Lightweight thermal insulation and waterproof membrane and its preparation method
By introducing EVA and POE insulation core layers into waterproof membranes, and utilizing the synergistic effect of polymer microspheres expanding to form hollow microcavities and phase change energy storage microcapsules, combined with online production processes of four-channel co-extrusion and electron beam irradiation crosslinking, the problems of heavy weight, low interlayer bonding strength, and insufficient thermal insulation performance of waterproof membranes have been solved, achieving a combination of lightweight, thermal insulation, and temperature regulation functions, as well as efficient production.
Patent Information
- Application Number
- CN202611359066.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-07-31
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing waterproof membranes, while fulfilling both waterproofing and thermal insulation functions, suffer from problems such as excessive weight, low interlayer bonding strength, limited thermal insulation performance, and high energy consumption and low efficiency in production processes, failing to meet the demands of modern buildings for lightweight, integrated, and efficient construction.
The insulation core layer, containing EVA and/or POE, is combined with composite lightweight fillers and foaming agents. Hollow microcavities are formed through the irreversible expansion of polymer microspheres at high temperatures, synergistically working with phase change energy storage microcapsules to reduce density and improve insulation performance. Simultaneously, an online production process employing four-channel co-extrusion and electron beam irradiation crosslinking achieves interface strengthening and continuous production.
It combines lightweight, heat insulation, and temperature regulation functions, reduces density and energy consumption, and improves the bonding strength of the interface, making it suitable for integrated waterproofing and heat insulation projects for various building roofs.
Smart Images

Figure CN123104191A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building waterproofing materials, specifically relating to a composite waterproofing membrane for roofing that combines lightweight, heat insulation, and waterproofing functions, and its continuous online production process. Background Technology
[0002] Roof waterproofing is a crucial aspect of building construction. Traditional roof waterproofing membranes are mainly divided into bitumen-based and polymer-based types. Bitumen-based membranes offer high waterproofing reliability and moderate cost, but their high filler content and density significantly increase the roof load. They also have poor thermal insulation performance, requiring an additional insulation layer and making the construction process cumbersome. On the other hand, polymer-based membranes are lighter and have better weather resistance, but their thermal insulation performance is insufficient. Furthermore, polymer-based membranes typically require mechanical fixing and cannot achieve full adhesion to the roof substrate for waterproofing.
[0003] In existing technologies, to balance waterproofing and insulation functions, a layered construction method of "waterproof membrane + insulation board" is usually adopted. This method is not only complex and time-consuming, but also prone to leakage or insulation layer detachment due to interlayer adhesion failure. At the same time, some waterproof and thermal insulation composite membrane products still have defects such as excessive weight, low bonding strength between the insulation and waterproof layers, and high energy consumption in the production process, which cannot meet the modern building requirements for "lightweight, integrated, and efficient construction".
[0004] Existing technologies involve adding a separate "temperature control layer" containing phase change materials to waterproof membranes to achieve localized optimization of temperature regulation, relying on physical adhesion or interlayer bonding methods based on the asphalt's own bonding. For example, patent CN217803714U discloses an elastomeric modified bitumen waterproof membrane containing a nano-phase change temperature control layer. However, the additional layer in this patent adds thickness, weight, and the risk of interlayer delamination.
[0005] Meanwhile, existing technologies also involve applying polymer microspheres to waterproof membranes. For example, patents CN108215371A and CN108081706A disclose a waterproof membrane and its preparation method. The microspheres work synergistically with thermoplastic elastomers to increase the rheological properties and flexibility of the adhesive, thereby improving the toughness and bonding performance of the adhesive.
[0006] For example, CN112440533A discloses a high-viscosity modified bitumen waterproof membrane and its preparation method. It utilizes polymer microspheres between layers as "balls" to change the internal friction mode to rolling friction, which is conducive to the "pseudo-low viscosity" phenomenon of internal components, so that the bitumen can be effectively spread and wetted on the concrete substrate surface. Furthermore, the construction process is accompanied by heating. Under the action of heat, the polymer microspheres undergo a certain degree of volume expansion. During the expansion process, the spacing between silanol groups increases and the hydrogen bonding force is weakened, making it easier for the layered silicate layers to slip relative to each other, reducing the viscosity of the system and facilitating wetting and spreading.
[0007] Patent CN109721323A discloses a nanoporous thermal insulation material, in which polymer hollow microspheres and paraffin / porous perlite-urea-formaldehyde resin phase change microcapsules are simultaneously added to the base layer. The porous structure of the polymer hollow microspheres creates steric hindrance to block heat conduction, while the phase change microcapsules utilize their heat storage and release properties to achieve temperature regulation. However, this solution disperses the two types of microspheres in a cement-based or inorganic cementitious system, and its application is for rigid wall insulation. The two types of microspheres independently perform their insulation and temperature regulation functions, which cannot meet the requirements of roof waterproofing membranes for flexibility, rollability, integrated waterproofing and insulation, and continuous production.
[0008] It is evident that the polymer microspheres in the aforementioned patents do not contribute to improving thermal insulation performance or reducing density in waterproof membranes.
[0009] The above background information is provided only to aid in understanding the inventive concept and technical solution of this invention. It does not necessarily belong to the prior art of this invention. In the absence of clear evidence that the above information was disclosed before the filing date of this invention, the above background information should not be used to evaluate the novelty and inventiveness of this invention. Summary of the Invention
[0010] In view of this, in order to overcome the shortcomings of the prior art, the purpose of this invention is to provide a thermal insulation core layer suitable for waterproof membranes, which has low density and good thermal insulation effect.
[0011] To achieve the above objectives, the present invention adopts the following technical solution: An insulating core layer suitable for waterproof membranes is disclosed, comprising EVA (ethylene-vinyl acetate copolymer) and / or POE (polyolefin elastomer), composite lightweight fillers, and a foaming agent. The composite lightweight fillers include polymer microspheres and phase change energy storage microcapsules. The polymer microspheres are internally encapsulated with a low-boiling-point hydrocarbon foaming agent. These polymer microspheres expand in volume during the preparation of the waterproof membrane, forming hollow microcavities that remain within the insulating core layer. Specifically, the polymer microspheres of this invention undergo irreversible plastic expansion at the foaming temperature, increasing in volume to 3-5 times their original size. Upon cooling, this expansion is permanently fixed, thereby forming numerous hollow microcavities within the insulating core layer. These microcavities, together with closed-cell bubbles generated by the decomposition of the chemical foaming agent, constitute a hierarchical porous structure, significantly reducing the core layer density and improving insulation performance.
