A method for preparing electronic-grade phosphorus oxychloride for integrated circuits
By employing a synergistic process of pre-distillation, anhydrous oxidation via oxygen/ozone microchannels, membrane degassing, and two-stage fixed-bed impurity trapping, and using anhydrous zirconium pyrophosphate-titanium phosphate/PFA composite impurity trapping material, the problem of insufficient purity and reliability of electronic-grade phosphorus oxychloride in existing technologies has been solved, achieving the preparation of phosphorus oxychloride with high purity and high stability.
Patent Information
- Application Number
- CN202611178669.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing electronic-grade phosphorus oxychloride are ineffective in removing trace metal impurities, moisture, and acidic impurities, resulting in insufficient product purity and reliability. Furthermore, traditional methods may introduce new impurities or increase the separation burden.
A synergistic process of pre-distillation, oxygen/ozone microchannel anhydrous oxidation, membrane degassing, and two-stage fixed-bed impurity trapping is adopted. Anhydrous zirconium pyrophosphate-titanium phosphate/PFA composite impurity trapping material is used. The oxidation efficiency is improved by microchannel reactor, dissolved impurities are removed by membrane degassing, and deep purification is achieved by two-stage fixed-bed impurity trapping columns.
It achieves synergistic control of trace metal impurities, moisture and acidic impurities, improves the purity and batch stability of phosphorus oxychloride, reduces the risk of metal leaching contamination, and increases the first-pass yield of the product.
Smart Images

Figure CN123105570A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of phosphorus compound technology, and more specifically to a method for preparing electronic-grade phosphorus oxychloride for use in integrated circuits. Background Technology
[0002] Phosphorus oxychloride is an important phosphorus-containing inorganic compound widely used in integrated circuit manufacturing, including phosphorus source diffusion doping, preparation of phosphorus-containing electrolyte materials and electrolyte additives, synthesis of pharmaceutical and pesticide intermediates, and preparation of flame retardants and other phosphorus-containing functional materials. In integrated circuit manufacturing, phosphorus oxychloride is commonly used as a phosphorus source in silicon wafer diffusion doping processes. Its purity, moisture content, free acid content, metal ion content, and particulate impurities directly affect phosphorus diffusion uniformity, wafer surface cleanliness, and device reliability. As integrated circuits develop towards higher integration and higher reliability, the requirements for impurity control of electronic-grade phosphorus oxychloride are becoming increasingly stringent, especially the need to simultaneously reduce trace metal impurities such as Fe, Cu, Ni, Cr, Na, K, and Al, as well as moisture, hydrogen chloride, phosphorus trichloride residues, and particulate contamination.
[0003] Existing methods for preparing electronic-grade phosphorus oxychloride typically include steps such as phosphorus trichloride oxidation, distillation, rectification, sub-boiling distillation, or the addition of complexing agents to remove metals. While these methods can increase the main content of phosphorus oxychloride, they still have certain shortcomings: Firstly, traditional reaction or purification processes easily introduce moisture and acidic chlorides, leading to the hydrolysis of phosphorus oxychloride and the production of byproducts such as hydrogen chloride. Secondly, when using complexing agents or soluble auxiliaries for impurity removal, new ions, organic residues, or particulate contamination may be introduced, increasing the burden on subsequent separation processes. Furthermore, relying solely on rectification is insufficient to effectively remove low-content metal impurities and polar chlorides, easily resulting in impurity tailing and reducing the first-pass yield of electronic-grade products. Summary of the Invention
[0004] In view of the shortcomings of the existing technology, the purpose of this invention is to provide a method for preparing electronic-grade phosphorus oxychloride for integrated circuits.
[0005] A method for preparing electronic-grade phosphorus oxychloride for integrated circuits includes the following steps: (1) High-purity phosphorus trichloride is pre-distilled to obtain refined phosphorus trichloride; (2) The refined phosphorus trichloride is fed into the PFA-lined microchannel reactor and oxygen / ozone mixture is introduced at the same time to carry out anhydrous oxidation reaction. The reaction product is collected by condensation of PFA receiver to obtain crude phosphorus oxychloride. (3) The crude phosphorus oxychloride was fed into a PFA hollow fiber membrane degasser for degassing to obtain degassed phosphorus oxychloride. (4) Transfer the degassed phosphorus oxychloride into the PFA circulating tank, and let the degassed phosphorus oxychloride circulate through the two-stage series-connected PFA fixed bed impurity collection column to obtain phosphorus oxychloride after impurity collection treatment. (5) The phosphorus oxychloride after impurity removal treatment is distilled, the middle fraction is collected, filtered and bottled to obtain electronic grade phosphorus oxychloride for integrated circuits; The two-stage series-connected PFA fixed-bed impurity trapping column includes a first-stage main impurity trapping column and a second-stage protective impurity trapping column. Both stages of the PFA fixed-bed impurity trapping column are filled with anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material.
[0006] In step (1), the parameters of the pre-distillation are as follows: the pre-distillation is carried out under normal pressure, the bottom temperature of the column is 76-85℃, the top temperature of the column is 74.5-76.5℃, the total reflux is 0.5-1.5h, 1-3wt% of the fore-distillate is discarded, and the fraction with the top temperature of 74.5-76.5℃ is collected.
[0007] In step (2), the volumetric flow rate during the transport of refined phosphorus trichloride is 250-380 ml / h; the molar flow rate of oxygen is 0.5-0.55 times that of refined phosphorus trichloride; and the volume fraction of ozone is 0.1-0.3% of the total volume of the oxygen / ozone mixture.
[0008] In step (2), the reaction temperature of the anhydrous oxidation reaction is 60-70℃, the time is 60-120s, and the reaction gauge pressure is 0.2-0.3MPa.
