A method for embedding water-based decal paint film on the surface of a workpiece

By constructing an integrated sandwich composite structure of protective paint film, pattern layer and primer film in the water decal process, the problems of poor adhesion and insufficient weather resistance caused by direct exposure of the pattern layer are solved, achieving high adhesion and wear resistance of the workpiece and extending its service life.

CN123104271APending Publication Date: 2026-11-17GREAT WALL SOUL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611526916.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing water decal processes, the pattern layer is directly exposed on the outermost layer of the workpiece, resulting in poor adhesion, easy wear, edge curling, peeling off after washing, and insufficient weather resistance, which affects the appearance quality and service life of the product.

Method used

An integrated sandwich composite structure consisting of a protective coating film, a pattern layer, and a primer film is constructed. By precisely controlling the surface drying window of the primer baking, the interface fusion between the pattern layer and the primer film is achieved by utilizing the rheological properties of the material. In step S4, a protective clear varnish is sprayed to seal the pattern layer between the two cured coating films.

Benefits of technology

It improves the adhesion, wear resistance, and weather resistance of the pattern layer, extends the service life of the workpiece product's appearance, avoids pattern wear and water washing peeling, and achieves high-precision pattern reproduction and environmentally friendly production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104271A_ABST
    Figure CN123104271A_ABST
Patent Text Reader

Abstract

This invention relates to the field of water transfer printing decorative processing technology, specifically disclosing a method for embedding a water-based decal paint film on a workpiece surface. The method includes immersing a water-based decal in water to obtain an activated water-based decal; during the surface drying window after applying a primer to the substrate workpiece, attaching the activated water-based decal to the surface of the substrate workpiece to obtain a water transfer printed workpiece; baking the water transfer printed workpiece and peeling off the coating to obtain a pre-cured transfer printed workpiece; and spraying a protective clear varnish onto the pre-cured transfer printed workpiece for curing to obtain a workpiece product with an embedded water-based decal paint film. This invention constructs an integrated sandwich composite structure formed by a protective paint film, a pattern layer, and a primer film. Utilizing the micro-wetting force during the surface drying window of the paint film, it achieves the penetration and bonding of ink and paint film molecules, solving the technical problems of weak adhesion and easy peeling of traditional decals. The resulting workpiece product has a completely embedded pattern, excellent adhesion, and good weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water transfer printing decoration processing technology, and relates to a method for embedding water decal paint film on the surface of a workpiece. Background Technology

[0002] As consumers' demand for personalized exterior parts of motorcycles and electric vehicles continues to increase, water transfer printing decoration technology, due to its ability to reproduce complex patterns with high precision, is widely used in the surface decoration of plastic parts, plastic shells, and small metal exterior parts of motorcycles and electric vehicles.

[0003] Currently, the commonly used water-based decal process in this field involves applying a primer to the workpiece surface and allowing it to fully cure. The decal is then directly applied to the primer surface, dried, and the film is removed, exposing the decal pattern layer directly on the outermost layer of the workpiece. However, this process creates a simple laminated structure between the primer and the pattern layer, relying solely on physical adhesion for bonding, resulting in weak interfacial bonding. In practical use, the pattern layer is directly exposed to the external environment without effective protection, leading to poor adhesion, easy wear, edge curling, and easy detachment after washing. Furthermore, it lacks sufficient weather resistance for long-term outdoor use, severely impacting the product's appearance quality and lifespan.

[0004] Therefore, how to solve the problems of easy wear and tear, poor adhesion, edge curling, water washing and peeling, insufficient weather resistance, orange peel defects, and delamination of surface decals, and extend the service life of product appearance, has become an urgent technical problem to be solved in this field. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a method for embedding a water-based decal paint film into the surface of a workpiece. This invention constructs an integrated sandwich composite structure consisting of a protective paint film, a pattern layer, and a primer film. This solves the technical problems in existing water-based decal processes, such as poor pattern adhesion, easy wear, edge curling, water washing detachment, insufficient weather resistance, orange peel defects, and delamination, which are caused by the pattern layer being directly exposed on the outermost layer of the workpiece and relying solely on physical adhesion to the primer surface. This improves the adhesion, wear resistance, and weather resistance of the pattern layer, extending the service life of the workpiece product.

