A closed-loop circulation process for multi-element staged extraction of deep-well black brine
By using a closed-loop circulation process for multi-element cascade extraction of deep-well black brine, the problems of low element extraction, high energy consumption, and safety risks in the development of deep-well black brine resources have been solved. This process achieves full element extraction and closed-loop circulation, reducing equipment investment and operating costs.
Patent Information
- Application Number
- CN202611426191.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for the development of deep-well black brine resources suffer from several problems, including limited extraction of elements, lack of treatment for high-sulfur brine, high energy consumption, failure to achieve true closed-loop circulation, limited product variety, poor economic efficiency, and unresolved safety risks associated with high-sulfur brine.
The closed-loop circulation process of multi-element cascade extraction of deep-well black brine is adopted, which includes steps such as raw brine pretreatment, two-stage desulfurization, brine refining, MVR evaporation and crystallization, boron extraction, iodine extraction, bromine extraction, lithium extraction and rubidium and cesium recovery. Through a closed structure and negative pressure operation, the process achieves full-element cascade extraction and closed-loop circulation, avoids mother liquor discharge, and reduces energy consumption and cost.
It has achieved the stepwise and orderly extraction of 13 elements from deep-well black brine, making full use of resources, reducing equipment investment and operating costs, and realizing zero-emission and safe and efficient utilization.
Smart Images

Figure CN123105555A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of salt chemical technology, specifically relating to a closed-loop circulation process for multi-element cascade extraction of deep-well black brine, which is suitable for the comprehensive development and utilization of deep brine containing high levels of hydrogen sulfide and high levels of calcium and magnesium components, such as deep natural black brine in the Zigong area. Background Technology
[0002] Brine is a liquid mineral rich in various elements such as potassium, sodium, lithium, boron, bromine, iodine, strontium, rubidium, and cesium. Currently, the development and utilization of brine in China generally involves selectively extracting some high-value-added components, while the unextracted components are discarded with the old brine, resulting in serious waste of resources and environmental pollution.
[0003] Some mining areas are rich in deep black brine resources, which, in addition to being rich in sodium chloride, also contain potassium, lithium, boron, bromine, iodine, strontium, rubidium, cesium, as well as calcium, magnesium and other valuable elements. The deep black brine in Zigong is a typical example. It also contains high concentrations of hydrogen sulfide (about 1000 mg / L), polysulfides, organic matter and iron salts and other impurities. Its composition is extremely complex and has not been developed and utilized on a large scale for a long time.
[0004] The main shortcomings of existing technologies are: (1) Few types of elements are extracted: Most processes only extract 2-3 elements, and a large number of associated elements are not utilized; (2) Not targeting high-sulfur brine: Existing processes are mostly for salt lake brine or oil and gas field brine, and lack systematic treatment solutions for deep well black brine with high hydrogen sulfide and high calcium and magnesium content; (3) High energy consumption: Traditional processes use multi-effect evaporation, which consumes a lot of energy and has high operating costs; (4) Failure to achieve true closed-loop circulation: Some processes still have mother liquor discharge, resulting in resource waste and environmental pollution; (5) Few product types and poor economic efficiency: Due to the limited number of extractable elements and the high extraction cost of a single element, the development of deep-well black brine has long been regarded as "more bark than meat" and economically unfeasible. (6) Pursuing single-pass yield leads to excessive equipment investment: Traditional processes pursue the maximization of single-pass yield, which forces the equipment to be enlarged and results in high investment intensity; (7) The safety risks of high-sulfur brine have not been systematically addressed: Existing technologies for treating H2S mostly involve "blowing out and then burning", which poses safety risks.
[0005] Therefore, we still need to conduct research and development in order to achieve efficient utilization of underground natural black brine resources and maximize their value. Summary of the Invention
[0006] The purpose of this invention is to provide a closed-loop recycling process for the multi-element cascade extraction of deep-well black brine, a liquid mineral rich in various elements such as sodium, potassium, lithium, boron, bromine, iodine, strontium, rubidium, cesium, calcium, and magnesium. In this process, the main components are extracted stepwise and in an orderly manner, achieving a closed-loop process, no mother liquor discharge, low cost, high yield, energy saving, and environmental protection.
[0007] To achieve the above-mentioned objectives, the specific technical solution of this invention is as follows: A closed-loop circulation process for multi-element cascade extraction of deep-well black brine includes the following steps: (1) Physical filtration of raw brine pretreatment: The raw brine is subjected to closed multi-stage filtration to remove suspended solids and obtain filtered brine; (2) Two-stage desulfurization: The filtered brine obtained in step (1) is degassed under negative pressure to release H2S gas, resulting in degassed brine and H2S-containing gas; The H2S-containing gas is recovered and converted into sulfur by a complexing iron-sulfur recovery device, and then processed into industrial sulfur products by a sulfur melting kettle; The degassed brine is subjected to deep desulfurization with FeCl3, and then separated by air flotation to obtain a clear liquid with H2S ≤ 10 mg / L; Steps (1) and (2) All equipment in contact with sulfur-containing raw brine is a closed structure, with a negative pressure extraction system connected to the top to maintain a slight negative pressure operation; the extracted H2S-containing gas is sent to the complex iron-sulfur recovery device for treatment; (3) Brine refining: the clear liquid obtained from the air flotation separation in step (2) is successively subjected to NaOH precipitation to remove magnesium to obtain Mg(OH)2 product, and Na2CO3 precipitation to remove calcium and strontium to obtain refined brine and CaCO3+SrCO3 mixed residue; the obtained CaCO3+SrCO3 mixed residue is leached with NH4Cl, plate and frame filter, and Na2CO3 is added to the filtrate for precipitation. The amount of sodium carbonate added is 1.05 to 1.05 of the stoichiometric ratio of strontium ions in the filtrate.SrCO3 product and calcium carbonate residue were obtained by 10-fold separation; the calcium carbonate residue was reacted with citric acid to obtain food-grade calcium citrate product. (4) MVR evaporation crystallization: The refined brine obtained in step (3) is subjected to MVR forced circulation evaporation crystallization; the MVR forced circulation evaporation crystallization adopts a DTB crystallizer and achieves graded separation of gypsum, sodium chloride and potassium chloride through three-stage washing of the salt leg; the obtained product enters the three-stage washing of the salt leg, the bottom of the salt leg is CaSO4 slurry, which enters the hydrocyclone and horizontal screw centrifuge in sequence, and then is washed and crystallized to obtain α-type high-strength gypsum; the upper part of the salt leg is NaCl slurry, which is centrifuged to produce NaCl product, and the residue is NaCl centrifugal mother liquor and washing water; the NaCl centrifugal mother liquor and washing water are diluted to unsaturation, crystallized by KCl flash crystallizer and treated by KCl centrifuge to obtain KCl product and KCl centrifugal mixed mother liquor; in the above evaporation crystallization process, valuable elements such as lithium, boron, bromine, iodine, rubidium and cesium do not enter the sodium chloride and potassium chloride products, and are naturally enriched in the evaporation mother liquor; (5) Boron extraction: The KCl centrifuged mixed mother liquor obtained in step (4) is acidified, extracted, back-extracted, and evaporated by a heat pump to crystallize, to obtain boric acid product and raffinate after boron extraction; (6) Iodine extraction: Acidification, oxidation, resin adsorption, and sublimation are performed on part of the raffinate after boron extraction to obtain iodine product and tail liquor after iodine extraction; (7) Bromine extraction: Acidification, oxidation, resin adsorption, and distillation are performed on part of the tail liquor after iodine extraction to obtain bromine product and tail liquor after bromine extraction; (8) Lithium extraction: Precision filtration, nanofiltration, calcium and magnesium removal by chelating resin, and lithium precipitation by adding Na2CO3 are performed on part of the tail liquor after bromine extraction to obtain lithium carbonate product and lithium precipitation mother liquor; (9) Rubidium and cesium recovery: A portion of the lithium precipitation mother liquor is concentrated by evaporation, crystallized, and filtered while hot to obtain NaCl / KCl filter cake and filtrate. The filtrate is further concentrated and then vacuum dried to obtain rubidium and cesium mixed salt; (10) Closed-loop recycling of mother liquor: A portion of the bromine extraction tail liquor from step (7) is returned to step (3); a portion of the raffinate after boron extraction from step (5) is returned to step (3); a portion of the lithium precipitation mother liquor from step (8) is returned to step (3); a portion of the KCl centrifuged mixed mother liquor from step (4) is returned to the front end of step (4) to participate in MVR recirculation; the filtrate after NH4Cl leaching in step (3) is recycled within the strontium recovery section; the NaCl / KCl filter cake dissolved in step (9) is returned to the MVR in step (4).
[0008] As a preferred embodiment of this application, in step (2) of the process, the vacuum degree of the negative pressure degassing is -0.06 to -0.08 MPa, the H2S conversion rate of the complexed iron-sulfur recovery is ≥99%, the operating temperature of the sulfur melting kettle is 120-140℃, and the FeCl3 dosage is 1.2 to 1.8 times the theoretical stoichiometric ratio of H2S.
[0009] In a preferred embodiment of this application, in step (3) of the process, the pH for precipitating magnesium with NaOH is 10.5-11.0; the pH for precipitating calcium and strontium with Na2CO3 is 9.0-9.5; and the magnesium ions in the refined brine are Mg. 2+ ≤40mg / L; calcium ions are not deeply removed, and the calcium ion concentration is controlled according to the sulfate ion concentration in the brine, with the molar amount of calcium ions controlled to be 1.05 to 1.15 times the molar amount of sulfate ions.
[0010] As a preferred embodiment of this application, in step (3) of the process, the NH4Cl leaching conditions are as follows: NH4Cl mass fraction 15-20%, NH4Cl to SrCO3 molar ratio 1:1~5:1, liquid-solid mass ratio 1:1~5:1, reaction temperature 20~80℃, reaction time 1~3h; SrCO3 leaching rate ≥95%, product purity ≥98%.
[0011] As a preferred embodiment of this application, in step (3) of the process, the conditions for the citric acid reaction are: the molar ratio of citric acid to calcium carbonate is 2:3, the excess of citric acid is 1%~5%, the reaction temperature is 50-70℃, the reaction time is 2-3h, and the product purity is ≥99%.