[0009] In step (3), the degassing treatment temperature is 25-35℃, the liquid side gauge pressure is 0.04-0.06MPa, the absolute pressure outside the membrane is 30-50kPa, and the time is 20-30min.
[0010] The anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity catching material is prepared by the following method: S1: Ultrapure water and zirconium oxychloride octahydrate were stirred and mixed, phosphoric acid was added, and then tetraisopropyl titanate was added. The mixture was heated to reflux and then subjected to hydrothermal reaction. The mixture was then placed in a tube furnace for dehydration pyrophosphorylation treatment to obtain anhydrous zirconium pyrophosphate-titanium phosphate composite powder. S2: Anhydrous zirconium pyrophosphate-titanium phosphate composite powder is mixed with electronic-grade PFA micro powder, and then subjected to pre-pressing, hot pressing, cooling, demolding, crushing and sieving to obtain anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity-catching material.
[0011] In step S1, the mass ratio of zirconium oxychloride octahydrate, phosphoric acid, and tetraisopropyl titanate is 1.6:1.5:0.7.
[0012] In step S2, the mass ratio of the anhydrous zirconium pyrophosphate-titanium phosphate composite powder to electronic-grade PFA micro powder is 7:13.
[0013] The total loading of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is 8-15 wt% of the crude phosphorus oxychloride mass, wherein the loading mass of the first-stage main impurity trapping column is 60%-70% of the total loading mass, and the loading mass of the second-stage protective impurity trapping column is 30%-40% of the total loading mass.
[0014] In step (5), the distillation parameters are as follows: the absolute pressure at the top of the column is 40-60 kPa, the total reflux is carried out for 2-4 hours, and then the fraction is cut at a reflux ratio of (8-12):1. The temperature at the top of the column is 80-90℃, and the temperature at the bottom of the column is 87-97℃.
[0015] Due to the adoption of the above technical solutions, the beneficial effects of the present invention include: This application achieves synergistic control of moisture, acidic impurities, residual phosphorus trichloride, and metallic impurities in electronic-grade phosphorus oxychloride through a synergistic process of pre-distillation of high-purity phosphorus trichloride, anhydrous oxidation via oxygen / ozone microchannels, membrane degassing, two-stage fixed-bed impurity removal, and distillation. Specifically, the microchannel reactor improves the contact efficiency and heat transfer efficiency between phosphorus trichloride and oxygen / ozone, allowing the oxidation reaction to proceed uniformly within a shorter residence time, reducing unreacted phosphorus trichloride residue and side reactions. The membrane degassing step pre-removes dissolved oxygen, ozone, hydrogen chloride, and low-boiling volatile impurities, reducing the load on subsequent impurity removal and distillation. The composite impurity trapping material of this application comprises anhydrous zirconium pyrophosphate-titanium phosphate inorganic phase with structures such as Zr-OP, Ti-OP, and POP, which can coordinate, immobilize, ion exchange, or surface adsorb trace metallic impurities such as Na, K, Ca, Mg, Al, Fe, Cu, Ni, and Pb, as well as acidic and polar trace impurities in phosphorus oxychloride. The PFA phase can immobilize and support the inorganic impurity trapping phase, reducing the risk of powder shedding and secondary pollution, and improving the structural stability of the impurity trapping material in the highly corrosive phosphorus oxychloride system. Furthermore, this application employs a two-stage PFA fixed-bed series structure. The first-stage main impurity trapping column bears the main impurity trapping load, while the second-stage protective impurity trapping column performs secondary interception of trace impurities that penetrate through the first stage, reducing the risk of impurity penetration caused by local saturation, bed channeling, or raw material fluctuations in a single-stage fixed bed. By leveraging the synergistic effect of composite impurity-catching materials and a two-stage PFA fixed-bed series structure, the removal depth of impurities such as metal impurities, free acid, residual phosphorus trichloride, and TOC can be improved, while reducing metal leaching contamination from fixed-bed and piping materials. This, in turn, enhances the purity, batch stability, and process cleanliness of electronic-grade phosphorus oxychloride. Attached Figure Description
[0016] Figure 1The infrared spectrum of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1; Figure 2 The image shows the X-ray diffraction pattern of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1. Detailed Implementation
[0017] Example 1: Preparation of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material S1: Mix 6L of ultrapure water and 320g of zirconium oxychloride octahydrate, stir at 300rpm for 20min, and under nitrogen protection, slowly add 2000g of 15wt% phosphoric acid aqueous solution at 10℃ for 3h. After the addition is complete, stir at 300rpm for 20min, and slowly add 1200ml of anhydrous isopropanol solution containing 140g of tetraisopropyl titanate at 10℃ for 2h. After the addition is complete, stir at 300rpm for 30min, and heat to reflux for 6h. Then transfer to a polytetrafluoroethylene-lined hydrothermal reactor and hydrothermally react at 130℃ for 8h. Cool to room temperature, filter, and wash the filter cake with 60℃ ultrapure water (3×1L) and anhydrous isopropanol (3×1L). The zirconium titanium phosphate precursor was obtained by vacuum drying at 120℃ for 12h. The zirconium titanium phosphate precursor was placed in a tube furnace and nitrogen gas was introduced (nitrogen flow rate of 200mL / min). The temperature was first increased to 180℃ at a heating rate of 2℃ / min and held for 1h. Then the temperature was increased to 750℃ at a heating rate of 1.5℃ / min and held for 3h. The furnace was then naturally cooled to room temperature under nitrogen protection. The powder was ground at 100rpm for 5min and passed through a 200-mesh sieve to obtain anhydrous zirconium pyrophosphate-titanium phosphate composite powder. S2: Under nitrogen protection, 350g of anhydrous zirconium pyrophosphate-titanium phosphate composite powder and 650g of electronic-grade PFA micro powder were mixed and dried under vacuum at 120℃ for 6h. The mixture was then added to a mold with a PFA film lining the inner wall and pressed at 5MPa for 5min at room temperature. The temperature was then raised to 340℃ and hot-pressed at 5MPa for 20min. After hot pressing, the pressure was maintained and the mixture was allowed to cool naturally to 70℃. The mold was then demolded and pre-cooled with liquid nitrogen for 15min under dry nitrogen protection. The mixture was then crushed at 200rpm for 5min using a PFA lining crusher. After sieving, anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity-catching material with a particle size of 0.8-2mm was obtained.
