A biaxially oriented polypropylene pearlescent film and its preparation method
By introducing polyurethane microspheres into the upper surface of biaxially oriented polypropylene pearl film to form a raised structure, the problems of low production efficiency and high energy consumption caused by corona treatment and primer coating are solved, enabling direct spreading and bonding of inks, and improving production efficiency and compatibility.
Patent Information
- Application Number
- CN202611560618.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing biaxially oriented polypropylene pearlescent films require corona treatment and primer coating before printing, resulting in low production efficiency, high energy consumption, and poor compatibility between ink and film.
By introducing polyurethane microspheres of appropriate particle size into the upper surface of the film, they are uniformly dispersed to form a raised structure, increasing polarity and enabling the ink to spread and bond directly without additional corona treatment or primer.
It improves production efficiency, reduces energy consumption, and ensures that the ink spreads evenly and bonds firmly on the film surface, avoiding additional processing steps.
Smart Images

Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of thin films, and in particular to a biaxially oriented polypropylene pearlescent film and its preparation method. Background Technology
[0002] Biaxially oriented polypropylene (BOPP) pearlescent film has a special gloss effect, which makes it easy for product manufacturers to design colorful and eye-catching patterns to showcase their brand image. Therefore, this type of film has a wide range of applications in the consumer goods labeling industry.
[0003] The information on consumer product labels is generally presented on BOPP pearlescent film through printing. Currently, the inks used in label printing have a very different polarity from polypropylene, and most highly polar polymers are incompatible with polypropylene. Therefore, in order to ensure that the ink can spread and bond well on the film surface, the BOPP pearlescent film production process not only requires corona treatment of the surface to be printed to ensure that its surface tension reaches more than 36 dynes, but also the surface tension will gradually decrease after corona treatment due to the gradual migration of polar groups on the surface into the film, the precipitation of low molecular weight substances, and environmental temperature and humidity. Therefore, before printing, a second corona treatment or a layer of polar acrylic ester material that is compatible with commonly used inks and can firmly adhere to the surface of BOPP pearlescent film is usually applied to the corona-treated surface to ensure the ink spreading and bonding.
[0004] However, performing corona treatment and primer coating before film printing not only leads to a longer production process, which is not conducive to improving production efficiency, but also increases production energy consumption. Summary of the Invention
[0005] Based on this, the purpose of this invention is to provide a biaxially oriented polypropylene pearlescent film and its preparation method. By introducing polyurethane microspheres of appropriate particle size into the upper surface layer and dispersing them uniformly therein, the polyurethane microspheres can form a uniformly distributed protruding structure on the surface of the upper surface layer after the film is stretched laterally. This protruding structure can, on the one hand, play an anti-adhesion role, making it less likely for the films to stick together when they come into contact; on the other hand, it is equivalent to adding a polyurethane layer to the upper surface layer of the film. The uniformly distributed and highly polar polyurethane microsphere protruding structure allows the ink printed on the upper surface layer to spread evenly on the film surface and bond firmly, without the need for additional corona treatment and primer treatment during printing.
[0006] The technical solution of the present invention is achieved in the following ways: A biaxially oriented polypropylene pearlescent film comprises an upper surface layer, a core layer, and a lower surface layer arranged sequentially. The upper surface layer comprises copolymer polypropylene and 30-40 wt% polyurethane microsphere masterbatch, and the thickness of the upper surface layer is 2-3 μm. The core layer comprises homopolymer polypropylene and 20-30 wt% calcium carbonate masterbatch. The lower surface layer comprises homopolymer polypropylene and 3-5% anti-blocking masterbatch. The polyurethane microsphere masterbatch comprises 41-44 wt% copolymer polypropylene, 53-55 wt% polyurethane microspheres, and 1-6 wt% aromatic polyester polyol grafted polyolefin elastomer. The particle size of the polyurethane microspheres is 5-7 μm.
[0007] The biaxially oriented polypropylene pearlescent film of this invention introduces polar polyurethane microspheres of suitable particle size into the upper surface layer and disperses them uniformly. This allows the polyurethane microspheres to form a uniformly distributed raised structure on the surface of the upper surface after the film is laterally stretched. This raised structure serves two purposes: firstly, it prevents adhesion, making it less likely for the films to stick together when in contact, thus facilitating smooth unwinding; secondly, it effectively adds a polyurethane layer to the upper surface of the film. The uniformly distributed and highly polar polyurethane microsphere raised structure allows the ink printed on the upper surface to spread evenly and bond firmly directly to the film surface without the need for additional corona treatment or primer. Furthermore, controlling the amount of polyurethane microsphere masterbatch added to 30-40 wt% ensures a sufficient number of polyurethane microspheres to be uniformly and densely distributed on the upper surface, which is beneficial for the uniform spreading of subsequent inks.
[0008] Specifically, the polyurethane microsphere masterbatch uses copolymer polypropylene as a carrier, which has good compatibility with the main resin of the upper surface layer, thus helping the polyurethane microspheres in the masterbatch to be better dispersed in the upper surface layer. As the main component of the polyurethane microsphere masterbatch, the polyurethane microspheres ultimately form polyurethane microsphere protrusions on the surface of the upper surface layer, which plays the role of anti-adhesion and acting as a film undercoating layer. The aromatic polyester polyol grafted polyolefin elastomer acts as a compatibilizer between the polyurethane microspheres and the copolymer polypropylene carrier resin. The polyolefin elastomer segment is similarly compatible with the copolymer polypropylene, and the aromatic polyester polyol segment (prepared from the second aromatic polyester polyol) is similarly compatible with the polyurethane microspheres (the raw materials include the first aromatic polyester polyol).