[0012] As a preferred embodiment of this application, in step (4) of the process, the temperature of the MVR forced circulation evaporation crystallization is 106-109℃, and the operating pressure is -0.02 to -0.05MPa; the temperature of the KCl flash evaporation crystallization is 40-50℃, and the vacuum degree is 7-12kPa absolute pressure.
[0013] As a preferred embodiment of this application, in step (5) of the process, the extractant used for extraction is 50% isooctanol + 50% sulfonated kerosene by volume, the extraction ratio O / A = 1:1 to 2:1, the number of extraction stages is 5, and the extraction rate is ≥97%; the back-extraction ratio O / A = 1:1 to 2:1, the number of back-extraction stages is 4, and the back-extraction rate is ≥98%.
[0014] As a preferred embodiment of this application, in step (6) of the process, the oxidation ORP of iodine extraction is 520-550 mV, and the effluent I... - ≤0.2mg / L, sublimation temperature is 98-100℃.
[0015] As a preferred embodiment of this application, in step (7) of the process, the oxidation ORP of bromine extraction is 700-800mV, the distillation temperature is 58-60℃, and the purity of the bromine product is ≥99.8%.
[0016] As a preferred embodiment of this application, in step (8) of the process, the chelating resin is CH-93 type, and the effluent Ca 2+ +Mg 2+ ≤5mg / L; the lithium precipitation temperature is 85-95℃, the pH is 10-11; the sodium carbonate dosage is 1.05-1.10 times the theoretical amount, and the lithium carbonate product purity is ≥99.5%.
[0017] As a preferred embodiment of this application, in step (10) of the process, the closed-loop circulation of the mother liquor includes: at least a portion of the bromine extraction tail liquor is returned to step (3), at least a portion of the raffinate is returned to step (3), and at least a portion of the lithium precipitation mother liquor is returned to step (3); the return ratio is automatically adjusted by the system material balance.
[0018] As a preferred embodiment of this application, in steps (1) and (2) of the process, all equipment in contact with the sulfur-containing brine is a closed structure, with a negative pressure extraction system connected to the top to maintain a slight negative pressure operation; the extracted H2S-containing gas is sent to a complex iron-sulfur recovery device for processing.
[0019] As a preferred embodiment of this application, in step (4) of the process, the MVR forced circulation evaporation crystallization uses a DTB crystallizer and achieves graded separation of gypsum, sodium chloride and potassium chloride through three-stage washing with salt legs; the enriched mother liquor enters the step-by-step extraction section in steps (5) to (9).
[0020] As a preferred embodiment of this application, in step (10) of the process, the closed-loop circulation of the mother liquor ensures that the single-pass yield of each extraction section does not need to be maximized, and the total yield is gradually approached through multiple cycles.
[0021] Analysis of the necessity of sequential processing in this process section: The sequence of processes in the deep-well black brine multi-element cascade extraction closed-loop circulation process of this invention is determined comprehensively based on the composition of the black brine material, the chemical behavior of each element, the phase precipitation law, reagent interference, separation selectivity, and the material balance of the closed-loop circulation system. Changing the sequence of processes or deviating the key process parameters from the set range will cause problems such as reagent interference, decreased product purity, reduced recovery rate of target elements, equipment scaling and blockage, and inability of the system to achieve closed-loop circulation.
[0022] (1) Raw brine pretreatment → Two-stage desulfurization must be placed at the very beginning. Deep well black brine contains high concentrations of H2S, polysulfides, and suspended solids. If the closed negative pressure two-stage desulfurization is not completed first, the brine containing H2S will directly enter the subsequent refining and MVR evaporation stages: under the evaporation and heating conditions, a large amount of H2S will escape, destroying the micro-negative pressure safety control of the entire set of equipment; H2S and polysulfides will consume the NaOH and Na2CO3 added in the subsequent magnesium removal and calcium and strontium removal processes, and at the same time generate colloidal precipitates of metal sulfides, making solid-liquid separation difficult; sulfides will cause poisoning and inactivation of the subsequent extraction resin and chelating resin. Therefore, suspended solids filtration and H2S removal must be completed at the very beginning, and the H2S of the clear liquid must be controlled to be ≤10mg / L.
[0023] (2) The necessity of placing the brine refining section before MVR. The core objective of this section is to strictly and deeply remove magnesium ions, retain calcium ions according to the sulfate concentration at a molar ratio of 1.05~1.15:1, separate calcium and strontium slag, and utilize them as resources. Magnesium ions must be deeply removed to Mg2+ before MVR. 2+ ≤40mg / L; otherwise, under evaporation conditions, magnesium hydroxide and magnesium silicate-like gelatinous sludge will form, adhering to the walls of the MVR heat exchanger tubes and the inside of the DTB crystallizer, reducing heat exchange efficiency and, in severe cases, causing equipment blockage. Calcium ions are not deeply removed and remain in the MVR, causing Ca... 2+ With SO4 in the system 2- Calcium sulfate is directionally generated at the salt leg of the DTB crystallizer, and gypsum and sodium salt are separated by three-stage washing at the salt leg. If all the calcium is precipitated and removed beforehand, sulfate ions in the brine cannot precipitate as gypsum, and will continue to accumulate in the closed-loop mother liquor. This results in a large amount of lithium sulfate co-precipitated impurities in the later lithium precipitation stage, directly reducing the purity of the lithium carbonate product. The calcium-strontium mixed residue must be separated on-site in the refining stage; otherwise, strontium salts will mix into sodium chloride, potassium chloride, and gypsum products, causing cross-contamination among multiple products.
[0024] (3) The core logic of placing MVR evaporation and crystallization before the extraction of valuable elements. Most existing brine processes first extract and separate boron, iodine, and bromine, and then evaporate to produce salt. This invention first uses MVR to produce salt and enrich the brine, and then carries out the extraction of rare and dispersed elements. The initial concentrations of lithium, boron, bromine, iodine, rubidium, and cesium in brine are low. If the original brine is directly extracted to extract boron, iodine, and bromine, the volume of the processed liquid is huge, and the scale of the extraction equipment and resin adsorption equipment is multiplied. This process takes advantage of the characteristic that sodium chloride and potassium chloride crystallize out first with the solubility of evaporation and concentration. By using MVR to produce salt, boron, lithium, bromine, iodine, rubidium, and cesium are retained in the mother liquor to achieve natural enrichment. The product benefits of salt production cover the energy consumption of evaporation. If the order is reversed, and boron, iodine, and bromine are extracted first and then MVR is used to produce salt, the volume of the liquid is large and the equipment investment is greatly increased. Moreover, if the raffinate after extraction is then evaporated, the organic extractant will be carried into the MVR evaporator. At high temperature, the organic phase decomposes and carbonizes, causing coking in the evaporator and the salt product contains organic impurities.
[0025] (4) Boron extraction must be performed before iodine and bromine extraction. The boron extraction system is isooctanol esterification extraction under acidic conditions. Boron extraction should be prioritized to separate and remove boron from the mother liquor in advance. If iodine and bromine extraction are performed before boron extraction, chlorine gas needs to be introduced for oxidation, which will generate a large amount of hypohalous acid and halogen elements in the system. When halogen elements enter the boron extraction process, they will cause the isooctanol extractant to be oxidized and destroyed by halogens, resulting in increased extractant loss, decreased extraction efficiency, and the introduction of halogen impurities into the boric acid product. If boron is not separated in advance, the mother liquor will continue to circulate in a closed loop, and boron will continue to accumulate. Under the high pH alkaline conditions of subsequent lithium precipitation, lithium borate co-precipitate will be generated, directly contaminating the lithium carbonate product.
[0026] (5) The necessity of iodine extraction preceding bromine extraction. The oxidation potential of iodide ions is lower than that of bromide ions. - Preferably oxidized to I2 by Cl2; bromide ions have a higher oxidation potential and require a higher ORP to oxidize to Br2. The process control for the iodine extraction section maintains an ORP of 520~550mV, under which only I2 is oxidized. - Iodine is oxidized and Br is released. - It is basically not oxidized; when the ORP is increased to 700~800mV, Br - Only then is a large amount of bromine produced through oxidation. If the order is reversed, with bromine extracted first and then iodine extracted, the ORP needs to be increased to 700-800mV to oxidize bromide ions. Iodine and bromine will be oxidized simultaneously, and I2 will be mixed into the bromine material system. Iodine impurities will be difficult to separate, the purity of the bromine product will decrease, and a large amount of iodine will be consumed, making it impossible to recover the iodine product separately later.
[0027] (6) The necessity of placing lithium precipitation after iodine and bromine precipitation. The lithium precipitation section is a strongly alkaline high-temperature environment (pH 10~11, 85~95℃). If lithium precipitation is carried out in advance, iodine and bromide ions in the system will undergo disproportionation reaction under alkaline and heated conditions to generate iodate and bromate. Some of these will co-precipitate with lithium carbonate and enter the lithium carbonate product, causing the lithium salt product to exceed the impurity standard. Lithium precipitation requires a large amount of sodium carbonate, which increases the pH of the system. Under alkaline conditions, iodine and bromine cannot be efficiently recovered by resin adsorption oxidation process.
[0028] (7) Rubidium and cesium recovery is performed after lithium precipitation. Rubidium and cesium carbonates have relatively high solubility and will not precipitate under lithium precipitation conditions, with most of them remaining in the lithium precipitation mother liquor; after multiple rounds of closed-loop circulation, Rb + Cs + Continuous enrichment. If rubidium and cesium recovery is set before lithium precipitation, before lithium is separated, lithium salts will crystallize and precipitate together with rubidium and cesium salts, and the rubidium and cesium mixed salt will be contaminated with a large amount of lithium salts.
[0029] (8) Necessity of controlling key process parameters. Oxidation-reduction potential (ORP): Iodine and bromine extraction rely on ORP for selective oxidation. Too low an ORP results in incomplete oxidation of the target ion and low recovery rate; too high an ORP leads to excessive chlorine, increased side reactions, and excessive resin degradation. pH control in each stage: Desulfurization, refining, extraction, and lithium precipitation all have strict pH windows. pH deviations from these windows can cause incomplete precipitation, failure to extract, and the formation of large amounts of co-precipitated impurities. Calcium to sulfate molar ratio n(Ca) in the refining stage. 2+ ):n(SO4 2- =1.05~1.15:1: If the ratio is too low, there is an excess of sulfate ions, which continue to accumulate in the mother liquor circulation, resulting in lithium sulfate impurities at the downstream lithium precipitation stage; if the ratio is too high, there is an excess of calcium ions, resulting in calcium sulfate scale forming on the MVR heat exchange surface.
