Method for preparing yellow phosphorus by reduction of phosphate rock

By using the synergistic effect of crude silicon and flux in the process of reducing phosphate rock to prepare yellow phosphorus, the byproduct of ferrophosphorus is converted into ferrosilicon, which solves the problems of phosphorus loss and low phosphorus yield, achieves high-efficiency phosphorus yield and resource utilization of waste, and reduces energy consumption.

CN123105567APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611157267.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing carbothermic reduction technologies for phosphate rock, phosphorus is lost in the solid residue, resulting in low phosphorus yield, and it is difficult to simultaneously achieve fluxing strengthening and resource utilization of solid waste.

Method used

By utilizing the synergistic effect of crude silicon containing elemental silicon and flux, the phosphorus-iron byproduct generated in the reduction reaction is converted into ferrosilicon, reducing phosphorus loss. Furthermore, by controlling the slag phase composition, the contact state of the reaction interface is improved, thus promoting the reduction reaction.

Benefits of technology

To improve phosphorus yield, reduce residual P2O5 content, realize the resource utilization of industrial solid waste, and reduce energy consumption of reduction reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105567A_ABST
    Figure CN123105567A_ABST
Patent Text Reader

Abstract

This invention relates to the technical field of comprehensive utilization of mineral resources and energy conservation and consumption reduction, specifically to a method for preparing yellow phosphorus by reducing phosphate rock. The method comprises the following steps: (1) mixing phosphate rock, a reducing agent, crude silicon, and a flux to obtain a mixture; (2) subjecting the mixture to a reduction reaction in the presence of a non-oxidizing atmosphere to obtain yellow phosphorus and ferrosilicon; wherein the crude silicon contains elemental silicon. This method can effectively improve phosphorus yield, reduce the P2O5 content in the residue, and has low production costs, enabling the resource utilization of industrial solid waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of comprehensive utilization of mineral resources and energy conservation and consumption reduction, specifically to a method for preparing yellow phosphorus by reducing phosphate rock. Background Technology

[0002] Yellow phosphorus is an important basic chemical raw material, widely used in agricultural phosphate fertilizers, fine chemicals, electronic chemicals, and new materials. Current yellow phosphorus production typically employs the carbothermic reduction process from phosphate rock, which is characterized by high reaction temperatures, high energy consumption, high carbon emission intensity, and strong resource dependence. Due to the stability of the P-O bond in phosphate, the release and reduction of phosphorus from phosphate rock requires high temperatures and a strong reducing atmosphere, making the yellow phosphorus extraction process quite complex. The carbothermic reduction of phosphate rock to produce yellow phosphorus usually uses silica (mainly SiO2) as a flux, employing a carbonaceous reducing agent at high temperatures to reduce calcium fluorophosphate (Ca5(PO4)3F) to gaseous elemental phosphorus. The main reactions can be represented as follows: 4Ca5(PO4)3F+30C+21SiO2=6P2(g)+20CaSiO3+SiF4(g)+30CO(g) This process is a typical high-temperature, high-energy-consumption reaction, highly dependent on phosphate rock grade, flux composition, reducing agent activity, and power supply. At lower temperatures, phosphate rock decomposition, calcium silicate formation, and phosphorus oxide reduction are difficult to complete, easily leading to low phosphate rock reduction efficiency, high energy consumption per unit product, and low energy efficiency levels, which no longer meets the development requirements of energy conservation, carbon reduction, and green manufacturing. Furthermore, natural phosphate rock has a complex composition, containing not only CaO, P2O5, and SiO2, but also certain amounts of Fe2O3, Al2O3, MgO, and alkali metal oxides as impurities. Iron oxides or other iron-containing minerals are easily reduced to metallic iron during high-temperature reduction, and further react with phosphorus vapor or phosphorus-containing intermediates released during the reduction process to generate phosphate-iron byproducts. These phosphate-iron byproducts fix some phosphorus in the residue or byproducts, reducing the amount of effective phosphorus entering the gas phase and being condensed and recovered, thus lowering the phosphorus yield in the yellow phosphorus production process. Therefore, improving the reduction efficiency of phosphate rock while reducing or suppressing phosphorus loss caused by iron-containing components is a crucial issue for improving the production efficiency of yellow phosphorus during the carbothermic reduction of phosphate rock. To address this issue, researchers have conducted extensive research on the carbothermic reduction process of phosphate rock, mainly focusing on areas such as additive enhancement, carbon source formulation, raw material pretreatment, and reactor optimization. How to reduce the reaction temperature, improve resource utilization efficiency, and reduce phosphorus loss while ensuring a high phosphorus conversion level has become a key problem urgently needing to be solved in this field.