[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: This invention provides a method for embedding water-based decal paint film on the surface of a workpiece, the key being that it includes the following steps: S1. Soak the water decals in water at 25℃~30℃ for 15s~25s to obtain activated water decals; The water decal includes a PVA film-coated base paper, a water-based ink intermediate layer, an acrylic resin isolation varnish layer, and a film coating. S2. During the surface drying window period after the primer is sprayed onto the substrate workpiece, the activated water decal is applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece. The surface drying window period is within 2 hours after the substrate workpiece is sprayed with primer and baked to a touch-dry state. S3. Bake the water transfer printed workpiece at 75℃~80℃, peel off the coating, and obtain the pre-cured transfer printed workpiece; S4. Spray a protective varnish onto the surface of the pre-cured transfer workpiece and cure it to obtain a workpiece product with an embedded water decal paint film.

[0007] In this invention, the surface drying window period refers to the time between when the primer surface reaches a touch-dry state (as measured by GB / T1728-2020, it is not sticky to the touch, has no fingerprints, no loss of gloss or haze, and leaves no marks when lightly scraped with a scraper) and when the micro-wetting force of the primer surface significantly decreases. After the substrate workpiece is coated with primer and baked, its surface is in a surface-dry state, while a trace amount of unvolatile solvent remains inside, forming micro-wetting force. This micro-wetting force can drive the resin molecules in the water-based pattern layer to penetrate and diffuse into the primer layer network, achieving interfacial fusion between the pattern layer and the primer layer.

[0008] This invention is not a simple superposition of steps in traditional decal processes. Instead, it precisely grasps the surface drying window after the primer is baked and uses the rheological properties of the material to achieve interface fusion between the pattern layer and the primer film. This allows the ink to penetrate and bond with the primer film at the molecular level, solving the technical problem of weak adhesion and easy peeling caused by traditional decals that rely solely on physical bonding.

[0009] This invention achieves controllable separation between the water-based ink intermediate layer and the base paper by precisely controlling the water temperature and soaking time for water-based decal activation. Simultaneously, it ensures the pattern layer achieves optimal extensibility under hydration, providing the necessary interface conditions for wetting and penetration during bonding. This invention avoids the VOC emissions and operator health risks associated with organic activators, while also ensuring environmental friendliness and high-precision pattern reproduction by matching the wetting and penetration mechanism.

[0010] This invention pre-cures and shapes the water-based decals after application. By controlling the baking temperature in step S3, the rate of moisture evaporation is controlled, allowing the pattern layer to achieve initial shaping while preserving the interfacial activity between the primer layer and the pattern layer. After baking in step S3, the coating can be completely peeled off, ensuring the pattern layer remains undamaged and preventing coating displacement.

[0011] Step S4 is the core step in constructing an integrated sandwich composite structure consisting of a protective varnish film, a pattern layer, and a primer film. By spraying a protective clear coat, the pattern layer is completely sealed and embedded between two cured varnish films. The pattern layer is not in direct contact with air, water, or friction media, structurally preventing pattern wear, water washing off, and environmental erosion, thus improving the product's resistance to washing, friction, weathering, and solvents.

[0012] Specifically, the baking temperature in step S2 is 75℃~85℃, and the baking time is 25min~35min.

[0013] Specifically, the baking time in step S3 is 20 to 30 minutes.

[0014] Furthermore, the substrate workpiece includes at least one of iron or plastic parts.

[0015] In some embodiments, the iron part includes any one of carbon steel workpiece, galvanized steel workpiece, aluminum alloy workpiece, magnesium alloy workpiece, or titanium alloy workpiece; when the base material workpiece is an iron part, the curing temperature in step S4 is 145℃~155℃ and the time is 35min~45min.

[0016] In some embodiments, the plastic part includes any one of ABS, PP, PC / ABS alloy, CFRP or GFRP; when the substrate workpiece is a plastic part, the curing temperature in step S4 is 80℃~90℃ and the time is 35min~45min.

[0017] This invention employs differentiated curing based on the workpiece material, allowing the primer film, pattern layer, and protective coating film to fully cross-link and cure under suitable curing conditions. During the curing process in step S4, the protective varnish and pattern layer undergo a cross-linking reaction at the interface, forming a dense cross-linked network structure. This integrates the primer film, pattern layer, and protective coating film into a unified composite structure. This cross-linked network structure also disperses interlayer stress, preventing stress concentration at the interface and avoiding delamination caused by temperature changes or mechanical stress.

[0018] Specifically, the dry film thickness of the protective varnish after curing in step S5 is 30μm to 40μm; optionally, it is 35μm.