[0012] According to some preferred embodiments of the present invention, the composite lightweight filler is obtained by compounding polymer microspheres and phase change energy storage microcapsules in a mass ratio of 3~5:1~2.
[0013] According to some preferred embodiments of the invention, the polymer microspheres have an average particle size of 20-50 μm, a wall thickness of 0.5-2 μm, and a true density of 0.1-0.3 g / cm³. 3 The outer shell of the polymer microspheres is made of polyacrylonitrile and / or polymethyl methacrylate, and is internally encapsulated with a low-boiling-point hydrocarbon foaming agent. These polymer microspheres can expand twice at 120-150°C, with a volume expansion ratio of 3-5 times, further reducing the density of the insulation core layer.
[0014] Preferably, in the polymer microspheres, the proportion of low-boiling-point hydrocarbon foaming agent is 10-20 wt%, and the proportion of shell is 80-90 wt%.
[0015] In this invention, the outer shell of the polymer microspheres is made of thermoplastic polyacrylonitrile or polymethyl methacrylate, and the interior is encapsulated with a low-boiling-point hydrocarbon foaming agent. At room temperature, the polymer shell is in a glassy state, exhibiting high rigidity and modulus. Although the internal foaming agent has already vaporized and generated pressure, this pressure is far from sufficient to break or deform the rigid shell, and the microsphere size remains essentially unchanged. When the masterbatch for preparing the insulating core layer is prepared at 120–140°C, the outer shell material gradually softens above its glass transition temperature, entering a highly elastic state; simultaneously, the vapor pressure of the internal low-boiling-point hydrocarbon foaming agent increases sharply with increasing temperature. When the internal pressure exceeds the yield strength of the outer shell material at that temperature, the shell undergoes uniform plastic expansion, and the microsphere volume increases. Because the outer shell material has sufficient melt strength within the foaming temperature range, the expansion process does not cause the shell to rupture, and the foaming agent is continuously encapsulated inside the microspheres. When the composite roll material enters the foaming box, the online foaming temperature rises to 140~150℃, and the microspheres expand again (secondary expansion). At this temperature, the molecular chains are fully extended. After cooling, the molecular chains are frozen in new positions, the outer shell regains rigidity, and the volume is permanently fixed, forming a large number of hollow microcavities. At the same time, together with the closed-cell bubbles generated by the decomposition of the chemical foaming agent, they form a multi-level porous structure, thus further reducing the density and weight of the insulation core layer.
[0016] According to some preferred embodiments of the present invention, the low-boiling-point hydrocarbon blowing agent is isobutane and / or isopentane. At room temperature, it exists in a gaseous state and continuously applies internal pressure to the outer shell of the polymer microspheres. As the temperature rises, the vapor pressure of the gaseous hydrocarbon blowing agent inside the microspheres increases exponentially with increasing temperature, forming a strong internal pressure of several megapascals within the sealed microsphere cavity. At this point, the softened outer shell can no longer confine the high-pressure gas inside, forcing it to undergo isotropic uniform plastic tensile deformation, causing the microsphere volume to expand rapidly.
[0017] According to some preferred embodiments of the present invention, the core material of the phase change energy storage microcapsule is paraffin wax, and the wall material is urea-formaldehyde resin and / or melamine-formaldehyde resin; the average particle size is 10-30 μm, and the latent heat of phase change is ≥120 J / g. The function of the phase change energy storage microcapsule is to utilize the characteristic of phase change materials to absorb / release a large amount of latent heat near the phase change temperature to achieve temperature regulation of building roofs. It absorbs excess heat during the day and releases it at night, effectively suppressing roof temperature fluctuations and reducing air conditioning energy consumption.
[0018] According to some preferred embodiments of the present invention, the thermal insulation core layer comprises, by weight: 40-50 parts of EVA, 20-25 parts of POE, 15-20 parts of polymer microspheres, 5-10 parts of phase change energy storage microcapsules, and 1-2 parts of chemical foaming agent.
[0019] The present invention also provides a lightweight thermal insulation and waterproof membrane comprising the thermal insulation core layer as described above; comprising a weather-resistant surface layer, wherein ultraviolet absorbers and / or anti-aging agents are added to the weather-resistant surface layer; and / or comprising an adhesive transition layer, wherein the adhesive transition layer contains SBS modified bitumen, 10 to 15 parts of polyolefin elastomer based on 100 parts of SBS modified bitumen, 5 to 8 parts of silane coupling agent, and 0.3 to 0.5 parts of antioxidant; and / or comprising a bitumen underlayer, wherein the bitumen underlayer contains rubber tackifying resin and an anti-sticking release film.
[0020] According to some preferred embodiments of the present invention, the weather-resistant surface layer, the bonding transition layer, the thermal insulation core layer and the asphalt underlayer are arranged sequentially, and the thickness of each layer is as follows: weather-resistant surface layer 0.3-0.4 mm, bonding transition layer 0.2-0.3 mm, thermal insulation core layer 3-5 mm, and asphalt underlayer 0.3-0.4 mm.
[0021] The lightweight thermal insulation and waterproof membrane of this invention is compositely formed from top to bottom as follows: a TPO polymer weather-resistant surface layer, a modified bitumen bonding transition layer, a lightweight foamed polymer thermal insulation core layer, and a self-adhesive modified bitumen base layer. The lightweight foamed polymer thermal insulation core layer uses an EVA / POE blend as the matrix, compounded with hollow polymer microspheres and paraffin phase change energy storage microcapsules, and is prepared through chemical closed-cell foaming. The modified bitumen bonding transition layer is an SBS modified bitumen layer incorporating POE elastomer and a silane coupling agent, used to achieve interfacial compatibility and high-strength bonding between the TPO surface layer and the foamed thermal insulation core layer. The overall density of the thermal insulation core layer is 0.08–0.12 g / cm³. 3 Thermal conductivity ≤0.020W / (m・K), density of finished roll material 0.4~0.6g / cm³ 3 The roll material has a composite strength of ≥0.8MPa, combining lightweight heat insulation, thermal insulation and temperature regulation, high bonding reliability and excellent weather resistance; the production process is continuous and efficient, reducing energy consumption by more than 40%; the roll material can be cold-applied for full adhesion and hot-air welding for overlapping of the surface layer, making it suitable for integrated waterproofing and thermal insulation projects for various building roofs.