[0030] (9) Overall logic of closed-loop mother liquor circulation. This process does not pursue high single-step yield, and the mother liquor is partially recycled in multiple stages; if the mother liquor is completely discharged, valuable elements will be lost with the waste liquid, generating a large amount of saline wastewater; if all mother liquor is forcibly circulated without diversion and extraction, elements such as rubidium, cesium, and boron will accumulate indefinitely, the salinity and viscosity of the system will continue to rise, and the material balance of the system will collapse. Therefore, a diversion mode of "partial return and circulation, and partial entry into the next extraction stage" is adopted.
[0031] In summary, the sequence of processes in this invention is not a simple combination of processes, but is determined based on the chemical characteristics of each component, reagent compatibility, impurity transmission paths, and closed-loop material balance. Changing the sequence of processes or causing key parameters to deviate from the control range will lead to a series of technical consequences, such as deterioration of product purity, increased reagent consumption, equipment scaling and failure, resource loss, and safety hazards.
[0032] Compared with existing technologies, the present invention has the following advantages: (1) Full element stepwise extraction: The stepwise and orderly extraction of 13 products, including sodium, potassium, lithium, boron, bromine, iodine, strontium, rubidium, cesium, calcium, magnesium and sulfur, from deep well black brine has been realized, making full use of the resources; (2) Concentrate first and then extract, enrichment cost approaches zero: Sodium chloride and potassium chloride are extracted first by MVR evaporation and crystallization, and valuable elements are naturally enriched in the mother liquor. The enrichment process is completed simultaneously with salt production, and the enrichment cost is covered by the salt production revenue, without the need for additional enrichment process and energy consumption. (3) Closed-loop circulation does not pursue single-pass yield, and equipment is operated in a down-level manner: Through the closed-loop circulation of mother liquor, the single-pass yield is not deliberately pursued to maximize. For every 10 percentage point reduction in single-pass yield, equipment investment can be reduced by 15-20 percentage points, operating energy consumption is reduced, and maintenance cycle is extended. (4) Truly closed-loop circulation and zero discharge: all mother liquor, washing water, raffinate and tail liquor are returned to the system for recycling, and there is no process wastewater discharge; (5) MVR heat pump evaporation and significant energy saving: No boiler is required, saving about 70% more energy than traditional multi-effect evaporation; (6) Multi-product co-production and superior economic efficiency: The cost of one set of processes is shared by 13 products, and the extraction cost of a single element is greatly reduced, making the development of deep well black brine industrial and economically feasible. (7) Closed negative pressure operation and safety assurance: All equipment in contact with sulfur-containing brine is a closed structure and maintains a slight negative pressure operation, which fundamentally eliminates the risk of H2S leakage. (8) Synergistic removal of impurities: Through multi-stage precipitation, filtration and adsorption units, the system solves the problem of deep well black brine treatment with high sulfur, high calcium and magnesium, organic matter and iron and silicon impurities; (9) Waste heat utilization: The steam from the outlet of the MVR compressor is used in stages for lithium precipitation heating, bromine distillation, rubidium and cesium evaporation and concentration processes to achieve energy utilization in stages. Attached Figure Description
[0033] Figure 1 This is a schematic diagram of a closed-loop circulation process for multi-element cascade extraction of deep-well black brine according to the present invention.
[0034] Figure 2 This is a schematic flowchart of a closed-loop process for multi-element cascade extraction of deep-well black brine according to the present invention.
[0035] Figure 3 This is a simplified flow chart of a closed-loop circulation process for multi-element cascade extraction of deep-well black brine according to the present invention.
[0036] like Figure 1 As shown, the raw brine, after pretreatment and physical filtration, enters the desulfurization section. The desulfurized brine then enters the brine refining section, and the refined brine enters the MVR evaporation and crystallization section, producing sodium chloride, potassium chloride, α-type high-strength gypsum, and by-product freshwater. The KCl centrifuged mixed mother liquor enters the boron extraction section, producing boric acid. At least a portion of the raffinate is returned to the brine refining section for recycling, and the remainder enters the iodine extraction section. The iodine extraction tail liquor enters the bromine extraction section, producing bromine. At least a portion of the bromine extraction tail liquor is returned to the brine refining section for recycling, and the remainder enters the lithium extraction section, producing lithium carbonate. At least a portion of the lithium precipitation mother liquor is returned to the brine refining section for recycling, and the remainder enters the rubidium-cesium recovery section, producing a rubidium-cesium mixed salt.
[0037] Figure 1 The dashed arrow indicates the mother liquor return path, and the solid arrow indicates the forward flow direction of the material. Detailed Implementation
[0038] A closed-loop circulation process for multi-element staged extraction of deep-well black brine includes the following steps: Step S0: Physical filtration for raw brine pretreatment. After the raw brine is pumped to the surface from the well, it passes through a screen to remove large particles ≥1mm, a vibrating screen to separate coarse sand, and a self-cleaning disc filter (filtration accuracy 50-100μm) to remove fine suspended solids. All equipment is a closed structure with a negative pressure air extraction system connected to the top.
[0039] Step S1: Two-stage desulfurization.
[0040] S1-1: The brine filtered in step S0 is sent to a negative pressure degassing tower to release dissolved hydrogen sulfide from the liquid phase under a vacuum of -0.06 to -0.08 MPa. S1-2: The released H2S-containing gas (gas phase) is sent to the complexed iron-sulfur recovery device, where H2S is oxidized to elemental sulfur under the action of a liquid-phase catalyst to obtain sulfur paste; the liquid-phase catalyst is a complexed iron desulfurization catalyst with trivalent iron as the active center and EDTA as the ligand.
[0041] S1-3: Sulfur paste is fed into a sulfur melting kettle, heated to 120-140℃ to melt, and cooled to form industrial sulfur products; S1-4: The liquid phase (degassed brine with residual H2S of about 200-300 mg / L) is treated with FeCl3 solution (the dosage is 1.2 to 1.8 times the theoretical stoichiometric ratio of H2S) for deep desulfurization, and then a clear liquid with H2S ≤ 10 mg / L is obtained by air flotation separation.
[0042] Step S2: Brine refining (without removing SO4) 2- ).
[0043] S2-1 magnesium removal: Add NaOH solution to the clarified liquid obtained by air flotation to control the pH to 10.5-11.0, and Mg... 2+ The Mg(OH)2 product was obtained by sedimentation separation in a Dorr clarifier (Φ30m) and dehydration in a horizontal screw centrifuge. S2-2 calcium and strontium removal: Add Na2CO3 solution to control pH = 9.0-9.5, Ca 2+ and Sr 2+ The purified brine (Mg) is obtained by precipitation in the form of carbonates. 2+ ≤40mg / L; Ca 2+ According to n(Ca) 2+ ):n(SO4 2- (1.05~1.15:1 matching retention) and CaCO3+SrCO3 mixed residue; S2-3 Strontium Recovery: The mixed residue of CaCO3 and SrCO3 is leached with NH4Cl (NH4Cl mass fraction 15-20%, NH4Cl / SrCO3 molar ratio 1:1~5:1, liquid-solid ratio 1:1~5:1, 20~80℃, 1~3h), followed by plate and frame filtration to obtain filtrate and calcium carbonate residue; Na2CO3 is added to the filtrate for precipitation, with the sodium carbonate dosage being 1.05~1.10 times the stoichiometric ratio of strontium ions in the filtrate to obtain SrCO3 product (purity ≥98%). S2-4 Calcium Slag Production of Food-Grade Calcium Citrate: Calcium carbonate slag undergoes three-stage countercurrent washing until Cl... - ≤0.05%, add food-grade citric acid (50-70℃) and react for 2-3 hours. After plate and frame filtration, activated carbon decolorization, cooling crystallization, scraper centrifugation, and fluidized bed drying, food-grade calcium citrate product (purity ≥99%) is obtained.
[0044] Step S3: MVR evaporation and crystallization – concentration followed by extraction.
[0045] The refined brine is fed into an MVR forced circulation evaporator (evaporation temperature 106-109℃), and then evaporated and crystallized in a DTB crystallizer (with a salt leg and three-stage washing process). S3-1. Gypsum slurry is discharged from the bottom of the salt leg and then crystallized to obtain α-type high-strength gypsum; S3-2. NaCl slurry is discharged from the upper part of the salt leg and obtained as industrial salt NaCl by HR centrifuge; S3-3. Part of the NaCl centrifuged mother liquor is returned to the MVR for recirculation, and part is sent to a KCl flash crystallizer (40-50℃, vacuum 7-12kPa) to obtain the KCl product. The KCl is then centrifuged and mixed with the mother liquor (105ml). 3 / h); S3-4 MVR condensate (2.76 million m³) 3 a) Freshwater produced as a byproduct is supplied externally; S3-5. The KCl centrifuged and mixed mother liquor is then transferred to step S4.
[0046] The key feature of this step is that valuable elements such as lithium, boron, bromine, iodine, rubidium, and cesium do not enter the sodium chloride and potassium chloride crystals, but are naturally enriched in the evaporation mother liquor, and the cost of this enrichment is covered by the salt production revenue.
[0047] Step S4: Boron extraction. The KCl centrifuged mixed mother liquor was acidified (pH=3-4), subjected to 5-stage countercurrent extraction (50% isooctanol + 50% sulfonated kerosene), followed by 4-stage countercurrent back-extraction, and heat pump evaporation crystallization (50-70℃, electrically driven) to obtain boric acid product (purity ≥99%) and raffinate; raffinate (62.5m... 3 At least a portion of the ( / h) returns to step S2 loop, and the remainder goes to step S5.
[0048] Step S5: Iodine extraction. Acidification (pH=1.5-2.5), chlorination oxidation (ORP=520-550mV), D201 resin adsorption, Na2SO3 desorption, and electric heating sublimation (98-100℃) are performed to obtain iodine product and iodine extraction tail liquid; the iodine extraction tail liquid proceeds to step S6.
[0049] Step S6: Bromine extraction. Extract iodine from the tailings (62.5 ml). 3 The product is obtained by acidification (pH=3-4), chlorination oxidation (ORP=700-800mV), D301 resin adsorption, alkaline elution, and distillation (58-60℃) to obtain bromine product (purity ≥99.8%) and bromine extraction tail liquid (I). - (≤0.2mg / L); at least a portion of the bromine extraction tail liquid is returned to step S2 for recycling, and the remaining portion enters step S7.