[0003] CN115744846A discloses a method for preparing yellow phosphorus by enhancing the carbothermic reduction process of phosphate rock with the addition of additives. The method involves finely grinding and mixing phosphate rock, silica, and a carbonaceous reducing agent. Under conditions where the carbon excess coefficient is controlled at approximately 1.03-1.13, a small amount of additives is added before a high-temperature reduction reaction to prepare yellow phosphorus. The phosphate rock used must have a grade higher than 20%, and the additives mainly include metallic manganese, magnesium oxide, elemental sulfur, and molybdenum-based compounds, with an addition amount of 0.5%-8% of the total mass of the mixture. Patent examples show that this type of additive can reduce the phosphate rock reduction temperature while maintaining a high phosphorus release rate; specifically, when m(MgO):m(S) = 1:4 and the additive addition amount is 8%, the phosphorus yield is 96.08%, and the required reaction temperature is reduced from 1450℃ to 1350℃, a reduction of 100℃.

[0004] CN108178136A discloses a carbothermic reduction technology for phosphate rock using alkali metal compounds as catalytic components. The technology aims to improve the utilization efficiency of phosphate rock resources and reduce reaction energy consumption. By pretreating phosphate rock, silica, and coke, and impregnating and modifying the carbonaceous reducing agent with alkali metal compounds, the reducing agent exhibits a significant catalytic effect under high temperature conditions. By holding the reaction at approximately 1300°C for several hours under an argon protective atmosphere, the phosphorus yield can be increased to over 90%.

[0005] CN104016321A discloses a method for enhancing the molten reduction of phosphate rock using a compound carbon source, which effectively solves the problem of insufficient reactivity of low- and medium-grade phosphate rock during high-temperature reduction. This method uses phosphate rock powder, silica, and a compound carbon source as raw materials, and performs molten reduction under high-temperature conditions. The reduction reaction behavior of phosphate rock is improved by adjusting the ratio of different carbonaceous raw materials. Example results show that, after using a compound carbon source, the phosphorus reduction rate can be increased from 67.8% to 95.5%, while the reaction temperature is reduced from 1300℃ to 1200℃.

[0006] CN223404888U presents a systematic design for the carbothermic reduction of phosphate rock to produce yellow phosphorus from the perspective of reaction apparatus and process integration, constructing a continuous reaction system with a fluidized bed reactor as its core. This system feeds pulverized coal and phosphate rock powder separately into the fluidized bed to complete the high-temperature reduction reaction. The resulting high-temperature gas-solid mixture flows through a cyclone separator and a return unit to achieve solid recycling. The gaseous products are converted into phosphoric acid through dust removal and hydration absorption processes. An airflow is introduced at the bottom of the reactor using a blower to maintain the fluidized bed state, thereby enhancing reaction and mass transfer. Related design results indicate that this fluidized bed system helps improve the utilization efficiency of phosphate rock and has certain advantages in terms of continuous operation and economics.

[0007] In summary, while existing carbothermic reduction technologies for phosphate rock can improve the reduction process to some extent through additives, carbon source blending, raw material pretreatment, or reactor optimization, achieving effects such as lowering reaction temperature, increasing phosphorus release rate, improving phosphorus reduction rate, or improving continuous operation, certain limitations remain. First, existing additives are mostly metal, alkali metal compounds, or other specific chemical additives, and the cost, source stability, and industrial applicability of raw materials still need improvement. Second, current technologies do not fully utilize low-cost silicon-containing solid waste, magnesium-aluminum mineral solid waste, and traditional silicon-based fluxing agents to synergistically construct composite fluxing systems, making it difficult to simultaneously achieve fluxing strengthening and solid waste resource utilization. Third, natural phosphate rock has a complex composition and usually contains a certain amount of iron components, which easily generate phosphorus-iron byproducts during high-temperature reduction, fixing some phosphorus in the residue or byproducts, thus reducing the amount of effective phosphorus entering the gas phase and being condensed and recovered. Existing technologies mainly focus on lowering the reduction temperature or increasing the overall phosphorus conversion level, lacking effective control over the generation of phosphorus-iron byproducts caused by iron components and their impact on the product phosphorus yield. Summary of the Invention