[0018] Figure 1 The image shows the infrared spectrum of the prepared anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trap. As can be seen from the image, at 3435 cm⁻¹... -1 Only a weak, broad absorption peak appears nearby, at 1640 cm⁻¹. -1 The weak water bending vibration peaks nearby indicate that the material has relatively little residual adsorbed water after dehydration and pyrophosphorylation treatment. (1221 cm⁻¹) -1 and 1150cm-1 A strong -CF2- stretching vibration absorption peak appears nearby, at 842 cm⁻¹. -1 and 638cm -1 The presence of -CF2--related vibrational peaks in the vicinity of PFA indicates the introduction of the PFA framework. (1062 cm⁻¹) -1 The nearby absorption peak is mainly attributed to the PO stretching vibration in the phosphate structure, 936 cm⁻¹. -1 and 756cm -1 The nearby absorption peak can be attributed to the POP pyrophosphate structural vibration, indicating the presence of a pyrophosphate structure. (585 cm⁻¹) -1 and 535cm -1 The nearby absorption peaks can be attributed to vibrations in the Ti-OP and Zr-OP structures.
[0019] Figure 2 The X-ray diffraction pattern of the prepared anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is shown in the figure. As can be seen from the figure, the main characteristic diffraction peaks related to the semi-crystalline structure of PFA appear near diffraction angles of 17°, 33°, 50°, 53° and 71°, indicating that the PFA framework structure is retained in the composite impurity trapping material. At the same time, the main diffraction peaks related to zirconium phosphate / zirconium pyrophosphate appear near diffraction angles of 22°, 28°, 29°, 40°, 46°, 57°, 62° and 68°, indicating that the zirconium source forms a zirconium pyrophosphate inorganic phase after phosphorylation, hydrothermal aging and high-temperature dehydration treatment. In addition, diffraction signals related to titanium phosphate / titanium pyrophosphate can be observed near diffraction angles of 21°, 47° and 58°, indicating that the titanium source participates in the formation of an inorganic impurity trapping phase containing Ti-OP structure. Since the PFA semi-crystalline peak, zirconium pyrophosphate peak, and titanium phosphate peak overlap in some angular regions, the remaining diffraction peaks in the figure can be attributed to the combined effect of the multiphase phosphate structure, the PFA semi-crystalline structure, and their peak overlap. Both the X-ray diffraction pattern and the infrared spectrum indicate that the prepared anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material retains the PFA framework structure and contains the zirconium titanium phosphate inorganic impurity trapping phase.
[0020] Example 2: Preparation of electronic-grade phosphorus oxychloride for integrated circuits (1) Add 3500g of high-purity phosphorus trichloride to a quartz distillation column and carry out atmospheric pressure pre-distillation under nitrogen protection. The actual number of trays in the distillation column is 20, the bottom temperature is 76℃, the top temperature is 74.5℃, and the total reflux is carried out for 0.5h. 35g of the first fraction is discarded, and the fraction with the top temperature of 74.5℃ is collected to obtain 3304g of refined phosphorus trichloride. The remaining material is used as bottom residue and liquid holdup in the column and does not enter the subsequent oxidation reaction. (2) All the obtained purified phosphorus trichloride was fed into a PFA-lined microchannel reactor at a flow rate of 250 ml / h, while an oxygen / ozone mixture was introduced. The oxygen purity was 99.999%, the oxygen dew point was -70℃, the ozone volume fraction was 0.1% of the total volume of the oxygen / ozone mixture, the oxygen molar flow rate was 1.43 mol / h, the reaction temperature was 60℃, the reaction gauge pressure was 0.2 MPa, and the average residence time of the material was 120 s. The reaction product was condensed and collected in a PFA receiver at 5℃ to obtain 3561 g of crude phosphorus oxychloride. (3) All the obtained crude phosphorus oxychloride was fed into a PFA hollow fiber membrane degasser and degassed for 30 min at 25°C, liquid side gauge pressure of 0.04 MPa and membrane outside absolute pressure of 30 kPa. The membrane outside was purged with nitrogen at a flow rate of 0.3 L / min, and 3547 g of degassed phosphorus oxychloride was obtained. (4) All the degassed phosphorus oxychloride obtained was transferred into a PFA circulating tank purged with dry nitrogen, and the temperature was controlled at 20°C. Two-stage PFA fixed-bed impurity traps were set up in series. The first stage was the main impurity trap (inner diameter 30 mm, effective filling height 400 mm), and the second stage was the protective impurity trap (inner diameter 30 mm, effective filling height 180 mm). Both stages of the fixed bed were filled with anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1. The total filling amount of the composite impurity trapping material was 285 g, the filling mass of the first-stage main impurity trapping column was 171 g, and the filling mass of the second-stage protective impurity trapping column was 114 g. The degassed phosphorus oxychloride was circulated through the first-stage main impurity trapping column and the second-stage protective impurity trapping column sequentially by a PFA diaphragm pump. The circulation flow rate was 0.5 L / h, the fixed bed gauge pressure was 0.05 MPa, and the circulation treatment was carried out for 4 h to obtain 3520 g of phosphorus oxychloride after impurity trapping treatment. (5) All the obtained phosphorus oxychloride after impurity removal treatment was transferred into a quartz distillation column with 20 actual trays and an absolute pressure of 40 kPa at the top. The column was first refluxed for 4 hours, and then the fraction was cut at a reflux ratio of 8:1. 176 g of the first fraction was discarded, and 3133 g of the middle fraction was collected. 211 g of the residue in the bottom of the column was not included in the product. During the distillation process, the temperature at the top of the column was controlled at 80°C and the temperature in the bottom of the column was controlled at 87°C. The bottom of the column must not be dried. The obtained middle fraction was filtered through a 0.03 μm PFA membrane filter and filled into PFA containers that had been dried at 120°C and purged with nitrogen in a local Class 100 clean environment. The relative humidity of the filling environment was 1%. After filling, the container was kept under a slight positive pressure of nitrogen to obtain electronic grade phosphorus oxychloride for integrated circuits.