[0009] If the polyurethane microsphere content in the polyurethane microsphere masterbatch is >55wt%, due to the difference in polarity between the microspheres and the copolymer polypropylene, the polyurethane microspheres tend to agglomerate rather than be uniformly dispersed in the carrier. This will prevent them from effectively playing an anti-blocking role in the upper surface layer. If the polyurethane microsphere content in the polyurethane microsphere masterbatch is <53wt%, there may not be a sufficient number of polyurethane microspheres in the upper surface layer, affecting its final anti-blocking effect on the film and its role as a base coating. To achieve a uniform distribution of microspheres on the upper surface of the film to play a base coating role, a large amount of masterbatch needs to be added, which will affect the smoothness of production.
[0010] If the content of aromatic polyester polyol grafted polyolefin elastomer in the polyurethane microsphere masterbatch is <1wt%, the compatibility layer between the polyurethane microspheres and the copolymerized polypropylene carrier resin will be too thin, and some microspheres and copolymerized polypropylene carrier resin will agglomerate, failing to disperse evenly and affecting its anti-blocking and base coating effect. If the content of aromatic polyester polyol grafted polyolefin elastomer in the polyurethane microsphere masterbatch is >6wt%, on the one hand, a separate third phase will be formed in the mixed system, affecting the compatibility between the polyurethane microspheres and copolymerized polypropylene carrier resin. On the other hand, the excess may cause poor film surface appearance and affect the dispersion of polyurethane microspheres in the upper surface of the film, thus failing to achieve the effect of no corona discharge and no base coating.
[0011] Furthermore, this invention specifies that the particle size of the polyurethane microspheres is 5-7 μm. If the particle size of the polyurethane microspheres is <5 μm, the portion of the microspheres exposed on the upper surface is too small, making it difficult to effectively prevent adhesion and spread the ink on the upper surface. If the particle size of the polyurethane microspheres is >7 μm, it will significantly reduce the surface smoothness of the film, resulting in defects such as fisheye spots, and is also prone to forming stress weak points during biaxial stretching, thus causing film breakage. Therefore, selecting a particle size range of 5-7 μm allows the microspheres to protrude from the upper surface of the film, primarily acting as an anti-adhesion agent, while simultaneously promoting and driving the ink to spread on the upper surface through the polarity of the microspheres themselves, ensuring good printability of the film.
[0012] Further, the preparation method of the polyurethane microspheres includes the following steps: preparing an aqueous phase with a dispersant content of 2-4 wt% using deionized water; mixing polyisocyanate and a first aromatic polyester polyol uniformly at a molar ratio of NCO / OH = 1.1, then adding a chain extender at a molar ratio of NCO / NH2 = 10 and stirring rapidly to obtain an oil phase; adding the oil phase dropwise at a uniform rate over 3-5 minutes to the aqueous phase containing the dispersant at a temperature of 60°C at a weight ratio of aqueous phase:oil phase = 3:1, while continuously stirring at a speed of not less than 900 rpm during the dropwise addition; after the dropwise addition is complete, homogenizing the droplets at a high shear rate of 10000-15000 rpm for 30 seconds to refine the droplets, then reducing the speed to 400-600 rpm to maintain suspension, and after crosslinking and curing, filtering out the solid product, washing and drying to obtain the polyurethane microspheres. Preferably, to ensure the thermal stability of the polyurethane microspheres, the first aromatic polyester polyol is selected with a weight-average molecular weight ≥ 4000 g / mol for preparing the polyurethane microspheres.
[0013] Further, the preparation method of the aromatic polyester polyol grafted polyolefin elastomer includes the following steps: maleic anhydride grafted polyolefin elastomer, a second aromatic polyester polyol, and an antioxidant are melt-premixed at 180°C, and a catalyst is added to continue the grafting reaction to obtain the aromatic polyester polyol grafted polyolefin elastomer; the molar ratio of MAH in the maleic anhydride grafted polyolefin elastomer to OH in the second aromatic polyester polyol is 1.2:1, the amount of antioxidant is 0.2~0.4 wt% of the amount of maleic anhydride grafted polyolefin elastomer, and the amount of catalyst is 0.1~0.2 wt% of the amount of maleic anhydride grafted polyolefin elastomer. Preferably, to ensure a certain grafting rate, the second aromatic polyester polyol is selected with a weight-average molecular weight ≤2000 g / mol for preparing the aromatic polyester polyol grafted polyolefin elastomer.
[0014] Furthermore, the preparation method of the polyurethane microsphere masterbatch includes the following steps: adding the copolymer polypropylene, the polyurethane microspheres and the aromatic polyester polyol grafted polyolefin elastomer into a mixer in a certain proportion, mixing them in a mixer at 155~165℃, and then extruding and granulating them through a single screw extruder at 175~185℃ to obtain the polyurethane microsphere masterbatch.