[0022] To address the interfacial compatibility issue, this invention employs a "modified bitumen bonding transition layer" as a means to resolve the interface problem between TPO and the foamed core layer, unlike traditional bitumen rolls or composite rolls where bitumen plays the primary role in waterproofing. Furthermore, the irradiation in this invention is "online," occurring sequentially online with "co-extrusion" and "foaming," which can be used to address the interfacial strength issues arising from online cross-linking.
[0023] The present invention also provides a method for preparing the above-mentioned lightweight thermal insulation and waterproof membrane, comprising the following steps: The raw materials corresponding to the weather-resistant surface layer, bonding transition layer, thermal insulation core layer and asphalt base layer are melt-blended separately; Four layers of material are simultaneously extruded using a multi-channel co-extrusion equipment and hot-bonded at the equipment outlet to form a composite roll. The composite roll material enters the foaming box and is foamed online to obtain the insulation core layer; Electron beam irradiation is then performed to cross-link the bonding transition layer and the thermal insulation core layer, resulting in the lightweight thermal insulation and waterproof membrane.
[0024] According to some preferred embodiments of the present invention, the melt blending temperature of the weather-resistant surface layer is 180–200°C; the melt blending temperature of the bonding transition layer is 160–170°C; and the extrusion temperature or melt blending temperature of the masterbatch for the thermal insulation core layer is 120–140°C. The material for the thermal insulation core layer can be prepared in the form of a masterbatch, or the raw materials can be directly heated, melt-blended, and then extruded.
[0025] According to some preferred embodiments of the present invention, the foaming box is a closed segmented temperature-controlled tunnel oven, which sequentially includes a preheating zone, a foaming zone and a shaping zone along the direction of roll material travel.
[0026] According to some preferred embodiments of the present invention, the online foaming temperature is 140-150°C and the foaming pressure is 0.3-0.5 MPa.
[0027] According to some preferred embodiments of the present invention, the online foaming includes the following steps: In the preheating zone, the temperature of the roll material gradually rises to 140~145℃, and the chemical foaming agent begins to decompose. The roll material enters the foaming zone and is foamed at a temperature of 140-150℃ and a foaming pressure of 0.3-0.5MPa; the chemical foaming agent decomposes to produce gas, forming bubble nuclei in the melt of the insulation core layer; the bubble nuclei grow and form a closed-cell structure; When the roll material enters the setting zone, the temperature is 120~130℃. The melt viscosity of the insulation core layer increases, the growth of the foam cells stops, and the foaming process ends.
[0028] According to some preferred embodiments of the invention, the dose of electron beam irradiation is 50 to 100 kGy.
[0029] In some embodiments, the production process of the lightweight thermal insulation and waterproof membrane of the present invention adopts a one-step continuous production method after four-channel co-extrusion composite, online foaming and electron beam irradiation crosslinking, including the following steps: (1) Raw material pretreatment The raw materials for the corresponding weather-resistant surface layer, bonding transition layer, thermal insulation core layer and asphalt base layer are obtained by melt blending.
[0030] (2) Four-channel co-extrusion molding Four layers of material are extruded simultaneously using a four-channel co-extrusion machine, and each layer is hot-bonded at the machine exit to obtain a composite roll material.
[0031] (3) Online closed-cell foaming The composite roll material enters the foaming chamber, where temperature-controlled foaming forms a closed-cell insulation structure. The online foaming chamber is a sealed, segmented, temperature-controlled tunnel oven, which includes a preheating zone, a foaming zone, and a setting zone along the direction of roll material travel. Specifically, at the exit of the four-channel co-extrusion die, after the core layer (containing 1-2 parts of AC chemical foaming agent) is hot-bonded with the other three layers, it immediately enters the foaming chamber. The foaming process consists of the following three steps: Preheating activation: In the preheating zone, the core temperature gradually rises from 120~140℃ during extrusion to 140~145℃, and the AC foaming agent begins to decompose, releasing gases such as N2.
[0032] Constant temperature foaming: The core layer enters the foaming zone (140~150℃, 0.3~0.5MPa), and the foaming agent decomposes in large quantities to produce gas, forming countless tiny bubble nuclei in the EVA / POE melt; the bubble nuclei grow uniformly under constant temperature and pressure conditions to form a closed-cell structure.
[0033] Cell shaping: When the core layer enters the shaping zone (120~130℃), the melt viscosity increases, cell growth stops, and foaming ends.
[0034] (4) Electron beam irradiation crosslinking This allows for radiation-induced cross-linking and strengthening of the interface between the bonding transition layer and the core layer.
[0035] (5) Cooling, calendering, winding and slitting to obtain finished rolls.
[0036] The entire production process described above is a continuous online molding process, with a single roll production cycle of ≤1 hour. Through online extrusion of multi-layer thermal lamination, combined with electron beam irradiation for online cross-linking molding, the interfacial bonding strength is effectively increased. Furthermore, the dual action of hollow polymer microspheres internally encapsulated with low-boiling-point hydrocarbon foaming agents and chemical foaming agents further reduces the density and weight of the insulation core layer, achieving excellent lightweight and thermal insulation effects.