[0021] The obtained electronic-grade phosphorus oxychloride had a phosphorus oxychloride content of 99.99999% as determined by gas chromatography area normalization; moisture content was 38.1 ppb; free acid (calculated as HCl) was 12.2 ppb; residual phosphorus trichloride was 0.6 ppb; and TOC was 5.8 ppb. Moisture content was determined using a coulometric Karl Fischer moisture analyzer; free acid was determined using acid-base titration; residual phosphorus trichloride was determined using gas chromatography; and TOC was determined using a TOC analyzer. ICP-MS analysis revealed the following metal impurities: Li 1.13 ppb, Na 2.51 ppb, and Mg 1. The total content of the 20 metals is 28.63 ppb, with Al at 2.24 ppb, K at 1.81 ppb, Ca at 2.10 ppb, Ti at 0.89 ppb, V at 0.63 ppb, Cr at 0.80 ppb, Mn at 0.94 ppb, Fe at 1.55 ppb, Co at 0.71 ppb, Ni at 1.02 ppb, Cu at 1.28 ppb, Zn at 1.35 ppb, Zr at 0.93 ppb, As at 2.01 ppb, Cd at 0.50 ppb, Ba at 1.46 ppb, and Pb at 3.12 ppb. Based on the crude phosphorus oxychloride product, the yield of electronic-grade phosphorus oxychloride in a single pass is 87.98%.
[0022] Example 3: Preparation of electronic-grade phosphorus oxychloride for integrated circuits (1) Add 3500g of high-purity phosphorus trichloride to a quartz distillation column and carry out atmospheric pressure pre-distillation under nitrogen protection. The actual number of trays in the distillation column is 20, the bottom temperature is 80℃, the top temperature is 75.5℃, and the total reflux is carried out for 1 hour. 52.5g of the first fraction is discarded, and the fraction with the top temperature of 75.5℃ is collected to obtain 3361g of refined phosphorus trichloride. The remaining material is used as bottom residue and liquid holdup in the column and does not enter the subsequent oxidation reaction. (2) All the obtained purified phosphorus trichloride was fed into a PFA-lined microchannel reactor at a flow rate of 320 ml / h, while an oxygen / ozone mixture was introduced. The oxygen purity was 99.999%, the oxygen dew point was -70℃, the ozone volume fraction was 0.2% of the total volume of the oxygen / ozone mixture, the oxygen molar flow rate was 1.91 mol / h, the reaction temperature was 65℃, the reaction gauge pressure was 0.25 MPa, and the average residence time of the material was 90 s. The reaction product was condensed and collected in a PFA receiver at 5℃ to obtain 3684 g of crude phosphorus oxychloride. (3) All the obtained crude phosphorus oxychloride was fed into a PFA hollow fiber membrane degasser and degassed for 25 min at 30°C, liquid side gauge pressure of 0.05 MPa and membrane outside absolute pressure of 40 kPa. The membrane outside was purged with nitrogen at a flow rate of 0.5 L / min, and 3629 g of degassed phosphorus oxychloride was obtained. (4) All the degassed phosphorus oxychloride obtained was transferred into a PFA circulating tank purged with dry nitrogen, and the temperature was controlled at 25°C. Two-stage PFA fixed-bed impurity traps were set up in series. The first stage was the main impurity trap (inner diameter 30 mm, effective filling height 400 mm), and the second stage was the protective impurity trap (inner diameter 30 mm, effective filling height 180 mm). Both stages of the fixed bed were filled with anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1. The total filling amount of the composite impurity trapping material was 442 g, the filling mass of the first-stage main impurity trapping column was 287 g, and the filling mass of the second-stage protective impurity trapping column was 155 g. The degassed phosphorus oxychloride was circulated through the first-stage main impurity trapping column and the second-stage protective impurity trapping column in sequence by a PFA diaphragm pump. The circulation flow rate was 1 L / h, the fixed bed gauge pressure was 0.1 MPa, and the circulation treatment was carried out for 3 h to obtain 3601 g of phosphorus oxychloride after impurity trapping treatment. (5) All the obtained phosphorus oxychloride after impurity removal treatment was transferred into a quartz distillation column with 20 actual plates and an absolute pressure of 50 kPa at the top. The column was first refluxed for 3 hours, and then the fraction was cut at a reflux ratio of 10:1. 108 g of the first fraction was discarded, and 3349 g of the middle fraction was collected. 144 g of the residue in the bottom of the column was not included in the product. During the distillation process, the temperature at the top of the column was controlled at 85°C and the temperature in the bottom of the column was controlled at 92°C. The bottom of the column must not be dried. The obtained middle fraction was filtered through a 0.03 μm PFA membrane filter and filled into PFA containers that had been dried at 120°C and purged with nitrogen in a local Class 100 clean environment. The relative humidity of the filling environment was 1%. After filling, the container was kept under a slight positive pressure of nitrogen to obtain electronic grade phosphorus oxychloride for integrated circuits.