[0015] Furthermore, the maleic anhydride grafting rate in the maleic anhydride-grafted polyolefin elastomer is 0.5-1%, and the number-average molecular weight of the second aromatic polyester polyol is 1800 g / mol, with a hydroxyl mass fraction of 0.15%. The maleic anhydride-grafted polyolefin elastomer is selected from one or more of DuPont N416, Mitsui Chemicals MA8510, and ExxonMobil VA1803, and the second aromatic polyester polyol is selected from BGI CMA-3.
[0016] Furthermore, the melt index of the copolymer polypropylene was measured to be 7~9 g / 10min at 230℃ and 2.16 kg. This specification of copolymer polypropylene can ensure efficient operation of biaxial stretching and is also conducive to better and more uniform mixing of polyurethane microsphere masterbatch in the upper surface layer.
[0017] Furthermore, the particle size of calcium carbonate in the calcium carbonate masterbatch is 1~2μm. If the particle size of calcium carbonate in the calcium carbonate masterbatch is <1μm, on the one hand, it becomes difficult to disperse calcium carbonate in homopolymer polypropylene, and excessive calcium carbonate agglomerates will cause problems such as production difficulties and uneven pearlescent effect of the film. On the other hand, it is difficult to form large-sized cavities, resulting in an unsatisfactory pearlescent effect of the film. If the particle size of calcium carbonate in the calcium carbonate masterbatch is >2μm, stress concentration is easily generated during stretching, leading to film breakage during production. At the same time, excessively large calcium carbonate will also make it difficult to form a uniform cavitation effect in the film, which will lead to large fluctuations in the overall performance of the film.
[0018] Furthermore, the lower surface layer also includes 3-5 wt% anti-blocking masterbatch, wherein the anti-blocking masterbatch uses homopolymer polypropylene as a carrier and the particle size of the anti-blocking agent in the anti-blocking masterbatch is 4-5 μm. The anti-blocking masterbatch includes one or more of Constance AB6018PP and Best ABPP905A.
[0019] This invention also provides a method for preparing any of the above-mentioned biaxially oriented polypropylene pearlescent films, comprising the following steps: mixing each layer of raw materials evenly, metering them with a metering pump, and then extruding them by extruders; after metering, the extruded melt layers are combined into a film sheet at the die head; the film sheet is cooled by a quenching roller and enters a quenching water tank; after passing through a blowing chamber, it is first stretched longitudinally, then stretched laterally; after being shaped, the laterally stretched film is wound up, and then subjected to aging treatment, slitting, and packaging into finished products. In the preparation process of the biaxially oriented polypropylene pearlescent film of this invention, a high surface tension can be obtained on the upper surface of the film used as the printing surface without corona treatment, and no additional corona treatment or base coating is required during subsequent ink printing.
[0020] Furthermore, the extrusion temperature of the upper surface layer is 180~200℃, the extrusion temperature of the lower surface layer is 220~240℃, and the extrusion temperature of the core layer is 220~240℃; the temperature of the chilling roller is 30~50℃, the longitudinal stretching temperature is 130~140℃, the transverse stretching temperature is 150~160℃, and the longitudinal stretching ratio and the transverse stretching ratio are both 4~5 times.
[0021] To better understand and implement this invention, the invention will be described in detail below. Detailed Implementation
[0022] It should be understood that the described embodiments are merely some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of the embodiments of this application.
[0023] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to limit the embodiments of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any or all possible combinations of one or more of the associated listed items.
[0024] The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims. In the description of this application, it should be understood that the terms "first," "second," "third," etc., are used only to distinguish similar objects and are not necessarily used to describe a specific order or sequence, nor should they be construed as indicating or implying relative importance. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0025] Furthermore, in the description of this application, unless otherwise stated, "multiple" means two or more. "And / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A alone, A and B simultaneously, or B alone. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.
[0026] It should be understood that the embodiments of this application are not limited to the precise structures described above, and various modifications and changes can be made without departing from their scope. The scope of the embodiments of this application is limited only by the appended claims.
[0027] This invention provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer arranged sequentially. The upper surface layer comprises copolymer polypropylene and 30-40 wt% polyurethane microsphere masterbatch, with a thickness of 2-3 μm. The core layer comprises homopolymer polypropylene and 20-30 wt% calcium carbonate masterbatch. The lower surface layer comprises homopolymer polypropylene and 3-5% anti-blocking masterbatch. The polyurethane microsphere masterbatch comprises 41-44 wt% copolymer polypropylene, 53-55 wt% polyurethane microspheres, and 1-6 wt% aromatic polyester polyol grafted polyolefin elastomer. The particle size of the polyurethane microspheres is 5-7 μm.
[0028] Further, the preparation method of polyurethane microspheres includes the following steps: preparing an aqueous phase with a dispersant content of 2-4 wt% using deionized water; mixing polyisocyanate and a first aromatic polyester polyol uniformly at a molar ratio of NCO / OH = 1.1, then adding a chain extender at a molar ratio of NCO / NH2 = 10 and stirring rapidly to obtain an oil phase; adding the oil phase dropwise at a weight ratio of water phase: oil phase = 3:1 over 3-5 minutes to the aqueous phase containing the dispersant at a temperature of 60°C and a stirring speed of not less than 900 rpm, then homogenizing the droplets at a high shear rate of 10000-15000 rpm for 30 seconds, then reducing the speed to 400-600 rpm to maintain suspension, and after crosslinking and curing, filtering out the solid product, washing and drying to obtain the polyurethane microspheres.