[0037] Due to the adoption of the above technical solutions, the advantages of the present invention compared with the prior art are as follows: The lightweight thermal insulation and waterproof membrane of the present invention contains both polymer microspheres and phase change energy storage microcapsules in its thermal insulation core layer, and the polymer microspheres are encapsulated with low-boiling-point hydrocarbon foaming agents, which enables the polymer microspheres to expand twice at 120~150℃, with a volume expansion ratio of 3~5 times, further reducing the density of the thermal insulation core layer and improving the thermal insulation effect. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0039] Figure 1 This is a schematic diagram of the cross-sectional structure of the lightweight thermal insulation and waterproof membrane in an embodiment of the present invention. Detailed Implementation
[0040] To enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0041] To address the shortcomings of existing roof waterproofing and insulation composite membranes, such as excessive weight, low interlayer bonding strength, limited insulation performance, and high energy consumption and low efficiency in production processes, this invention provides an integrated composite membrane and an efficient production solution. The waterproof membrane of this invention has a four-layer composite structure, consisting of, from top to bottom: a TPO polymer weather-resistant top layer, a modified bitumen bonding transition layer, an EVA / POE lightweight foamed insulation core layer composed of composite hollow polymer microspheres and paraffin phase change energy storage microcapsules, and a self-adhesive modified bitumen bottom layer. The production process employs a one-step continuous production method involving four-channel co-extrusion composite, online closed-cell foaming, and electron beam irradiation crosslinking, achieving simultaneous molding and interfacial strengthening of each layer.
[0042] First, this invention provides an insulating core layer suitable for waterproof membranes. The insulating core layer contains EVA, POE, a composite lightweight filler, and a foaming agent. The composite lightweight filler includes polymer microspheres and phase change energy storage microcapsules. The composite lightweight filler is obtained by compounding polymer microspheres and phase change energy storage microcapsules at a mass ratio of 3~5:1~2.
[0043] The polymer microspheres have an average particle size of 20–50 μm, a wall thickness of 0.5–2 μm, and a true density of 0.1–0.3 g / cm³. 3The polymer microspheres have an outer shell made of polyacrylonitrile and / or polymethyl methacrylate, and are internally encapsulated with a low-boiling-point hydrocarbon foaming agent; preferably, isobutane and / or isopentane. These polymer microspheres can expand twice at 120-150°C, with a volume expansion ratio of 3-5 times, further reducing the density of the insulation core layer. Preferably, the low-boiling-point hydrocarbon foaming agent accounts for 10-20 wt% of the polymer microspheres, and the outer shell accounts for 80-90 wt%.
[0044] The core material of the phase change energy storage microcapsules is paraffin wax, and the wall material is urea-formaldehyde resin and / or melamine-formaldehyde resin; the average particle size is 10-30 μm, and the latent heat of phase change is ≥120 J / g. The function of the phase change energy storage microcapsules is to utilize the characteristic of phase change materials to absorb / release a large amount of latent heat near the phase change temperature to achieve temperature regulation of building roofs. They absorb excess heat during the day and release it at night, effectively suppressing roof temperature fluctuations and reducing air conditioning energy consumption.
[0045] Traditional phase change materials, such as paraffin, suffer from inherent defects during phase change processes, including easy leakage, large volume changes, and low thermal conductivity. The phase change energy storage microcapsules used in this invention fundamentally solve these problems through microencapsulation technology, offering the following specific advantages: Leakage prevention and encapsulation stability: Microencapsulation technology encapsulates the phase change core material within a dense polymer wall material, forming a "core-shell" structure. Even if the core material undergoes a solid-liquid phase change, the molten paraffin remains confined within the microcapsules, preventing leakage and ensuring the roll material's performance does not degrade over long-term use. A large specific heat transfer surface area: The microencapsulated phase change material particles are tiny, and the outer shell provides a large specific heat transfer surface, significantly improving the heat exchange efficiency between the phase change material and the matrix, resulting in faster heat storage and release responses. Good compatibility with the matrix material: The microcapsule shell (urea-formaldehyde resin or melamine-formaldehyde resin) has certain polarity and reactivity, enabling it to form a good interfacial bond with the matrix and be uniformly dispersed in the core layer without agglomeration or sedimentation. Volume change constraint: Traditional phase change materials undergo significant volume changes (expansion or contraction) during solid-liquid phase changes, which can lead to material cracking or detachment from the matrix after repeated cycles. The microcapsule shell provides mechanical constraints, limiting volume changes within the microcapsules and ensuring the overall dimensional stability of the roll material.
[0046] By weight, the thermal insulation core layer comprises: 40-50 parts EVA, 20-25 parts POE, 15-20 parts polymer microspheres, 5-10 parts phase change energy storage microcapsules, and 1-2 parts AC chemical foaming agent.
[0047] This invention utilizes both hollow polymer microspheres and paraffin phase change energy storage microcapsules in the thermal insulation core layer. These two components are not simply superimposed but exhibit a significant synergistic effect. In addition to their high-temperature expansion during fabrication, the hollow polymer microspheres, through their expanded internal hollow cavities, provide continuous and stable thermal insulation during the application of the waterproof membrane, acting consistently day and night. The phase change energy storage microcapsules only trigger a solid-liquid phase change when the ambient temperature exceeds their phase change temperature, buffering temperature shocks by absorbing or releasing latent heat, thus providing a transient thermal regulation effect. The combination of the two mechanisms reduces the average heat flow throughout the day, while the phase change microcapsules mitigate the midday peak temperature, achieving dual protection of "steady-state insulation + transient buffering." Faced with the complex climatic conditions of sustained high temperatures and significant diurnal temperature variations in summer, a single mechanism either cannot cope with continuous heat conduction or cannot buffer sudden temperature changes; the synergy of both mechanisms enables all-day, multi-scenario thermal management coverage.
[0048] Secondly, this invention provides a lightweight thermal insulation and waterproof membrane comprising the above-mentioned thermal insulation core layer. This invention employs a four-layer composite structure consisting of a "polymer weather-resistant surface layer + modified bitumen bonding transition layer + lightweight foamed polymer thermal insulation core layer + self-adhesive bitumen bottom layer." Through a one-step co-extrusion composite process and online cross-linking thermal bonding technology, simultaneous molding and high-strength interfacial bonding of each layer are achieved. Simultaneously, polymer microspheres and phase change energy storage microcapsules are introduced into the thermal insulation core layer to enhance its thermal insulation and temperature regulation performance. Structurally, the weather-resistant surface layer, bonding transition layer, thermal insulation core layer, and bitumen bottom layer are arranged sequentially, as follows: TPO polymer weather-resistant surface layer (thickness 0.3-0.4mm): Modified with weather-resistant TPO (thermoplastic polyolefin) blend, and with the addition of UV absorbers and anti-aging agents, providing excellent weather resistance, puncture resistance, and surface decoration. Preferably, it includes 90-110 parts TPO resin, 0.2-1 parts UV absorber, and 0.2-1 parts anti-aging agent.
