A multilayer co-extruded degradable composite film, its preparation method and application

By employing a five-layer structure design and chemical bonding technology, the problems of poor interlayer bonding strength and uncontrollable degradation rate in biodegradable plastic films have been solved, achieving high barrier performance and stable degradation, making it suitable for packaging materials and agricultural mulch films.

CN123104202APending Publication Date: 2026-11-17ANHUI YINGKE NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611301570.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing biodegradable plastic films suffer from a tradeoff between mechanical properties and degradation performance, poor interlayer bonding strength, insufficient barrier properties, uncontrollable degradation rate, and the tendency for multilayer co-extruded films to delaminate.

Method used

The device employs a five-layer structure design. The outer layer is composed of polylactic acid and modified montmorillonite, while the core layer consists of polybutylene succinate and modified montmorillonite. Polybutylene adipate/terephthalate is grafted with glycidyl methacrylate to form chemical bonds with polybutylene succinate. The inner layer is composed of polybutylene adipate/terephthalate and polycaprolactone. Degradation promoters are added to control the degradation rate.

Benefits of technology

A multilayer co-extruded degradable composite film with high interlayer bonding strength, outstanding barrier performance, controllable degradation rate, and good mechanical properties has been achieved, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses a multilayer co-extruded degradable composite film, its preparation method, and its application, relating to the field of degradable composite film technology. The multilayer co-extruded degradable composite film provided by this application achieves a balance between interlayer bonding strength, barrier properties, and degradation performance; a balance between stable performance during use and rapid degradation after disposal; and a balance between mechanical properties and degradation performance. It solves common industry problems such as easy delamination between layers, poor montmorillonite dispersion, and uncontrollable degradation initiation in existing degradable polyester multilayer co-extruded films. The product exhibits high interlayer bonding strength, good oxygen and water vapor barrier properties, controllable degradation induction period, stable mechanical properties, and a controllable preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of biodegradable composite film technology, and in particular to a multilayer co-extruded biodegradable composite film, its preparation method, and its application. Background Technology

[0002] Biodegradable plastic films have received widespread attention in recent years as an important alternative to traditional non-biodegradable plastics. Currently, commercially available biodegradable film materials mainly include starch-based plastics, polylactic acid, polybutylene adipate / terephthalate copolymer, and polybutylene succinate, among other biodegradable resins. These general-purpose biodegradable materials are predominantly ester-bonded in their molecular structure and can be hydrolyzed or degraded by microorganisms. However, from a material property perspective, they generally suffer from the difficulty of simultaneously achieving both mechanical and degradation performance. Furthermore, the oxygen and water vapor barrier properties of these biodegradable resins are generally lower than those of traditional high-barrier materials such as polyolefins and ethylene-vinyl alcohol copolymers, limiting their application in packaging and agricultural films where a certain shelf life is required.

[0003] To address the performance deficiencies of single biodegradable resins, current technologies often employ multilayer co-extrusion to combine different materials, aiming to integrate functions such as mechanical support, barrier properties, and heat sealing. However, commonly used multilayer co-extruded biodegradable films still suffer from several drawbacks. Firstly, significant polarity differences between different biodegradable resins lead to weak interlayer bonding, resulting in easy delamination after co-extrusion. Secondly, conventionally added layered fillers, such as montmorillonite, often exhibit poor dispersibility in the resin matrix without effective organic treatment, making it difficult to form effective barrier pathways. Thirdly, current methods for controlling degradation rates largely rely on the resin's molecular structure or the addition of common degradation aids, lacking effective control over degradation initiation time and rate.

[0004] To address the aforementioned technical shortcomings, there is an urgent need to improve existing technologies. Summary of the Invention

[0005] In view of this, this application provides a multilayer co-extruded degradable composite film, its preparation method and application. The multilayer co-extruded degradable composite film achieves a balance of high interlayer bonding strength, outstanding barrier performance and controllable degradation rate, solving common industry problems such as interlayer delamination, poor montmorillonite dispersion and uncontrollable degradation start-up time of existing biodegradable polyester multilayer co-extruded films. The product has good mechanical properties, barrier performance and degradation regulation ability, and the preparation process is controllable and suitable for large-scale production.

[0006] In the first aspect, this application provides a multilayer co-extruded degradable composite film, the technical solution of which is as follows:

[0007] A multilayer co-extruded degradable composite film includes an outer layer, a first adhesive layer, a core layer, a second adhesive layer, and an inner layer arranged sequentially.

[0008] The outer layer, by mass parts, comprises the following raw materials: 60-80 parts of polylactic acid, 20-40 parts of poly(butylene adipate / terephthalate) copolymer, 0.5-2 parts of modified montmorillonite, 0.3-1 parts of styrene-acrylate copolymer, and 0.5-1 parts of tributyl citrate.

[0009] The first adhesive layer and the second adhesive layer, by mass parts, each independently comprise the following raw materials: 70-90 parts of glycidyl methacrylate grafted poly(butylene adipate / terephthalate), and 10-30 parts of polybutylene succinate.

[0010] The core layer, by mass parts, comprises the following raw materials: 55-75 parts of polybutylene succinate, 10-25 parts of polycaprolactone, 3-8 parts of modified montmorillonite, 2-8 parts of degradation accelerator, and 2-5 parts of tributyl citrate.

[0011] The inner layer, by mass parts, comprises the following raw materials: 70-90 parts of poly(butylene adipate / terephthalate) copolymer, 10-30 parts of polycaprolactone, and 0.5-1 parts of silica.

[0012] Optionally, the outer layer has a thickness of 8~20μm, the first adhesive layer and the second adhesive layer each have a thickness of 3~10μm, the core layer has a thickness of 12~40μm, and the inner layer has a thickness of 8~20μm.

[0013] Optionally, the preparation method of the glycidyl methacrylate grafted poly(adipate / butylene terephthalate) includes the following steps:

[0014] Poly(butylene adipate) / butylene terephthalate copolymer, glycidyl methacrylate and benzoyl peroxide are mixed and stirred to obtain a premix.

[0015] The premixed material is subjected to melt reaction extrusion and then vacuum devolatilization to obtain the glycidyl methacrylate-grafted poly(adipate / butylene terephthalate).

[0016] Optionally, the mass ratio of the poly(adipic acid / butylene terephthalate) copolymer, glycidyl methacrylate, and benzoyl peroxide is 1:0.01~0.05:0.001~0.005.

[0017] Optionally, the stirring speed is 300~500 r / min, the temperature is 25~40℃, and the time is 10~20 min.

[0018] Optionally, the melt reactive extrusion is carried out in a twin-screw extruder with a length-to-diameter ratio ≥40, a zone temperature of 140~170℃, and a screw speed of 50~150 r / min.

[0019] Optionally, the vacuum degree of the vacuum devolatilization treatment is -0.06 to -0.09 MPa, the temperature is 140 to 170°C, and the time is 1 to 5 min.

[0020] Optionally, the method for preparing the degradation promoter includes the following steps:

[0021] Modified malic acid was obtained by mixing malic acid, aqueous ethanol solution and γ-aminopropyltriethoxysilane and stirring the mixture.

[0022] The modified malic acid and polyvinyl alcohol aqueous solution were mixed and stirred to obtain the degradation promoter.

[0023] Optionally, the mass-to-volume ratio of malic acid, aqueous ethanol solution, and γ-aminopropyltriethoxysilane is 1 g: (5~15) mL: (0.05~0.2) g, and the volume concentration of the aqueous ethanol solution is 20%~50%.

[0024] Optionally, the stirring reaction is carried out at a speed of 200-400 r / min, a temperature of 40-60℃, and a time of 1-3 h.

[0025] Optionally, the mass-to-volume ratio of the modified malic acid and the polyvinyl alcohol aqueous solution is 1 g: (10~30) mL, and the mass concentration of the polyvinyl alcohol aqueous solution is 5%~15%.

[0026] Optionally, the stirring speed is 200~400 r / min, the temperature is 60~80℃, and the time is 30~60 min.

[0027] Optionally, the preparation method of the modified montmorillonite includes the following steps:

[0028] Sodium-based montmorillonite and water were mixed and stirred to obtain a montmorillonite suspension.

[0029] The montmorillonite suspension and octadecyltrimethylammonium chloride were mixed and stirred to obtain the modified montmorillonite.

[0030] Optionally, the mass-to-volume ratio of the sodium-based montmorillonite to water is 1 g: (20~100) mL.

[0031] Optionally, the stirring speed is 200~400 r / min, the temperature is 25~40℃, and the time is 10~30 min.