[0023] The obtained electronic-grade phosphorus oxychloride contained 99.99999% phosphorus oxychloride, as determined by gas chromatography area normalization; moisture content was 32.6 ppb; free acid (calculated as HCl) was 9.8 ppb; residual phosphorus trichloride was 0.4 ppb; and TOC was 4.5 ppb. The contents of various metal impurities were as follows: Li 0.92 ppb, Na 2.18 ppb, Mg 1.40 ppb, Al 1.98 ppb, K 1.55 ppb, and Ca 1.82 ppb. The concentrations of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Cd, Ba, and Pb were 0.70 ppb, 0.48 ppb, 0.62 ppb, 0.76 ppb, 0.55 ppb, 0.82 ppb, 1.05 ppb, 1.10 ppb, 0.72 ppb, 1.68 ppb, 0.38 ppb, 1.20 ppb, and 2.58 ppb, respectively; the total concentration of the 20 metals was 23.71 ppb. Based on the crude phosphorus oxychloride product, the first-pass yield of electronic-grade phosphorus oxychloride was 90.91%.
[0024] Example 4: Preparation of electronic-grade phosphorus oxychloride for integrated circuits (1) Add 3500g of high-purity phosphorus trichloride to a quartz distillation column and carry out atmospheric pressure pre-distillation under nitrogen protection. The actual number of trays in the distillation column is 20, the bottom temperature is 85℃, the top temperature is 76.5℃, and the total reflux is carried out for 1.5h. 70g of the first fraction is discarded, and the fraction with the top temperature of 76.5℃ is collected to obtain 3390g of refined phosphorus trichloride. The remaining material is used as bottom residue and liquid holdup in the column and does not enter the subsequent oxidation reaction. (2) All the obtained purified phosphorus trichloride was fed into a PFA-lined microchannel reactor at a flow rate of 380 ml / h, while an oxygen / ozone mixture was introduced. The oxygen purity was 99.999%, the oxygen dew point was -70℃, the ozone volume fraction was 0.3% of the total volume of the oxygen / ozone mixture, the oxygen molar flow rate was 2.40 mol / h, the reaction temperature was 70℃, the reaction gauge pressure was 0.3 MPa, and the average residence time of the material was 60 s. The reaction product was condensed and collected in a PFA receiver at 10℃ to obtain 3782 g of crude phosphorus oxychloride. (3) All the obtained crude phosphorus oxychloride was fed into a PFA hollow fiber membrane degasser and degassed for 20 min at 35°C, liquid side gauge pressure of 0.06 MPa and membrane outside absolute pressure of 50 kPa. The membrane outside was purged with nitrogen at a flow rate of 1 L / min to obtain 3751 g of degassed phosphorus oxychloride. (4) All the degassed phosphorus oxychloride obtained was transferred into a PFA circulating tank purged with dry nitrogen, and the temperature was controlled at 30°C. Two-stage PFA fixed-bed impurity traps were set up in series. The first stage was the main impurity trap (inner diameter 30 mm, effective filling height 400 mm), and the second stage was the protective impurity trap (inner diameter 30 mm, effective filling height 180 mm). Both stages of the fixed bed were filled with anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1. The total filling amount of the composite impurity trapping material was 567 g, the filling mass of the first-stage main impurity trapping column was 396.9 g, and the filling mass of the second-stage protective impurity trapping column was 170.1 g. The degassed phosphorus oxychloride was circulated through the first-stage main impurity trapping column and the second-stage protective impurity trapping column by a PFA diaphragm pump. The circulation flow rate was 1.5 L / h, the fixed bed gauge pressure was 0.15 MPa, and the circulation treatment was carried out for 2 h to obtain 3735 g of impurity-treated phosphorus oxychloride. (5) All the obtained phosphorus oxychloride after impurity removal treatment was transferred into a quartz distillation column with 20 actual plates and an absolute pressure of 60 kPa at the top. The column was first refluxed for 2 hours, and then the fraction was cut at a reflux ratio of 12:1. 149 g of the first fraction was discarded, and 3399 g of the middle fraction was collected. 187 g of the residue in the bottom of the column was not included in the product. During the distillation process, the temperature at the top of the column was controlled at 90°C and the temperature in the bottom of the column was controlled at 97°C. The bottom of the column must not be dried. The obtained middle fraction was filtered through a 0.03 μm PFA membrane filter and filled into PFA containers that had been dried at 120°C and purged with nitrogen in a local Class 100 clean environment. The relative humidity of the filling environment was 1%. After filling, the container was kept under a slight positive pressure of nitrogen to obtain electronic grade phosphorus oxychloride for integrated circuits.
[0025] The obtained electronic-grade phosphorus oxychloride contained 99.99999% phosphorus oxychloride, as determined by gas chromatography area normalization; moisture content was 40.2 ppb; free acid (calculated as HCl) was 12.7 ppb; residual phosphorus trichloride was 0.8 ppb; and TOC was 6.8 ppb. The contents of various metal impurities were as follows: Li 1.38 ppb, Na 3.05 ppb, Mg 1.92 ppb, Al 2.82 ppb, K 2.27 ppb, and Ca 2.65 ppb. The content of phosphorus oxychloride (Pb) was as follows: Ti 1.12 ppb, V 0.86 ppb, Cr 1.05 ppb, Mn 1.18 ppb, Fe 1.94 ppb, Co 0.95 ppb, Ni 1.36 ppb, Cu 1.62 ppb, Zn 1.74 ppb, Zr 1.20 ppb, As 2.48 ppb, Cd 0.72 ppb, Ba 1.88 ppb, and Pb 3.64 ppb; the total content of the 20 metals was 35.83 ppb. Based on the mass of crude phosphorus oxychloride, the yield of electronic-grade phosphorus oxychloride in a single pass was 89.87%.
