g / m 2 and 300~350g / m 2This low-frequency sound-absorbing layer creates an acoustic impedance gradient through a progressively increasing surface density from the inside out. This causes low-frequency sound waves entering the layer to be repeatedly reflected, refracted, and scattered within the three-layer polyester fiber network, and the sound energy is gradually dissipated through inter-fiber friction. Compared to a single-density sound-absorbing layer, the stepped increasing density structure reduces abrupt changes in acoustic impedance, increases the probability of low-frequency sound waves entering the fiber layer and being absorbed, thereby improving the reduction effect of low-frequency human voice components in the 250Hz–500Hz range.

[0019] Preferably, the plastic sound insulation layer is the outermost layer of the mask, integrally molded from an acrylonitrile-butadiene-styrene copolymer to form the outer shell, and the wall thickness of the plastic sound insulation layer is 1.5-3 mm. The ABS shell has good rigidity, formability, and structural support performance, which can provide stable support for the inner flexible sound-absorbing layer, and physically block and reflect the residual sound energy that still propagates outward after being treated by the high-frequency sound-absorbing layer and the low-frequency sound-absorbing layer.

[0020] Preferably, the four-layer structure is composited using ultrasonic bonding. The ultrasonic bonding employs high-frequency vibration waves with a frequency of 20–40 kHz, fusing the layers together at their edges and critical stress areas. Ultrasonic bonding eliminates the need for large areas of adhesive between the four layers, ensuring interlayer bonding strength and operational stability while preserving as much of the internal pore connectivity and acoustic dissipation channels of the sound-absorbing layer as possible.

[0021] Preferably, a voice acquisition and communication interaction module is fixedly installed inside the mask cavity. The module consists of an omnidirectional electret microphone, a Bluetooth wireless communication unit, and a rechargeable lithium battery. The microphone acquires the wearer's voice signal, and the Bluetooth wireless communication unit transmits the voice signal to an external smart terminal to enable real-time communication.

[0022] In a second aspect of the present invention, the organic / inorganic composite nanofiber membrane of the aforementioned high-frequency sound-absorbing layer is prepared by electrospinning after mixing a polyurethane solution with an alumina nanoparticle dispersion. The fiber diameter is distributed in the range of 300–2000 nm, and the porosity is 85%–90%. Polyurethane, as the organic continuous phase, provides the nanofiber membrane with flexibility, film-forming properties, and a porous three-dimensional framework; alumina nanoparticles, as the inorganic component, can increase the micro-interface and roughness of the fiber surface, enhancing the scattering and dissipation of sound waves in the fiber network, which is beneficial for improving the high-frequency sound absorption effect. The electrospinning process specifically includes the following steps:

[0023] S1) Polyurethane is dissolved in N,N-dimethylformamide to prepare a concentrated solution with a mass fraction of 18% to 25%, and alumina nanoparticles with a particle size of 1 to 50 nm are added at a mass of 0.2% to 5% of the mass of the polyurethane to obtain a spinning solution.

[0024] S2) Transfer the spinning solution into the injection pump of the electrospinning device, set the spinning voltage to 20-35kV, the receiving distance between the spinneret and the collecting substrate to 20-40cm, and the solution propulsion rate to 0.5-1.5mL / h.

[0025] S3) The nanofibers are uniformly stacked in multiple layers on the collecting substrate, and after curing, they are peeled off to obtain an ultrafine ceramic fiber / polyurethane composite nanofiber membrane, which is the high-frequency sound-absorbing layer.

[0026] Preferably, in step S1, the polyurethane (PU) is used to provide a three-dimensional structure for the nanofiber membrane and improve the elasticity and porosity of the membrane.

[0027] Preferably, in step S2, the electrospinning process parameters are: voltage 20-35kV, and charged droplets are formed at the spinneret and drawn into a fine jet, followed by solvent evaporation, fiber solidification and deposition on the collecting substrate.