[0032] Optionally, the mass-to-volume ratio of the montmorillonite suspension to octadecyltrimethylammonium chloride is 1 mL: (0.002~0.03) g.

[0033] Optionally, the stirring reaction is carried out at a speed of 200-400 r / min, a temperature of 60-90℃, and a time of 2-6 h.

[0034] Secondly, this application provides a method for preparing the multilayer co-extruded degradable composite film described in the foregoing scheme, comprising the following steps:

[0035] After mixing polylactic acid, poly(butylene adipate / terephthalate) copolymer, modified montmorillonite, styrene-acrylate copolymer and tributyl citrate, the mixture is subjected to a first stirring treatment to obtain the outer layer premix.

[0036] After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a second stirring treatment is performed to obtain the first adhesive layer premix.

[0037] After mixing polybutylene succinate, polycaprolactone, modified montmorillonite, degradation accelerator and tributyl citrate, a third stirring treatment is carried out to obtain the core layer premix.

[0038] After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a fourth stirring treatment is performed to obtain the second adhesive layer premix.

[0039] After mixing poly(adipate) / butylene terephthalate copolymer, polycaprolactone and silica, a fifth stirring treatment is performed to obtain the inner layer premix.

[0040] The outer layer premix, the first adhesive layer premix, the core layer premix, the second adhesive layer premix, and the inner layer premix are melted and plasticized by five single-screw extruders, and then merged by five co-extrusion dies to form a five-layer melt. The melt is then cast to form a multi-layer co-extruded degradable composite film.

[0041] Optionally, the first stirring treatment is performed at a speed of 300~500 r / min, a temperature of 25~40℃, and a time of 5~10 min.

[0042] Optionally, the second stirring treatment is performed at a speed of 300-500 r / min, a temperature of 25-40℃, and a time of 5-10 min.

[0043] Optionally, the third stirring treatment is performed at a speed of 300-500 r / min, a temperature of 25-40℃, and a time of 5-10 min.

[0044] Optionally, the fourth stirring treatment has a rotation speed of 300~500 r / min, a temperature of 25~40℃, and a time of 5~10 min.

[0045] Optionally, the fifth stirring process is carried out at a speed of 300-500 r / min, a temperature of 25-40℃, and a time of 5-10 min.

[0046] Optionally, the outer layer corresponds to a temperature of 165~200℃ in each zone of the extruder, and a screw speed of 15~30 r / min.

[0047] Optionally, the temperatures of each zone of the extruder corresponding to the first adhesive layer and the second adhesive layer are 155~185℃, and the screw speed is 15~30r / min.

[0048] Optionally, the core layer corresponds to a temperature of 150~190℃ in each zone of the extruder, and a screw speed of 15~30r / min.

[0049] Optionally, the inner layer corresponds to a temperature of 150~180℃ in each zone of the extruder, and a screw speed of 15~30r / min.

[0050] Optionally, the temperature of the cooling roller for casting is 15~30℃.

[0051] Thirdly, this application provides the application of the multilayer co-extruded degradable composite film described in the aforementioned scheme in packaging materials or agricultural mulch films.

[0052] The multilayer co-extruded degradable composite membrane provided in this application achieves a synergistic improvement in interlayer bonding strength, barrier properties, and degradation performance through a five-layer structural design and functional division of labor among the layers. Compared with existing technologies, this multilayer co-extruded degradable composite membrane features high interlayer bonding strength, good oxygen and water vapor barrier properties, controllable degradation induction period, and stable mechanical properties. Furthermore, the preparation process is simple, and all raw materials for each layer are conventional degradable materials, demonstrating good feasibility and industrial application prospects. Detailed Implementation

[0053] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, it should be understood that the specific implementation methods described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0054] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish an order.

[0055] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0056] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0057] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0058] In the first aspect, this application provides a multilayer co-extruded degradable composite film, the technical solution of which is as follows:

[0059] A multilayer co-extruded degradable composite film includes an outer layer, a first adhesive layer, a core layer, a second adhesive layer, and an inner layer arranged sequentially.

[0060] The outer layer, by mass parts, comprises the following raw materials: 60-80 parts of polylactic acid, 20-40 parts of poly(butylene adipate / terephthalate) copolymer, 0.5-2 parts of modified montmorillonite, 0.3-1 parts of styrene-acrylate copolymer, and 0.5-1 parts of tributyl citrate.

[0061] The first adhesive layer and the second adhesive layer, by mass parts, each independently comprise the following raw materials: 70-90 parts of glycidyl methacrylate grafted poly(butylene adipate / terephthalate), and 10-30 parts of polybutylene succinate.

[0062] The core layer, by mass parts, comprises the following raw materials: 55-75 parts of polybutylene succinate, 10-25 parts of polycaprolactone, 3-8 parts of modified montmorillonite, 2-8 parts of degradation accelerator, and 2-5 parts of tributyl citrate.

[0063] The inner layer, by mass parts, comprises the following raw materials: 70-90 parts of poly(butylene adipate / terephthalate) copolymer, 10-30 parts of polycaprolactone, and 0.5-1 parts of silica.

[0064] This application uses polylactic acid (PLA) and polybutylene adipate / terephthalate (PET) copolymer to form the outer layer bimatrix system. PLA serves as the main rigid component, providing the outer layer with the required stiffness, heat resistance, and printability. PET copolymer acts as the toughening component; its flexible molecular chains effectively absorb and dissipate stress concentration under external forces, improving the outer layer's flexibility and impact resistance. Both components have similar processing temperature windows in the molten state, ensuring uniform blending and interlayer co-extrusion stability, while also considering the outer layer's strength, toughness, and heat-sealing adaptability. Modified montmorillonite is added to the outer layer, utilizing its layered structure to block gas molecules and ensure that the outer layer has a certain ability to block oxygen and water vapor. Styrene-acrylate copolymers are used as chain extenders. Their molecular chains contain epoxy functional groups, which can react with the terminal carboxyl and terminal hydroxyl groups of polylactic acid and poly(butylene adipate / terephthalate) copolymers to improve the melt strength and molecular weight of the outer layer resin and improve film stability. Tributyl citrate is used as a plasticizer to improve the processing fluidity and flexibility of polylactic acid and reduce the risk of thermal degradation at processing temperatures.

[0065] This application uses glycidyl methacrylate grafted with polybutylene adipate / terephthalate (PBAT-g-GMA) and polybutylene succinate to form the first and second adhesive layers. The main chain of the glycidyl methacrylate-grafted polybutylene adipate / terephthalate is polybutylene adipate / terephthalate, and its side chains contain epoxy groups. During the five-layer co-extrusion process, these epoxy groups can react in situ with the terminal carboxyl and hydroxyl groups of the polyester in adjacent outer and core layers, generating graft copolymers at the layer interfaces and improving interlayer peel strength. Polybutylene succinate, as an auxiliary component, has a melt viscosity close to that of the main component, which can adjust the flowability and processing window of the adhesive layer, ensuring that the adhesive layer can be uniformly spread between adjacent layers during co-extrusion, forming a continuous and uniform adhesive interface. This adhesive layer design enables chemical bonding between the outer layer, core layer, and inner layer, rather than simple physical adhesion, fundamentally solving the problems of poor compatibility and easy delamination between different biodegradable polyesters.

[0066] This application uses polybutylene succinate (PBS) and polycaprolactone (PCL) as the core layer matrix system. PBS is the main matrix resin of the core layer, possessing good mechanical and degradation properties. PCL, as a flexible component, imparts good flexibility and film-forming properties to the core layer. Simultaneously, PCL degrades rapidly, which is beneficial for the overall degradation of the membrane after disposal. Modified montmorillonite is added to the core layer. Utilizing its high aspect ratio after organic intercalation and good dispersibility in the matrix, it forms a layered, tortuous barrier path within the core layer, extending the diffusion distance of gas and water vapor molecules and reducing oxygen and water vapor permeability. A degradation promoter is added to the core layer. This promoter remains stable during membrane use, preventing premature release. When the membrane is disposed of and enters the degradation environment, the microcapsule wall material gradually ruptures under the action of the medium, releasing the degradation promoter, promoting the hydrolysis of polyester molecular chains, and achieving timed initiation and self-acceleration of the degradation rate. The degradation accelerator works synergistically with tributyl citrate. Tributyl citrate is both a plasticizer and has a certain degree of acidity, which can help promote the hydrolysis of the core polyester.

[0067] This application uses a poly(butylene adipate) / butylene terephthalate copolymer and polycaprolactone to form the inner layer matrix system. The poly(butylene adipate) / butylene terephthalate copolymer provides the required heat-sealing performance and flexibility of the inner layer, while polycaprolactone further improves the flexibility and degradation performance of the inner layer. Silica is added to the inner layer as an opening agent to prevent film sticking during winding and use, while silica also improves the slip properties and processing stability of the inner layer surface.