[0029] Specifically, the polyurethane microsphere preparation method of the embodiments and comparative examples of the present invention includes the following steps: Raw material pretreatment: The first aromatic polyester polyol was dehydrated at 120℃ under vacuum (-0.095MPa) for 2 hours, then cooled to room temperature and protected with N2. The polyisocyanate was stored in a sealed container. Deoxygenation was achieved by bubbling N2 into deionized water for 10 minutes.
[0030] Aqueous phase preparation: Add 2-4 wt% dispersant to deionized water, heat to 40°C, and dissolve completely to obtain the aqueous phase.
[0031] Oil phase preparation: Add the first aromatic polyester polyol to a three-necked flask, stir until dissolved, and purge with nitrogen for 10 minutes to remove oxygen. Add polyisocyanate at a molar ratio of NCO / OH = 1.1:1, stir at 300 rpm for 5 minutes, then add catalyst dropwise at a ratio of 0.2~0.4 wt% of the oil phase, continue stirring for 5 minutes, and then raise the system temperature to 50℃. Quickly add chain extender at a molar ratio of NCO / NH2 = 10:1, continue stirring for 1~2 minutes to obtain the oil phase, and immediately transfer to the dispersion process.
[0032] Suspension and dispersion: First, heat the aqueous phase to 60°C and stir at high speed (at least 900 rpm) to create a vortex. This prevents the oil phase from being excessively sheared due to excessive speed or from being difficult to suspend due to slow speed. The oil phase is added dropwise through a dropping funnel at a uniform rate over 3-5 minutes. After the oil phase is added, switch to high-shear homogenization (10000-15000 rpm, 30 s) to refine the droplets, ensuring that the two monomers can react fully without explosive polymerization. Then, reduce the speed to 400-600 rpm to maintain suspension. This relatively lower speed allows the polymer microspheres to continue growing. If the speed is too low, the microspheres may become too large, while if the speed is too high, the microspheres may not reach the required 5-7 μm size.
[0033] Cross-linking and curing: After maintaining the temperature at 60℃ for 1 hour, the temperature is increased to 90℃ and reacted for 1 hour. A portion of the mixture is filtered and sampled. The particle size of the microspheres is observed and measured under SEM. Once the particle size is confirmed to be within the expected range, the temperature is increased again to 130℃ and reacted for 3 hours to ensure complete cross-linking and curing of the microspheres. Infrared analysis is performed on the sample. The reaction can be stopped once the isocyanate peak disappears. The entire reaction is carried out under N2 protection, and reflux condensation is performed simultaneously to prevent the entry of oxygen and moisture.
[0034] Post-processing: The reaction product was cooled to below 60℃, filtered, washed 2-3 times with hot water, and then washed once with ethanol. It was then vacuum dried at 60℃ for 12 hours, sieved (100 / 200 mesh) to obtain polyurethane microspheres, and then sealed and dried for storage.
[0035] Specifically, in the preparation of the polyurethane microspheres in the embodiments and comparative examples of the present invention, the polyisocyanate used is polymethylene polyphenyl polyisocyanate (PAPI), specifically Wanhua PM-200 (isocyanate mass fraction of 30~32%); the first aromatic polyester polyol used is Huada MX-4028 (hydroxyl mass fraction of 0.14~0.16%, Mw of 4000g / mol); the dispersant used is polyvinyl alcohol (PVA), specifically Wanwei 17-88 (L); the chain extender used is diethyltoluene diamine (DETDA), specifically Yarui Chemical E100; and the catalyst used is dibutyltin dilaurate (DBTDL), specifically Qiguang T-12.
[0036] Specifically, the preparation conditions of the 5μm polyurethane microspheres of the present invention are as follows: high-speed stirring at 900rpm to form a vortex, uniform dripping of the oil phase within 5min, high-shear homogenization at a speed of 15000rpm, and then reduced to 500rpm.
[0037] Specifically, the preparation conditions of the 6μm polyurethane microspheres of the present invention are as follows: high-speed stirring at 900rpm to form a vortex, uniform dripping of the oil phase within 4min, high-shear homogenization at a speed of 12000rpm, and then reduced to 500rpm.
[0038] Specifically, the preparation conditions of the 7μm polyurethane microspheres of the present invention are as follows: high-speed stirring at 900rpm to form a vortex, uniform dripping of the oil phase within 3min, high-shear homogenization at a speed of 10000rpm, and then reduced to 500rpm.
[0039] Structural stability evaluation: (1) High-temperature chemical structural stability: 10 mg of the prepared polyurethane microspheres were placed in a crucible and dried under vacuum at 60 °C for 1 hour. Then, under a nitrogen atmosphere, the microspheres were placed in a thermogravimetric analyzer to test the thermogravimetric curves of the microspheres from room temperature to 210 °C. A weight loss of <0.1% indicates that the chemical structural stability of the prepared polyurethane microspheres under heat meets the standard. (2) 0.5 mg of the prepared polyurethane microspheres were placed on a glass slide and transferred to a hot stage. The process of the microspheres rising from room temperature to 210 °C was observed using an optical microscope. The shape of the prepared polyurethane microspheres did not collapse significantly, and there was no obvious aggregation between the microspheres, indicating that the size and structural stability of the prepared polyurethane microspheres met the standard.