[0026] Comparative Example 1 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of phosphoric acid-ammonium dihydrogen phosphate / PFA composite filler. The preparation method of the phosphoric acid-ammonium dihydrogen phosphate / PFA composite filler is as follows: Under nitrogen protection, 100g of 87wt% phosphoric acid and 90g of ammonium dihydrogen phosphate were mixed and stirred at 300rpm for 20min. Then, 300g of electronic-grade PFA micro powder was added and stirred at 300rpm for 30min. The mixture was then poured into a mold with a PFA film lining the inner wall and pressed at 5MPa for 5min at room temperature. The temperature was then raised to 280℃ and hot-pressed at 5MPa for 20min. After hot pressing, the pressure was maintained and the mixture was allowed to cool naturally to 70℃. The mold was then demolded and pre-cooled with liquid nitrogen for 15min under dry nitrogen protection. Finally, the mixture was crushed at 200rpm for 5min using a PFA lining crusher. After sieving, phosphoric acid-ammonium dihydrogen phosphate / PFA composite filler with a particle size of 0.8-2mm was obtained.
[0027] The electronic-grade phosphorus oxychloride obtained in Comparative Example 1 contained 99.99994% phosphorus oxychloride; 210.5 ppb of moisture; 120.2 ppb of free acid (calculated as HCl); 44.8 ppb of residual phosphorus trichloride; 69.5 ppb of TOC; and a total of 68.40 ppb of 20 metallic impurities.
[0028] Comparative Example 1 uses ordinary phosphate / PFA composite filler, which lacks a stable pyrophosphate framework and has insufficient coordination and fixation ability for trace metal impurities. At the same time, the phosphate component has strong hygroscopicity and mobility, which easily introduces moisture and acidic impurities, promotes the local hydrolysis of phosphorus oxychloride, and increases the levels of free acid, phosphorus trichloride residues and metal impurities.
[0029] Comparative Example 2 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared by the following method. The preparation method of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is basically the same as that in Example 1. The difference is that the step S1 "heat to 750°C at a heating rate of 1.5°C / min and hold for 3 hours" is replaced with "heat to 300°C at a heating rate of 1.5°C / min and hold for 3 hours". The electronic-grade phosphorus oxychloride obtained in Comparative Example 2 contained 99.99991% phosphorus oxychloride; 360.4 ppb of moisture; 180.2 ppb of free acid (calculated as HCl); 55.1 ppb of residual phosphorus trichloride; 99.3 ppb of TOC; and a total of 49.86 ppb of 20 metallic impurities.
[0030] In Comparative Example 2, the calcination temperature was reduced from 750℃ to 300℃. The dehydration condensation and crystal phase transformation of the inorganic precursor were insufficient, making it difficult to form a stable anhydrous zirconium pyrophosphate-titanium phosphate framework, which reduced the coordination and fixation ability of metal impurities. At the same time, there were more residual hydroxyl groups and adsorbed water in the material, which easily caused trace hydrolysis of phosphorus oxychloride, resulting in an increase in the content of water, free acid and metal impurities.
[0031] Comparative Example 3 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared by the following method. The preparation method of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is basically the same as that in Example 1, except that the amount of tetraisopropyl titanate in step S1 is replaced with 70g.
[0032] The electronic-grade phosphorus oxychloride obtained in Comparative Example 3 contained 99.99996% phosphorus oxychloride; 80.2 ppb of moisture; 31.8 ppb of free acid (calculated as HCl); 15.9 ppb of residual phosphorus trichloride; 45.1 ppb of TOC; and a total of 40.96 ppb of 20 metallic impurities.
[0033] In Comparative Example 3, after reducing the amount of tetraisopropyl titanate, the content of titanium phosphate phase in the material was insufficient, which weakened the adsorption and coordination fixation ability of transition metal impurities such as Fe, Cu, Ni, and Cr, thus weakening the effect of controlling metal impurities.
[0034] Comparative Example 4 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared by the following method. The preparation method of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is basically the same as that in Example 1, except that the amount of tetraisopropyl titanate in step S1 is replaced with 280g.
[0035] The electronic-grade phosphorus oxychloride obtained in Comparative Example 4 contained 99.99995% phosphorus oxychloride; 88.4 ppb of moisture; 38.2 ppb of free acid (calculated as HCl); 18.1 ppb of residual phosphorus trichloride; 47.3 ppb of TOC; and a total of 46.82 ppb of 20 metallic impurities.
[0036] In Comparative Example 4, increasing the amount of tetraisopropyl titanate resulted in an excessively high proportion of titanium phosphate phase and a relatively insufficient proportion of zirconium-based pyrophosphate phase. This reduced the ability to fix impurities such as Na, K, Ca, Mg, and Al. At the same time, excessive titanium phase may reduce the utilization rate of effective sites, leading to a poorer impurity capture effect.
[0037] Comparative Example 5 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared by the following method. The preparation method of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is basically the same as that in Example 1. The difference is that the amount of anhydrous zirconium pyrophosphate-titanium phosphate composite powder in step S2 is replaced with 550g, and the amount of electronic grade PFA micro powder is replaced with 450g.
[0038] The electronic-grade phosphorus oxychloride obtained in Comparative Example 5 contained 99.99997% phosphorus oxychloride; 72.3 ppb of moisture; 25.8 ppb of free acid (calculated as HCl); 12.1 ppb of residual phosphorus trichloride; 41.8 ppb of TOC; and a total of 45.79 ppb of 20 metallic impurities.
[0039] In Comparative Example 5, after reducing the amount of electronic-grade PFA micro powder, the PFA provided insufficient support for the immobilization of inorganic impurity-collecting powders. During the fixed-bed circulation process, fine powder was easily detached and particles migrated, increasing the risk of Zr and Ti leaching. Therefore, the metal impurity-collecting effect was weakened.