[0050] Step S7: Lithium Extraction. The bromine extraction tail liquid is subjected to precision filtration (5μm + 1μm), nanofiltration, and chelation resin (CH-93 type) to remove calcium and magnesium (calcium in the effluent). 2+ +Mg 2+ ≤5mg / L), lithium precipitation (85-95℃, Na2CO3, pH=10-11), sedimentation aging, scraper centrifugation, and disc drying to obtain lithium carbonate product (purity ≥99.5%, battery grade); at least a portion of the lithium precipitation mother liquor is returned to step S2 for recycling, and the remaining portion enters step S8.
[0051] Step S8: Rubidium and Cesium Recovery. Evaporation and concentration (80-100℃), crystallization and hot filtration (NaCl / KCl filter cake dissolved and returned to MVR), further concentration to Rb + +Cs + =500-800g / L, vacuum dried (80-100℃, -0.08~-0.09MPa), to obtain rubidium-cesium mixed salt for strategic reserve.
[0052] Step S9: Closed-loop circulation of mother liquor. At least a portion of the bromine extraction tail liquor from Step S6 is returned to Step S2; at least a portion of the raffinate from Step S4 is returned to Step S2; at least a portion of the lithium precipitation mother liquor from Step S7 is returned to Step S2; a portion of the NaCl centrifugation mother liquor from Step S3 is returned to the MVR for recycling; the NH4Cl mother liquor from Steps S2-3 is recycled within the strontium recovery section; the NaCl / KCl filter cake from Step S8 is returned to the MVR after dissolution. The amount of mother liquor returned is automatically adjusted by the system's material balance, and the return ratio is determined comprehensively based on the concentration of valuable elements, system water balance, and equipment load. There is no process wastewater discharge from the entire system.
[0053] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and examples. It should be understood that the specific embodiments listed in this invention are merely examples, and this invention is not limited to the specific embodiments described below. For those skilled in the art, any equivalent modifications and substitutions to the embodiments described below are also within the scope of this invention. Therefore, all equivalent transformations and modifications made without departing from the spirit and scope of this invention should be covered within the protection scope of this invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. All reagents or instruments without specified manufacturers are commercially available conventional products. To better illustrate this invention, numerous specific details are given in the following specific embodiments. Those skilled in the art should understand that this invention can also be implemented without certain specific details. In some other embodiments, methods, means, equipment, and steps well known to those skilled in the art are not described in detail in order to highlight the main points of this invention.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. Unless otherwise specified, all units used in this specification are International Standard Units (SI), and all numerical values and ranges appearing in this invention should be understood to include unavoidable systematic errors in industrial production.
[0055] The present invention will be further described in detail below with reference to embodiments, but the implementation of the present invention is not limited thereto.
[0056] In this application, all percentages not explicitly marked are mass percentages.
[0057] The liquid-to-solid ratio is the mass ratio.
[0058] Example 1: Using deep black brine from a mining area in Zigong as raw material, the system processes 3 million cubic meters of brine annually, operating for 8,000 hours per year. The main component of the raw brine is Na. + 79320mg / L, K + 2822 mg / L, Mg 2+ 646 mg / L, Ca 2+ 2913 mg / L, Sr 2+ 79.6 mg / L, Cl - 138306 mg / L, B 741 mg / L, Li + 80mg / L, Br - 700mg / L, I - 20mg / L, Rb + 5.22 mg / L, Cs +0.02 mg / L, H2S ~1000 mg / L, SO4 2- ≈2,270 mg / L.
[0059] Perform the operations according to steps S0 to S9 in the specific implementation method: S0: Original brine (375m) 3 The brine is filtered through a screen (≥1mm) to remove large particles of impurities, then through a vibrating screen to separate coarse sand, and then through a self-cleaning disc filter (50-100μm) to remove fine suspended solids. All three stages of treatment are closed filtration. A negative pressure extraction system is connected to the top to maintain a slight negative pressure at the top of the equipment, resulting in filtered brine. Section 1, namely S1 two-stage desulfurization: The filtered brine is degassed in a negative pressure degassing tower. During degassing, dissolved hydrogen sulfide is released from the liquid phase under a vacuum of -0.07 MPa. The released H2S gas enters a complex iron-sulfur recovery device, where H2S is oxidized to elemental sulfur by a liquid-phase catalyst (commercially available from Hebei Jingliu Environmental Protection Technology Co., Ltd., complex iron desulfurization catalyst). The H2S conversion rate is ≥99%. The sulfur paste is then processed into industrial sulfur (product) in a sulfur melting kettle (130℃). The degassed brine (with a residual H2S content of approximately 200-300 mg / L) is sent to an FeCl3 oxidation tank. FeCl3 (1.2 times the stoichiometric ratio of the liquid to be treated) is added to the FeCl3 oxidation tank. The material is then sent to an integrated air flotation and sedimentation machine for air flotation separation. After air flotation separation, air flotation (sent to a sulfuric acid plant) and clear liquid (H2S ≤10 mg / L) are obtained. Section 2, namely S2 brine refining: S2-1: The clear liquid in S1 is sent to the baffled reaction tank. NaOH is added to the tank to adjust the pH to 10.8, generating Mg(OH)2 precipitate. The Mg(OH)2 precipitate is treated by the Daur clarifier (Φ30m). The underflow enters the horizontal screw centrifuge for dehydration, obtaining 4,325 t / a of magnesium hydroxide product (purity 95-98%). The supernatant enters the next stage. S2-2: The supernatant from S2-1 is passed into a baffled reaction tank. Na2CO3 is added to the tank to adjust the pH to 9.2, resulting in a solution containing Ca. 2+ 、Sr 2 + The precipitate was then sent to a Doer clarification tank (Φ30m) for further treatment, yielding a supernatant (refined brine Mg). 2+ ≤40mg / L, Ca 2+ According to SO4 2- The mixture is retained at a molar ratio of 1.05 to 1.15:1 and the underflow is fed into a horizontal screw centrifuge for dewatering to obtain a mixed residue (15,800 t / a). S2-3: The mixed residue from S2-2 was leached with an 18% NH4Cl solution (NH4Cl / SrCO3 molar ratio 3.8:1, liquid-solid mass ratio 3.3:1, 40℃, 2h), filtered by plate and frame press, and the filtrate was treated with Na2CO3 (addition amount 1.08 times the stoichiometric ratio of strontium ions) to precipitate and obtain 340 t / a of strontium carbonate (SrCO3) (purity ≥98%) and calcium carbonate residue; S2-4: The calcium carbonate slag obtained from S2-3 is subjected to three-stage countercurrent washing until Cl - ≤0.05%, add food-grade citric acid (60℃, 2.5h, 5% excess citric acid), filter through plate and frame filter, decolorize with activated carbon, cool and crystallize, centrifuge, and dry in a fluidized bed to obtain 14,000 t / a of food-grade calcium citrate (purity ≥99%). Section 3, namely S3 MVR evaporation and crystallization: The refined brine obtained in S2-2 enters the MVR forced circulation evaporator (4 units, 3 operating, 1 standby, 108℃) for evaporation and crystallization. Then it enters the DTB crystallizer (three-stage washing of the salt leg). The bottom of the salt leg (CaSO4 slurry) → hydrocyclone → horizontal screw centrifuge → washing → crystallization → 10,371 t / a of α-type high-strength gypsum. The NaCl slurry discharged from the top of the salt leg is centrifuged by an HR centrifuge to obtain 586,694 t / a of industrial salt. The remaining NaCl centrifugal mother liquor is partially returned to the MVR forced circulation evaporator and partially enters the KCl flash crystallizer (vacuum flash evaporation, feed temperature approximately 85℃, post-flash temperature approximately 45℃, absolute pressure 10 kPa). The resulting material is then centrifuged in a KCl centrifuge to obtain 13,724 t / a of KCl product and a KCl centrifugal mixed mother liquor (105 m³). 3 / h). A portion of the KCl centrifuged mixed mother liquor is returned to the MVR forced circulation evaporator; the MVR forced circulation evaporator yields 2.76 million m³ of MVR condensate. 3 / a, can be used as a by-product freshwater for external supply; Section 4, namely S4 boron extraction: The KCl centrifuged mixed mother liquor obtained in S3 was acidified to pH 3.5, followed by 5-stage countercurrent extraction (50% isooctanol + 50% sulfonated kerosene, O / A = 1.5:1), 4-stage countercurrent back-extraction (O / A = 1.5:1), and heat pump evaporation crystallization to obtain 10,817 t / a of boric acid product (purity ≥ 99%); the raffinate was split, with a portion (42.5 m) 3 / h) returns to S2, part (62.5m) 3 / h) Enter S5; Section 5, or S5 iodine extraction: The raffinate from S4 was acidified to pH 2.0, chlorinated to ORP 535mV, and then adsorbed using D201 resin. The resulting effluent (iodine extraction tail liquid) was then used for further processing. -≤ 0.2mg / L) enters the next stage, saturates the resin, decomposes it with Na2SO3, and sublimates it at 98-100℃ to obtain 48t / a of iodine product and iodine extraction tail liquid; Section 6, or S6 bromine extraction: The iodine extraction tailings obtained from S5 (62.5m) 3 The solution was acidified to pH 3.5, chlorinated to ORP 750 mV, adsorbed onto D301 resin, eluted with alkaline solution, and distilled at 59 °C. Iodine was removed by alkaline elution to obtain 1,785 t / a of bromine (purity ≥ 99.8%) and a bromine extraction tail liquid. The bromine extraction tail liquid was split, with a portion (55.8 m³) being distilled. 3 / h) returns to S2, part (6.7m) 3 / h) Enter S7; Section 7, or S7 lithium extraction: The bromine tailings obtained from S6 were subjected to 5μm+1μm precision filtration, nanofiltration, and CH-93 chelating resin to remove calcium and magnesium (Ca in the effluent). 2+ +Mg 2+ ≤5mg / L), add Na2CO3 (2 units in parallel, V=8m 3 One unit is used and one unit is prepared. Na₂CO₃ (1.08 times the theoretical amount) is slowly added dropwise. Lithium is precipitated at 90℃ and pH=10.5, and then transferred to a settling tank (8-10m). 3 After sedimentation and aging, the underflow enters a scraper centrifuge for centrifugation, followed by drying in a disc dryer to obtain 1,086 t / a of lithium carbonate (purity ≥99.5%, battery grade). The overflow is the lithium precipitation mother liquor. The lithium precipitation mother liquor is then split, with a portion (4.7 m...) 3 / h) returns to S2, part (2.0m) 3 / h) Enter S8; Section 8, namely S8 rubidium and cesium recycling: Lithium precipitation mother liquor (2.0m) 3 / h) The solution is evaporated and concentrated in a 90℃ evaporation and concentration vessel, filtered while hot, and then crystallized and filtered again using NaCl / KCl to obtain a filtrate and a NaCl / KCl filter cake (the NaCl / KCl filter cake is dissolved and returned to the NaCl centrifugal mother liquor tank). The filtrate is further concentrated to Rb + +Cs + =650g / L, vacuum dried at 90℃ and -0.085MPa, yielding 20.3t / a of rubidium-cesium mixed salt for strategic reserve.