[0049] Modified asphalt bonding transition layer (thickness 0.2-0.3mm): 100 parts of SBS modified asphalt are used as the base material, and 10-15 parts of POE (polyolefin elastomer), 5-8 parts of silane coupling agent, and 0.3-0.5 parts of antioxidant are added to improve the interfacial compatibility and bonding strength with TPO surface layer and foamed core layer.
[0050] Lightweight foamed polymer insulation core layer (thickness 3-5mm): EVA / POE blend as matrix, with 15-20% hollow polymer microspheres (density 0.1-0.3g / cm³) added. 3 The thermal insulation core layer, containing 5-10% paraffin phase change energy storage microcapsules, is chemically foamed into a closed-cell foam. The density of the insulation core layer is controlled at 0.08-0.12 g / cm³. 3Thermal conductivity ≤0.020W / (m・K).
[0051] Self-adhesive asphalt base layer (thickness 0.3-0.4mm): Uses self-adhesive modified asphalt as the base material, with added rubber tackifying resin for easy bonding to the roof substrate. No open flame heating is required during construction. Preferably, use 90-110 parts self-adhesive modified asphalt and 6-15 parts rubber tackifying resin.
[0052] This invention directly disperses phase change energy storage microcapsules within the EVA / POE foam core layer, rather than stacking them as a separate additional layer in the structure. This allows the same material layer to simultaneously perform the triple functions of lightweight support, physical insulation, and phase change temperature regulation. This avoids the thickness, weight, and interlayer delamination risks associated with adding an extra layer. Simultaneously, a modified asphalt bonding transition layer based on SBS-modified asphalt, with added POE elastomer and silane coupling agent, is introduced to solve the interfacial compatibility problem. Furthermore, electron beam irradiation crosslinking forms chemical bonds at the interface, improving the composite strength.
[0053] Furthermore, based on the aforementioned structure of the lightweight thermal insulation and waterproof membrane, this invention also provides a method for preparing the aforementioned lightweight thermal insulation and waterproof membrane, comprising the following steps: Step 1: Raw material pretreatment Polymer surface layer: TPO raw materials are melt-blended in a mixer at 180-200℃ and then fed into an extruder; Modified asphalt bonding transition layer: SBS modified asphalt, POE, silane coupling agent and antioxidant are put into a mixing tank and mixed evenly at 160-170℃ to prepare molten binder.
[0054] Insulating core layer: EVA, POE, hollow polymer microspheres, phase change energy storage microcapsules, and chemical foaming agent (AC foaming agent) are fed into a twin-screw extruder and co-extruded at 120-140°C to produce foaming masterbatch. Preparing masterbatch is the preferred embodiment. Under specific conditions, the components can also be directly mixed and melt-dried.
[0055] Base layer: Self-adhesive asphalt raw materials are mixed evenly at 150-160℃ to form a molten binder.
[0056] Step 2: One-step co-extrusion composite molding Using a four-channel co-extrusion die, TPO top layer, modified asphalt adhesive layer, thermal insulation core layer, and self-adhesive asphalt bottom layer are extruded simultaneously. The four layers are thermally bonded at the die exit to obtain composite roll material.
[0057] The composite roll material is immediately fed into an online foaming chamber after extrusion, where the temperature is controlled at 140–150℃ and the pressure at 0.3–0.5MPa to complete the closed-cell foaming process.
[0058] In some embodiments, the online foaming box is a closed-type segmented temperature-controlled tunnel oven, which sequentially includes a preheating zone, a foaming zone, and a shaping zone along the roll material's travel direction. Specifically, at the exit of the four-channel co-extrusion die, after the insulation core layer (containing 1-2 parts of AC chemical foaming agent) is hot-pressed with the other three layers, it immediately enters the foaming box. The foaming process consists of the following three steps: Preheating activation: In the preheating zone, the temperature of the composite roll material gradually increases from 120~140℃ during extrusion to 140~145℃, and the AC foaming agent begins to decompose, releasing gases such as N2.
[0059] Constant temperature foaming: When the composite roll material enters the foaming zone (140~150℃, 0.3~0.5MPa), the foaming agent decomposes in large quantities to produce gas, forming countless tiny bubble nuclei in the EVA / POE melt; the bubble nuclei grow uniformly under constant temperature and pressure conditions to form a closed-cell structure.
[0060] Cell setting: When the composite roll enters the setting zone (120~130℃), the melt viscosity increases, cell growth stops, and foaming ends.
[0061] The polymer microspheres are encapsulated with a low-boiling-point hydrocarbon foaming agent. At the high temperatures used in the preparation of the insulation core layer or waterproof membrane, the foaming agent vaporizes, generating internal pressure that causes irreversible plastic expansion of the microsphere shell, increasing its volume to 3-5 times its original size. Upon cooling, this expansion is permanently fixed, forming numerous hollow microcavities within the insulation core layer. Simultaneously, the chemical foaming agent decomposes in the EVA / POE melt, releasing gas and forming a closed-cell bubble structure. Through the synergistic effect of the permanent hollow cavities of the hollow polymer microspheres and the closed-cell bubbles generated by the chemical foaming agent, a multi-level porous structure is formed within the core layer, significantly reducing its density and achieving excellent lightweight and thermal insulation properties.
[0062] Step 3: Online cross-linking thermal bonding After foaming, the roll material enters an electron beam irradiation crosslinking device, which irradiates and crosslinks the interface between the bonding transition layer and the insulation core layer, improving the interfacial molecular chain entanglement strength and achieving a bonding composite strength ≥0.8MPa. Subsequently, it is cooled and shaped using a three-roll calender, with the cooling rate controlled at 5-10℃ / min to prevent warping and deformation of the roll material.
[0063] Step 4: Rewinding and Slitting After the roll material is shaped and inspected for surface defects, it is rolled up and then cut into standard widths (such as 1m and 2m) according to requirements, and then packaged and stored.
[0064] In existing technologies, foaming and cross-linking are typically independent processes completed offline. This invention couples "four-channel co-extrusion" with "online closed-cell foaming" and "electron beam irradiation cross-linking" online. The core layer foams at 140-150℃, and the interface is cross-linked and strengthened under the action of an electron beam (50-100kGy), achieving integration of molding and functionalization. Existing two-step processes (first fabricating the insulation board → then hot-pressing composite) have a production cycle of 8-12 hours per batch. This invention achieves continuous one-step production, with a single roll production cycle of ≤1 hour and energy consumption reduced by more than 40%.