[0068] The five-layer structure of this application provides mechanical support and printing load through the outer layer, the first and second adhesive layers provide interlayer chemical bonding, the core layer performs dual functions of barrier and degradation regulation, and the inner layer provides heat-sealing performance, thus achieving a reasonable division of labor and synergy among the functions of each layer. The outer and inner layers are respectively disposed on both sides of the core layer, and the adhesive layer is located between each functional layer, ensuring the overall symmetry of the composite film structure and avoiding warping deformation caused by differences in the shrinkage rates of each layer.

[0069] Optionally, the outer layer has a thickness of 8-20 μm, the first adhesive layer and the second adhesive layer each have a thickness of 3-10 μm, the core layer has a thickness of 12-40 μm, and the inner layer has a thickness of 8-20 μm. This thickness distribution ensures that the core layer, as a functional layer, has sufficient thickness to achieve barrier and degradation regulation functions. The adhesive layer has a moderate thickness, providing enough epoxy groups to participate in the interfacial reaction, without being too thick and causing excessive interlayer adhesion that would affect the overall flexibility of the film. The matching thickness of the outer and inner layers ensures the mechanical symmetry and processing stability of the film.

[0070] In some embodiments, the preparation method of the glycidyl methacrylate-grafted poly(butylene adipate) / terephthalate (PBAT-g-GMA) includes the following steps:

[0071] Poly(butylene adipate) / butylene terephthalate copolymer, glycidyl methacrylate and benzoyl peroxide are mixed and stirred to obtain a premix.

[0072] The premixed material is subjected to melt reaction extrusion and then vacuum devolatilization to obtain the glycidyl methacrylate grafted poly(adipate adipate / butylene terephthalate) (PBAT-g-GMA).

[0073] This preparation method involves mixing followed by reactive extrusion to uniformly adsorb glycidyl methacrylate and benzoyl peroxide onto the surface of poly(adipate adipate / butylene terephthalate) copolymer particles. Melt reactive extrusion is then performed in a twin-screw extruder, where benzoyl peroxide decomposes upon heating to generate free radicals, initiating a grafting reaction between glycidyl methacrylate and poly(adipate adipate / butylene terephthalate) molecular chains, introducing epoxy functional groups into the side chains of the matrix resin. Vacuum devolatilization removes unreacted glycidyl methacrylate monomers, preventing residual monomers from causing adverse effects during subsequent film processing and use.

[0074] In some embodiments, the mass ratio of the poly(butylene adipate / terephthalate) copolymer, glycidyl methacrylate, and benzoyl peroxide is 1:0.01~0.05:0.001~0.005. This ratio ensures grafting reaction efficiency and grafting rate. If the amount of glycidyl methacrylate is too low, the grafting rate will be insufficient; if the amount is too high, homopolymerization may occur and the residual monomer content will increase. Benzoyl peroxide, as an initiator, is used at a low level to ensure the initiation reaction while avoiding excessive degradation of the matrix resin.

[0075] In some embodiments, the stirring speed is 300-500 r / min, the temperature is 25-40℃, and the time is 10-20 min. These stirring conditions ensure that glycidyl methacrylate and benzoyl peroxide are fully dispersed on the surface of the poly(adipate) / butylene terephthalate copolymer particles, and the moderate temperature prevents premature decomposition of the peroxide and self-polymerization of glycidyl methacrylate.

[0076] In some embodiments, the melt reactive extrusion is carried out in a twin-screw extruder with an aspect ratio ≥40, a zone temperature of 140~170°C, and a screw speed of 50~150 r / min. The twin-screw extruder provides strong shear mixing and self-cleaning capabilities, and the aspect ratio ≥40 ensures sufficient reaction residence time. The zone temperature is set above the decomposition temperature of benzoyl peroxide but below the boiling point of glycidyl methacrylate, allowing the initiator to continuously decompose and initiate the grafting reaction, while avoiding excessively high temperatures that could lead to material degradation.

[0077] In some embodiments, the vacuum devolatilization process is performed at a vacuum level of -0.06 to -0.09 MPa, a temperature of 140 to 170°C, and a time of 1 to 5 minutes. Vacuum devolatilization is carried out in the later stage of the extruder, where unreacted monomers and low-molecular-weight volatiles are released from the melt through negative pressure. The temperature is maintained near the reaction temperature, and the time is less than 5 minutes to avoid prolonged thermal degradation of the material.

[0078] In some embodiments, the method for preparing the degradation promoter includes the following steps:

[0079] Modified malic acid was obtained by mixing malic acid, aqueous ethanol solution and γ-aminopropyltriethoxysilane and stirring the mixture.

[0080] The modified malic acid and polyvinyl alcohol aqueous solution were mixed and stirred to obtain the degradation promoter.

[0081] This preparation method yields a coated degradation accelerator through a two-step process. First, malic acid is modified with γ-aminopropyltriethoxysilane. After hydrolysis, the γ-aminopropyltriethoxysilane reacts with the carboxyl groups of malic acid, introducing an organosilicon layer onto the surface of the malic acid, thus enhancing its interfacial bonding with the polyvinyl alcohol (PVA) shell. Then, the modified malic acid is mixed with an aqueous PVA solution. Under stirring, the PVA coats the surface of the modified malic acid, forming a microcapsule shell. This microcapsule structure ensures the stability of the degradation accelerator during co-extrusion processing, preventing premature release.

[0082] In some embodiments, the mass-to-volume ratio of malic acid, aqueous ethanol solution, and γ-aminopropyltriethoxysilane is 1 g : (5~15) mL : (0.05~0.2) g, and the volume concentration of the aqueous ethanol solution is 20%~50%. This ratio ensures that γ-aminopropyltriethoxysilane forms a suitable silane-modified layer on the surface of malic acid. The aqueous ethanol solution serves as a dispersion medium, and a volume concentration of 20%~50% is beneficial for silane hydrolysis and sufficient contact with malic acid. If the concentration is too high, silane hydrolysis will be insufficient; if the concentration is too low, the loss of malic acid due to dissolution will increase.

[0083] In some embodiments, the stirring speed is 200-400 r / min, the temperature is 40-60°C, and the time is 1-3 h. These reaction conditions are carried out at a mild temperature, allowing the silane coupling agent to complete hydrolysis and condensation and react with malic acid. If the temperature is too low, the reaction rate is slow; if the temperature is too high, the silane self-condensation intensifies, and the time is insufficient to form a uniform modified layer.

[0084] In some embodiments, the mass-to-volume ratio of the modified malic acid to the polyvinyl alcohol aqueous solution is 1 g: (10~30) mL, and the mass concentration of the polyvinyl alcohol aqueous solution is 5%~15%. This ratio ensures that the polyvinyl alcohol forms a coating layer of appropriate thickness on the surface of the modified malic acid. The polyvinyl alcohol aqueous solution with a mass concentration of 5%~15% has a suitable viscosity, which is beneficial to the uniformity of coating. If the concentration is too low, the coating will be incomplete; if the concentration is too high, the solution viscosity will be too high, the coating layer will be too thick, and particle adhesion will easily occur.

[0085] In some embodiments, the stirring speed is 200~400 r / min, the temperature is 60~80℃, and the time is 30~60 min. Under these stirring conditions, the viscosity of the polyvinyl alcohol aqueous solution decreases with auxiliary heating, which is beneficial for its uniform coating on the modified malic acid surface. If the temperature is too high, the water evaporates too quickly, and the coating layer is prone to defects. If the time is too long, the coating layer tends to be saturated and the particles are prone to collision and aggregation.

[0086] In some embodiments, the method for preparing the modified montmorillonite includes the following steps:

[0087] Sodium-based montmorillonite and water were mixed and stirred to obtain a montmorillonite suspension.

[0088] The montmorillonite suspension and octadecyltrimethylammonium chloride were mixed and stirred to obtain the modified montmorillonite.

[0089] The preparation method first involves exfoliating sodium-based montmorillonite into a suspension to fully disperse the montmorillonite sheets. Then, octadecyltrimethylammonium chloride is added as an organic intercalating agent. The long alkyl chains on its molecular chain enter the spaces between the montmorillonite sheets, replacing sodium ions through ion exchange, thereby increasing the interlayer spacing and obtaining organically modified montmorillonite. Organically modified montmorillonite exhibits good compatibility with the polymer matrix, a high aspect ratio, and can form a well-dispersed and barrier structure in the core layer.