[0019] Furthermore, step S2 further includes roughening and degreasing the surface of the substrate workpiece after the baking is completed and before the active water decal is applied.

[0020] Furthermore, step S4 also includes grinding and polishing the cured workpiece.

[0021] This invention eliminates surface micropores and orange peel texture through a mirror polishing process after the protective varnish is applied, so that the appearance of the workpiece product with water-based decal paint film embedded in it can achieve a mirror-like high-gloss effect. The orange peel mirror effect can reach short-wave S≤15, long-wave L≤8 and DOI≥90. Attached Figure Description

[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0023] Figure 1 Motorcycles that are part products in which a water-based decal paint film prepared by the method of the present invention is embedded. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0025] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of the invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified. In the description of the present invention, "a number" means at least one, such as one, two, etc., unless otherwise explicitly specified.

[0026] The terms "preferred," "more preferably," etc., used in this invention refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this invention.

[0027] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0028] Water decals The water-based decals used in this invention comprise a PVA film-coated base paper, a water-based ink intermediate layer, an acrylic resin varnish layer, and a lamination, conforming to the first-class standard of GB / T 29283-2012 "Water Transfer Printing Base Paper". In this field, water-based decals, also known as water-based transfer decals, are decorative materials that use water as a transfer medium to transfer a pattern layer from base paper to the surface of a workpiece.

[0029] It should be noted that those skilled in the art should understand that any water-based decal can be used in this invention as long as it has a water-swellable and activatable PVA film layer, a water-based pattern layer carrying the pattern, and a release varnish layer and a coating that can be completely peeled off after pre-curing. When there are differences in the thickness of the PVA film, the water swelling rate, the thickness of the pattern layer, or the resin system used, the soaking time in step S2 and the bonding timing in step S3 can be appropriately adjusted according to the actual material characteristics to ensure that the pattern layer and the primer layer can still achieve wetting penetration and interface fusion, thereby obtaining the same technical effect.

[0030] Furthermore, this invention does not limit the specific type or source of water decals. Water decals of different brands, different types of backing (white backing, transparent backing, or dark opaque backing) or different adhesive activity can all be used as the source of water decals in this invention, as long as they can achieve controllable separation of the pattern layer and the backing paper under the pure water immersion conditions in step S2, and form wetting and penetration with the primer layer in step S3.

[0031] The above-described requirements for first-class products conforming to GB / T 29283-2012 are merely illustrative examples of the present invention and do not constitute a limitation thereof. Those skilled in the art should understand that as long as the PVA film layer of the base paper can detach completely from the base paper without damage after immersion in pure water at 25°C to 30°C for 15 to 25 seconds, it can be used in the present invention.

[0032] Method for embedding water-based decal paint film on workpiece surface This invention provides a method for embedding water-based decal paint film on a workpiece surface, specifically including the following steps: S1. Water decal constant temperature immersion activation: Immerse the water decal in pure water at 25℃~30℃ for 15s~25s to obtain activated water decals.

[0033] For example, the soaking temperature can be 25°C, 28°C, or 30°C; the soaking time can be 15s, 20s, or 25s, preferably 20s. This step achieves controllable separation of the pattern layer and the base paper, allowing for full wetting and penetration of the paint film molecules when the water decal's extensibility is at its optimal level.

[0034] S2, Precise alignment and embedded transfer: S2-1. During the surface drying window period after the primer is applied to the substrate workpiece, roughen, remove dust and degrease the substrate workpiece after the primer is applied.

[0035] The specific steps for roughening, dust removal, and degreasing are as follows: use 2000-grit sandpaper to finely sand the surface of the primer layer until it changes from a glossy state to a matte state, without sanding through the primer layer or exposing the substrate, and then wipe it with anhydrous ethanol to remove oil.

[0036] This invention involves spraying a primer onto the substrate workpiece and baking it at 75℃~85℃ for 25min~35min until it reaches a touch-dry state, followed by decal application within 2 hours. After the primer is sprayed and baked, the surface of the substrate workpiece is in a surface-dry state, while a trace amount of unevaporated solvent remains inside, forming a micro-wetting force. This micro-wetting force can drive the resin molecules in the water-based pattern layer to penetrate and diffuse into the primer layer network, achieving interfacial fusion between the pattern layer and the primer layer.