[0008] The purpose of this invention is to overcome the problems of excessive phosphorus loss in solid residue, low phosphorus yield, and difficulty in simultaneously achieving fluxing strengthening and solid waste resource utilization in existing technologies. This invention provides a method for preparing yellow phosphorus by reducing phosphate rock. This method effectively reduces the P2O5 content in the residue, increases the phosphorus yield, and enables the resource utilization of industrial solid waste.

[0009] To achieve the above objectives, the present invention provides a method for preparing yellow phosphorus by reducing phosphate rock, wherein the method includes the following steps: (1) The phosphate rock, reducing agent, crude silicon and flux are mixed to obtain a mixture; (2) The mixture is subjected to a reduction reaction in the presence of a non-oxidizing atmosphere to obtain yellow phosphorus and ferrosilicon; The crude silicon contains elemental silicon.

[0010] The method for preparing yellow phosphorus by reducing phosphate rock provided by this invention can convert as much of the phosphorus-iron byproduct generated by the reduction reaction as possible into ferrosilicon by introducing crude silicon containing elemental silicon and a flux, thereby reducing the loss of phosphorus in the solid phase. Furthermore, the iron element in ferrosilicon has a low ability to fix phosphorus, which is beneficial to further reduce the formation of phosphorus-iron byproducts and thus effectively improve the phosphorus yield. In addition, the synergistic effect of crude silicon and flux can effectively improve the melt fluidity and the contact state of the reaction interface, effectively promote the reduction reaction, shorten the reduction reaction time, and reduce the energy consumption of the reduction reaction.

[0011] The method provided by this invention uses readily available raw materials, has low production costs, and can realize the resource utilization of industrial solid waste. Attached Figure Description

[0012] Figure 1 These are X-ray diffraction patterns of the materials prepared by the methods of Example 3 and Comparative Example 3. Detailed Implementation

[0013] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0014] This invention provides a method for preparing yellow phosphorus by reducing phosphate rock, wherein the method includes the following steps: (1) The phosphate rock, reducing agent, crude silicon and flux are mixed to obtain a mixture; (2) The mixture is subjected to a reduction reaction in the presence of a non-oxidizing atmosphere to obtain yellow phosphorus and ferrosilicon; The crude silicon contains elemental silicon.

[0015] The method for preparing yellow phosphorus by reducing phosphate rock provided by this invention can convert as much of the phosphorus-iron byproduct generated by the reduction reaction as possible into ferrosilicon by introducing crude silicon containing elemental silicon and a flux, thereby reducing the loss of phosphorus in the solid phase. Furthermore, the iron element in ferrosilicon has a low ability to fix phosphorus, which is beneficial to further reduce the formation of phosphorus-iron byproducts and thus effectively improve the phosphorus yield. In addition, the synergistic effect of crude silicon and flux can effectively improve the melt fluidity and the contact state of the reaction interface, effectively promote the reduction reaction, shorten the reduction reaction time, and reduce the energy consumption of the reduction reaction.

[0016] In this invention, the type of phosphate rock is not particularly limited, and conventional phosphate rocks in the art are all applicable to this invention. Preferably, the phosphate rock is selected from at least one of sedimentary phosphate rock, magmatic phosphate rock, metamorphic phosphate rock, and weathered phosphate rock; more preferably, the phosphate rock is selected from at least one of collophane, phosphorite, apatite, siliceous phosphate rock, calcareous phosphate rock, magnesian phosphate rock, and iron-bearing phosphate rock.

[0017] In this invention, preferably, in step (1), the phosphate rock contains P2O5, SiO2, MgO, Al2O3, Fe2O3 and CaO.

[0018] In this invention, preferably, in step (1), based on the total weight of the phosphate rock, the content of P2O5 is 20-35%, the content of SiO2 is 5-30%, the content of MgO is 0.1-6%, the content of Al2O3 is 0.1-6%, the content of Fe2O3 is 0.05-3%, and the content of CaO is 30-50%.