[0090] In some embodiments, the mass-to-volume ratio of sodium-based montmorillonite to water is 1 g: (20~100) mL. This ratio ensures that the montmorillonite suspension has a suitable concentration, guaranteeing that the sheets are fully dispersed without severe aggregation, and providing a uniform reaction environment for subsequent organic intercalation reactions.

[0091] In some embodiments, the stirring speed is 200-400 r / min, the temperature is 25-40°C, and the time is 10-30 min. These stirring conditions ensure that the montmorillonite flakes are fully dispersed, the temperature is moderate to prevent excessive evaporation of moisture, and the time is sufficient to form a uniform suspension.

[0092] In some embodiments, the mass-to-volume ratio of the montmorillonite suspension to octadecyltrimethylammonium chloride is 1 mL: (0.002~0.03) g. This ratio controls the amount of octadecyltrimethylammonium chloride used to ensure sufficient organic intercalation. If the amount is too low, the intercalation will be insufficient; if the amount is too high, there will be an excess of organic intercalating agent, which may remain on the surface of the modified montmorillonite and affect subsequent processing performance.

[0093] In some embodiments, the stirring speed is 200-400 r / min, the temperature is 60-90°C, and the time is 2-6 h. These reaction conditions, carried out at a higher temperature, are beneficial for the dissolution of octadecyltrimethylammonium chloride and the intercalation reaction. Sufficient time ensures adequate ion exchange, while excessively high temperatures can affect the stability of the organic intercalating agent.

[0094] Secondly, this application provides a method for preparing the multilayer co-extruded degradable composite film described in the foregoing scheme, comprising the following steps:

[0095] After mixing polylactic acid, poly(butylene adipate / terephthalate) copolymer, modified montmorillonite, styrene-acrylate copolymer and tributyl citrate, the mixture is subjected to a first stirring treatment to obtain the outer layer premix.

[0096] After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a second stirring treatment is performed to obtain the first adhesive layer premix.

[0097] After mixing polybutylene succinate, polycaprolactone, modified montmorillonite, degradation accelerator and tributyl citrate, a third stirring treatment is carried out to obtain the core layer premix.

[0098] After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a fourth stirring treatment is performed to obtain the second adhesive layer premix.

[0099] After mixing poly(adipate) / butylene terephthalate copolymer, polycaprolactone and silica, a fifth stirring treatment is performed to obtain the inner layer premix.

[0100] The outer layer premix, the first adhesive layer premix, the core layer premix, the second adhesive layer premix, and the inner layer premix are melted and plasticized by five single-screw extruders, and then merged by five co-extrusion dies to form a five-layer melt. The melt is then cast to form a multi-layer co-extruded degradable composite film.

[0101] The preparation method provided in this application involves preparing premixes for each layer separately, ensuring thorough and uniform mixing of raw materials. Five single-screw extruders are used to melt and plasticize each premix, with independent temperature control to prevent degradation or uneven flow caused by temperature differences between different layers. When the five melt layers converge in the co-extrusion die, the epoxy groups in the adhesive layer react in situ with the end groups of the adjacent polyester layer in the molten state, forming chemical bonds and achieving interlayer compatibilization. The casting process is a one-step film formation, simple in process and highly efficient in production.

[0102] In some embodiments, the stirring speed of the first, second, third, fourth, and fifth stirring processes is 300-500 r / min, the temperature is 25-40°C, and the time is 5-10 min. These stirring conditions ensure that the raw materials in each layer are mixed evenly at a mild temperature, avoiding adverse effects such as premature release of degradation promoters and volatilization and degradation of silane coupling agents caused by excessive stirring speed or temperature.

[0103] In some embodiments, the outer layer corresponds to an extruder zone temperature of 165~200℃ and a screw speed of 15~30 r / min; the first and second adhesive layers correspond to an extruder zone temperature of 155~185℃ and a screw speed of 15~30 r / min; the core layer corresponds to an extruder zone temperature of 150~190℃ and a screw speed of 15~30 r / min; and the inner layer corresponds to an extruder zone temperature of 150~180℃ and a screw speed of 15~30 r / min. These temperature ranges are set according to the melting characteristics and processing heat sensitivity of each resin layer to ensure that each layer is fully plasticized and has a suitable melt viscosity, forming a clear and stable five-layer structure in the co-extrusion die, avoiding blurred interlayer interfaces or melt fracture.

[0104] In some embodiments, the temperature of the cooling roller for casting is 15~30°C. This cooling temperature allows the molten film to cool and solidify rapidly, preventing excessive crystallization or uneven shrinkage, and ensuring uniform film thickness and surface smoothness.

[0105] Thirdly, this application provides the application of the multilayer co-extruded degradable composite film described in the aforementioned scheme in packaging materials or agricultural mulch films.

[0106] The multilayer co-extruded degradable composite membrane provided in this application achieves a synergistic improvement in interlayer bonding strength, barrier performance, and degradation performance through a five-layer structural design and functional division of each layer. Specifically, the first and second adhesive layers are composed of glycidyl methacrylate grafted with poly(adipate / butylene terephthalate) and polybutylene succinate. During co-extrusion, the epoxy groups react in situ with the end groups of adjacent polyester layers to form an interfacial graft copolymer, improving interlayer peel strength. In the core layer, organically intercalated montmorillonite forms a lamellar dispersion structure, extending the diffusion path of gas molecules and enhancing barrier performance. The degradation promoter is a microcapsule structure of malic acid modified with γ-aminopropyltriethoxysilane and coated with polyvinyl alcohol. This structure remains stable during membrane use and releases organic acids under the action of a medium after disposal, promoting polyester hydrolysis and achieving timed initiation and self-acceleration of the degradation rate. Compared with existing technologies, this multilayer co-extruded degradable composite film has the characteristics of high interlayer bonding strength, good oxygen and water vapor barrier performance, controllable degradation induction period and stable mechanical properties. At the same time, the preparation process is simple and the raw materials of each layer are all conventional degradable materials, which has good feasibility and industrial application prospects.

[0107] The present application will be specifically described below through specific embodiments. The following embodiments are only some embodiments of the present application and are not intended to limit the present application.

[0108] Example 1

[0109] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0110] 70g polylactic acid, 25g PBAT, 1.0g modified montmorillonite, 0.5g styrene-acrylate copolymer (epoxy functionalized, ADR-4370) and 0.5g tributyl citrate were mixed and stirred at 400r / min and 30℃ for 8min to obtain the outer layer premix.

[0111] After mixing 80g PBAT-g-GMA and 20g polybutylene succinate, the mixture was stirred at 400r / min and 30℃ for 8min to obtain the first adhesive layer premix.

[0112] 65g of polybutylene succinate, 15g of polycaprolactone, 5g of modified montmorillonite, 4g of degradation accelerator and 3g of tributyl citrate were mixed and stirred at 400r / min and 30℃ for 8min to obtain the core layer premix.

[0113] After mixing 80g PBAT-g-GMA and 20g polybutylene succinate, the mixture was stirred at 400r / min and 30℃ for 8min to obtain the second adhesive layer premix.

[0114] Mix 80g PBAT, 15g polycaprolactone and 0.8g silica, and stir at 400r / min and 30℃ for 8min to obtain the inner layer premix.

[0115] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 170 / 180 / 190 / 190 / 185℃ for the outer layer, 160 / 170 / 175 / 175 / 170℃ for the first and second adhesive layers, 155 / 165 / 175 / 175 / 170℃ for the core layer, and 155 / 165 / 170 / 170 / 165℃ for the inner layer. The screw speed was 20 r / min for all zones.

[0116] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 20°C. The total film thickness is 50 μm, with an outer layer thickness of 10 μm, a first adhesive layer thickness of 5 μm, a core layer thickness of 20 μm, a second adhesive layer thickness of 5 μm, and an inner layer thickness of 10 μm.

[0117] The preparation method of the glycidyl methacrylate-grafted poly(butylene adipate) / terephthalate (PBAT-g-GMA) includes the following steps:

[0118] 500g of poly(butylene adipate) / terephthalate copolymer (PBAT, melt index 4g / 10min), 10g of glycidyl methacrylate (GMA) and 2.5g of benzoyl peroxide were mixed and stirred at 400r / min and 30℃ for 15min to obtain a premix.

[0119] The premixed material was fed into a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 48, and the temperatures in each zone were 150 / 160 / 170 / 170 / 165℃. The screw speed was 100 r / min. Vacuum devolatilization was then performed in the rear section of the extruder at a vacuum degree of -0.08 MPa, a temperature of 160℃, and a time of 2 min to obtain PBAT-g-GMA.