[0040] Comparative Example 6 The preparation method of electronic-grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3, except that the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is replaced with an equal weight of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared by the following method. The preparation method of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is basically the same as that in Example 1. The difference is that the amount of anhydrous zirconium pyrophosphate-titanium phosphate composite powder in step S2 is replaced with 200g, and the amount of electronic grade PFA micro powder is replaced with 800g.
[0041] The electronic-grade phosphorus oxychloride obtained in Comparative Example 6 contained 99.99995% phosphorus oxychloride; 65.4 ppb of moisture; 24.1 ppb of free acid (calculated as HCl); 20.2 ppb of residual phosphorus trichloride; 84.3 ppb of TOC; and a total of 41.82 ppb of 20 metallic impurities.
[0042] In Comparative Example 6, although increasing the amount of electronic-grade PFA micro powder reduced the risk of particle detachment, excessive PFA would coat some of the pyrophosphate and phosphate trapping sites, making it difficult for metal impurities to fully contact the effective sites, resulting in a decrease in the trapping effect. At the same time, an excessively high PFA ratio reduced the content of the effective inorganic trapping phase in the bed, and the TOC control effect deteriorated.
[0043] Comparative Example 7 The preparation method of electronic grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3. The difference is that in step (4), no second-stage protective impurity trapping column is set, only a first-stage PFA fixed bed impurity trapping column is set, and 442g of anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in Example 1 is loaded into the fixed bed at one time.
[0044] The electronic-grade phosphorus oxychloride obtained in Comparative Example 7 contained 99.99995% phosphorus oxychloride; 95.3 ppb of moisture; 44.9 ppb of free acid (calculated as HCl); 22.7 ppb of residual phosphorus trichloride; 57.4 ppb of TOC; and a total of 52.63 ppb of 20 metallic impurities.
[0045] Comparative Example 7 uses only a single-stage fixed bed for impurity capture. Although the total amount of impurity capture material is the same, it lacks a secondary interception of penetrating impurities by the protective impurity capture column. When the main impurity capture column is close to saturation in some areas, metallic impurities are more likely to enter the subsequent rectification section, resulting in a decrease in the metal control effect.
[0046] Comparative Example 8 The preparation method of electronic grade phosphorus oxychloride for integrated circuits is basically the same as that in Example 3. The difference is that the PFA hollow fiber membrane degassing treatment in step (3) is not performed. Instead, the crude phosphorus oxychloride obtained in step (2) is directly transferred to the PFA circulating tank in step (4) for two-stage fixed bed impurity removal treatment to obtain 3650g of phosphorus oxychloride after impurity removal treatment.
[0047] The electronic-grade phosphorus oxychloride obtained in Comparative Example 8 contained 99.99988% phosphorus oxychloride; 248.7 ppb of moisture; 150.4 ppb of free acid (calculated as HCl); 87.5 ppb of residual phosphorus trichloride; 79.0 ppb of TOC; and a total of 39.85 ppb of 20 metallic impurities.
[0048] Comparative Example 8 did not undergo PFA hollow fiber membrane degassing treatment. Dissolved oxygen, ozone, hydrogen chloride, and unreacted phosphorus trichloride in the crude phosphorus oxychloride could not be removed in time. After entering the fixed bed, it would increase the consumption of impurity-collecting materials and promote the slight hydrolysis of phosphorus oxychloride, thus increasing the free acid and moisture content.
[0049] The anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material prepared in this application was loaded into the first-stage main impurity trapping column and the second-stage protective impurity trapping column before use. High-purity nitrogen gas (nitrogen flow rate of 200 mL / min) was introduced and activated at atmospheric pressure and 200℃ for 6 h. After cooling, it was pre-distilled with phosphorus oxychloride at a rate of 0.5 h. -1 One bed volume of liquid volume hourly space velocity (LHSV) was used for pre-rinsing. The pre-rinsing solution was discarded, and after pre-rinsing, all free pre-rinsing solution in the bed was drained. The bed was then purged with nitrogen until no continuous droplets remained at the outlet of the impurity trap column. The pre-distilled phosphorus oxychloride was prepared by the following method: 1500g of high-purity phosphorus oxychloride was added to a quartz distillation column under nitrogen protection. The absolute pressure at the bottom of the column was controlled at 50kPa, and total reflux was applied for 1 hour. 30g of the forerunner was discarded, and 1400g of the intermediate distillate was collected. The obtained intermediate distillate was filtered through a 0.03μm PFA membrane filter and stored in a PFA container that had been dried at 120℃ for 1 hour and purged with nitrogen for use as pre-distilled phosphorus oxychloride.
[0050] In this application, during the two-stage PFA fixed-bed impurity collection and circulation process, the content of metal impurities in phosphorus oxychloride at the outlets of the first-stage main impurity collection column and the second-stage protective impurity collection column is measured every 1 hour. The first-stage main impurity collection column is replaced when the total amount of metal impurities at the outlet exceeds 40 ppb or any single metal impurity exceeds 5 ppb; the second-stage protective impurity collection column is replaced when the total amount of metal impurities at the outlet of the first-stage main impurity collection column is ≤40 ppb and any single metal impurity is ≤5 ppb, while the total amount of metal impurities at the outlet of the second-stage protective impurity collection column exceeds 40 ppb or any single metal impurity exceeds 5 ppb.
[0051] The high-purity phosphorus trichloride used in the embodiments and comparative examples of this application has a purity of 99.99% and a moisture content of 20 ppm. The microchannel reactor is model PL-WT06, with a custom-made PFA lining, manufactured by KINTEK. The hollow fiber membrane degasser is model TYSEI TY-77100, manufactured by Taisei Corporation. The fixed bed is model KMCFRF-L1GM, with a custom-made PFA material, manufactured by Anhui Kemi Instrument Co., Ltd. The PFA circulation tank is model RNKJ003000, manufactured by Nanjing Ruinike Technology Development Co., Ltd. The quartz distillation column is an electronic-grade quartz distillation column, model RFJL-S5L, with a volume of 5L and 20 trays, manufactured by Xuchang Ruitaifeng Technology Co., Ltd.