[0060] Resource utilization of calcium slag: The mixed residue obtained in S2-2 (15,800 t / a) → Plate and frame filter press dewatering (20% water content, about 60 t / d) → Ammonium chloride leaching (40% solid content, 60-80℃, 2h) → Solid-liquid separation → Liquid phase (SrCl2 solution, 1.51%) → MVR evaporation and concentration (15%) → Sodium carbonate precipitation → SrCO3 product (340 t / a); Solid phase (calcium carbonate filter cake) → Three-stage countercurrent washing (wash water returned to prepare NH4Cl) → Citric acid reaction (2 mol / L, 5% excess, 65℃) → Crystallization (30-40℃) → Centrifugation → Drying → Pulverization → Food-grade calcium citrate product (14,000 t / a, GB 1903.14-2016).
[0061] Testing revealed that the entire system discharged no process wastewater, and all MVR condensate was supplied to the industrial park. All product specifications met design requirements.
[0062] In the above embodiments, the main equipment of section 1 is: negative pressure degassing tower (2 units, FRP, Φ2400×H14000mm), brine plate heat exchanger (2 units, TA2 titanium material, 200m). 2 Water ring vacuum unit (2 sets, 316L), skid-mounted complexed iron desulfurization unit (2 sets, 316L, 5000Nm) 3 / h), sulfur grease filtration system (1 set, 60m) 2 ), sulfur melting kettle (2 units, Q345R, V=5m) 3 ), sulfur molding and packaging system (1 set), FeCl3 oxidation reaction tanks (2 units, steel lined with rubber, V=20m) 3 ), air flotation sedimentation unit (1 set, FRP / 316L, 400m) 3 / h), desulfurization circulating pump sets (6 units, fluoroplastics), and online H2S analyzers (3 sets).
[0063] The technological principle is as follows: The original brine contains approximately 1,000 mg / L of H2S, which must be removed to ≤10 mg / L. The first stage uses negative pressure degassing to extract H2S from the brine, which is then oxidized to elemental sulfur in a complexed iron desulfurization unit, producing sulfur paste (30%-50% moisture content). This paste is then refined into industrial sulfur products in a sulfur melting kettle (130-150℃). The second stage uses FeCl3 oxidation and precipitation to oxidize the remaining H2S to elemental sulfur and partially generate FeS precipitate. This precipitate is separated by an integrated air flotation and sedimentation unit, and the clarified liquid with H2S ≤10 mg / L enters section 2.
[0064] The actual consumption of FeCl3 is approximately 1.5 to 1.8 times the stoichiometric ratio of H2S. Note: In addition to dissolved H2S, the brine also contains reducing components such as polysulfides and reducing organic matter, which will consume additional ferric chloride; therefore, the actual dosage is higher than the theoretical stoichiometric ratio of H2S alone, and should be controlled at 1.2 to 1.8 times the theoretical stoichiometric ratio of H2S to ensure that the H2S in the treated brine is ≤10mg / L.
[0065] Material balance: Industrial sulfur production is approximately 2,300 t / a, FeCl3 consumption is approximately 23,000 t / a, and flotation slag is approximately 500-800 t / a (sent to sulfuric acid plants).
[0066] Section 2: The principle of brine refining process is: SO4 2- Magnesium ions are not removed in this stage; they all enter the MVR system and naturally precipitate as gypsum at the bottom of the salt leg of the DTB crystallizer during the evaporation and concentration process. The refining section only performs deep removal of magnesium ions to control the magnesium content in the refined brine. 2+ ≤40mg / L; calcium ions are not deeply removed and are retained in the MVR evaporation system; the calcium ion concentration is adjusted according to the sulfate concentration in the brine to control n(Ca 2+ ):n(SO4 2- The ratio of calcium ions to gypsum is 1.05 to 1.15:1, which causes sulfate ions to precipitate as calcium sulfate in the salt leg of the DTB crystallizer. The gypsum and salt slurry are separated by three-stage washing in the salt leg. Excess calcium ions should not be too high to prevent the formation of calcium sulfate scale on the MVR heat exchange surface.
[0067] Magnesium removal: NaOH is used for precipitation, and the reaction of Mg... 2+ +2NaOH→Mg(OH)2↓+2Na + pH=10.5-11.0.
[0068] Main equipment: Baffled reactor (1 unit, ≥160m) 3 The facility includes a Dow clarifier (1 unit, Φ30m) and two horizontal screw centrifuges (1 in use and 1 on standby). Approximately 4,325 t / a of Mg(OH)2 product is produced, and approximately 22,330 t / a of NaOH (30% liquid alkali) is consumed.
[0069] Removal of calcium and strontium: Precipitation with Na₂CO₃, Ca 2+ +CO3 2- →CaCO3↓, Sr 2+ +CO3 2- →SrCO3↓, pH=9.0-9.5. Equipment: Baffled reactor (1 unit, ≥160m²) 3The facility includes: a Dorr clarifier (1 unit, Φ30m), two horizontal screw centrifuges (1 unit, 1 unit in operation, 1 unit on standby), and two plate and frame filter presses. Na2CO3 consumption is approximately 16,390 t / a, and the CaCO3+SrCO3 mixed residue is approximately 15,800 t / a (approximately 48 t / d). The mixed residue composition is: CaCO3 97.47%, SrCO3 2.16%.
[0070] Strontium recovery: Leaching with NH4Cl, reaction SrCO3 + 2NH4Cl → SrCl2 + 2NH3↑ + CO2↑ + H2O. Approximately 340 t / a of SrCO3 product is produced, and approximately 80-100 t / a of NH4Cl is replenished.
[0071] Section 3: MVR Evaporation and Crystallization Process principle: The MVR system is the core hub, with a total evaporation capacity of 345t / h, and uses four large centrifugal compressors (three in operation and one on standby). Secondary steam is compressed by the steam compressors, and its temperature and pressure are increased before being recycled as a heat source, without the need for a boiler.
[0072] Calcium sulfate scaling control: adopts seed crystal method (maintaining seed crystal concentration of 20-40g / L), salt leg separation (utilizing the difference between gypsum density 2.32 and NaCl density 2.16), CIP online acid washing (once every 30-45 days), and annual mother liquor purification bypass four-layer protection.
[0073] To prevent NaCl co-precipitation during KCl flash evaporation: NaCl centrifuge wash water (fresh water, approximately 15 ml) 3 The NaCl mother liquor (at a concentration of 10 m / h) is mixed with the NaCl centrifuged mother liquor in a mixing pipe (L≥10 m) to dilute the NaCl concentration to an unsaturated state. The concentration is then measured using an online density meter and NaCl... + The concentration analyzer monitors in real time, and the DCS automatically adjusts.
[0074] Gypsum separation and crystallization: Concentrated gypsum slurry from the bottom of the salt leg → washing within the salt leg → hydrocyclone (concentrating to 30-40%) → horizontal screw centrifuge → water washing for desalination → hydrothermal crystallization (120-150℃, 0.3-0.5MPa, with crystallization agent added) → centrifugal separation → flash drying → ball milling → α-type high-strength gypsum. The crystallization agent is an organic acid (citric acid, succinic acid, etc.), used at a dosage of 0.01%-0.5%.
[0075] Main equipment: MVR forced circulation evaporators (4 sets, TA2 tube bundle + 2205 shell, 115-120 t / h), centrifugal steam compressors (4 units, duplex stainless steel), MVR forced circulation pump sets (8 sets, 2205), NaCl DTB crystallizers (2 units, 2205, 300-400 m³ / h). 3 KCl flash crystallizer (1 unit, 2205, 650m) 3), NaCl HR centrifuges (4 units, Hastelloy C276), KCl HR centrifuges (2 units, Hastelloy C276), fluidized bed drying system (1 set for NaCl, 1 set for KCl), CIP online pickling system (1 set), DCS automatic control system (1 batch), gypsum separation and washing system (1 set), gypsum crystallization section (1 set).
[0076] Material balance: Industrial salt 586,694 t / a, α-type high-strength gypsum 10,371 t / a, potassium chloride 13,724 t / a, by-product freshwater 2.76 million m³ 3 / a.
[0077] Section 4: Boron Extraction Process Principle: Boric acid undergoes an esterification reaction with isooctanol under acidic conditions to generate borate esters, which enter the organic phase. After back-extraction with pure water, a boron-rich solution is obtained. Extraction: H₃BO₃ + 3R⁻OH B(OR)3+3H2O; stripping: B(OR)3+3H2O H3BO3 + 3R-OH. The boron-rich back-extraction solution is evaporated and concentrated at low temperature under conditions of 50-70℃ and 10-40kPa absolute pressure. Boric acid crystallizes out after reaching supersaturation (boric acid begins to dehydrate at 100-105℃, and the operating temperature must be much lower than 100℃).
[0078] Process flow: KCl centrifugation to mix mother liquor (105m) 3 / h, B≈741mg / L) → Acidification (pH 3-4) → 5-stage centrifugal extraction (50% isooctanol + 50% sulfonated kerosene) → Back-extraction → Heat pump evaporation crystallization (electrically driven) → Boric acid product (10,817t / a). Mother liquor is returned to the heat pump evaporator for continued circulation; raffinate is diverted → 62.5m 3 / h→Iodine extraction, 42.5m 3 / h → Return to section 2.