[0065] In the following examples, the manufacturers and batches of some of the raw materials used are as follows: Thermoplastic polyolefin NS06, Sino-Korean (Wuhan) Petrochemical Co., Ltd.; UV absorbers UV-326 and UV-327, Qingdao Xuxin Chemical Co., Ltd.; POE elastomer PN-2070, Mitsui Chemicals; Silane coupling agent KH-550, Nanjing Silicon Innovation Materials Co., Ltd.; Antioxidant 1010 and Antioxidant 168, BASF; Polymer microspheres, Haiyi Enterprise Development Co., Ltd.; AC chemical foaming agent AC7000, Taizhou Kaixin Chemical Co., Ltd.; Rubber tackifying resin C5 / C9, Shanghai Yiyong New Materials Technology Co., Ltd.
[0066] Example 1 (I) The raw material composition of each layer in the lightweight thermal insulation and waterproof membrane of this embodiment is as follows: TPO polymer weather-resistant surface layer: 100 parts TPO resin, 0.5 parts ultraviolet absorber, and 0.5 parts anti-aging agent.
[0067] Modified asphalt bonding transition layer: 100 parts SBS modified asphalt, 12 parts POE elastomer, 6 parts silane coupling agent, and 0.4 parts antioxidant.
[0068] Lightweight foamed polymer insulation core layer: 45 parts EVA, 22 parts POE, and 18 parts hollow polymer microspheres (average particle size 35μm, wall thickness 1.2μm, true density 0.18g / cm³). 3 The material consists of a polyacrylonitrile shell, encapsulated internally with isobutane foaming agent, 8 parts of paraffin phase change energy storage microcapsules (average particle size 20μm, phase change temperature 28℃, latent heat of phase change ≥120J / g), and 1.5 parts of AC chemical foaming agent.
[0069] Self-adhesive modified bitumen base layer: 100 parts self-adhesive modified bitumen, 10 parts rubber tackifying resin.
[0070] (II) The preparation method of the lightweight thermal insulation and waterproof membrane in this embodiment is as follows: (1) Raw material pretreatment TPO raw materials are melt-blended at 190°C and then fed into an extruder; SBS modified asphalt, POE, silane coupling agent, and antioxidant are mixed evenly at 165°C to prepare a molten binder; EVA, POE, hollow polymer microspheres, phase change energy storage microcapsules, and AC foaming agent are blended and extruded at 130°C using a twin-screw extruder to prepare foaming masterbatch; self-adhesive asphalt raw materials are mixed evenly at 155°C to prepare a molten binder.
[0071] (2) Four-channel co-extrusion molding Four layers of material are extruded simultaneously through a four-channel co-extrusion die. The thickness of each layer is controlled as follows: TPO top layer 0.35mm, modified asphalt bonding transition layer 0.25mm, foamed core layer 4mm, and self-adhesive asphalt bottom layer 0.35mm. Thermal bonding is achieved at the die exit to obtain composite roll material.
[0072] (3) Online closed-cell foaming The composite roll material enters the online foaming chamber (a closed, segmented, temperature-controlled tunnel oven, which includes a preheating zone, a foaming zone, and a setting zone along the direction of roll material travel). The foaming process consists of the following three steps: Preheating activation: In the preheating zone, the temperature of the composite roll material gradually rises from 130°C during extrusion to 145°C, and the AC foaming agent begins to decompose, releasing gases such as N2.
[0073] Constant temperature foaming: The composite roll material enters the foaming zone (temperature 145℃, pressure 0.4MPa), where the foaming agent decomposes in large quantities to produce gas, forming countless tiny bubble nuclei in the EVA / POE melt; the bubble nuclei grow uniformly under constant temperature and pressure conditions, forming a closed-cell structure.
[0074] Cell shaping: When the composite roll enters the shaping zone (120℃), the melt viscosity increases, cell growth stops, and closed-cell foaming is completed.
[0075] (4) Electron beam irradiation crosslinking The interface between the bonding transition layer and the thermal insulation core layer was subjected to irradiation crosslinking at an irradiation dose of 75 kGy.
[0076] (5) Cooling, calendering, winding and slitting The product is cooled and shaped using a three-roll calender at a cooling rate of 8℃ / min, and then wound up and slit to obtain the finished product.
[0077] (III) Performance test results of the lightweight thermal insulation and waterproof membrane in this embodiment The lightweight thermal insulation and waterproof membrane of this embodiment was subjected to the following tests. The test results are shown in Table 1.
[0078] Table 1 Test Results of Example 1 Example 2 The difference between this embodiment and the previous embodiment is that the raw material composition of each layer in the lightweight thermal insulation and waterproof membrane of this embodiment is as follows: TPO polymer weather-resistant surface layer: 100 parts TPO resin, 0.2 parts ultraviolet absorber, and 1 part anti-aging agent.
[0079] Modified asphalt bonding transition layer: 100 parts SBS modified asphalt, 10 parts POE elastomer, 5 parts silane coupling agent, and 0.3 parts antioxidant.
[0080] Lightweight foamed polymer insulation core layer: 40 parts EVA, 25 parts POE, 15 parts polymer microspheres, 5 parts phase change energy storage microcapsules, and 1 part AC chemical foaming agent.
[0081] Self-adhesive modified bitumen base layer: 100 parts self-adhesive modified bitumen, 6 parts rubber tackifying resin.
[0082] The preparation process conditions of the lightweight thermal insulation and waterproof membrane in this embodiment are basically the same as those in Example 1.
[0083] Example 3 The difference between this embodiment and the previous embodiment is that the raw material composition of each layer in the lightweight thermal insulation and waterproof membrane of this embodiment is as follows: TPO polymer weather-resistant surface layer: 100 parts TPO resin, 1 part ultraviolet absorber, and 0.2 parts anti-aging agent.
[0084] Modified asphalt bonding transition layer: 100 parts SBS modified asphalt, 15 parts POE elastomer, 8 parts silane coupling agent, and 0.5 parts antioxidant.