[0037] The baking and subsequent curing steps involved in this invention can all be achieved using heating methods known in the art, including but not limited to circulating air drying ovens, hot plate contact heating, and infrared radiation heating. The choice of heating method is not limited to specific equipment, as long as the workpiece is heated uniformly within a set time and the baking temperature is controlled within ±2℃ of the set value and the baking time is controlled within ±1min of the set value.

[0038] Those skilled in the art should understand that different heating methods differ in their heat conduction mechanisms, but as long as the following conditions are met, they can be used in the baking steps of this invention: First, the temperature distribution of the workpiece to be baked is uniform, avoiding uneven curing due to local overheating or insufficient heating; Second, the baking temperature and time can be precisely set and stably maintained, ensuring that the primer layer, pattern layer and protective varnish layer are fully cross-linked and cured under their respective suitable conditions.

[0039] For example, when using a circulating air drying oven, the hot air can form a directional circulating airflow within the oven through a circulating fan and a guide structure, uniformly blowing onto the workpiece surface from multiple angles; when using infrared radiation heating, the workpiece surface can be heated uniformly by reasonably arranging the radiation sources and adjusting the radiation distance; when using hot plate contact heating, uniform heat transfer can be achieved by ensuring the workpiece is in close contact with the constant-temperature hot plate. The specific heating methods described above are merely illustrative examples of the present invention and do not constitute a limitation thereof.

[0040] S2-2. Using a flexible scraping process, activated water decals are applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece.

[0041] In this invention, the surface drying window period refers to the time period between when the primer surface reaches a touch-dry state (as measured by GB / T1728-2020, it is not sticky to the touch, has no fingerprints, no loss of gloss or haze, and leaves no marks when lightly scraped with a scraper) and when the micro-wetting power of the primer surface decreases significantly.

[0042] The flexible scraping process described in this invention refers to applying gentle and uniform pressure to the water-based decal after activation and when the primer layer is in its surface drying window. This pressure is achieved using an elastic scraping tool, ensuring close adhesion between the decal and the primer layer surface. Simultaneously, air bubbles and excess moisture are removed from the interface. The residual micro-wetting force on the primer layer surface drives ink molecules to penetrate the primer network, achieving interface fusion. This process differs from traditional mechanical pressing or roller pressing. Its core lies in the combination of flexibility and scraping pressure: flexibility avoids damage to the pattern layer and primer layer, while scraping pressure ensures a continuous, bubble-free contact interface between the water-based decal and the primer layer.

[0043] S3, Pre-curing and Shaping, and Coating Peeling: The water transfer print workpiece is pre-cured and shaped by baking at 75℃~80℃ for 20min~30min, and the film of the water decal is peeled off to obtain the pre-cured transfer print workpiece.

[0044] For example, the pre-curing temperature can be 75°C, 78°C or 80°C, and the baking time can be 20 min, 25 min or 30 min.

[0045] This step involves gently peeling off the film immediately after pre-curing and stabilization of the pattern layer. At this point, the film can be completely peeled off without any residue or raised edges, and the ink remains intact and undamaged, achieving a qualitative change of "wetting force-driven penetration" rather than "mechanical bonding".

[0046] S4, Double-layer clear varnish sealing and differentiated curing: S4-1. Spray a transparent protective varnish onto the pre-cured transfer workpiece and cure it differently according to the material of the substrate workpiece. The dry film thickness of the protective varnish is 30μm to 40μm, preferably 35μm.

[0047] In some embodiments, the substrate workpiece is an iron part, which is cured at 145°C to 155°C for 35 to 45 minutes. The iron part includes any one of carbon steel workpieces, galvanized steel workpieces, aluminum alloy workpieces, magnesium alloy workpieces, or titanium alloy workpieces. Exemplarily, the substrate workpiece is a galvanized steel workpiece.

[0048] In some embodiments, the substrate workpiece is a plastic part, cured at 80°C to 90°C for 35 to 45 minutes. The plastic part includes any one of ABS (acrylonitrile-butadiene-styrene copolymer), PP (polypropylene), PC / ABS alloy (polycarbonate / acrylonitrile-butadiene-styrene copolymer alloy), CFRP (carbon fiber reinforced plastic), or GFRP (glass fiber reinforced plastic). Exemplarily, the substrate workpiece is PP.