[0028] A third aspect of the present invention provides an application of the aforementioned sound-reducing mask based on a four-layer sound-reducing structure in privacy protection and real-time multi-person interactive communication. In use, the four-layer composite structure physically reduces the volume of the wearer's voice, decreasing the intensity of speech diffusion into the surrounding environment. This is suitable for open-plan offices, libraries, study rooms, and other scenarios requiring reduced sound leakage or less interference with surrounding individuals. Simultaneously, the voice acquisition and communication interaction module can transmit the wearer's voice to an external smart terminal and, combined with terminal software, enable real-time multi-person calls, thereby maintaining clear communication while protecting voice privacy and reducing environmental noise.

[0029] Compared with the prior art, the present invention has the following advantages:

[0030] 1) The sound-reducing mask of the present invention uses a hydrophilic ultrafine polypropylene meltblown nonwoven fabric drying layer to effectively trap water molecules generated by breathing by utilizing its high specific surface area, preventing water vapor from clogging the fiber micropores in the high-frequency and low-frequency sound-absorbing layers, thus ensuring the long-term stability of the sound-reducing performance.

[0031] 2) The high-frequency sound-absorbing layer of the present invention is an organic / inorganic nanofiber composite membrane prepared by electrospinning technology. By utilizing its high porosity and nanoscale fiber diameter, the friction area between the sound wave and the fiber is increased, thereby efficiently converting high-frequency sound energy into heat energy. The thickness of 5-15mm ensures a significant noise reduction coefficient.

[0032] 3) The low-frequency sound-absorbing layer of the present invention adopts a stepped density polyester fiber structure, which, together with the physical reflection effect of the ABS plastic sound insulation shell, achieves effective capture and blocking of low-frequency sound waves. The overall measured sound reduction effect can reach 10-15 decibels.

[0033] 4) This invention achieves physical noise reduction structure and WebRTC communication system through deep integration, which ensures clear and low-latency voice interaction between users while realizing physical acoustic shielding, filling the technological gap of integrated intelligent noise reduction mask in China. Attached Figure Description

[0034] Figure 1 : Schematic diagram of the overall structure of the sound-reducing mask.

[0035] Figure 2 WebRTC technology architecture diagram.

[0036] Figure 3 Audio and video call structure logic diagram (showing the signaling channel exchange process).

[0037] Figure 4 : UI interface and volume adjustment logic diagram of the software auxiliary system. Detailed Implementation

[0038] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0039] A first aspect of this invention provides a sound-reducing mask based on a four-layer sound-reducing structure, characterized in that it comprises a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer stacked sequentially from the inside out. The four layers are composited by ultrasonic bonding, synergistically reducing sound to achieve a reduction of ≥10dB in the human voice frequency range of 250Hz to 4000Hz. The drying layer utilizes hydrophilic ultrafine polypropylene meltblown nonwoven fabric to absorb moisture generated by respiration, preventing moisture from clogging the pores of subsequent nanofiber layers and maintaining sound absorption performance. The high-frequency sound-absorbing layer uses an organic / inorganic composite nanofiber material prepared by electrospinning technology, utilizing a high-porosity three-dimensional mesh structure to convert sound energy into heat energy. The low-frequency sound-absorbing layer utilizes the three-dimensional mesh structure of polyester fiber sound-absorbing cotton to absorb low-frequency sound waves through multiple reflections and scattering. The plastic sound-insulating layer uses ABS material as the outer shell, utilizing its rigidity to block residual sound energy and support the mask structure.

[0040] Example 1

[0041] The sound-reducing mask based on the four-layer sound-reducing structure in this embodiment includes a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer stacked sequentially from the inside to the outside.

[0042] (1) The drying layer is the innermost layer of the face mask, made of hydrophilic ultrafine polypropylene meltblown nonwoven fabric with a surface density of 30 g / m³.2 The thickness is 0.5mm;

[0043] (2) The high-frequency sound-absorbing layer is closely attached to the outside of the drying layer and is composed of an organic / inorganic composite nanofiber membrane with a thickness of 10 mm and a porosity of 87%.