[0120] The preparation method of the modified montmorillonite includes the following steps:

[0121] 100g of sodium montmorillonite and 5000mL of deionized water were mixed and stirred at 300r / min and 30℃ for 20min to obtain a montmorillonite suspension.

[0122] The montmorillonite suspension was mixed with 30g of octadecyltrimethylammonium chloride and stirred at 300r / min and 80℃ for 4h. After filtration, the mixture was washed three times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 80℃ for 10h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0123] The method for preparing the degradation promoter includes the following steps:

[0124] 100g of malic acid, 800mL of ethanol aqueous solution (volume concentration 30%) and 12g of γ-aminopropyltriethoxysilane were mixed and stirred at 300r / min and 50℃ for 2h. After filtration, the mixture was dried at 60℃ to obtain modified malic acid.

[0125] The modified malic acid and 2000 mL of polyvinyl alcohol aqueous solution (mass concentration 10%) were mixed and stirred at 300 r / min and 70 °C for 45 min, and then spray dried with an inlet air temperature of 140 °C and an outlet air temperature of 70 °C to obtain a degradation accelerator.

[0126] Example 2

[0127] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0128] 75g polylactic acid, 20g PBAT, 1.5g modified montmorillonite, 0.8g styrene-acrylate copolymer (epoxy functionalized, ADR-4368) and 0.8g tributyl citrate were mixed and stirred at 350r / min and 25℃ for 10min to obtain the outer layer premix.

[0129] 85g of PBAT-g-GMA and 15g of polybutylene succinate were mixed and stirred at 350r / min and 25℃ for 10min to obtain the first adhesive layer premix.

[0130] 70g of polybutylene succinate, 20g of polycaprolactone, 6g of modified montmorillonite, 6g of degradation accelerator and 4g of tributyl citrate were mixed and stirred at 350r / min and 25℃ for 10min to obtain the core layer premix.

[0131] After mixing 85g PBAT-g-GMA and 15g polybutylene succinate, the mixture was stirred at 350r / min and 25℃ for 10min to obtain the second adhesive layer premix.

[0132] Mix 85g PBAT, 20g polycaprolactone and 1.0g silica, and stir for 10min at 350r / min and 25℃ to obtain the inner layer premix.

[0133] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 175 / 185 / 195 / 195 / 190℃ for the outer layer, 165 / 175 / 180 / 180 / 175℃ for the first and second adhesive layers, 160 / 170 / 180 / 180 / 175℃ for the core layer, and 160 / 170 / 175 / 175 / 175 / 170℃ for the inner layer. The screw speed was 18 r / min for all zones.

[0134] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 18°C. The total film thickness is 40 μm, with an outer layer thickness of 8 μm, a first adhesive layer thickness of 4 μm, a core layer thickness of 16 μm, a second adhesive layer thickness of 4 μm, and an inner layer thickness of 8 μm.

[0135] The preparation method of the PBAT-g-GMA includes the following steps:

[0136] 500g PBAT (melt index 5g / 10min), 20g glycidyl methacrylate and 4g benzoyl peroxide were mixed and stirred at 300r / min and 35℃ for 12min to obtain a premix.

[0137] The premixed material was added to a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 42, and the temperatures in each zone were 155 / 165 / 170 / 170 / 165℃. The screw speed was 80 r / min. Vacuum devolatilization was performed in the latter part of the extruder at a vacuum degree of -0.07 MPa, a temperature of 165℃, and a time of 2.5 min to obtain PBAT-g-GMA.

[0138] The preparation method of the modified montmorillonite includes the following steps:

[0139] 100g of sodium montmorillonite and 3000mL of deionized water were mixed and stirred at 250r / min and 28℃ for 25min to obtain a montmorillonite suspension.

[0140] The montmorillonite suspension was mixed with 50g of octadecyltrimethylammonium chloride and stirred at 250r / min and 70℃ for 3h. After filtration, the mixture was washed 4 times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 90℃ for 8h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0141] The method for preparing the degradation promoter includes the following steps:

[0142] 100g of malic acid, 600mL of ethanol aqueous solution (volume concentration 25%) and 8g of γ-aminopropyltriethoxysilane were mixed and stirred at 250r / min and 45℃ for 2.5h. After filtration and drying at 60℃, modified malic acid was obtained.

[0143] The modified malic acid was mixed with 1500 mL of polyvinyl alcohol aqueous solution (mass concentration 8%), stirred at 250 r / min and 65 °C for 50 min, and then spray dried with an inlet air temperature of 130 °C and an outlet air temperature of 65 °C to obtain a degradation accelerator.

[0144] Example 3

[0145] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0146] 65g polylactic acid, 30g PBAT, 0.8g modified montmorillonite, 0.6g styrene-acrylate copolymer (epoxy functionalized, ADR-4370) and 0.6g tributyl citrate were mixed and stirred at 450r / min and 40℃ for 6min to obtain the outer layer premix.

[0147] After mixing 90g PBAT-g-GMA and 10g polybutylene succinate, the mixture was stirred at 450r / min and 40℃ for 6min to obtain the first adhesive layer premix.

[0148] 60g of polybutylene succinate, 25g of polycaprolactone, 8g of modified montmorillonite, 2g of degradation accelerator and 4g of tributyl citrate were mixed and stirred at 450r / min and 40℃ for 6min to obtain the core layer premix.

[0149] After mixing 90g PBAT-g-GMA and 10g polybutylene succinate, the mixture was stirred at 450r / min and 40℃ for 6min to obtain the second adhesive layer premix.

[0150] 75g PBAT, 25g polycaprolactone and 0.6g silica were mixed and stirred at 450r / min and 40℃ for 6min to obtain the inner layer premix.

[0151] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 180 / 190 / 200 / 200 / 195℃ for the outer layer, 170 / 180 / 185 / 185 / 180℃ for the first and second adhesive layers, 165 / 175 / 185 / 185 / 180℃ for the core layer, and 165 / 175 / 180 / 180 / 175℃ for the inner layer. The screw speed was 25 r / min for all zones.

[0152] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 25°C. The total film thickness is 60 μm, with the outer layer being 12 μm, the first adhesive layer being 6 μm, the core layer being 25 μm, the second adhesive layer being 6 μm, and the inner layer being 11 μm.

[0153] The preparation method of the PBAT-g-GMA includes the following steps:

[0154] 500g PBAT (melt index 6g / 10min), 30g glycidyl methacrylate and 5g benzoyl peroxide were mixed and stirred at 500r / min and 25℃ for 18min to obtain a premix.

[0155] The premixed material was fed into a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 45, zone temperatures of 160 / 170 / 175 / 175 / 170℃, and a screw speed of 120 r / min. Vacuum devolatilization was then performed in the rear section of the extruder at a vacuum degree of -0.06 MPa, a temperature of 170℃, and a time of 1.5 min to obtain PBAT-g-GMA.

[0156] The preparation method of the modified montmorillonite includes the following steps:

[0157] 100g of sodium montmorillonite and 8000mL of deionized water were mixed and stirred at 400r / min and 35℃ for 15min to obtain a montmorillonite suspension.

[0158] The montmorillonite suspension was mixed with 60g of octadecyltrimethylammonium chloride and stirred at 400r / min and 85℃ for 5h. After filtration, the mixture was washed 5 times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 100℃ for 6h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0159] The method for preparing the degradation promoter includes the following steps:

[0160] 100g of malic acid, 1000mL of ethanol aqueous solution (volume concentration 40%) and 15g of γ-aminopropyltriethoxysilane were mixed and stirred at 400r / min and 55℃ for 1.5h. After filtration and drying at 60℃, modified malic acid was obtained.

[0161] The modified malic acid and 2500 mL of polyvinyl alcohol aqueous solution (mass concentration 12%) were mixed and stirred at 400 r / min and 75 °C for 35 min, and then spray dried with an inlet air temperature of 150 °C and an outlet air temperature of 75 °C to obtain the degradation accelerator.

[0162] Example 4

[0163] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0164] 60g polylactic acid, 35g PBAT, 2.0g modified montmorillonite, 1.0g styrene-acrylate copolymer (epoxy functionalized, ADR-4370) and 1.0g tributyl citrate were mixed and stirred at 300r / min and 35℃ for 9min to obtain the outer layer premix.

[0165] After mixing 70g PBAT-g-GMA and 30g polybutylene succinate, the mixture was stirred at 300r / min and 35℃ for 9min to obtain the first adhesive layer premix.

[0166] 55g of polybutylene succinate, 10g of polycaprolactone, 3g of modified montmorillonite, 8g of degradation accelerator and 2g of tributyl citrate were mixed and stirred at 300r / min and 35℃ for 9min to obtain the core layer premix.