[0049] It should be noted that the specific materials of the aforementioned iron and plastic parts are merely illustrative examples of the present invention and do not constitute a limitation thereof. Those skilled in the art should understand that the iron parts are not limited to the carbon steel, galvanized steel, aluminum alloy, magnesium alloy, or titanium alloy listed above; any metal substrate capable of withstanding the curing temperature without deformation or performance degradation can be used in the present invention. Similarly, the plastic parts are not limited to the ABS, PP, PC / ABS alloy, CFRP, or GFRP listed above; any plastic part capable of withstanding the curing temperature without softening or deformation can be used in the present invention.

[0050] S4-2, Overall grinding, polishing and finishing: The workpiece is sanded with 2000-grit sandpaper and then mirror polished to obtain a workpiece product with an embedded water decal paint film; its orange peel mirror effect can achieve: short wave S≤15; long wave L≤8; DOI≥90.

[0051] The purpose of sanding is to remove minor imperfections such as tiny particles, orange peel texture, and dust spots from the surface of the clear coat, providing a smooth and uniform surface base for subsequent mirror polishing. Sanding can be done dry or wet, with wet sanding being preferred to reduce heat and dust generated during the process, preventing the clear coat from softening or being damaged due to localized overheating. The sanding pressure should be even and gentle, aiming for a uniform matte finish on the clear coat surface, avoiding excessive sanding in certain areas that could thin the clear coat or even sand it through. After sanding, the workpiece surface can be rinsed with water to remove sanding debris and dust, then dried with compressed air or allowed to air dry naturally.

[0052] Mirror polishing gives the workpiece surface a mirror-like gloss. Polishing can be performed mechanically, manually, or a combination of both. For mechanical polishing, a polishing machine is used with a polishing pad and polishing compound to polish the workpiece surface. The polishing pad is preferably a wool pad or sponge pad, and the polishing compound is preferably a water-based or oil-based mirror polishing compound with abrasive particles preferably in the nanometer or submicron range. During polishing, the polishing machine should move at a moderate speed across the workpiece surface to avoid prolonged contact in the same position, which could lead to localized overheating or over-polishing of the varnish layer. The polishing pressure should be uniform and moderate, aiming to gradually achieve a mirror-like gloss on the varnish layer surface. For manual polishing, a lint-free cloth or microfiber cloth is applied to the workpiece surface with mirror polishing compound, and the surface is repeatedly wiped in a circular or reciprocating motion until a mirror-like gloss is achieved. Manual polishing is suitable for areas with complex shapes or those difficult to reach with mechanical polishing. During the polishing process, multiple passes can be performed as needed. First, use a coarser polishing compound to remove grinding marks, and then use a finer polishing compound for fine polishing, ultimately obtaining a mirror-like surface without visible scratches, haze, and uniform gloss.

[0053] It should be noted that the 2000-grit sandpaper and mirror polishing process described are merely one exemplary embodiment of the present invention. Those skilled in the art should understand that the grit of the sandpaper can be appropriately adjusted according to the degree of surface defects in the varnish layer and the desired finishing effect; for example, 1500-grit or 3000-grit sandpaper can also be used. The polishing method and polishing agent can also be flexibly determined according to the workpiece material, shape, and production volume requirements, as long as the finishing and mirror-like treatment of the varnish layer surface can be achieved.

[0054] The following are specific embodiments. Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0055] Example 1 This embodiment provides a method for embedding water-based decal paint films on the surface of a workpiece, specifically including the following steps: S1. Water decal constant temperature immersion activation: The water decals were soaked in pure water at 28°C for 20 seconds to obtain activated water decals.

[0056] S2, Precise alignment and embedded transfer: S2-1. Spray primer onto the substrate workpiece and bake at 80℃ for 30 minutes. Immediately use 2000 grit sandpaper to finely sand the surface of the primer layer until it changes from a glossy state to a matte state, without sanding through the primer layer or exposing the substrate. Wipe off the oil with anhydrous ethanol.

[0057] S2-2. Using a flexible scraping process, activated water decals are applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece.

[0058] S3, Pre-curing and Shaping, and Coating Peeling: The water transfer print workpiece is pre-cured and shaped by baking at 78℃ for 25 minutes. The film of the activated water decal is then peeled off to obtain the pre-cured transfer print workpiece.

[0059] S4, Double-layer clear varnish sealing and differentiated curing: The pre-cured transfer workpiece is sprayed with a transparent protective varnish and cured at 150℃ for 40 minutes. The dry film thickness of the protective varnish is 35μm. The entire workpiece is sanded with 2000-grit sandpaper and then mirror polished to obtain a workpiece product with an embedded water decal paint film. The orange peel mirror effect is achieved as follows: short wave S=1.9; long wave L=5.6; DOI=94.9.