[0040] Testing showed that the microspheres prepared in the embodiments and comparative examples of this invention met the standards for chemical and dimensional structural stability under heating. This result indicates that the polyurethane microspheres prepared in the embodiments and comparative examples of this invention can maintain structural stability at the extrusion temperature (180~200℃) of the upper surface layer. It should also be noted that although the extrusion temperatures of other layers are higher, the stability of the polyurethane microspheres in the upper surface layer is not affected because the extrusion dies of each layer are independent.
[0041] Furthermore, the preparation method of aromatic polyester polyol grafted polyolefin elastomer includes the following steps: maleic anhydride grafted polyolefin elastomer, second aromatic polyester polyol and antioxidant are melt-premixed at 180°C, and then a catalyst is added to continue the grafting reaction to obtain aromatic polyester polyol grafted polyolefin elastomer; the molar ratio of MAH in maleic anhydride grafted polyolefin elastomer to OH in second aromatic polyester polyol is 1.2:1, the amount of antioxidant is 0.2~0.4wt% of the amount of maleic anhydride grafted polyolefin elastomer, and the amount of catalyst is 0.1~0.2wt% of the amount of maleic anhydride grafted polyolefin elastomer.
[0042] Specifically, the preparation method of the aromatic polyester polyol grafted polyolefin elastomer in the embodiments and comparative examples of the present invention includes the following steps: Maleic anhydride-grafted polyolefin elastomer was vacuum dried at 80°C for 8 hours to completely remove moisture. The second aromatic polyester polyol was vacuum dried at 110°C for 4 hours. Antioxidant, dried maleic anhydride-grafted polyolefin elastomer, and a second aromatic polyester polyol were added to a mixer, with the molar ratio of MAH in the maleic anhydride-grafted polyolefin elastomer to OH in the aromatic polyester polyol being 1.2:1. The antioxidant content was 0.2~0.4 wt% of the maleic anhydride-grafted polyolefin elastomer feed amount. The mixer temperature was set to 180℃, the rotor speed to 300 rpm, and the mixture was premixed for 30 min. Then, 0.1~0.2 wt% of catalyst was added, the processing temperature was maintained, the rotor speed was increased to 450 rpm, and the reaction was continued for 30 min. Finally, the mixture was transferred to a single-screw extruder and extruded to granulate, yielding the aromatic polyester polyol-grafted polyolefin elastomer.
[0043] The processing temperature and time selected in this invention ensure that the grafting rate of the second aromatic polyester polyol in the final aromatic polyester polyol-grafted polyolefin elastomer reaches 3%. If the grafting rate is <3%, the polyol content in the system is too low, resulting in insufficient polar functional groups to be compatible with the polyurethane microspheres, leading to poor compatibility. Conversely, when the grafting rate is >4%, the polyol content in the system is too high, resulting in insufficient non-polar functional groups compatible with the copolymerized polypropylene, also leading to poor compatibility.
[0044] Specifically, in the preparation of the aromatic polyester polyol-grafted polyolefin elastomers in the embodiments and comparative examples of the present invention, the maleic anhydride-grafted polyolefin elastomer is DuPont N416; the second aromatic polyester polyol is Huada CMA-3 (hydroxyl mass fraction of 0.14~0.16%, Mw of 1800g / mol); the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], specifically RIANOX1010, used at 0.2wt% of the maleic anhydride-grafted polyolefin elastomer; the catalyst is dibutyltin dilaurate, specifically Qiguang T-12, used at 0.2wt% of the maleic anhydride-grafted polyolefin elastomer.
[0045] Furthermore, the preparation method of polyurethane microsphere masterbatch includes the following steps: adding copolymer polypropylene and polyurethane microsphere aromatic polyester polyol grafted polyolefin elastomer into a continuous internal mixer according to the ratio, mixing them at 155~165℃ and 400rpm, and then extruding them through a single screw extruder at 175~185℃ and water-cooled granulation to obtain polyurethane microsphere masterbatch.
[0046] Further, the maleic anhydride grafting rate in the maleic anhydride-grafted polyolefin elastomer is 0.5-1%, and the number-average molecular weight of the second aromatic polyester polyol is 1800 g / mol, with a hydroxyl mass fraction of 0.15%. The maleic anhydride-grafted polyolefin elastomer is selected from one or more of DuPont N416, Mitsui Chemicals MA8510, and ExxonMobil VA1803. Specifically, the maleic anhydride-grafted polyolefin elastomer is selected from DuPont N416, and the second aromatic polyester polyol is selected from BGI CMA-3.
[0047] Furthermore, the melt index of the copolymer polypropylene was measured to be 7-9 g / 10 min at 230°C and 2.16 kg. The melt index of the copolymer polypropylene in the embodiments and comparative examples of this invention was 8 g / 10 min.
[0048] Furthermore, the calcium carbonate particle size in the calcium carbonate masterbatch is 1~2μm. The calcium carbonate masterbatch used in the embodiments and comparative examples of this invention is Suxing ZG904E.
[0049] Furthermore, the thickness of the lower surface layer is 2~3 μm.
[0050] Furthermore, the lower surface layer also includes 3-5 wt% anti-blocking masterbatch, which uses homopolymer polypropylene as a carrier, and the particle size of the anti-blocking agent in the anti-blocking masterbatch is 4-5 μm. The anti-blocking agent can be silica.