[0167] 70g of PBAT-g-GMA and 30g of polybutylene succinate were mixed and stirred at 300r / min and 35℃ for 9min to obtain the second adhesive layer premix.

[0168] Mix 70g PBAT, 10g polycaprolactone and 0.5g silica, and stir at 300r / min and 35℃ for 9min to obtain the inner layer premix.

[0169] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 165 / 175 / 185 / 185 / 180℃ for the outer layer, 155 / 165 / 170 / 170 / 165℃ for the first and second adhesive layers, 150 / 160 / 170 / 170 / 165℃ for the core layer, and 150 / 160 / 165 / 165 / 165℃ for the inner layer. The screw speed was 15 r / min for all zones.

[0170] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 15°C. The total film thickness is 30 μm, with the outer layer being 6 μm thick, the first adhesive layer being 3 μm thick, the core layer being 12 μm thick, the second adhesive layer being 3 μm thick, and the inner layer being 6 μm thick.

[0171] The preparation method of the glycidyl methacrylate-grafted poly(butylene adipate) / terephthalate (PBAT-g-GMA) includes the following steps:

[0172] 500g of poly(butylene adipate) / terephthalate copolymer (PBAT, melt index 4g / 10min), 10g of glycidyl methacrylate (GMA) and 2.5g of benzoyl peroxide were mixed and stirred at 400r / min and 30℃ for 15min to obtain a premix.

[0173] The premixed material was fed into a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 48, and the temperatures in each zone were 150 / 160 / 170 / 170 / 165℃. The screw speed was 100 r / min. Vacuum devolatilization was then performed in the rear section of the extruder at a vacuum degree of -0.08 MPa, a temperature of 160℃, and a time of 2 min to obtain PBAT-g-GMA.

[0174] The preparation method of the modified montmorillonite includes the following steps:

[0175] 100g of sodium montmorillonite and 5000mL of deionized water were mixed and stirred at 300r / min and 30℃ for 20min to obtain a montmorillonite suspension.

[0176] The montmorillonite suspension was mixed with 30g of octadecyltrimethylammonium chloride and stirred at 300r / min and 80℃ for 4h. After filtration, the mixture was washed three times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 80℃ for 10h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0177] The method for preparing the degradation promoter includes the following steps:

[0178] 100g of malic acid, 800mL of ethanol aqueous solution (volume concentration 30%) and 12g of γ-aminopropyltriethoxysilane were mixed and stirred at 300r / min and 50℃ for 2h. After filtration, the mixture was dried at 60℃ to obtain modified malic acid.

[0179] The modified malic acid and 2000 mL of polyvinyl alcohol aqueous solution (mass concentration 10%) were mixed and stirred at 300 r / min and 70 °C for 45 min, and then spray dried with an inlet air temperature of 140 °C and an outlet air temperature of 70 °C to obtain a degradation accelerator.

[0180] Example 5

[0181] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0182] 80g polylactic acid, 20g PBAT, 0.5g modified montmorillonite, 0.3g styrene-acrylate copolymer (epoxy functionalized, ADR-4368) and 0.5g tributyl citrate were mixed and stirred at 500r / min and 25℃ for 5min to obtain the outer layer premix.

[0183] 75g of PBAT-g-GMA and 25g of polybutylene succinate were mixed and stirred at 500r / min and 25℃ for 5min to obtain the first adhesive layer premix.

[0184] 75g of polybutylene succinate, 15g of polycaprolactone, 4g of modified montmorillonite, 5g of degradation accelerator and 5g of tributyl citrate were mixed and stirred at 500r / min and 25℃ for 5min to obtain the core layer premix.

[0185] After mixing 75g PBAT-g-GMA and 25g polybutylene succinate, the mixture was stirred at 500r / min and 25℃ for 5min to obtain the second adhesive layer premix.

[0186] After mixing 90g PBAT, 30g polycaprolactone and 1.0g silica, the mixture was stirred at 500r / min and 25℃ for 5min to obtain the inner layer premix.

[0187] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 175 / 185 / 195 / 195 / 190℃ for the outer layer, 165 / 175 / 180 / 180 / 175℃ for the first and second adhesive layers, 160 / 170 / 180 / 180 / 175℃ for the core layer, and 160 / 170 / 175 / 175 / 175℃ for the inner layer; the screw speed was 30 r / min for all zones.

[0188] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 30°C. The total film thickness is 80 μm, with the outer layer being 16 μm thick, the first adhesive layer being 8 μm thick, the core layer being 32 μm thick, the second adhesive layer being 8 μm thick, and the inner layer being 16 μm thick.

[0189] The preparation method of the PBAT-g-GMA includes the following steps:

[0190] 500g PBAT (melt index 5g / 10min), 20g glycidyl methacrylate and 4g benzoyl peroxide were mixed and stirred at 300r / min and 35℃ for 12min to obtain a premix.

[0191] The premixed material was added to a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 42, and the temperatures in each zone were 155 / 165 / 170 / 170 / 165℃. The screw speed was 80 r / min. Vacuum devolatilization was performed in the latter part of the extruder at a vacuum degree of -0.07 MPa, a temperature of 165℃, and a time of 2.5 min to obtain PBAT-g-GMA.

[0192] The preparation method of the modified montmorillonite includes the following steps:

[0193] 100g of sodium montmorillonite and 3000mL of deionized water were mixed and stirred at 250r / min and 28℃ for 25min to obtain a montmorillonite suspension.

[0194] The montmorillonite suspension was mixed with 50g of octadecyltrimethylammonium chloride and stirred at 250r / min and 70℃ for 3h. After filtration, the mixture was washed 4 times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 90℃ for 8h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0195] The method for preparing the degradation promoter includes the following steps:

[0196] 100g of malic acid, 600mL of ethanol aqueous solution (volume concentration 25%) and 8g of γ-aminopropyltriethoxysilane were mixed and stirred at 250r / min and 45℃ for 2.5h. After filtration and drying at 60℃, modified malic acid was obtained.

[0197] The modified malic acid was mixed with 1500 mL of polyvinyl alcohol aqueous solution (mass concentration 8%), stirred at 250 r / min and 65 °C for 50 min, and then spray dried with an inlet air temperature of 130 °C and an outlet air temperature of 65 °C to obtain a degradation accelerator.

[0198] Example 6

[0199] This embodiment provides a method for preparing a multilayer co-extruded degradable composite film, comprising the following steps:

[0200] 70g polylactic acid, 25g PBAT, 1.2g modified montmorillonite, 0.5g styrene-acrylate copolymer (epoxy functionalized, ADR-4370) and 0.7g tributyl citrate were mixed and stirred at 400r / min and 30℃ for 8min to obtain the outer layer premix.

[0201] After mixing 80g PBAT-g-GMA and 20g polybutylene succinate, the mixture was stirred at 400r / min and 30℃ for 8min to obtain the first adhesive layer premix.

[0202] 65g of polybutylene succinate, 20g of polycaprolactone, 5g of modified montmorillonite, 4g of degradation accelerator and 3g of tributyl citrate were mixed and stirred at 400r / min and 30℃ for 8min to obtain the core layer premix.

[0203] After mixing 80g PBAT-g-GMA and 20g polybutylene succinate, the mixture was stirred at 400r / min and 30℃ for 8min to obtain the second adhesive layer premix.

[0204] Mix 80g PBAT, 15g polycaprolactone and 0.8g silica, and stir at 400r / min and 30℃ for 8min to obtain the inner layer premix.

[0205] The outer layer premix, first adhesive layer premix, core layer premix, second adhesive layer premix, and inner layer premix were respectively added to five single-screw extruders for melt plasticization. The temperatures of each zone of the extruders were as follows: 170 / 180 / 190 / 190 / 185℃ for the outer layer, 160 / 170 / 175 / 175 / 170℃ for the first and second adhesive layers, 155 / 165 / 175 / 175 / 170℃ for the core layer, and 155 / 165 / 170 / 170 / 165℃ for the inner layer. The screw speed was 22 r / min for all zones.

[0206] Five layers of melt are combined through a five-layer co-extrusion die to form a multi-layer co-extruded degradable composite film, which is then cast and molded at a cooling roller temperature of 20°C. The total film thickness is 100 μm, with an outer layer thickness of 20 μm, a first adhesive layer thickness of 10 μm, a core layer thickness of 40 μm, a second adhesive layer thickness of 10 μm, and an inner layer thickness of 20 μm.

[0207] The preparation method of the PBAT-g-GMA includes the following steps:

[0208] 500g PBAT (melt index 6g / 10min), 30g glycidyl methacrylate and 5g benzoyl peroxide were mixed and stirred at 500r / min and 25℃ for 18min to obtain a premix.