[0079] Main equipment: Acidification reaction tanks (2 units, glass-lined, V=20m) 3 ), acid metering pumps (3 units, fluoroplastic), centrifugal extractors (5 extraction sections + 4 back-extraction sections + 1 washing section, TA10 / 2507), extractant preparation tank (1 unit, carbon steel, 30m³). 3 Extractant storage tanks (2 units, carbon steel, 50m³) 3 ), independent heat pump evaporator crystallizer (1 set, TA2 / 2205, 2-3t / h), small steam compressor (1 unit, duplex stainless steel), boric acid centrifuge (2 units, 1 for use and 1 for standby, 316L), fluidized bed dryer (1 unit, 304, 1-2t / h).
[0080] Material balance: Boric acid product is approximately 10,817 t / a.
[0081] Section 5: Iodine Extraction Process Principle: Iodide ions are preferentially oxidized to iodine molecules (I₂) during chlorination. These molecules are then adsorbed using a D201 type macroporous strong-base anion exchange resin, desorbed by sodium sulfite, and purified by sublimation. Oxidation: 2I₂ - +Cl2→I2+2Cl - ; Liberation: Na2SO3 + I2 + H2O → Na2SO4 + 2HI.
[0082] Process flow: Boron extraction residue (62.5m) 3 / h,I - ≈20mg / L) → Acidification (pH 1.5-2.5) → Chlorination oxidation (ORP 520-550mV, interlock control) → D201 resin adsorption → Discharge (I - ≤0.2mg / L) All enter section 6; Saturated resin → Na2SO3 desorption → secondary oxidation → sublimation purification (98-100℃) → iodine product (48t / a).
[0083] Main equipment: Acidification reaction tanks (2 units, glass-lined, V=10m) 3 Oxidation reaction vessels (2 units, glass-lined, with ORP monitoring), D201 resin adsorption towers (3 units, rubber-lined steel, Φ1800×H4000), D201 macroporous resin (20m³) 3 ), Decomposition fluid storage tank (1 unit, PE / glass enamel, V=5m) 3 Sodium sulfite preparation tank (1 unit, PE, V=3m) 3 ), Iodine sublimation refining apparatus (1 unit, glass-lined, V=2m) 3 ), iodine product collector (1 unit, 316L), corrosion-resistant pump set (6 units, fluoroplastic).
[0084] Material balance: Iodine product: approximately 48 t / a.
[0085] Section 6: Bromine Extraction Process principle: Under acidification conditions, Br is oxidized by chlorination. - The bromine is obtained by adsorption with D301 macroporous anion exchange resin, followed by elution with alkaline solution and distillation. Oxidation: 2Br - +Cl2→Br2+2Cl - Elution: Resin - R·Br2 + 2OH - →Resin-R+Br - +BrO - +H2O.
[0086] Process flow: Iodine extraction tailings (62.5m) 3 / h, Br -≈700mg / L) → Acidification (pH 3-4) → Chlorination oxidation (ORP 700-800mV, interlock control) → D301 resin adsorption → Alkali elution → Distillation (58-60℃) → Alkali elution of iodine (2-5% NaOH, 30-50℃) → Bromine product (1,785t / a, purity ≥99.8%); Tailings diversion → 6.7m 3 / h → Lithium extraction, 55.8m 3 / h → Return to section 2. Secondary distillation is reserved (depending on product quality).
[0087] Main equipment: Acidification reaction tanks (2 units, glass-lined, V=10m) 3 Oxidation reaction vessels (2 units, glass-lined, with ORP monitoring), D301 resin adsorption towers (3 units, steel lined with rubber, Φ2000×H4000), D301 resin (20m³) 3 Eluent storage tank (1 unit, PE / glass enamel, V=5m) 3 ), bromine-rich intermediate tank (1 unit, glass-lined, V=5m) 3 ), bromine distillation column (1 unit, glass-lined, Φ1000×H6000), bromine finished product storage tanks (2 units, glass-lined, V=5m) 3 Alkali washing and iodine removal tower (1 unit, glass-lined / PTFE-lined, DN600-800), alkali circulation pump (2 units, fluoroplastic), tail gas alkali absorption tower (1 set, PP), corrosion-resistant pump set (6 units, fluoroplastic).
[0088] Material balance: bromine product approximately 1,785 t / a.
[0089] Section 7: Lithium Extraction Process Principle: Utilizing the characteristic that the solubility of lithium carbonate decreases with increasing temperature (1.29 g / 100 g water at 25℃, 0.72 g / 100 g water at 100℃), sodium carbonate is added at a high temperature of 85-95℃, causing Li to... + It precipitates as Li₂CO₃. Reaction: 2Li + +CO3 2- →Li2CO3↓.
[0090] Process flow: Bromine extraction tail liquid (6.7m) 3 / h, Li + ≈80mg / L) → Precision filtration (5μm + 1μm) → Nanofiltration → Chelating resin to remove calcium and magnesium (eluent Ca 2+ +Mg 2+ ≤5mg / L) → Lithium precipitation reactor (2 units in parallel, V=8m) 3 1 for use, 1 for standby, 85-95℃, slowly add Na2CO3 (pH=10-11) → settling tank (8-10m) 3Sedimentation + heat preservation aging, 85-90℃) → Underflow → Scraper centrifuge → Disc dryer → Lithium carbonate product (1,086t / a, purity ≥99.5%); Overflow → Diverter (2.0m) 3 / h→Rudium and cesium recovery, 4.7m 3 / h→Return to Section 2).
[0091] Main equipment: Precision filtration unit (2 sets, PP / PVDF, 5μm+1μm), nanofiltration system (1 set, 8040 type, 30 units), NF high-pressure feed pump (2 units, 316L, 50m³). 3 / h), chelation resin tower (4 units, 2 in operation and 2 on standby, steel lined with rubber, Φ1800×H4000), CH-93 chelation resin (15m 3 Lithium precipitation reactor (2 units, 1 in use and 1 on standby, glass-lined, V=8m) 3 ), Settling tank (1 unit, 316L, 8-10m) 3 ), horizontal scraper centrifuge (1 unit, 316L, 200-300kg / h), disc dryer (1 unit, 304, 200-300kg / h), mother liquor tank (1 unit, 304, 5-10m³). 3 ), Lithium carbonate automatic packaging system (1 set, 304, 25kg / bag).
[0092] Material balance: Lithium carbonate product is approximately 1,086 t / a.
[0093] Section 8: Rubidium and Cesium Recycling Process principle: Utilizing Rb in the MVR closed-loop cycle + and Cs + Without an extraction path, it continuously and naturally accumulates in the circulating mother liquor. Once the controlled concentration is reached, a separate stream is continuously diverted from the lithium precipitation mother liquor for independent evaporation and concentration, followed by vacuum drying to form solid mixed salts. Rb + The annual total is approximately 17.8 t / a, Cs + Approximately 0.06 t / a, while the actual production of RbCl is approximately 20.2 t / a.
[0094] Process flow: Lithium precipitation mother liquor (6.7m) 3 / h) → Continuous diversion → Small amount (2.0m) 3 / h) → Section 8; Remaining (4.7m) 3 / h) → Return to Section 2 → Evaporation and Concentration Kettle (V=5m) 3 → NaCl / KCl crystallization → hot filtration → dissolve the filter cake with a small amount of MVR cooling water → return to the NaCl centrifuge mother liquor tank; the filtrate is further concentrated to Rb + +Cs +=500-800g / L → Vacuum drying oven (80-100℃, -0.085MPa) → Rubidium-cesium mixed salt (20.3t / a) → Strategic reserve.
[0095] Main equipment: Evaporation and concentration kettle (1 unit, glass-lined, V=5m) 3 Small centrifuge (1 unit, 316L, 50-100kg / batch), small dissolving tank (1 unit, 304 stainless steel, 0.5-1.0m³) 3 Vacuum oven (1 unit, 316L inner liner, 1-2m) 3 Vacuum pump (1 unit, ≥100L / s), sealing packaging system (1 set), and matching pump set pipeline valves (1 batch).
[0096] Material balance: Rubidium-cesium mixed salt approximately 20.3 t / a.
[0097] Supplementary explanation on the resource utilization of calcium slag: Process principle: SrCO3 + 2NH4Cl → SrCl2 + 2NH3↑ + CO2↑ + H2O. CaCO3 does not react under these conditions. Ammonium chloride circulates in a closed loop within the system and is not consumed; the annual replenishment is 70-120 t / a (irreversible loss). Citric acid reaction: 3CaCO3 + 2C6H8O7 → Ca3(C6H5O7)2 + 3CO2↑ + 3H2O. Optimal conditions: citric acid concentration 2 mol / L, 5% excess, reaction temperature 65℃, product yield 92.68%.
[0098] Process flow: Mixed residue → Plate and frame filter press dewatering (20% water content) → Leaching reactor (add three-stage washing water + supplement NH4Cl, solid content 40%, 60-80℃, 2h) → Solid-liquid separation → Liquid phase (SrCl2 solution, 1.51%) → MVR evaporation and concentration (15%) → Sodium carbonate precipitation → SrCO3 product (340t / a); Solid phase (calcium carbonate filter cake) → Three-stage countercurrent washing (fresh MVR condensate 59.9t / d, 50-70℃, wash water returned to prepare NH4Cl) → Washed filter cake → Slurry preparation → Citric acid reaction → Filtration → Crystallization (30-40℃) → Centrifugation → Washing → Drying (≤80℃) → Crushing → Food-grade calcium citrate product (14,000t / a, GB 1903.14-2016).
[0099] Core data for material balance: Mixed slag composition: CaCO3 15,400 t / a, SrCO3 342 t / a, others 58 t / a. Filter cake moisture content 20%, wet weight 59.9 t / d, leaching and pulping water consumption 59.9 t / d, pulp solids content 40%. Annual NH4Cl recycling rate approximately 472 t / a, annual replenishment 70-120 t / a. SrCl2 solution concentration 1.51%, annual SrCl2 consumption 367 t / a. After concentration, SrCl2 solution 15% (7.4 t / d), evaporation water consumption 66.3 t / d. Na2CO3 consumption 245 t / a, SrCO3 product 340 t / a. Citric acid consumption 10,300 t / a, calcium citrate product 14,000 t / a.