[0051] As a specific implementation method, the anti-blocking masterbatch can be selected from one or more of Constance AB6018PP and Best ABPP905A. In the embodiments and comparative examples of the present invention, Best ABPP905A is used as the anti-blocking masterbatch.
[0052] Furthermore, the melt index of the homopolymer polypropylene was measured to be 2-4 g / 10 min at 230°C and 2.16 kg. The melt index of the homopolymer polypropylene in the embodiments and comparative examples of the present invention was 3 g / 10 min.
[0053] The present invention also provides a method for preparing any of the above-mentioned biaxially oriented polypropylene pearl film, comprising the following steps: mixing each layer of raw materials evenly, metering them with a metering pump, and then extruding them by extruders; after metering with a metering pump, the extruded melt layers are combined into a film sheet at the die head; the film sheet is cooled by a quenching roller and enters a quenching water tank; after passing through a blowing chamber, it is first stretched longitudinally, and then stretched laterally; after being shaped, the film is wound up, and then subjected to aging treatment, slitting, and packaging into finished products.
[0054] Furthermore, the extrusion temperature of the upper surface layer is 180~200℃, the extrusion temperature of the lower surface layer is 220~240℃, and the extrusion temperature of the core layer is 220~240℃; the temperature of the chilling roller is 30~50℃, the longitudinal stretching temperature is 130~140℃, the transverse stretching temperature is 150~160℃, and the longitudinal stretching ratio and the transverse stretching ratio are both 4~5 times.
[0055] The physical properties and testing methods of the embodiments or comparative examples of the present invention are as follows: Membrane surface quality: Five samples from a 50×50cm area of the finished film were randomly selected. The defects such as crystal points, bright spots, and protrusions on the surface were observed by the naked eye. The total number of defects in each sample was recorded, and the average total number was calculated. If the number of defects is less than 5, it is rated as excellent; if the number of defects is less than 10, it is rated as good; if the number of defects is less than 15, it is rated as average; if the number of defects is greater than or equal to 15, it is rated as poor. Interfilm adhesion: According to ISO 4587:2003, two film samples were selected and cut into 25mm pieces. Ten 100mm long strips were prepared, with the top surface containing polyurethane microspheres marked as the main surface and the other side as the secondary surface. Two strips were selected, and the left end of the main surface of one strip and the right end of the secondary surface of the other strip were aligned at a 25° angle. The samples were overlapped with a 25mm area, and the remaining four groups of strips were overlapped in the same way. The overlap positions of all five groups of strips were fixed, and they were placed in an 80℃ oven. After 24 hours, all samples were taken out, and the free ends (i.e., non-overlapping ends) of each group of samples were clamped on a universal testing machine and stretched at a speed of 5mm / min. The maximum load force was recorded. After testing all five groups of data, the average value was calculated. The average value was used as the inter-film adhesion force. This index is used to evaluate whether the polyurethane microspheres have an anti-adhesion effect. The adhesion force is specified as <2N for excellent effect, <3N for good effect, <5N for moderate effect, and ≥5N for poor effect.
[0056] Surface dyne value of the upper surface layer after 12 hours of aging treatment on the master roll: used to evaluate whether the added polyurethane microspheres can effectively eliminate corona discharge and aid ink spreading before printing. A dyne value > 45 is considered acceptable (meaning printing can be performed without corona treatment and primer corona treatment). If the dyne content is ≤45, it is considered unqualified (i.e., corona treatment or primer is required for printing).
[0057] The components and contents of the upper surface layer in the embodiments and comparative examples of the present invention are shown in Table 1 below.
[0058] Table 1
[0059] Example 1 This embodiment provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film in this embodiment includes the following steps: Preparation of the upper surface resin: 70 wt% copolymer polypropylene and 30 wt% polyurethane microsphere masterbatch (44 wt% copolymer polypropylene, 55 wt% polyurethane microspheres, and 1 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 5 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0060] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0061] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0062] The BOPP film preparation method of this embodiment includes the following steps: each layer of raw material is mixed evenly and then metered by a metering pump and then melted and extruded by each extruder. After being metered by the metering pump, the extruded melt layers are combined into a film sheet at the die head. The film sheet is cooled by a chilling roller and enters a chilling water tank. After passing through a blowing chamber, it is first stretched longitudinally and then stretched laterally. After being shaped, the film is wound up, and then subjected to aging treatment, slitting, and packaging into finished products.
[0063] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0064] Example 2 This embodiment provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film in this embodiment includes the following steps: Preparation of the upper surface resin: 65 wt% copolymer polypropylene and 35 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the polyurethane microspheres had a particle size of 6 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%. Preparation of the core layer resin: 80 wt% homopolymer polypropylene and 20 wt% ZG904E were mixed evenly to obtain the core layer resin.
[0065] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0066] The preparation method of the biaxially oriented polypropylene pearl film in this embodiment is the same as that in Example 1, so it will not be described again.
[0067] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0068] Example 3 This embodiment provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film in this embodiment includes the following steps: Preparation of the upper surface resin: 60 wt% copolymer polypropylene and 40 wt% polyurethane microsphere masterbatch (41 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 6 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the polyurethane microspheres had a particle size of 7 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%. Preparation of the core layer resin: 80 wt% homopolymer polypropylene and 20 wt% ZG904E were mixed evenly to obtain the core layer resin.