[0052] Electronic-grade PFA micro powder was prepared by the following method: 1000g of Teflon™ PFA 950HP Plus resin particles were placed in a PFA cleaning basket in a local Class 100 clean environment and rinsed sequentially with ultrapure water (3×1L), electronic-grade isopropanol (2×1L), and ultrapure water (2×1L). The particles were then placed in a nitrogen-purified vacuum drying oven and vacuum dried at 100℃ for 12h. The particles were then transferred to a nitrogen-purified cryogenic pulverizing system, pre-cooled with liquid nitrogen for 30min, and then cryogenically pulverized under nitrogen protection. The parts in contact with the material in the pulverizing equipment were lined with PFA. The pulverizing speed was controlled at 8000rpm and the feeding speed at 30g / min. The resulting powder was sieved through a PFA sieve under nitrogen protection, and the particles with a particle size of 20-80μm were collected. The powder was then vacuum dried at 100℃ for 8h and cooled to obtain electronic-grade PFA micro powder.
[0053] Unless otherwise stated, the nitrogen gas used in this application has a purity of 99.999% and a dew point of -70°C.
[0054] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. However, any modifications, alterations, and variations made by those skilled in the art without departing from the scope of the present invention based on the disclosed technical content are equivalent embodiments of the present invention. Furthermore, any modifications, alterations, and variations made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the present invention.
Claims
1. A process for the production of electronic grade phosphorus oxychloride for integrated circuits, characterized in that, Includes the following steps: (1) High-purity phosphorus trichloride is pre-distilled to obtain refined phosphorus trichloride; (2) The refined phosphorus trichloride is fed into the PFA-lined microchannel reactor and oxygen / ozone mixture is introduced at the same time to carry out anhydrous oxidation reaction. The reaction product is collected by condensation of PFA receiver to obtain crude phosphorus oxychloride. (3) The crude phosphorus oxychloride was fed into a PFA hollow fiber membrane degasser for degassing to obtain degassed phosphorus oxychloride. (4) Transfer the degassed phosphorus oxychloride into the PFA circulating tank, and let the degassed phosphorus oxychloride circulate through the two-stage series-connected PFA fixed bed impurity collection column to obtain phosphorus oxychloride after impurity collection treatment. (5) The phosphorus oxychloride after impurity removal treatment is distilled, the middle fraction is collected, filtered and bottled to obtain electronic grade phosphorus oxychloride for integrated circuits; The two-stage series-connected PFA fixed-bed impurity trapping column includes a first-stage main impurity trapping column and a second-stage protective impurity trapping column. Both stages of the PFA fixed-bed impurity trapping column are filled with anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material.
2. A process for the production of electronic grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, In step (1), the parameters of the pre-distillation are as follows: the pre-distillation is carried out under normal pressure, the bottom temperature of the column is 76-85℃, the top temperature of the column is 74.5-76.5℃, the total reflux is 0.5-1.5h, 1-3wt% of the fore-distillate is discarded, and the fraction with the top temperature of 74.5-76.5℃ is collected.
3. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, In step (2), the volumetric flow rate during the transport of refined phosphorus trichloride is 250-380 ml / h; the molar flow rate of oxygen is 0.5-0.55 times that of refined phosphorus trichloride; and the volume fraction of ozone is 0.1-0.3% of the total volume of the oxygen / ozone mixture.
4. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, In step (2), the reaction temperature of the anhydrous oxidation reaction is 60-70℃, the time is 60-120s, and the reaction gauge pressure is 0.2-0.3MPa.
5. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, In step (3), the degassing treatment temperature is 25-35℃, the liquid side gauge pressure is 0.04-0.06MPa, the absolute pressure outside the membrane is 30-50kPa, and the time is 20-30min.
6. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, The anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity catching material is prepared by the following method: S1: Ultrapure water and zirconium oxychloride octahydrate were stirred and mixed, phosphoric acid was added, and then tetraisopropyl titanate was added. The mixture was heated to reflux and then subjected to hydrothermal reaction. The mixture was then placed in a tube furnace for dehydration pyrophosphorylation treatment to obtain anhydrous zirconium pyrophosphate-titanium phosphate composite powder. S2: Anhydrous zirconium pyrophosphate-titanium phosphate composite powder is mixed with electronic-grade PFA micro powder, and then subjected to pre-pressing, hot pressing, cooling, demolding, crushing and sieving to obtain anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity-catching material.
7. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 6, characterized in that, In step S1, the mass ratio of zirconium oxychloride octahydrate, phosphoric acid, and tetraisopropyl titanate is 1.6:1.5:0.
7.
8. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 6, characterized in that, In step S2, the mass ratio of the anhydrous zirconium pyrophosphate-titanium phosphate composite powder to electronic-grade PFA micro powder is 7:
13.
9. The method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, The total loading of the anhydrous zirconium pyrophosphate-titanium phosphate / PFA composite impurity trapping material is 8-15 wt% of the crude phosphorus oxychloride mass, wherein the loading mass of the first-stage main impurity trapping column is 60%-70% of the total loading mass, and the loading mass of the second-stage protective impurity trapping column is 30%-40% of the total loading mass.
10. A method for preparing electronic-grade phosphorus oxychloride for integrated circuits according to claim 1, characterized in that, In step (5), the distillation parameters are as follows: the absolute pressure at the top of the column is 40-60 kPa, the total reflux is carried out for 2-4 hours, and then the fraction is cut at a reflux ratio of (8-12):
1. The temperature at the top of the column is 80-90℃, and the temperature at the bottom of the column is 87-97℃.