[0044] (3) The low-frequency sound-absorbing layer is closely attached to the outside of the high-frequency sound-absorbing layer. It is composed of three layers of polyester fibers with a thickness of 15 mm and a density that increases in a stepped manner. The average diameter of the polyester fibers is 1.5 μm, and the areal density of the three layers from the inside to the outside is 120 g / m³. 2 220g / m 2 and 320g / m 2 ;

[0045] (4) The plastic sound insulation layer is the outermost layer of the mask. It is formed by integral molding of acrylonitrile-butadiene-styrene copolymer to form a shell with a wall thickness of 2mm.

[0046] The method for preparing the high-frequency sound-absorbing layer specifically includes the following steps:

[0047] S1) Polyurethane is dissolved in N,N-dimethylformamide to prepare a concentrated solution with a mass fraction of 22%, and alumina nanoparticles with a particle size of 20 nm are added at a mass of 2% of the polyurethane to obtain a spinning solution.

[0048] S2) Transfer the spinning solution into the injection pump of the electrospinning device, set the spinning voltage to 28kV, the receiving distance between the spinneret and the collecting substrate to 30cm, and the solution propulsion rate to 1.0mL / h.

[0049] S3) Nanofibers are uniformly stacked in multiple layers on the collecting substrate, cured, and then peeled off to obtain an organic / inorganic composite nanofiber membrane with a fiber diameter distribution in the range of 300-2000 nm and a porosity of 87%, which is the high-frequency sound-absorbing layer.

[0050] The four-layer structure is ultrasonically fused together at the edges and key stress areas using a high-frequency vibration wave of 25kHz.

[0051] The mask's inner cavity is fixedly equipped with a voice acquisition and communication interaction module, which consists of an omnidirectional electret microphone, a Bluetooth wireless communication unit, and a rechargeable lithium battery. The microphone acquires the wearer's voice signal, and the Bluetooth wireless communication unit transmits the voice signal to an external smart terminal to enable real-time communication.

[0052] The mask obtained in Example 1 was subjected to the following performance tests: Referring to GB / T 18696.2-2002 standard, the normal incident sound absorption coefficient at different frequencies was determined using the impedance tube method. Before testing, the four-layer composite structure to be tested was cut into circular samples according to the inner diameter of the impedance tube. The edges of the samples were sealed with sealing rings or low-modulus sealant to prevent sound leakage at the edges. When installing the samples, the drying layer faced the sound source end and the plastic sound insulation layer faced the rigid backing end, thus simulating the sound propagation path from the inside to the outside when the mask is worn. For low-frequency testing, an impedance tube with an inner diameter of 100mm was used, corresponding to a circular sample diameter of 100mm and a microphone spacing of 50mm; for mid-to-high frequency testing, an impedance tube with an inner diameter of 30mm was used, corresponding to a circular sample diameter of 30mm and a microphone spacing of 20mm. The test sound source used was broadband random noise or a swept-frequency signal, with a sampling frequency of not less than 12.8 kHz. At least 32 average spectra were collected for each sample. The test environment was controlled at a temperature of 23±2℃ and a relative humidity of 50±5%. Before testing, the sensitivity of both microphones was calibrated using a 1 kHz, 94 dB sound level calibrator, and dual-channel amplitude and phase corrections were performed according to the equipment operating procedures to eliminate amplitude and phase deviations between the two channels. The test results are as follows:

[0053] Low-frequency sound absorption (250-500Hz): Average sound absorption coefficient 0.53;

[0054] Mid-to-high frequency sound absorption (500-4000Hz): average sound absorption coefficient 0.78;

[0055] Overall average sound absorption coefficient (250-4000Hz): 0.71.

[0056] Example 2

[0057] The difference between this embodiment and Embodiment 1 is that the thickness of the high-frequency sound-absorbing layer is 5mm, while the rest of the structure, material parameters and preparation method are the same.

[0058] Performance tests were conducted on Example 2, using the same impedance tube method parameters as in Example 1. The test results are as follows:

[0059] Low-frequency sound absorption (250-500Hz): Average sound absorption coefficient 0.50;

[0060] Mid-to-high frequency sound absorption (500-4000Hz): average sound absorption coefficient 0.70;

[0061] Overall average sound absorption coefficient (250-4000Hz): 0.64.