[0100] Control parameters: Moisture content of filter cake after pressure ≤20%, solid content of leaching slurry 40%, leaching reaction temperature 60-80℃, leaching reaction time 2h, Sr leaching rate ≥96%, washing water temperature 50-70℃, ammonium residue in filter cake after washing ≤50ppm, concentration of SrCl2 after concentration 15%, citric acid concentration 2mol / L, citric acid excess 5%, citric acid reaction temperature 65℃, and calcium citrate drying temperature ≤80℃.
[0101] Main equipment: Plate and frame filter press (1-2 units, 200-300m³) 2 ), Leaching reactors (2 units, glass-lined, V=20m) 3 ), Pulping tanks (6 units, 2 units per stage, 316L / steel lined with rubber, V=25m) 3 Plate and frame filter press (washing and filtration, 2 units, 150-200m³) 2 NH4Cl preparation tank (1 unit, PE / steel lined with rubber, 25m) 3 Wash water collection tanks (3 units, PE / steel lined with rubber, 25m³) 3 MVR evaporator (1 set, 316L / titanium material, 3-4t / h), precipitation reaction tank (1 unit, 316L, V=5m) 3 Small plate and frame filter press (1 unit, 10-20m) 2 Vacuum drying oven (1 unit, 316L inner liner, 1.0m) 3 ), mixing tank (1 unit, 304 stainless steel, 20-30m) 3 Citric acid preparation tank (1 unit, 304 stainless steel, 20-30m³) 3 Citric acid reactor (2 units in series, 316L, 10-20m³) 3 Plate and frame filter press (calcium citrate, 1-2 units, food-grade PP, 50-100m³) 2 ), crystallization tanks (2 units, 316L, 10-20m²) 3Centrifuges (calcium citrate, 1-2 units, 316L, 2-5t / h), fluidized bed dryer (1 unit, 316L, 2-5t / h), pulverizing, sieving and packaging system (1 set, 304 / 316L), food-grade cleanroom (1 room, meeting GMP requirements).
[0102] Example 2 (Annual brine treatment capacity of 1 million m³) 3 (Low load conditions) Using deep black brine from a mining area (Zigong mining area as an example) as raw material, the annual brine processing capacity is 1 million cubic meters, with an annual operation time of 8000 hours. The main component of the raw brine is Na. + 76100mg / L, K + 2510 mg / L, Mg 2+ 580mg / L, Ca 2+ 2620mg / L, Sr 2+ 72mg / L, Cl - 132000mg / L, B 660mg / L, Li + 72mg / L, Br - 630mg / L, I - 18mg / L, Rb + 4.7 mg / L, Cs + 0.018mg / L, H2S≈850mg / L, SO4 2- ≈1080mg / L.
[0103] Perform the operation using S0~S9: S0: Original brine (125m) 3 The brine is filtered through a screen (≥1mm), a vibrating screen, and a self-cleaning disc filter (100μm) in a closed system. The equipment maintains a slight negative pressure to obtain the filtered brine.
[0104] S1 Two-Stage Desulfurization: After filtration, the brine is sent to a negative pressure degassing tower with a vacuum of -0.06 MPa; the released H2S gas is then sent to a complexed iron-sulfur recovery unit (EDTA-Fe). 3+ Complexing catalyst), H2S conversion rate ≥99%; sulfur paste is fed into a sulfur melting kettle at 120℃ to obtain industrial sulfur; after degassing, FeCl3 is added to the brine, the addition amount is 1.2 times the theoretical stoichiometric ratio of H2S, and the H2S of the clear liquid after air flotation separation is ≤10mg / L.
[0105] S2 brine refining: S 2- 1. Add NaOH to adjust pH to 10.5, precipitate and remove magnesium, and control the Mg content in the refined brine. 2+ ≤40mg / L; S 2- 2. Add Na₂CO₃ to adjust pH to 9.0, precipitating some calcium and strontium. Calcium ions are added according to the molar ratio n(Ca). 2+):n(SO4 2- )=1.05:1 Match preserved; S 2- 3. The mixed residue was leached with a 15% NH4Cl solution (molar ratio of NH4Cl / SrCO3 1:1, liquid-to-solid mass ratio 1:1) at 20℃ for 1 hour. Na2CO3 (dosage 1.05 times the stoichiometric ratio of strontium ions) was added to the filtrate to precipitate SrCO3 product (purity ≥98%) and calcium carbonate residue. 2- 4. Calcium carbonate slag undergoes three-stage countercurrent washing until Cl - Add food-grade citric acid (citric acid to calcium carbonate molar ratio 2:3, citric acid excess 1%, 50℃, 2h) to obtain food-grade calcium citrate product (purity ≥99%).
[0106] S3 MVR evaporation crystallization: evaporation temperature 106℃, operating pressure -0.05MPa; DTB crystallizer + salt leg three-stage washing; KCl flash evaporation temperature 40℃, absolute pressure 12kPa; lithium, boron, bromine, iodine, rubidium, and cesium are enriched in the KCl centrifuged mixed mother liquor.
[0107] S4 Boron Extraction: Acidification pH=3.0; 5-stage countercurrent extraction (50% isooctanol + 50% sulfonated kerosene, O / A=1:1); 4-stage countercurrent back-extraction (O / A=1:1); heat pump evaporation crystallization to obtain boric acid (purity ≥99%).
[0108] Iodine extraction using S5: Acidification pH=1.5; Oxidation with chlorine ORP=520mV; Adsorption with D201 resin, desorption with Na2SO3, sublimation at 98℃ to obtain iodine product.
[0109] S6 bromine extraction: acidification pH=3.0; chlorination oxidation ORP=700mV; D301 resin adsorption, alkaline elution, and distillation at 58℃ to obtain bromine product (purity ≥99.8%).
[0110] S7 lithium extraction: 5μm + 1μm precision filtration, nanofiltration, CH-93 chelating resin for calcium and magnesium removal (outflow Ca... 2+ +Mg 2+ ≤5mg / L); lithium precipitation temperature 85℃, pH=10, sodium carbonate dosage 1.05 times the theoretical amount; battery-grade lithium carbonate (purity ≥99.5%) was obtained.
[0111] S8 Rubidium and Cesium Recovery: Evaporation and concentration, hot filtration, NaCl / KCl filter cake dissolved and returned to MVR; filtrate concentrated to Rb + +Cs + =500g / L; vacuum dried at 80℃ and -0.08MPa to obtain rubidium-cesium mixed salt.
[0112] S9 mother liquor closed-loop circulation: The return ratio of mother liquor in each section is automatically adjusted according to the material balance, and there is no process wastewater discharge from the entire system.
[0113] The main products produced in this embodiment are: magnesium hydroxide 1410 t / a, strontium carbonate 112 t / a, food-grade calcium citrate 4650 t / a, α-type high-strength gypsum 3420 t / a, industrial salt 194000 t / a, potassium chloride 4540 t / a, boric acid 3600 t / a, iodine 16 t / a, bromine 590 t / a, lithium carbonate 360 t / a, and rubidium-cesium mixed salt 6.8 t / a; 920,000 m³ of freshwater is produced as a byproduct of MVR. 3 / a.
[0114] Example 3 (Annual brine treatment capacity of 4 million m³) 3 ) Using deep black brine from a mining area (Zigong mining area as an example) as raw material, the annual brine processing capacity is 4 million cubic meters, with an annual operation time of 8000 hours. The main component of the raw brine is Na. + 82500mg / L, K + 3100mg / L, Mg 2+ 690mg / L, Ca 2+ 3150mg / L, Sr 2+ 86mg / L, Cl - 144000mg / L, B 810mg / L, Li + 88mg / L, Br - 770mg / L, I - 22mg / L, Rb + 5.7 mg / L, Cs + 0.022mg / L, H2S≈1150mg / L, SO4 2- ≈1320mg / L.
[0115] Perform the operation using S0~S9: S0: Original brine (500m) 3 The brine is filtered through a screen (≥1mm), a vibrating screen, and a self-cleaning disc filter (50μm) in a closed system. The equipment maintains a slight negative pressure to obtain the filtered brine.
[0116] S1 Two-Stage Desulfurization: After filtration, the brine is sent to a negative pressure degassing tower with a vacuum of -0.08 MPa; the released H2S gas is then sent to a complexed iron-sulfur recovery unit (EDTA-Fe). 3+ Complexing catalyst), H2S conversion rate ≥99%; sulfur paste is fed into a sulfur melting kettle at 140℃ to obtain industrial sulfur; after degassing, FeCl3 is added to the brine, the addition amount is 1.8 times the theoretical stoichiometric ratio of H2S, and the H2S of the clear liquid after air flotation separation is ≤10mg / L.
[0117] S2 brine refining: S2- 1. Add NaOH to adjust pH to 11.0, precipitate and remove magnesium, and control the Mg content in the refined brine. 2+ ≤40mg / L; S 2- 2. Add Na₂CO₃ to adjust pH to 9.5, precipitating some calcium and strontium. Calcium ions are added according to the molar ratio n(Ca). 2+ ):n(SO4 2- )=1.15:1 Match preserved; S 2- 3. The mixed residue was leached with a 20% NH4Cl solution (molar ratio of NH4Cl / SrCO3 5:1, liquid-to-solid mass ratio 5:1) at 80℃ for 3 hours. Na2CO3 (dosage 1.10 times the stoichiometric ratio of strontium ions) was added to the filtrate to precipitate SrCO3 product (purity ≥98%) and calcium carbonate residue. 2- 4. Calcium carbonate slag undergoes three-stage countercurrent washing until Cl - Add food-grade citric acid (citric acid to calcium carbonate molar ratio 2:3, citric acid excess 5%, 70℃, 3h) to obtain food-grade calcium citrate product (purity ≥99%).
[0118] S3 MVR evaporation crystallization: evaporation temperature 109℃, operating pressure -0.02MPa; DTB crystallizer + salt leg three-stage washing; KCl flash evaporation temperature 50℃, absolute pressure 7kPa; lithium, boron, bromine, iodine, rubidium, and cesium are enriched in the KCl centrifuged mixed mother liquor.
[0119] S4 Boron Extraction: Acidification pH=4.0; 5-stage countercurrent extraction (50% isooctanol + 50% sulfonated kerosene, O / A=2:1); 4-stage countercurrent back-extraction (O / A=2:1); heat pump evaporation crystallization to obtain boric acid (purity ≥99%).
[0120] Iodine extraction using S5: Acidification pH=2.5; Oxidation with chlorine ORP=550mV; Adsorption with D201 resin, desorption with Na2SO3, sublimation at 100℃ to obtain iodine product.