[0209] The premixed material was fed into a twin-screw extruder via a metering pump for melt reaction extrusion. The twin-screw extruder had an aspect ratio of 45, zone temperatures of 160 / 170 / 175 / 175 / 170℃, and a screw speed of 120 r / min. Vacuum devolatilization was then performed in the rear section of the extruder at a vacuum degree of -0.06 MPa, a temperature of 170℃, and a time of 1.5 min to obtain PBAT-g-GMA.

[0210] The preparation method of the modified montmorillonite includes the following steps:

[0211] 100g of sodium montmorillonite and 8000mL of deionized water were mixed and stirred at 400r / min and 35℃ for 15min to obtain a montmorillonite suspension.

[0212] The montmorillonite suspension was mixed with 60g of octadecyltrimethylammonium chloride and stirred at 400r / min and 85℃ for 5h. After filtration, the mixture was washed 5 times with deionized water until no chloride ions remained in the filtrate. The mixture was then vacuum dried at 100℃ for 6h and ground through a 200-mesh sieve to obtain modified montmorillonite.

[0213] The method for preparing the degradation promoter includes the following steps:

[0214] 100g of malic acid, 1000mL of ethanol aqueous solution (volume concentration 40%) and 15g of γ-aminopropyltriethoxysilane were mixed and stirred at 400r / min and 55℃ for 1.5h. After filtration and drying at 60℃, modified malic acid was obtained.

[0215] The modified malic acid and 2500 mL of polyvinyl alcohol aqueous solution (mass concentration 12%) were mixed and stirred at 400 r / min and 75 °C for 35 min, and then spray dried with an inlet air temperature of 150 °C and an outlet air temperature of 75 °C to obtain the degradation accelerator.

[0216] Comparative Example 1

[0217] This comparative example provides a method for preparing a multilayer co-extruded degradable composite film. The difference from Example 1 is that no degradation promoter is added to the core layer, while the other raw materials and steps are the same as in Example 1.

[0218] Comparative Example 2

[0219] This comparative example provides a method for preparing a multilayer co-extruded degradable composite film. The difference from Example 1 is that the first adhesive layer and the second adhesive layer use a blend of ungrafted PBAT (80g) and polybutylene succinate (20g) instead of PBAT-g-GMA. The remaining raw materials and steps are the same as in Example 1.

[0220] Comparative Example 3

[0221] This comparative example provides a method for preparing a multilayer co-extruded degradable composite film. The difference from Example 1 is that unmodified sodium-based montmorillonite is used instead of modified montmorillonite in the outer and core layers, while the other raw materials and steps are the same as in Example 1.

[0222] Comparative Example 4

[0223] This comparative example provides a method for preparing a multilayer co-extruded degradable composite film. The difference from Example 1 is that no styrene-acrylate copolymer is added to the outer layer, while the other raw materials and steps are the same as in Example 1.

[0224] Comparative Example 5

[0225] This comparative example provides a method for preparing a single-layer PBAT thin film, comprising the following steps:

[0226] Mix 70g PBAT, 15g polycaprolactone and 0.8g silica, and stir at 400r / min and 30℃ for 8min to obtain a mixture.

[0227] The mixture is melt-extruded through a single-screw extruder and cast into a film. The temperatures of each zone of the extruder are 150 / 160 / 170 / 170 / 165℃, the screw speed is 20r / min, and the temperature of the cooling roller is 20℃, resulting in a single-layer PBAT film with a thickness of 50μm.

[0228] The performance of the multilayer co-extruded degradable composite films prepared in Examples 1-6 and Comparative Examples 1-5 was tested, and the test results are shown in Table 1. Wherein:

[0229] Interlayer peel strength test: Cut the composite film into samples 150mm long and 15mm wide. Manually pre-peel the outer layer and the middle layer by about 10mm at one end of the sample. Clamp the pre-peeled ends on an electronic universal testing machine and perform a T-shaped peel test at a peeling speed of 200mm / min. Record the average peeling force during the peeling process. Divide the peeling force by the sample width to obtain the interlayer peel strength (N / 15mm). Test 5 samples in each group and take the average value.

[0230] Tensile strength and elongation at break tests: The composite film was cut into dumbbell-shaped specimens (gauge length 25 mm, width 6 mm). The specimens were clamped on an electronic universal testing machine and stretched uniformly along the longitudinal axis of the specimen at a tensile speed of 50 mm / min. The stress-strain curve was automatically recorded. The maximum tensile stress at the time of specimen breakage was read as the tensile strength (MPa). The percentage of the elongation of the gauge length at the time of specimen breakage relative to the original gauge length was read as the elongation at break (%). Five specimens were tested in each group, and the average value was taken.

[0231] Oxygen permeability test: The composite membrane was cut into circular samples with a diameter of 80 mm and clamped onto a differential pressure gas permeameter. The test was conducted at 23°C and 0% relative humidity. The test gas was oxygen with a purity ≥99.9%. The oxygen permeability was recorded in cm. 3 / (m 2 • 24h • 0.1MPa), 3 samples were tested in each group, and the average value was taken.

[0232] Water vapor transmission rate test: Cut the composite membrane into circular samples with a diameter of 80 mm, clamp them on an infrared water vapor transmission rate tester, and test them at 38℃ and 90% relative humidity. Record the water vapor transmission rate in g / (m²). 2 • 24h), 3 samples were tested in each group, and the average value was taken.

[0233] Composting degradation induction period test: The composite membrane was cut into 50mm×50mm samples and buried in the composting test device. The composting medium was commercial compost. The temperature was controlled at 58±2℃ and the relative humidity at 60%~70%. The samples were turned over every 7 days. The integrity of the samples was observed and the mass of the samples was weighed every 7 days. The degradation induction period (days) was defined as the number of days when the sample showed obvious damage and the weight loss rate reached more than 5%. Five samples were tested in each group, and the average value was taken.

[0234] 180-day composting degradation rate test: The composite membrane was cut into 50mm×50mm samples, the initial mass was weighed and then buried in the composting test device. The temperature was controlled at 58±2℃ and the relative humidity at 60%~70%. The samples were turned over every 7 days. After 180 days, the samples were taken out, washed with deionized water, dried and the residual mass was weighed. The degradation rate (%) was the percentage of the difference between the initial mass and the residual mass to the initial mass. Five samples were tested in each group and the average value was taken.

[0235] Table 1

[0236] project Interlayer peel strength (N / 15mm) Tensile strength (MPa) Elongation at break (%) <![CDATA[Oxygen transmission rate (cm 3 / (m 2 ·24h·0.1MPa))]]> <![CDATA[Water vapor transmission rate (g / (m 2 ·24h))]]> Degradation induction period (days) Degradation rate (%) after 180 days Example 1 3.2 28 260 650 120 45 92 Example 2 3.5 30 240 600 110 50 90 Example 3 3.0 26 280 700 130 40 94 Example 4 3.8 25 300 750 140 35 95 Example 5 3.1 32 230 580 105 55 89 Example 6 3.4 29 250 630 115 48 91 Comparative Example 1 3.3 28 255 660 122 — 45 Comparative Example 2 0.8 18 210 680 125 48 93 Comparative Example 3 3.1 26 240 1100 220 47 90 Comparative Example 4 3.2 27 250 670 123 46 89 Comparative Example 5 — 20 500 1500 300 60 80

[0237] The multilayer co-extruded degradable composite films from Examples 1-6 and Comparative Examples 1-5 were subjected to heat-sealing strength, right-angle tear strength, puncture strength, light transmittance, and accelerated UV aging tests. The test results are shown in Table 2. Among them:

[0238] Heat seal strength test: Cut the composite film into strips 150mm long and 15mm wide. Place the inner surfaces of two strips together and place them between the upper and lower heat seal blades of the heat seal testing machine. The heat seal blade temperature is 140℃, the heat seal pressure is 0.2MPa, and the heat seal time is 1s. After heat sealing, remove the sample and cool it at room temperature (23±2℃) for 1 hour. Then, clamp the heat-sealed sample on an electronic universal testing machine and perform a T-type peel test at a tensile speed of 200mm / min. Record the maximum peel force during the peeling process. Divide the maximum peel force by the sample width to obtain the heat seal strength (N / 15mm). Test 5 samples in each group and take the average value.

[0239] Right-angle tear strength test: The composite film is cut into right-angle tear-type specimens (the specimen size is 100mm×50mm, and a 50mm long cut is made in the center of one end of the specimen along the length direction). The specimen is clamped on an electronic universal testing machine and stretched at a tensile speed of 200mm / min along the longitudinal axis of the specimen. The force-displacement curve during the tearing process is automatically recorded, and the maximum tearing force during the tearing process is read. The right-angle tear strength (kN / m) is obtained by dividing the maximum tearing force by the specimen thickness. Five specimens are tested in each group, and the average value is taken.