[0062] Example 3

[0063] The difference between this embodiment and Embodiment 1 is that the thickness of the high-frequency sound-absorbing layer is 15mm, while the rest of the structure, material parameters and preparation method are the same.

[0064] Performance tests were conducted on Example 3, using the same impedance tube method parameters as in Example 1. The test results are as follows:

[0065] Low-frequency sound absorption (250-500Hz): Average sound absorption coefficient 0.54;

[0066] Mid-to-high frequency sound absorption (500-4000Hz): average sound absorption coefficient 0.82;

[0067] Overall average sound absorption coefficient (250-4000Hz): 0.74.

[0068] Example 4

[0069] The difference between this embodiment and Embodiment 1 is that the average diameter of the polyester fibers in the low-frequency sound-absorbing layer is 1 μm, while the rest of the structure, material parameters and preparation methods are the same.

[0070] Performance tests were conducted on Example 4, using the same impedance tube method parameters as in Example 1. The test results are as follows:

[0071] Low-frequency sound absorption (250-500Hz): Average sound absorption coefficient 0.58;

[0072] Mid-to-high frequency sound absorption (500-4000Hz): average sound absorption coefficient 0.79;

[0073] Overall average sound absorption coefficient (250-4000Hz): 0.74.

[0074] The four-layer composite sound-reducing masks prepared in Examples 1-4 above achieve graded absorption and synergistic reduction of noise in different frequency bands: The organic / inorganic composite nanofiber membrane in the high-frequency sound-absorbing layer enhances the viscous loss and heat dissipation of sound waves through a high-porosity fiber network, primarily improving the sound absorption performance in the mid-to-high frequency band (500-4000Hz); the stepped-density three-layer polyester fiber structure in the low-frequency sound-absorbing layer improves the sound absorption performance in the low-frequency band (250-500Hz) through acoustic impedance gradient, multiple reflections, and frictional dissipation; the outer ABS plastic sound insulation layer further blocks transmitted sound waves. Test results show that as the thickness of the high-frequency sound-absorbing layer increases from 5mm to 10mm and 15mm, the average sound absorption coefficient in the mid-to-high frequency band increases from 0.70 to 0.78 and 0.82, respectively; when the average diameter of the polyester fibers decreases from 1.5μm to 1μm, the average sound absorption coefficient in the low-frequency band increases from 0.53 to 0.58. The above structure achieves an overall average sound absorption coefficient of 0.64 to 0.74 in the 250 to 4000 Hz range, demonstrating good broadband sound absorption performance.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 1 is that the high-frequency sound-absorbing layer uses ordinary polyurethane open-cell sponge with a thickness of 10 mm and a porosity of approximately 75% instead of the organic / inorganic composite nanofiber membrane. All other structures, material parameters, and preparation methods are the same. The sound absorption performance was tested using the same GB / T 18696.2-2002 impedance tube method test conditions as in Example 1, and the results are as follows:

[0077] Low-frequency sound absorption (250-500Hz): average sound absorption coefficient 0.51;

[0078] Mid-to-high frequency sound absorption (500–4000 Hz): average sound absorption coefficient 0.61;

[0079] Overall average sound absorption coefficient (250~4000Hz): 0.57.

[0080] Further observation of the material's microstructure using scanning electron microscopy revealed the following results:

[0081] The composite nanofibers in Example 1 have an average fiber diameter of 300–2000 nm;

[0082] The average pore size of the polyurethane sponge in Comparative Example 1 is approximately 80–1500 μm.

[0083] Because ordinary polyurethane foam has a large pore size and a low specific surface area, the frictional dissipation effect of sound waves at the material interface is weakened, resulting in lower high-frequency sound absorption performance than in Example 1.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 1 is that the low-frequency sound-absorbing layer adopts a single-layer uniform density polyester fiber structure with an areal density of 220 g / m². 2 The total thickness is 15mm, and the remaining structure, material parameters, and preparation method are the same. The sound absorption performance was tested under the same GB / T 18696.2-2002 impedance tube method test conditions as in Example 1, and the results are as follows:

[0086] Low-frequency sound absorption (250-500Hz): average sound absorption coefficient 0.44;

[0087] Mid-to-high frequency sound absorption (500–4000 Hz): average sound absorption coefficient 0.74;

[0088] Overall average sound absorption coefficient (250~4000Hz): 0.63.