[0019] In this invention, preferably, in step (1), the phosphate rock further contains K2O and Na2O.

[0020] In this invention, preferably, in step (1), based on the total weight of the phosphate rock, the content of K2O is 0.01-4% and the content of Na2O is 0.01-1%.

[0021] It should be noted that the phosphate rock may also contain other trace elements, and the present invention does not specifically limit the types of other trace elements. When other trace elements are present, the total content of the other trace elements plus the content of P2O5, SiO2, MgO, Al2O3, Fe2O3, CaO, K2O and Na2O must satisfy 100%.

[0022] In this invention, the content of each component in the phosphate rock is obtained by X-ray fluorescence spectroscopy analysis.

[0023] In this invention, the type of reducing agent is not particularly limited. Preferably, in step (1), the reducing agent is selected from at least one of coke, white coal, and lignite; more preferably, the reducing agent is coke.

[0024] In this invention, preferably, the molar ratio of the reducing agent (calculated as carbon) to the phosphate rock (calculated as P2O5) is ≥5:1, more preferably 5.25-5.75:1. When the molar ratio is less than 5:1, because the phosphate rock contains iron and carbonates, some carbon is consumed, resulting in incomplete reduction of P2O5 in the phosphate rock, an increase in the P2O5 content in the residue, a decrease in the phosphate rock reduction rate, and a decrease in phosphorus yield. When the molar ratio is too high, there will be too much reducing agent, resulting in waste of raw materials. At the same time, it will also promote the occurrence of side reactions, increase power consumption, reduce the thermal efficiency of the electric furnace, and lead to an increase in phosphorus power consumption.

[0025] In this invention, preferably, in step (1), the content of elemental silicon is 90-98% based on the total weight of the crude silicon, and more preferably 92-96%. This preferred embodiment ensures that the crude silicon has a high effective silicon content, so that it can fully play its role in promoting the transformation of phosphorus-iron byproducts into silicon-iron phase during the reduction process, reducing the fixation and loss of phosphorus in the solid residue, thereby improving the phosphorus yield.

[0026] In this invention, preferably, in step (1), the crude silicon further comprises O, C and Fe elements.

[0027] In this invention, the selection range for the content of each component in the crude silicon is relatively wide. Preferably, based on the total weight of the crude silicon, the content of O element is 1-8%, the content of C element is 0.01-1.5%, and the content of Fe element is 0.001-0.5%; more preferably, based on the total weight of the crude silicon, the content of O element is 3-6%, the content of C element is 0.1-1.5%, and the content of Fe element is 0.01-0.5%. This preferred embodiment helps to ensure the effective content of elemental silicon in the crude silicon while reducing the amount of Fe introduced, thereby reducing the fixation effect of additional iron-containing components on phosphorus element and promoting the transformation of the phosphorus-iron byproduct generated during the reduction process into the silicon-iron phase, thus reducing the loss of phosphorus element in the solid residue and increasing the phosphorus yield.

[0028] In this invention, the content of each component in the crude silicon is obtained by X-ray fluorescence spectroscopy and ICP-OES analysis.

[0029] It should be noted that the crude silicon may also contain other trace elements, and the present invention does not specifically limit the types of other trace elements. When other trace elements are present, the total content of the other trace elements plus the content of elemental silicon, O, C and Fe must satisfy 100%.

[0030] In this invention, preferably, the type of flux is not particularly limited. Preferably, in step (1), the flux is selected from at least one of coal gangue, coal ash, silica, and feldspar, with coal gangue being the most preferred. This preferred embodiment is beneficial for enhancing melt fluidity and improving the fluxing effect, while promoting close contact between phosphate rock, reducing agent, and crude silica, thereby helping to promote the carbothermic reduction reaction of phosphate rock and thus increasing phosphorus yield.

[0031] In this invention, preferably, the flux contains SiO2, MgO, Al2O3, Fe2O3 and CaO.