[0085] Lightweight foamed polymer insulation core layer: 50 parts EVA, 20 parts POE, 20 parts polymer microspheres, 10 parts phase change energy storage microcapsules, and 2 parts AC chemical foaming agent.
[0086] Self-adhesive modified bitumen base layer: 100 parts self-adhesive modified bitumen, 15 parts rubber tackifying resin.
[0087] The preparation process conditions of the lightweight thermal insulation and waterproof membrane in this embodiment are basically the same as those in Example 1.
[0088] Comparative Example 1 The difference between this comparative example and the embodiment is that in this comparative example, the hollow polymer microspheres in the insulation core layer of embodiment 1 are replaced with the same mass fraction of ordinary hollow glass microspheres (average particle size 40 μm, true density 0.25 g / cm³). 3 (Without internal encapsulating foaming agent), the rest of the formulation and process conditions are basically the same as in Example 1.
[0089] Results: Because ordinary hollow glass microspheres do not have the ability to expand twice during the online foaming process, they cannot expand further at the foaming temperature to reduce density. As a result, the density of the finished roll increases, the thermal conductivity increases, and the mass per unit area increases, leading to increased product transportation costs.
[0090] Comparative Example 2 The difference between this comparative example and the embodiment is that the paraffin phase change energy storage microcapsules in the insulation core layer of embodiment 1 are replaced with the same mass fraction of ordinary paraffin, while the rest of the formulation and process conditions are basically the same as those of embodiment 1.
[0091] Results: Ordinary paraffin wax cannot be uniformly mixed with the matrix material during the preparation of EVA / POE foamed core layer, resulting in obvious agglomeration and precipitation; at the foaming temperature, paraffin wax melts and flows, and migrates to the core layer surface with the growth of bubbles during the foaming process. After cooling, waxy precipitates appear on the surface of the roll material, affecting the composite strength.
[0092] Comparative Example 3 The difference between this comparative example and the example is that: in this comparative example, the paraffin phase change energy storage microcapsules are not added to the insulation core layer of Example 1, and the amount of hollow polymer microspheres is increased to 26 parts (keeping the total amount of composite lightweight filler equivalent to that of Example 1). The rest of the formulation and process conditions are basically the same as those of Example 1.
[0093] Results: The thermal conductivity of the roll material was basically the same as that of Example 1, and the density was similar, but it did not have the function of phase change energy storage and temperature regulation. In the simulated solar radiation temperature rise test, the core layer temperature increased linearly with the ambient temperature, without the "temperature plateau" effect.
[0094] Comparative Example 4 The difference between this comparative example and the example is that hollow polymer microspheres are not added to the insulation core layer of Example 1 in this comparative example, and the amount of phase change energy storage microcapsules is increased to 26 parts (keeping the total amount of composite lightweight filler equivalent to that of Example 1). The rest of the formulation and process conditions are basically the same as those of Example 1.
[0095] Results: The roll material has good phase change temperature regulation function, but the thermal insulation performance is reduced, the density and thermal conductivity of the finished roll material are increased, and the increase in the unit area mass leads to an increase in product transportation costs.
[0096] Comparative Example 5 The difference between this comparative example and the example is that: in this comparative example, no silane coupling agent is added to the modified asphalt bonding transition layer of Example 1, while the rest of the formulation and process conditions are basically the same as those of Example 1.
[0097] Results: Due to the lack of bridging effect of silane coupling agent, the interfacial compatibility between the modified bitumen and the TPO surface layer decreased significantly, resulting in reduced composite strength. In simulated roof thermal cycling tests, the roofing membrane exhibited delamination between the surface layer and the core layer.
[0098] Comparative Example 6 This comparative example uses a traditional two-step process to prepare a four-layer roll material with the same structure as in Example 1, as detailed below: First, a TPO surface layer (extrusion molding), a foamed insulation core layer (EVA / POE + filler + AC foaming agent calendered and foamed), a modified asphalt bonding transition layer (coating molding), and a self-adhesive asphalt base layer (coating molding) are prepared separately. Then, the four layers are bonded together by hot pressing (temperature 170℃, pressure 0.5MPa). The formulations of the remaining raw materials are basically the same as those in Example 1.
[0099] Results: The two-step process resulted in low composite strength of the roll material; the production cycle for a single batch was approximately 8 hours; the core layer thickness uniformity was poor; and the roll material was prone to warping and deformation.
[0100] Tests and Results The waterproof membranes prepared in the examples and comparative examples were tested for relevant properties. The test results are shown in Table 2.
[0101] Table 2 Test results of the examples and comparative examples The data in Table 2 show that Comparative Examples 1 and 2 respectively demonstrate the performance enhancement of the hollow polymer microspheres' "secondary expansion capability" and the phase change energy storage microcapsules' "core-shell encapsulation" structure. Comparative Examples 3 and 4 jointly demonstrate the indispensable synergistic relationship between the two components in the hollow microsphere and phase change energy storage microcapsule composite system. Comparative Example 5 demonstrates the decisive role of the silane coupling agent in interlayer bonding strength; Comparative Example 6 demonstrates the significant superiority of the one-step continuous process of this invention compared to the traditional two-step process.
[0102] Existing waterproof membrane technologies suffer from excessive weight, weak interlayer adhesion, high production energy consumption, and insufficient thermal insulation performance. Therefore, this invention aims to provide a lightweight thermal insulation and waterproof membrane and its manufacturing process. The lightweight thermal insulation and waterproof membrane of this invention is compositely formed from top to bottom as follows: a TPO polymer weather-resistant surface layer, a modified bitumen bonding transition layer, a lightweight foamed polymer thermal insulation core layer, and a self-adhesive modified bitumen bottom layer. The lightweight foamed polymer thermal insulation core layer uses an EVA / POE blend as a matrix, compounded with hollow polymer microspheres and paraffin phase change energy storage microcapsules, and is produced through chemical closed-cell foaming. The core layer forms hollow microcavities, which, together with the closed-cell bubbles generated by the chemical foaming agent, constitute a multi-level porous structure. The modified bitumen bonding transition layer is an SBS modified bitumen layer incorporating POE elastomer and a silane coupling agent, used to achieve interfacial compatibility and high-strength adhesion between the TPO surface layer and the foamed thermal insulation core layer. The overall density of the thermal insulation core layer is 0.08–0.12 g / cm³. 3Thermal conductivity ≤0.020W / (m・K), density of finished roll material 0.4~0.6g / cm³ 3 Compared with existing waterproof membrane technologies, it reduces the load by more than 30%, significantly reducing the roof load; the composite strength of the membrane is ≥0.8MPa, avoiding delamination failure after long-term use, and it has the advantages of lightweight heat insulation, heat preservation and temperature regulation, high bonding reliability and excellent weather resistance, improving adaptability to extreme climates; the production process is continuous and efficient, reducing energy consumption by more than 40%, and the membrane can be fully bonded by cold construction and the surface layer can be hot-air welded and overlapped, making it suitable for integrated waterproof and thermal insulation projects for various building roofs.