[0060] Example 2 This embodiment provides a method for embedding water-based decal paint films on the surface of a workpiece, specifically including the following steps: S1. Water decal constant temperature immersion activation: Water decals are soaked in pure water at 30℃ for 15 seconds to obtain activated water decals.

[0061] S2, Precise alignment and embedded transfer: S2-1. Spray primer onto the substrate workpiece and bake at 85℃ for 25 minutes. Let it stand for 1 hour. Use 2000 grit sandpaper to finely sand the primer layer until the surface changes from glossy to matte, without sanding through the primer layer or exposing the substrate. Wipe off the oil with anhydrous ethanol.

[0062] S2-2. Using a flexible scraping process, activated water decals are applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece.

[0063] S3, Pre-curing and Shaping, and Coating Peeling: The water transfer print workpiece is pre-cured and shaped by baking at 80℃ for 20 minutes. The film covering the water decal is then peeled off to obtain the pre-cured transfer print workpiece.

[0064] S4, Double-layer clear varnish sealing and differentiated curing: The pre-cured transfer workpiece is sprayed with a transparent protective varnish and cured at 155℃ for 30 minutes. The dry film thickness of the protective varnish is 35μm. The entire workpiece is sanded with 2000-grit sandpaper and then mirror polished to obtain a workpiece product with an embedded water decal paint film. The orange peel mirror effect is achieved as follows: short wave S=1.7; long wave L=4.2; DOI=96.3.

[0065] Example 3 This embodiment provides a method for embedding water-based decal paint films on the surface of a workpiece, specifically including the following steps: S1. Water decal constant temperature immersion activation: Water decals are soaked in pure water at 25°C for 25 seconds to obtain activated water decals.

[0066] S2, Precise alignment and embedded transfer: S2-1. The substrate workpiece is baked at 75℃ for 35 minutes after the primer is applied, and left for 2 hours. Then, it is finely sanded with 2000 grit sandpaper until the surface of the primer layer changes from a glossy state to a matte state, without sanding through the primer layer or exposing the substrate. Finally, it is wiped with anhydrous ethanol to remove oil.

[0067] S2-2. Using a flexible scraping process, activated water decals are applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece.

[0068] S3, Pre-curing and Shaping, and Coating Peeling: The water transfer print workpiece is pre-cured and shaped by baking at 75℃ for 30 minutes. The film covering the water decal is then peeled off to obtain the pre-cured transfer print workpiece.

[0069] S4, Double-layer clear varnish sealing and differentiated curing: The pre-cured transfer workpiece is sprayed with a transparent protective varnish and cured at 145℃ for 40 minutes. The dry film thickness of the protective varnish is 35μm. The entire workpiece is sanded with 2000-grit sandpaper and then mirror polished to obtain a workpiece product with an embedded water decal paint film. The orange peel mirror effect is achieved as follows: short wave S=1.9; long wave L=6.3; DOI=95.7.

[0070] Example 4 This embodiment provides a method for embedding a water-based decal paint film on the surface of a workpiece. The specific steps are the same as in Embodiment 1, except that: the substrate workpiece selected in step S2 is a plastic part, the curing temperature in step S4 is 80°C, the curing time remains unchanged, and the thickness of the protective clear varnish dry film remains unchanged, resulting in a cured workpiece with an orange peel mirror effect of: short wave S=2.0; long wave L=5.9; DOI=95.9.

[0071] Example 5 This embodiment provides a method for embedding a water-based decal paint film on the surface of a workpiece. The specific steps are the same as in Embodiment 2, except that: the substrate workpiece selected in step S2 is a plastic part, the curing temperature in step S4 is 85°C, the curing time remains unchanged, and the thickness of the protective clear varnish dry film remains unchanged, resulting in a cured workpiece with an orange peel mirror effect of: short wave S=1.6; long wave L=4.5; DOI=96.0.

[0072] Example 6 This embodiment provides a method for embedding a water-based decal paint film on the surface of a workpiece. The specific steps are the same as in Embodiment 3, except that: the substrate workpiece selected in step S2 is a plastic part, the curing temperature in step S4 is 75°C, the curing time remains unchanged, and the thickness of the protective clear varnish dry film remains unchanged, resulting in a cured workpiece with an orange peel mirror effect of: short wave S=1.4; long wave L=4.5; DOI=96.0.