[0032] In this invention, preferably, based on the total weight of the flux, the content of SiO2 is 25-95%, the content of MgO is 0.01-10%, the content of Al2O3 is 0.1-50%, the content of Fe2O3 is 0.5-15%, and the content of CaO is 0.2-15%; more preferably, based on the total weight of the flux, the content of SiO2 is 25-50%, the content of MgO is 5-10%, the content of Al2O3 is 25-45%, the content of Fe2O3 is 5-10%, and the content of CaO is 8-15%. This preferred embodiment is advantageous in controlling the slag phase composition of the reduction system through the synergistic effect of MgO, Al2O3, SiO2 and CaO components, promoting the formation of low-melting-point silicate or aluminosilicate phases, improving the fluidity of high-temperature melts and the contact state of the reaction interface, while avoiding the excessive introduction of impurity components that would have an adverse effect on the reduction reaction and phosphorus recovery process, thereby improving the phosphorus yield.

[0033] It should be noted that the flux may also contain other trace elements. The present invention does not specifically limit the types of other trace elements. When other trace elements are present, the total content of these trace elements, combined with the content of SiO2, MgO, Al2O3, Fe2O3, and CaO, shall satisfy 100%.

[0034] In this invention, the content of each component in the flux is obtained by X-ray fluorescence spectroscopy analysis.

[0035] In this invention, preferably, in step (1), the mass ratio of the flux to crude silicon is 1:0.1-0.5, more preferably 1:0.1-0.2. This preferred embodiment helps ensure that elemental silicon in the crude silicon fully promotes the conversion of ferrophosphorus byproducts to the ferrosilicon phase, while appropriately introducing flux to regulate the slag phase composition of the reduction system, promoting the formation of low-melting-point silicate or aluminosilicate phases, improving the fluidity of the high-temperature melt and the contact state of the reaction interface, thereby strengthening the mass transfer and reaction process between phosphate rock, reducing agent, crude silicon, and flux, and increasing phosphorus yield.

[0036] In this invention, preferably, in step (1), the total mass of the crude silicon and the flux accounts for 5-30% of the mass of the phosphate rock on a dry basis, more preferably 6-10%. This preferred embodiment is advantageous in ensuring that elemental silicon promotes the conversion of ferrophosphate by-products to the ferrosilicon phase, while appropriately controlling the slag phase composition and melting characteristics of the reduction system, thus improving phosphorus yield. Using the above-mentioned preferred proportions of crude silicon and flux effectively avoids the problem of insufficient addition of crude silicon and flux affecting the conversion of ferrophosphate by-products to the ferrosilicon phase, and also effectively avoids the problems of excessive addition causing material system dilution, increased slag volume, and increased energy consumption.

[0037] In this invention, preferably, in step (1), the phosphate rock, reducing agent, crude silicon and flux are dried independently and then mixed to obtain the mixture with a water content ≤3wt%.

[0038] In this invention, preferably, in step (1), the mixture containing phosphate rock, reducing agent, crude silicon, and flux refers to a mixture that may contain other components besides phosphate rock, reducing agent, crude silicon, and flux. Preferably, the mixture is composed of phosphate rock, reducing agent, crude silicon, and flux.

[0039] In this invention, preferably, the mixing conditions in step (1) are not particularly limited, as long as the phosphate rock, reducing agent, crude silicon, and flux are mixed evenly. Preferably, the mixing conditions include a temperature of 0-60°C, more preferably 20-30°C.

[0040] In this invention, preferably, the reduction reaction is carried out in a reactor.

[0041] In this invention, the conditions for the reduction reaction in step (2) are not particularly limited. Preferably, the conditions for the reduction reaction include: a temperature of 1300-1650℃, for example, 1300℃, 1350℃, 1400℃, 1450℃, 1500℃, 1650℃, or any value within any range of two such values, preferably 1400-1500℃; and a time of 10-100 min, for example, 10 min, 20 min, 40 min, 60 min, 80 min, 100 min, or any value within any range of two such values, preferably 20-100 min. This preferred embodiment helps to reduce the P2O5 content in the residue and increase the phosphorus yield.

[0042] In this invention, step (2) further includes cooling the material obtained after the reduction reaction.

[0043] In this invention, the cooling method and conditions are not particularly limited, as long as the gaseous elemental phosphorus (P2) generated by the reduction reaction is converted into yellow phosphorus (P4).

[0044] The present invention will be described in detail below through embodiments.