[0069] Preparation of the lower surface resin: 95 wt% homopolymer polypropylene and 5 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0070] The preparation method of the biaxially oriented polypropylene pearl film in this embodiment is the same as that in Example 1, so it will not be described again.
[0071] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0072] Example 4 This embodiment provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film in this embodiment includes the following steps: Preparation of the upper surface resin: 70 wt% copolymer polypropylene and 30 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the polyurethane microspheres had a particle size of 6 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%. Preparation of the core layer resin: 70 wt% homopolymer polypropylene and 30 wt% ZG904E were mixed evenly to obtain the core layer resin.
[0073] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0074] The preparation method of the biaxially oriented polypropylene pearl film in this embodiment is the same as that in Example 1, so it will not be described again.
[0075] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0076] Comparative Example 1 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 40 wt% copolymer polypropylene and 60 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 6 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0077] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0078] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0079] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0080] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0081] Comparative Example 2 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 90 wt% copolymer polypropylene and 10 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 6 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0082] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0083] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0084] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0085] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0086] Comparative Example 3 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 60 wt% copolymer polypropylene and 40 wt% polyurethane microsphere masterbatch (47 wt% copolymer polypropylene, 53 wt% polyurethane microspheres) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 6 μm.
[0087] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0088] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0089] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0090] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0091] Comparative Example 4 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 60 wt% copolymer polypropylene and 40 wt% polyurethane microsphere masterbatch (37 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 10 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 6 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0092] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0093] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0094] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0095] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0096] Comparative Example 5 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 65 wt% copolymer polypropylene and 35 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 3 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0097] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0098] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0099] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0100] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0101] Comparative Example 6 This comparative example provides a biaxially oriented polypropylene pearlescent film, comprising an upper surface layer, a core layer, and a lower surface layer sequentially disposed therefrom. The preparation method of each resin layer of the biaxially oriented polypropylene pearlescent film of this comparative example includes the following steps: Preparation of the upper surface resin: 65 wt% copolymer polypropylene and 35 wt% polyurethane microsphere masterbatch (43 wt% copolymer polypropylene, 53 wt% polyurethane microspheres, and 4 wt% aromatic polyester polyol grafted polyolefin elastomer) were mixed evenly to obtain the upper surface resin; the particle size of the polyurethane microspheres was 10 μm, and the grafting rate of the second aromatic polyester polyol in the aromatic polyester polyol grafted polyolefin elastomer was 3%.
[0102] Core layer resin preparation: 80 wt% homopolymer polypropylene and 20 wt% ZG904E are mixed evenly to obtain the core layer resin.
[0103] Preparation of the lower surface resin: 97 wt% homopolymer polypropylene and 3 wt% ABPP905A were mixed evenly to obtain the lower surface resin.
[0104] The preparation method of the biaxially oriented polypropylene pearl film in this comparative example is the same as that in Example 1, so it will not be described again.
[0105] The total thickness of the film is 44µm, with the upper surface layer being 2µm thick and the lower surface layer being 2µm thick.
[0106] The performance test results of the biaxially oriented polypropylene pearl films of Examples 1-4 and Comparative Examples 1-6 are shown in Table 2 below.
[0107] Table 2
[0108] Compared with Example 2, the amount of polyurethane microsphere masterbatch added to the upper surface layer of Comparative Example 1 was too high, resulting in an excessively high content of polyurethane microspheres in the upper surface layer, which tended to agglomerate and had excessive adhesion between films. Consequently, it could not effectively play an anti-adhesion role in the upper surface layer, and the film surface quality was poor.
[0109] Compared with Example 2, the amount of polyurethane microsphere masterbatch in the upper surface layer of Comparative Example 2 is too low, and the number of protrusions on the surface of the upper surface layer is too small. As a result, the anti-blocking effect and the base coating effect are relatively limited. Therefore, the adhesion between the films is too large, the anti-blocking effect is not good, and the surface dyne value is small, so it is impossible to achieve corona-free and base coating-free treatment during printing.
[0110] Compared with Example 3, the polyurethane microsphere masterbatch added to the upper surface layer of Comparative Example 3 did not contain aromatic polyester polyol grafted polyolefin elastomer during preparation. As a result, the polyurethane microspheres could not be uniformly dispersed in the copolymer polypropylene, and agglomeration occurred. The adhesion between the films was too large, and thus they could not play an effective role in the upper surface layer. Therefore, the film quality was poor and the surface dyne value was small, and corona-free and primer-free treatment could not be achieved during printing.
[0111] Compared with Example 3, the content of aromatic polyester polyol grafted polyolefin elastomer in the polyurethane microsphere masterbatch added to the upper surface of Comparative Example 4 is too high. The aromatic polyester polyol grafted polyolefin elastomer in the polyurethane microsphere masterbatch forms an independent third phase and partially migrates to the surface of the upper surface, affecting the compatibility between polyurethane microspheres and copolymer polypropylene. In addition, it also affects the dispersion of polyurethane microspheres on the film surface. Therefore, the adhesion between films is too large, the film surface quality is poor, and the surface dyne value is small, making it impossible to achieve corona-free and primer-free treatment during printing.