[0073] Comparative Example 1 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the water-based decal constant temperature immersion activation in step S1 is 20°C, and the activation time remains unchanged; the remaining parameters and operations are the same as in Example 1, resulting in a cured workpiece.

[0074] Comparative Example 2 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the water-based decal constant temperature immersion activation in step S1 is 35°C, and the activation time remains unchanged; the remaining parameters and operations are the same as in Example 1, resulting in a cured workpiece.

[0075] Comparative Example 3 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the water-based decal constant temperature immersion activation temperature in step S1 remains unchanged, but the activation time is adjusted to 60s; the remaining parameters and operations are the same as in Example 1, resulting in a cured workpiece.

[0076] Comparative Example 4 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the pre-curing and shaping temperature in step S3 is 90°C and the baking time is 15 minutes, i.e., high-temperature short-time pre-curing is used; the remaining parameters and operations are the same as in Example 1, and a cured workpiece is obtained.

[0077] Comparative Example 5 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the pre-curing and shaping temperature in step S3 is 65°C and the baking time is 40 minutes, i.e., low-temperature long-time pre-curing is used; the remaining parameters and operations are the same as in Example 1, and a cured workpiece is obtained.

[0078] Comparative Example 6 This comparative example provides a method for embedding a water-based decal paint film on the surface of a workpiece. The difference from Example 1 is that the curing temperature in step S4 is 80°C, while the curing time remains unchanged. That is, the curing conditions for the iron part are the same as those for the plastic part. The remaining parameters and operations are the same as in Example 1, resulting in a cured workpiece.

[0079] Performance testing The properties of the cured workpieces prepared in Examples 1-6 and Comparative Examples 1-6 were evaluated.

[0080] The performance indicators, testing standards, and rating methods examined are shown in Table 1, and the test results are shown in Tables 2 and 3.

[0081] The grading criteria for adhesion are as follows: Grade 0: The cut edges are completely smooth, and there is no coating peeling within the mesh; Level 1: Only a small amount of coating peels off at the cross-shaped incision point, with an affected area ≤5%; Grade 2: Coating peels off at the intersection of incisions or along the edge of the blade, with a peeling area >5% and ≤15%; Level 3: Large fragments fall off along the edge of the blade, and some grids are peeled off in one piece; the area of ​​the peeling off is >15% and ≤35%. Level 4: Large areas of the blade have peeled off, with many square pieces falling off in one piece; the area of ​​peeling off is >35% and ≤65%. Level 5: The degree of detachment exceeds Level 4, and the detached area is greater than 65%.

[0082] The classification criteria for the overall damage level are as follows: Grade 1: The paint film is intact, without bubbles, rust spots, or cracks; there is only very slight loss of gloss, which is almost invisible to the naked eye; Level 2: Very few tiny bubbles, slight discoloration at the edges; no rust, no paint peeling, no cracking; Level 3: Localized noticeable discoloration, a small number of medium-sized bubbles, no substrate corrosion; minor cracks are permissible, but peeling and flaking are not allowed; Level 4: Numerous bubbles, localized paint film blistering, localized substrate rusting, and localized coating cracking; Level 5: Extensive blistering, peeling, and flaking of the paint film, and extensive corrosion of the substrate.

[0083] Table 1: Summary of Performance Indicators, Testing Standards, and Rating Methods Table 2: Performance test results for each embodiment Table 3: Performance test results of each comparative example As can be seen from the results in Table 2, under the precise control of the wetting temperature and wetting time for the activation of the water decals, and under the differentiated curing conditions after pre-curing and spraying of protective clear varnish, the embodiments of the present invention all meet the index requirements, namely, water resistance adhesion grade 0, stone impact resistance ≤ grade 2, damp heat comprehensive damage grade 1 with adhesion grade 0, and high and low temperature adhesion grade 0. This indicates that the method of the present invention forms a good interface fusion and integrated composite structure between the pattern layer, the primer film, and the protective varnish film.

[0084] As can be seen from the results in Table 3, in Comparative Example 1, the activation and wetting temperature of the water decal was lower than 25℃, the ink was not fully activated, and the wetting force with the primer film was insufficient, resulting in slight bubbles on the surface during the water resistance test. Its water resistance adhesion and high and low temperature adhesion were both reduced to level 1.

[0085] In Comparative Example 2, because the activation and wetting temperature of the water decal was higher than 30°C, the pattern layer was excessively dissolved. Not only did the water resistance and adhesion to high and low temperatures drop to level 1, but the pattern also diffused and shifted during application.