[0240] Puncture strength test: The composite film is cut into circular samples with a diameter of 80 mm and fixed on the sample clamp of the puncture test device. A stainless steel puncture needle with a diameter of 1 mm is used to puncture the sample at a uniform speed of 50 mm / min in a direction perpendicular to the sample surface. The force-displacement curve is automatically recorded, and the maximum puncture force when the puncture needle punctures the sample is read as the puncture strength (N). The greater the puncture strength, the better the film's ability to resist puncture by sharp objects. Five samples are tested in each group, and the average value is taken.

[0241] Transmittance test: Cut the composite film into 50mm×50mm square samples, place them on the transmittance test bracket of the spectrophotometer, and measure the transmittance of the sample at a wavelength of 550nm. The transmittance (%) is the percentage of transmitted light intensity to incident light intensity. The higher the transmittance, the better the transparency of the film. Three samples are tested in each group, and the average value is taken.

[0242] Tensile strength retention rate test after UV accelerated aging: The composite film was cut into rectangular samples of 100mm×50mm and placed in a UV accelerated aging test chamber. The UV lamp power was 40W and the wavelength was 300~400nm. The sample was 300mm away from the UV lamp tube. The temperature inside the test chamber was controlled at 40±2℃. The sample was continuously irradiated for 240h. After removal, the sample was placed at room temperature (23±2℃) for 2h to recover naturally. The tensile strength after irradiation was measured according to the above tensile strength test method. The percentage of the tensile strength after irradiation to the tensile strength before irradiation was taken as the tensile strength retention rate (%) after UV accelerated aging. The higher the retention rate, the better the UV aging resistance. Five samples were tested in each group, and the average value was taken.

[0243] Table 2

[0244] project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Heat seal strength (N / 15mm) 7.2 7.5 7.0 6.8 7.8 7.3 7.2 5.5 6.5 6.8 7.5 Right-angle tear strength (kN / m) 38 42 36 34 44 40 38 25 30 32 20 Puncture intensity (N) 4.5 4.8 4.2 4.0 5.0 4.6 4.5 3.2 3.5 3.8 2.5 Light transmittance (%) 82 85 78 75 86 83 82 83 65 84 90 Tensile strength retention rate after UV accelerated aging (%) 88 90 86 85 89 87 88 80 75 70 60

[0245] The technical solutions provided by the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A multilayer co-extruded degradable composite film, characterized in that, It includes an outer layer, a first adhesive layer, a core layer, a second adhesive layer, and an inner layer arranged sequentially; The outer layer, by mass parts, comprises the following raw materials: 60-80 parts of polylactic acid, 20-40 parts of poly(butylene adipate / terephthalate) copolymer, 0.5-2 parts of modified montmorillonite, 0.3-1 parts of styrene-acrylate copolymer, and 0.5-1 parts of tributyl citrate. The first adhesive layer and the second adhesive layer, by mass parts, each independently comprise the following raw materials: 70-90 parts of glycidyl methacrylate grafted poly(butylene adipate / terephthalate), and 10-30 parts of polybutylene succinate. The core layer, by mass parts, comprises the following raw materials: 55-75 parts of polybutylene succinate, 10-25 parts of polycaprolactone, 3-8 parts of modified montmorillonite, 2-8 parts of degradation accelerator, and 2-5 parts of tributyl citrate. The inner layer, by mass parts, comprises the following raw materials: 70-90 parts of poly(butylene adipate / terephthalate) copolymer, 10-30 parts of polycaprolactone, and 0.5-1 parts of silica.

2. The multilayer co-extruded degradable composite film according to claim 1, characterized in that, The outer layer has a thickness of 8~20μm, the first adhesive layer and the second adhesive layer each have a thickness of 3~10μm, the core layer has a thickness of 12~40μm, and the inner layer has a thickness of 8~20μm.

3. The multilayer co-extruded degradable composite film according to claim 1, characterized in that, The preparation method of the glycidyl methacrylate-grafted poly(adipate / butylene terephthalate) comprises the following steps: Poly(butylene adipate) / butylene terephthalate copolymer, glycidyl methacrylate and benzoyl peroxide are mixed and stirred to obtain a premix. The premixed material is subjected to melt reaction extrusion and then vacuum devolatilization to obtain the glycidyl methacrylate-grafted poly(adipate / butylene terephthalate).

4. The multilayer co-extruded degradable composite film according to claim 3, characterized in that, The mass ratio of the poly(butylene adipate / terephthalate) copolymer, glycidyl methacrylate, and benzoyl peroxide is 1:0.01~0.05:0.001~0.005; and / or The stirring process is carried out at a speed of 300-500 r / min, a temperature of 25-40℃, and a time of 10-20 min; and / or The melt reactive extrusion is carried out in a twin-screw extruder with a length-to-diameter ratio ≥40, a zone temperature of 140~170℃, and a screw speed of 50~150 r / min; and / or The vacuum devolatilization process is performed at a vacuum level of -0.06 to -0.09 MPa, a temperature of 140 to 170°C, and a time of 1 to 5 minutes.

5. The multilayer co-extruded degradable composite film according to claim 1, characterized in that, The method for preparing the degradation promoter includes the following steps: Modified malic acid was obtained by mixing malic acid, an aqueous ethanol solution and γ-aminopropyltriethoxysilane and stirring the mixture. The modified malic acid and polyvinyl alcohol aqueous solution were mixed and stirred to obtain the degradation promoter.

6. The multilayer co-extruded degradable composite film according to claim 5, characterized in that, The mass-to-volume ratio of the malic acid, the aqueous ethanol solution, and γ-aminopropyltriethoxysilane is 1 g : (5~15) mL : (0.05~0.2) g, and the volume concentration of the aqueous ethanol solution is 20%~50%; and / or The stirring reaction is carried out at a speed of 200-400 r / min, a temperature of 40-60℃, and a time of 1-3 h; and / or The modified malic acid and polyvinyl alcohol aqueous solution have a mass-to-volume ratio of 1 g:(10~30) mL, and the polyvinyl alcohol aqueous solution has a mass concentration of 5%~15%; and / or The stirring speed is 200~400 r / min, the temperature is 60~80℃, and the time is 30~60 min.

7. The multilayer co-extruded degradable composite film according to claim 1, characterized in that, The preparation method of the modified montmorillonite includes the following steps: Sodium-based montmorillonite and water were mixed and stirred to obtain a montmorillonite suspension. The montmorillonite suspension and octadecyltrimethylammonium chloride were mixed and stirred to obtain the modified montmorillonite.

8. The multilayer co-extruded degradable composite film according to claim 7, characterized in that, The mass-to-volume ratio of sodium-based montmorillonite to water is 1 g: (20~100) mL; and / or The stirring process is carried out at a speed of 200-400 r / min, a temperature of 25-40℃, and a time of 10-30 min; and / or The mass-to-volume ratio of the montmorillonite suspension to octadecyltrimethylammonium chloride is 1 mL: (0.002~0.03) g; and / or The stirring reaction is carried out at a speed of 200-400 r / min, a temperature of 60-90℃, and a time of 2-6 h.

9. A method for preparing the multilayer co-extruded degradable composite film according to any one of claims 1 to 8, characterized in that, Includes the following steps: After mixing polylactic acid, poly(butylene adipate / terephthalate) copolymer, modified montmorillonite, styrene-acrylate copolymer and tributyl citrate, the mixture is subjected to a first stirring treatment to obtain the outer layer premix. After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a second stirring treatment is performed to obtain the first adhesive layer premix. After mixing polybutylene succinate, polycaprolactone, modified montmorillonite, degradation accelerator and tributyl citrate, a third stirring treatment is carried out to obtain the core layer premix. After glycidyl methacrylate grafted poly(butylene adipate / terephthalate) and poly(butylene succinate) are mixed, a fourth stirring treatment is performed to obtain the second adhesive layer premix. After mixing poly(adipate) / butylene terephthalate copolymer, polycaprolactone and silica, a fifth stirring treatment is performed to obtain the inner layer premix. The outer layer premix, the first adhesive layer premix, the core layer premix, the second adhesive layer premix, and the inner layer premix are melted and plasticized by five single-screw extruders, and then merged by five co-extrusion dies to form a five-layer melt. The melt is then cast to form a multi-layer co-extruded degradable composite film.

10. The application of the multilayer co-extruded degradable composite film according to any one of claims 1 to 8 in packaging materials or agricultural mulch films.