[0045] Unless otherwise specified, room temperature in the following examples refers to 25±5℃.

[0046] In the following embodiments, unless otherwise specified, all raw materials are commercially available products.

[0047] In the following examples, the phosphorus yield is calculated using the following formula:

[0048] in, For phosphorus yield, The mass of the material before the reaction. The total phosphorus in the material before the reaction is The calculated mass fraction, The mass of the residue after the reaction, The total phosphorus in the residue after the reaction is The total phosphorus content is calculated as the mass fraction, which refers to the sum of all forms of phosphorus (phosphorus iron and phosphorus pentoxide) present in the material / residue.

[0049] Comparative Example 1 (1) Phosphate rock, coke, and silica are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.25:1, and the mass of silica accounts for 25% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the silica, the SiO2 content is 94.25%, the MgO content is 0.06%, the Al2O3 content is 0.32%, the Fe2O3 content is 0.7%, and the CaO content is 0.22%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1350℃, 1400℃, 1450℃ and 1500℃ for 20 min respectively. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed and the phosphorus yield was calculated. The experimental data are shown in Table 1.

[0050] Example 1 (1) Phosphate rock, coke, crude silicon and coal gangue A are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein, the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.25:1, and the mass ratio of the coal gangue A to the crude silicon is 1:0.1; the total mass of the crude silicon and the coal gangue A accounts for 9% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the crude silicon, the Si content is 93.25%, the O content is 4.79%, the C content is 0.21%, and the Fe content is 0.04%. Based on the total weight of the coal gangue A, the content of SiO2 is 41.45%, the content of MgO is 5.76%, the content of Al2O3 is 32.4%, the content of Fe2O3 is 8.05%, and the content of CaO is 10.11%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1350℃, 1400℃, 1450℃ and 1500℃ for 20 min respectively. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed and the phosphorus yield was calculated. The experimental data are shown in Table 1.

[0051] Table 1

[0052] As shown in Table 1, compared with Comparative Example 1, Example 1 exhibits a lower residual P2O5 content and a higher phosphorus yield at the same reaction temperature.

[0053] Comparative Example 2 (1) Phosphate rock, coke, and coal gangue B are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.5:1, and the mass of coal gangue B accounts for 6%, 7%, 8%, 9%, 10%, and 15% of the mass of the phosphate rock on a dry basis, respectively; Of which, based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, the content of SiO2 is 20.11%, the content of MgO is 2.31%, the content of Al2O3 is 1.24%, the content of Fe2O3 is 0.82%, the content of CaO is 37.49%, the content of K2O is 0.31%, and the content of Na2O is 0.54%. Based on the total weight of the coal gangue B, the content of SiO2 is 39.5%, the content of MgO is 6.5%, the content of Al2O3 is 35%, the content of Fe2O3 is 7.83%, and the content of CaO is 10.45%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1450°C for 60 minutes. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 2.

[0054] Example 2 (1) Phosphate rock, coke, crude silicon and coal gangue B are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein, the molar ratio of the coke (calculated as C) and the phosphate rock (calculated as P2O5) is 5.5:1, and the mass ratio of the coal gangue B and the crude silicon is 1:0.15; the total mass of the crude silicon and the coal gangue B accounts for 6%, 7%, 8%, 9%, 10% and 15% of the mass of the phosphate rock on a dry basis, respectively; Of which, based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, the content of SiO2 is 20.11%, the content of MgO is 2.31%, the content of Al2O3 is 1.24%, the content of Fe2O3 is 0.82%, the content of CaO is 37.49%, the content of K2O is 0.31%, and the content of Na2O is 0.54%. Based on the total weight of the crude silicon, the Si content is 93.25%, the O content is 4.79%, the C content is 0.21%, and the Fe content is 0.04%. Based on the total weight of the coal gangue B, the content of SiO2 is 39.5%, the content of MgO is 6.5%, the content of Al2O3 is 35%, the content of Fe2O3 is 7.83%, and the content of CaO is 10.45%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1450°C for 60 minutes. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 2.

[0055] Table 2

[0056] As shown in Table 2, the phosphorus yield of Example 2 and Comparative Example 2 showed a trend of first increasing and then decreasing with the increase of the total amount of crude silicon and flux. Compared with Comparative Example 2, the use of crude silicon and coal gangue composite addition in Example 2 can effectively reduce the residual P2O5 content and improve the phosphorus yield.