[0103] Compared with the prior art, the present invention has the following advantages: For the first time, a four-layer composite structure of "TPO weather-resistant surface layer + modified asphalt bonding transition layer + EVA / POE foamed insulation core layer + self-adhesive asphalt bottom layer" is adopted. The bonding transition layer solves the interfacial compatibility problem between polymer and asphalt materials.
[0104] A composite system of hollow polymer microspheres and phase change energy storage microcapsules is introduced into the thermal insulation core layer to achieve the dual effects of lightweighting and efficient thermal insulation and temperature regulation; POE and silane coupling agent are added to the modified asphalt bonding layer to significantly improve the interlayer bonding strength.
[0105] For the first time, a one-step continuous production process for this roll material, which combines four-channel co-extrusion, online closed-cell foaming, and electron beam irradiation crosslinking, has been publicly disclosed. This process enables simultaneous molding of multiple materials and interface strengthening, replacing the traditional two-step hot-pressing composite method and significantly improving production efficiency and product reliability.
[0106] The above embodiments prepared by the method of the present invention are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
[0107] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
Claims
1. A lightweight thermal insulation and waterproof membrane, characterized in that, The waterproof membrane comprises, in sequence, a weather-resistant surface layer, an adhesive transition layer, an insulating core layer, and an asphalt underlayer; the insulating core layer contains ethylene-vinyl acetate copolymer and / or polyolefin elastomer, composite lightweight filler, and foaming agent; the composite lightweight filler includes polymer microspheres and phase change energy storage microcapsules; the polymer microspheres are internally encapsulated with a low-boiling-point hydrocarbon foaming agent; and the polymer microspheres are used to expand in volume during the preparation of the waterproof membrane.
2. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, The composite lightweight filler is obtained by compounding polymer microspheres and phase change energy storage microcapsules at a mass ratio of 3~5:1~2.
3. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, The polymer microspheres have an average particle size of 20–50 μm, a wall thickness of 0.5–2 μm, and a true density of 0.1–0.3 g / cm³. 3 The outer shell of the polymer microspheres is made of polyacrylonitrile and / or polymethyl methacrylate.
4. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, The low-boiling-point hydrocarbon foaming agent is isobutane and / or isopentane.
5. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, In the polymer microspheres, the proportion of low-boiling-point hydrocarbon foaming agent is 10-20 wt%, and the proportion of shell is 80-90 wt%.
6. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, The core material of the phase change energy storage microcapsule is paraffin wax, and the wall material is urea-formaldehyde resin and / or melamine-formaldehyde resin; the average particle size is 10-30 μm, and the latent heat of phase change is ≥120 J / g.
7. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, By weight, the thermal insulation core layer comprises: 40-50 parts of ethylene-vinyl acetate copolymer, 20-25 parts of polyolefin elastomer, 15-20 parts of polymer microspheres, 5-10 parts of phase change energy storage microcapsules, and 1-2 parts of chemical foaming agent.
8. The lightweight thermal insulation and waterproof membrane according to claim 1, characterized in that, The weather-resistant surface layer contains ultraviolet absorbers and / or anti-aging agents; and / or the bonding transition layer contains SBS modified asphalt, 10 to 15 parts of polyolefin elastomer based on 100 parts of SBS modified asphalt, 5 to 8 parts of silane coupling agent, and 0.3 to 0.5 parts of antioxidant; and / or the asphalt underlayer contains rubber tackifying resin.
9. A method for preparing a lightweight thermal insulation and waterproof membrane as described in any one of claims 1-8, characterized in that, Includes the following steps: The raw materials corresponding to the weather-resistant surface layer, bonding transition layer, thermal insulation core layer and asphalt base layer are melt-blended separately; Four layers of material are simultaneously extruded using a multi-channel co-extrusion equipment and hot-bonded at the equipment outlet to form a composite roll. The composite roll material enters the foaming box and is foamed online to obtain the insulation core layer; Electron beam irradiation is then performed to cross-link the bonding transition layer and the thermal insulation core layer, resulting in the lightweight thermal insulation and waterproof membrane.
10. The preparation method according to claim 9, characterized in that, The melt blending temperature of the weather-resistant surface layer is 180–200°C; the melt blending temperature of the bonding transition layer is 160–170°C; and the melt blending temperature of the thermal insulation core layer is 120–140°C.
11. The preparation method according to claim 9, characterized in that, The foaming chamber is a closed, segmented, temperature-controlled tunnel oven, which includes a preheating zone, a foaming zone, and a shaping zone in sequence along the direction of roll material travel.
12. The preparation method according to claim 11, characterized in that, The online foaming process includes the following steps: In the preheating zone, the temperature of the roll material gradually rises to 140~145℃, and the chemical foaming agent begins to decompose. The roll material enters the foaming zone and is foamed at a temperature of 140-150℃ and a foaming pressure of 0.3-0.5MPa; the chemical foaming agent decomposes to produce gas, forming bubble nuclei in the melt of the insulation core layer; the bubble nuclei grow and form a closed-cell structure; When the roll material enters the setting zone, the temperature is 120~130℃. The melt viscosity of the insulation core layer increases, the growth of the foam cells stops, and the foaming process ends.
Citation Information
Patent Citations
Antibacterial waterproof roll and preparation method thereof
CN108081706A
Waterproof roll and preparation method thereof
CN108215371A
Nano-microporous thermal insulation material and preparation method thereof
CN109721323A
High-viscosity modified asphalt waterproof coiled material and preparation method thereof
CN112440533A