[0086] Comparative Example 3 had an excessively long activation and wetting time (60s) for the water decal, resulting in excessive separation between the pattern layer and the base paper during step S2. This caused the decal to tear easily and leave paper scraps during bonding, leading to surface blistering during the water resistance test. Not only did the water resistance adhesion and high / low temperature adhesion both drop to level 1, but the stone impact adhesion also dropped to level ≤3.

[0087] Comparative Example 4 suffered from premature curing of the primer film due to excessively high pre-curing temperature in step S3 (90℃ / 15min), even with a shortened time. This resulted in the loss of wetting power, with the pattern only physically adhering. Water resistance, resistance to damp heat, and resistance to high and low temperature adhesion all dropped to level 2, and stone chip adhesion dropped to ≤ level 3.

[0088] Comparative Example 5 had an excessively low pre-curing temperature in step S3 (65℃ / 40min), and the primer film did not reach the surface drying window. Even with extended time, the moisture in the pattern layer could not be fully evaporated, causing the pattern to float and fall off after washing. During the water resistance test, surface blistering occurred, and the water resistance, damp heat resistance, and high and low temperature adhesion all dropped to level 2.

[0089] Comparative Example 6 uses the same curing conditions as plastic parts for iron parts. The curing temperature is insufficient, resulting in incomplete cross-linking of the double-layer paint film. The thermal expansion of the iron parts causes the embedded pattern to delaminate. The water resistance adhesion drops to level 3, the stone chip resistance adhesion is ≤ level 3, and the wet heat resistance and high and low temperature resistance adhesion both drop to level 2.

[0090] In summary, the wetting parameters in step S1, the pre-curing parameters in step S3, and the differentiated curing conditions in step S4 of this invention are key to ensuring that the pattern layer wets and penetrates the primer film and the protective film, achieves interfacial fusion, and integrates cross-linking. Any deviation of the parameters from the specified range will lead to technical problems such as insufficient or excessive ink activation, loss of film wetting power, and insufficient cross-linking, which in turn will cause deterioration of product performance such as decreased adhesion, blistering, and delamination. The process parameter window of this invention can stably produce water-based decal film embedded workpieces with completely embedded patterns, excellent adhesion, and good weather resistance.

[0091] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for embedding a water-based decal paint film into the surface of a workpiece, characterized in that, Includes the following steps: S1. Soak the water decals in water at 25℃~30℃ for 15s~25s to obtain activated water decals; The water decal includes a PVA film-coated base paper, a water-based ink intermediate layer, an acrylic resin isolation varnish layer, and a film coating. S2. During the surface drying window period after the primer is sprayed onto the substrate workpiece, the activated water decal is applied to the surface of the substrate workpiece to obtain a water transfer printed workpiece. The surface drying window period is within 2 hours after the substrate workpiece is sprayed with primer and baked to a touch-dry state. S3. Bake the water transfer printed workpiece at 75℃~80℃, peel off the coating, and obtain the pre-cured transfer printed workpiece; S4. Spray a protective varnish onto the surface of the pre-cured transfer workpiece and cure it to obtain a workpiece product with an embedded water decal paint film.

2. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 1, characterized in that, The baking temperature in step S2 is 75℃~85℃, and the baking time is 25min~35min.

3. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 1, characterized in that, The baking time described in step S3 is 20 to 30 minutes.

4. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 1, characterized in that, The substrate workpiece includes at least one of iron or plastic parts.

5. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 3, characterized in that, The iron part includes any one of carbon steel workpiece, galvanized steel workpiece, aluminum alloy workpiece, magnesium alloy workpiece or titanium alloy workpiece; when the base material workpiece is an iron part, the curing temperature in step S4 is 145℃~155℃ and the time is 35min~45min.

6. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 3, characterized in that, The plastic part includes any one of ABS, PP, PC / ABS alloy, CFRP or GFRP; when the substrate workpiece is a plastic part, the curing temperature in step S4 is 80℃~90℃ and the time is 35min~45min.

7. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 1, characterized in that, The dry film thickness of the protective varnish described in step S4 after curing is 30μm to 40μm.

8. The method for embedding water-based decal paint film on the surface of a workpiece as described in claim 1, characterized in that, Step S2 further includes roughening and degreasing the surface of the substrate workpiece after baking and before applying the active water decal.