[0112] Compared with Example 2, the polyurethane microspheres in the polyurethane microsphere masterbatch added to the upper surface of Comparative Example 5 have too small a particle size and too little of the polyurethane microspheres are exposed on the upper surface. Therefore, the adhesion between the films is too large and the surface dyne value is small, making it difficult to play the role of anti-blocking and promoting the smoothing of ink on the upper surface.
[0113] Compared with Example 2, the polyurethane microspheres in the polyurethane microsphere masterbatch added to the upper surface of Comparative Example 6 have excessively large particle sizes, resulting in too much of the polyurethane microspheres being exposed on the upper surface. This reduces the surface smoothness of the upper surface, causing fish-eye crystal points and film breakage. Consequently, the film quality is poor, and the surface dyne value is too small, making it impossible to achieve corona-free and primer-free treatment during printing.
[0114] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and the present invention also intends to include these modifications and variations.
Claims
1. A biaxially oriented polypropylene pearlescent film, characterized in that, The material comprises an upper surface layer, a core layer, and a lower surface layer arranged sequentially. The upper surface layer comprises copolymer polypropylene and 30-40 wt% polyurethane microsphere masterbatch, and the thickness of the upper surface layer is 2-3 μm. The core layer comprises homopolymer polypropylene and 20-30 wt% calcium carbonate masterbatch. The lower surface layer comprises homopolymer polypropylene and 3-5% anti-blocking masterbatch. The polyurethane microsphere masterbatch comprises 41-44 wt% copolymer polypropylene, 53-55 wt% polyurethane microspheres, and 1-6 wt% aromatic polyester polyol grafted polyolefin elastomer. The particle size of the polyurethane microspheres is 5-7 μm.
2. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The preparation method of the polyurethane microspheres includes the following steps: preparing an aqueous phase with a dispersant content of 2-4 wt% using deionized water; mixing polyisocyanate and a first aromatic polyester polyol uniformly at a molar ratio of NCO / OH = 1.1, then adding a chain extender at a molar ratio of NCO / NH2 = 10 and stirring rapidly to obtain an oil phase; adding the oil phase dropwise at a uniform rate over 3-5 minutes to the aqueous phase containing the dispersant at a temperature of 60°C at a weight ratio of aqueous phase:oil phase = 3:1, while continuously stirring at a speed of not less than 900 rpm during the dropwise addition; after the dropwise addition is completed, homogenizing the droplets at a high shear rate of 10000-15000 rpm for 30 seconds to refine the droplets, then reducing the speed to 400-600 rpm to maintain suspension, and after cross-linking and curing, filtering out the solid product, washing and drying to obtain the polyurethane microspheres.
3. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The preparation method of the aromatic polyester polyol grafted polyolefin elastomer includes the following steps: maleic anhydride grafted polyolefin elastomer, a second aromatic polyester polyol and an antioxidant are melt-premixed at 180°C, and a catalyst is added to continue the grafting reaction to obtain the aromatic polyester polyol grafted polyolefin elastomer; the molar ratio of MAH in the maleic anhydride grafted polyolefin elastomer to OH in the second aromatic polyester polyol is 1.2:1, the amount of antioxidant is 0.2~0.4wt% of the amount of maleic anhydride grafted polyolefin elastomer, and the amount of catalyst is 0.1~0.2wt% of the amount of maleic anhydride grafted polyolefin elastomer.
4. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The preparation method of the polyurethane microsphere masterbatch includes the following steps: adding the copolymer polypropylene, the polyurethane microspheres and the aromatic polyester polyol grafted polyolefin elastomer into a mixer in a certain proportion, mixing them in a mixer at 155~165℃, and then extruding and granulating them through a single screw extruder at 175~185℃ to obtain the polyurethane microsphere masterbatch.
5. The biaxially oriented polypropylene pearlescent film according to claim 3, characterized in that, The maleic anhydride grafting rate in the maleic anhydride-grafted polyolefin elastomer is 0.5-1%, and the number average molecular weight of the second aromatic polyester polyol is 1800 g / mol, with a hydroxyl mass fraction of 0.15%.
6. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The melt index of the copolymer polypropylene was measured to be 7~9 g / 10min at 230℃ and 2.16 kg.
7. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The calcium carbonate masterbatch has a particle size of 1~2μm.
8. The biaxially oriented polypropylene pearlescent film according to claim 1, characterized in that, The lower surface layer also includes 3-5 wt% anti-blocking masterbatch.
9. A method for preparing a biaxially oriented polypropylene pearlescent film as described in any one of claims 1 to 8, characterized in that, The process includes the following steps: each layer of raw material is mixed evenly and then metered by a metering pump and fed into each extruder for melting and extrusion. The extruded melt layers are combined into a thin film at the die head. The film is cooled by a chilling roller and enters a chilling water tank. After passing through a blowing chamber, it is first stretched longitudinally and then stretched laterally. The film after being stretched laterally is shaped and then wound up. Finally, it undergoes aging treatment, slitting, and packaging into finished products.
10. The method for preparing biaxially oriented polypropylene pearlescent film according to claim 9, characterized in that, The extrusion temperature of the upper surface layer is 180~200℃, the extrusion temperature of the lower surface layer is 220~240℃, and the extrusion temperature of the core layer is 220~240℃; the temperature of the chilling roller is 30~50℃, the longitudinal stretching temperature is 130~140℃, the transverse stretching temperature is 150~160℃, and the longitudinal stretching ratio and the transverse stretching ratio are both 4~5 times.