[0089] The results show that the acoustic impedance change is relatively simple under the uniform density structure, and the multiple reflections and gradual dissipation of low-frequency sound waves after entering the fiber layer are insufficient; while after adopting the stepped increasing density structure in Example 1, a continuous acoustic impedance gradient can be formed, thereby improving the propagation path and dissipation efficiency of low-frequency sound waves inside the material.

[0090] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A sound-reducing mask based on a four-layer sound-reducing structure, characterized in that, The mask comprises, from the inside out, a drying layer, a high-frequency sound-absorbing layer, a low-frequency sound-absorbing layer, and a plastic sound-insulating layer. These four layers are bonded together using ultrasonic bonding, and their synergistic sound reduction ensures that the mask reduces the human voice frequency range (250Hz–4000Hz) by ≥10dB. (1) The drying layer is the innermost layer of the face mask, made of hydrophilic ultrafine polypropylene meltblown nonwoven fabric with a surface density of 25-35 g / m². 2 The thickness is 0.3–0.8 mm; (2) The high-frequency sound-absorbing layer is closely attached to the outside of the drying layer and is composed of an organic / inorganic composite nanofiber membrane with a thickness of 5-15 mm and a porosity of >80%. (3) The low-frequency sound-absorbing layer is closely attached to the outside of the high-frequency sound-absorbing layer and is composed of three layers of polyester fibers with a thickness of 10-20 mm and a density that increases in a stepped manner. The average diameter of the polyester fibers is 1-2 μm, and the areal density of the three layers from the inside to the outside is 100-150 g / m³. 2 200~250g / m 2 and 300~350g / m 2 ; (4) The plastic sound insulation layer is the outermost layer of the mask, which is integrally formed by acrylonitrile-butadiene-styrene copolymer to form the outer shell.

2. The sound-reducing mask according to claim 1, characterized in that, The mask's inner cavity is fixedly equipped with a voice acquisition and communication interaction module, which consists of an omnidirectional electret microphone, a Bluetooth wireless communication unit, and a rechargeable lithium battery. The microphone acquires the wearer's voice signal, and the Bluetooth wireless communication unit transmits the voice signal to an external smart terminal to enable real-time communication.

3. The sound-reducing mask according to claim 1, characterized in that, The organic / inorganic composite nanofiber membrane of the high-frequency sound-absorbing layer is prepared by electrospinning after mixing a polyurethane solution with an alumina nanoparticle dispersion. The fiber diameter is distributed in the range of 300-2000 nm, and the porosity is 85%-90%. The electrospinning process specifically includes the following steps: S1) Polyurethane is dissolved in N,N-dimethylformamide to prepare a concentrated solution with a mass fraction of 18% to 25%, and alumina nanoparticles with a particle size of 1 to 50 nm are added at a mass of 0.2% to 5% of the mass of the polyurethane to obtain a spinning solution. S2) Transfer the spinning solution into the injection pump of the electrospinning device, set the spinning voltage to 20-35kV, the receiving distance between the spinneret and the collecting substrate to 20-40cm, and the solution propulsion rate to 0.5-1.5mL / h; S3) Allow the nanofibers to be uniformly stacked in multiple layers on the collecting substrate, and after curing, peel them off to obtain an ultrafine ceramic fiber / polyurethane composite nanofiber membrane, which is the high-frequency sound-absorbing layer.

4. The sound-reducing mask according to claim 1, characterized in that, The ultrasonic bonding uses high-frequency vibration waves with a frequency of 20 to 40 kHz to fuse and bond the four-layer structure at its edges and key stress areas.

5. The sound-reducing mask according to claim 1, characterized in that, The wall thickness of the plastic sound insulation layer is 1.5 to 3 mm.