[0057] Comparative Example 3 (1) Phosphate rock, coke, and silica are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.75:1, and the mass of silica accounts for 23% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the silica, the SiO2 content is 94.25%, the MgO content is 0.06%, the Al2O3 content is 0.32%, the Fe2O3 content is 0.7%, and the CaO content is 0.22%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1500℃ for 20 min, 40 min, 60 min, 80 min, and 100 min. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 3.

[0058] Example 3 (1) Phosphate rock, coke, crude silicon and coal gangue C are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein, the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.75:1, and the mass ratio of the coal gangue C to the crude silicon is 1:0.2; the total mass of the crude silicon and the coal gangue C accounts for 9% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the crude silicon, the Si content is 93.25%, the O content is 4.79%, the C content is 0.21%, and the Fe content is 0.04%. Based on the total weight of the coal gangue C, the content of SiO2 is 42.5%, the content of MgO is 6%, the content of Al2O3 is 33.2%, the content of Fe2O3 is 6.88%, and the content of CaO is 11.06%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1500℃ for 20 min, 40 min, 60 min, 80 min, and 100 min. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 3.

[0059] Figure 1The X-ray diffraction patterns of the materials obtained by reacting the mixtures in Example 3 and Comparative Example 3 at 1500°C for 100 min are shown below. Figure 1 As can be seen, the material obtained in Example 3 showed characteristic diffraction peaks belonging to FeSi2 at 2θ of 29.44° and 46.07°, and characteristic diffraction peaks belonging to FeSi at 2θ of 45.34°, indicating that the material obtained in Example 3 contained ferrosilicon. In contrast to Example 3, the material obtained in Comparative Example 3 did not have characteristic diffraction peaks belonging to ferrosilicon, indicating that no ferrosilicon was generated in the material obtained in Comparative Example 3.

[0060] Table 3

[0061] As shown in Table 3, compared with Comparative Example 3, Example 3 exhibits a lower residual P2O5 content and a higher phosphorus yield at the same reaction temperature.

[0062] Comparative Example 4 (1) Phosphate rock, coke, and silica are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.75:1, and the mass of silica accounts for 23% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the silica, the SiO2 content is 94.25%, the MgO content is 0.06%, the Al2O3 content is 0.32%, the Fe2O3 content is 0.7%, and the CaO content is 0.22%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1450°C for 20 min, 40 min, 60 min, 80 min, and 100 min, respectively. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 4.

[0063] Comparative Example 5 (1) Phosphate rock, coke, and crude silicon are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.75:1, and the mass of the crude silicon accounts for 9% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the crude silicon, the Si content is 93.25%, the O content is 4.79%, the C content is 0.21%, and the Fe content is 0.04%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1450°C for 20 min, 40 min, 60 min, 80 min, and 100 min, respectively. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 4.

[0064] Example 4 (1) Phosphate rock, coke, crude silicon and coal gangue C are mixed and dried to obtain a mixture with a water content ≤3wt%; wherein, the molar ratio of the coke (calculated as C) to the phosphate rock (calculated as P2O5) is 5.75:1, the mass ratio of the coal gangue C to the crude silicon is 1:0.5; the total mass of the crude silicon and the coal gangue C accounts for 9% of the mass of the phosphate rock on a dry basis; Based on the total weight of the phosphate rock, the content of P2O5 is 25.16%, SiO2 is 20.11%, MgO is 2.31%, Al2O3 is 1.24%, Fe2O3 is 0.82%, CaO is 37.49%, K2O is 0.31%, and Na2O is 0.54%. Based on the total weight of the crude silicon, the Si content is 93.25%, the O content is 4.79%, the C content is 0.21%, and the Fe content is 0.04%. Based on the total weight of the coal gangue C, the content of SiO2 is 42.5%, the content of MgO is 6%, the content of Al2O3 is 33.2%, the content of Fe2O3 is 6.88%, and the content of CaO is 11.06%. (2) Under an argon atmosphere, the mixture was placed in a reactor and reacted at 1450°C for 20 min, 40 min, 60 min, 80 min, and 100 min, respectively. After the mixture was removed and cooled to room temperature, the P2O5 content in the residue was analyzed, and the phosphorus yield was calculated. The experimental data are shown in Table 4.