[0121] S6 bromine extraction: acidification pH=4.0; chlorination oxidation ORP=800mV; adsorption with D301 resin, alkaline elution, and distillation at 60℃ to obtain bromine product (purity ≥99.8%).
[0122] S7 lithium extraction: 5μm + 1μm precision filtration, nanofiltration, CH-93 chelating resin for calcium and magnesium removal (outflow Ca... 2+ +Mg 2+ ≤5mg / L); lithium precipitation temperature 95℃, pH=11, sodium carbonate dosage 1.10 times the theoretical amount; to obtain battery-grade lithium carbonate (purity ≥99.5%).
[0123] S8 Rubidium and Cesium Recovery: Evaporation and concentration, hot filtration, NaCl / KCl filter cake dissolved and returned to MVR; filtrate concentrated to Rb + +Cs + =800g / L; vacuum dried at 100℃ and -0.09MPa to obtain rubidium-cesium mixed salt.
[0124] S9 mother liquor closed-loop circulation: The return ratio of mother liquor in each section is automatically adjusted according to the material balance, and there is no process wastewater discharge from the entire system.
[0125] The main products produced in this embodiment are: magnesium hydroxide 5760 t / a, strontium carbonate 455 t / a, food-grade calcium citrate 18650 t / a, α-type high-strength gypsum 13830 t / a, industrial salt 782200 t / a, potassium chloride 18300 t / a, boric acid 14420 t / a, iodine 64 t / a, bromine 2380 t / a, lithium carbonate 1445 t / a, and rubidium-cesium mixed salt 27.2 t / a; 3.68 million m³ of freshwater is produced as a byproduct of MVR. 3 / a.
[0126] Examples 1-3 represent medium operating conditions, lower parameter limit operating conditions, and upper parameter limit operating conditions, respectively. These examples use brine from a certain mining area as an example raw material. The process of this invention is not limited to this specific mining area and can be adapted to other deep brines with similar component characteristics. The composition of the original brine fluctuates within a reasonable range, and all process parameters in each example fall within the protection range defined in the claims of this invention. Each example achieves a closed-loop circulation throughout the entire process with no process wastewater discharge, and all product indicators meet design requirements. In actual production, the parameters can be adjusted according to changes in the original brine composition, based on n(Ca... 2+ ):n(SO4 2- The concentration of residual calcium ions in the refined brine is dynamically adjusted to 1.05~1.15:1.
[0127] This invention is not limited to this specific scale. The mother liquor return rate is automatically adjusted by the system's material balance, and the return ratio is determined comprehensively based on the concentration of valuable elements, system water balance, and equipment load. In implementations of different scales, the above-mentioned flow rates can be adjusted proportionally, all of which fall within the scope of protection of this invention.
Claims
1. A closed-loop circulation process for multi-element cascade extraction of deep-well black brine, characterized in that, Includes the following steps: (1) Physical filtration of raw brine pretreatment: The raw brine is filtered through a closed multi-stage filtration system to remove suspended solids and obtain filtered brine. (2) Two-stage desulfurization: The filtered brine obtained in step (1) is degassed under negative pressure to release H2S gas, resulting in degassed brine and H2S-containing gas; the H2S-containing gas is recovered and converted into sulfur by a complexing iron-sulfur recovery device, and then processed into industrial sulfur products through a sulfur melting kettle; the degassed brine is subjected to deep desulfurization with FeCl3, and then separated by air flotation to obtain a clear liquid with H2S ≤ 10 mg / L; all equipment in steps (1) and (2) that comes into contact with the sulfur-containing raw brine is a closed structure, with the top... The part is connected to a negative pressure extraction system to maintain a slight negative pressure operation; the extracted H2S-containing gas is sent to a complex iron-sulfur recovery device for treatment; (3) Brine refining: the clear liquid obtained by air flotation separation in step (2) is successively subjected to NaOH precipitation to remove magnesium to obtain Mg(OH)2 product, and Na2CO3 precipitation to remove calcium and strontium to obtain refined brine and CaCO3+SrCO3 mixed residue; the obtained CaCO3+SrCO3 mixed residue is leached with NH4Cl, plate and frame filter, and Na2CO3 is added to the filtrate for precipitation and separation. SrCO3 product and calcium carbonate residue are obtained; calcium carbonate residue is reacted with citric acid to obtain food-grade calcium citrate product; (4) MVR evaporation crystallization: the refined brine obtained in step (3) is subjected to MVR forced circulation evaporation crystallization; the MVR forced circulation evaporation crystallization adopts DTB crystallizer and achieves graded separation of gypsum, sodium chloride and potassium chloride through three-stage washing of salt leg; the obtained product enters the three-stage washing of salt leg, the bottom of salt leg is CaSO4 slurry, which enters hydrocyclone and horizontal screw centrifuge in sequence, and then is washed and crystallized to obtain α-type high-strength gypsum; the upper part of salt leg is NaCl slurry, which is centrifuged to produce NaCl product, and the residue is NaCl centrifugal mother liquor and washing water; the NaCl centrifugal mother liquor and washing water are diluted to unsaturation, crystallized by KCl flash crystallizer and treated by KCl centrifuge to obtain KCl product and KCl centrifugal mixed mother liquor; in the above evaporation crystallization process, lithium, boron, bromine, iodine, rubidium and cesium valuable elements do not enter sodium chloride and potassium chloride products, and are naturally enriched in the evaporation mother liquor; (5) Boron extraction: The KCl centrifuged mixed mother liquor obtained in step (4) is acidified, extracted, back-extracted, and evaporated by a heat pump to crystallize, to obtain boric acid product and raffinate after boron extraction; (6) Iodine extraction: Acidification, oxidation, resin adsorption, and sublimation are performed on a portion of the raffinate after boron extraction to obtain iodine product and tail liquid after iodine extraction; (7) Bromine extraction: Acidification, oxidation, resin adsorption, and distillation are performed on a portion of the tail liquid after iodine extraction to obtain bromine product and tail liquid after bromine extraction; (8) Lithium extraction: After bromine extraction, the tail liquid is subjected to precision filtration, nanofiltration, chelation resin to remove calcium and magnesium, and Na2CO3 is added to precipitate lithium to obtain lithium carbonate product and lithium precipitation mother liquor; (9) Rubidium and cesium recovery: After evaporation and concentration, crystallization and hot filtration, a NaCl / KCl filter cake and filtrate are obtained. The filtrate is further concentrated and then vacuum dried to obtain rubidium and cesium mixed salt; (10) Mother liquor closed-loop circulation: A portion of the bromine extraction tail liquid in step (7) is returned to step (3); A portion of the raffinate after boron extraction in step (5) is returned to step (3); A portion of the lithium precipitation mother liquor in step (8) is returned to step (3); A portion of the KCl centrifuged mixed mother liquor in step (4) is returned to the front end of step (4) to participate in MVR recirculation; The filtrate after NH4Cl leaching in step (3) is recycled and reused in the strontium recovery section; The NaCl / KCl filter cake in step (9) is dissolved and returned to the MVR in step (4).
2. The process according to claim 1, characterized in that: The vacuum degree of the negative pressure degassing in step (2) is -0.06 to -0.08 MPa, the H2S conversion rate of the complexed iron-sulfur recovery is ≥99%, the operating temperature of the sulfur melting kettle is 120-140℃, and the FeCl3 dosage is 1.2 to 1.8 times the theoretical stoichiometric ratio of H2S.
3. The process according to claim 1, characterized in that: In step (3), the pH for magnesium removal by NaOH precipitation is 10.5-11.0; the pH for calcium and strontium removal by Na2CO3 precipitation is 9.0-9.5, and the Mg in the refined brine is... 2+ ≤40mg / L; calcium ions are not deeply removed, and the calcium ion concentration is controlled according to the sulfate ion concentration in the brine, with the molar amount of calcium ions controlled to be 1.05 to 1.15 times the molar amount of sulfate ions.
4. The process according to claim 1, characterized in that: In step (3), the NH4Cl leaching conditions are as follows: the mass fraction of NH4Cl is 15-20%, the molar ratio of NH4Cl to SrCO3 is 1:1 to 5:1, the liquid-solid mass ratio is 1:1 to 5:1, the reaction temperature is 20 to 80℃, and the reaction time is 1 to 3 hours; the leaching rate of SrCO3 is ≥95%, and the product purity is ≥98%.
5. The process according to claim 1, characterized in that, In step (3), the amount of sodium carbonate added is 1.05 to 1.10 times the stoichiometric ratio of strontium ions in the filtrate; the conditions for the citric acid reaction are: the molar ratio of citric acid to calcium carbonate is 2:3, the excess of citric acid is 1% to 5%, the reaction temperature is 50-70℃, the reaction time is 2-3h, and the product purity is ≥99%.
6. The process according to claim 1, characterized in that: The temperature of the MVR forced circulation evaporation crystallization in step (4) is 106-109℃ and the operating pressure is -0.02 to -0.05MPa; the temperature of the KCl flash evaporation crystallization is 40-50℃ and the vacuum degree is 7-12kPa absolute pressure.
7. The process according to claim 1, characterized in that: The extraction agent used in step (5) contains 50% isooctanol + 50% sulfonated kerosene by volume fraction, with an extraction ratio of O / A = 1:1 to 2:1, 5 extraction stages, and an extraction rate of ≥97%; the back-extraction ratio is O / A = 1:1 to 2:1, with 4 back-extraction stages and a back-extraction rate of ≥98%.
8. The process according to claim 1, characterized in that: In step (6), the ORP of iodine oxidation during extraction is 520-550 mV, and the effluent I... - ≤0.2mg / L, the sublimation temperature is 98-100℃; the ORP of oxidation in the bromine extraction in step (7) is 700-800mV, the distillation temperature is 58-60℃, and the purity of the bromine product is ≥99.8%.
9. The process according to claim 1, characterized in that: The chelating resin mentioned in step (8) is of type CH-93, and the effluent Ca²⁺ + +Mg² + ≤5mg / L; the lithium precipitation temperature is 85-95℃, the pH is 10-11; the sodium carbonate dosage is 1.05-1.10 times the theoretical amount, and the lithium carbonate product purity is ≥99.5%.
10. The process according to claim 1, characterized in that, The return ratio of each mother liquor in step (10) is automatically adjusted by the system material balance and determined comprehensively based on the concentration of valuable elements, system water balance and equipment load.