[0065] Table 4

[0066] As shown in Table 4, Comparative Example 4 did not add crude silicon, and Comparative Example 5 did not add flux. Compared with Example 4, under the same reduction reaction temperature and time conditions, Comparative Example 4 and Comparative Example 5 had higher residual P2O5 content and lower phosphorus yield. This also indicates that the combined use of crude silicon and flux can significantly promote the carbothermic reduction process of phosphate rock, which is beneficial to reducing the residual P2O5 content and increasing the phosphorus yield, and reducing the loss of phosphorus in the solid residue. In addition, compared with Comparative Example 4, Comparative Example 5 had higher residual P2O5 content and lower phosphorus yield. Crude silicon alone is difficult to achieve effective fluxing and slag formation. Crude silicon is more suitable for use in combination with fluxes such as silica and coal gangue to better exert its role in promoting the conversion of ferrophosphorus by-products to the ferrosilicon phase and improving the slag flowability.

[0067] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing yellow phosphorus by reducing phosphate rock, characterized in that, The method includes the following steps: (1) The phosphate rock, reducing agent, crude silicon and flux are mixed to obtain a mixture; (2) The mixture is subjected to a reduction reaction in the presence of a non-oxidizing atmosphere to obtain yellow phosphorus and ferrosilicon; The crude silicon contains elemental silicon.

2. The method according to claim 1, wherein, In step (1), the phosphate rock contains P2O5, SiO2, MgO, Al2O3, Fe2O3 and CaO; Preferably, in step (1), based on the total weight of the phosphate rock, the content of P2O5 is 20-35%, the content of SiO2 is 5-30%, the content of MgO is 0.1-6%, the content of Al2O3 is 0.1-6%, the content of Fe2O3 is 0.05-3%, and the content of CaO is 30-50%.

3. The method according to claim 1 or 2, wherein, In step (1), the reducing agent is selected from at least one of coke, white coal and lignite; Preferably, the molar ratio of the reducing agent (calculated as C) to the phosphate rock (calculated as P2O5) is ≥5:1, more preferably 5.25-5.75:

1.

4. The method according to any one of claims 1-3, wherein, In step (1), based on the total weight of the crude silicon, the content of elemental silicon is 90-98%, preferably 92-96%.

5. The method according to any one of claims 1-4, wherein, In step (1), the flux is selected from at least one of coal gangue, coal ash, silica and feldspar, preferably coal gangue; Preferably, the flux contains SiO2, MgO, Al2O3, Fe2O3 and CaO; Preferably, based on the total weight of the flux, the content of SiO2 is 25-95%, the content of MgO is 0.01-10%, the content of Al2O3 is 0.1-50%, the content of Fe2O3 is 0.5-15%, and the content of CaO is 0.2-15%. More preferably, based on the total weight of the flux, the content of SiO2 is 25-50%, the content of MgO is 5-10%, the content of Al2O3 is 25-45%, the content of Fe2O3 is 5-10%, and the content of CaO is 8-15%.

6. The method according to any one of claims 1-5, wherein, In step (1), the mass ratio of flux to crude silicon is 1:0.1-0.

5.

7. The method according to claim 6, wherein, In step (1), the mass ratio of flux to crude silicon is 1:0.1-0.

2.

8. The method according to any one of claims 1-7, wherein, In step (1), the total mass of the crude silicon and the flux accounts for 5-30% of the mass of the phosphate rock on a dry basis, preferably 6-10%.

9. The method according to any one of claims 1-8, wherein, In step (1), the phosphate rock, reducing agent, crude silicon and flux are dried independently and then mixed to obtain the mixture with a water content of ≤3wt%.

10. The method according to any one of claims 1-9, wherein, The conditions for the reduction reaction include: a temperature of 1300-1650℃, preferably 1350-1500℃; and a time of 10-100min, preferably 20-100min.

Citation Information

Patent Citations

  • Method of smelting reduction of middle- and low- grade phosphate ore by utilization of mixed carbon source

    CN104016321A

  • Method for catalyzing carbothermal reduction of phosphate rock by alkali metal compound