A pitch-based porous carbon with annular pore edges and its preparation method
By employing specific oxidative crosslinking, thermal migration, confined volatilization, and activation treatment steps, the problem of forming annular pore edges in open pore cavities, which is difficult to achieve in existing technologies, is solved, and pitch-based porous carbon with a continuous carbon framework and secondary pores is prepared, which is suitable for pollutant adsorption.
Patent Information
- Application Number
- CN202611548317.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
In existing processes for preparing pitch-based porous carbon, it is difficult to utilize the redistribution of migratable volatile components in the initial crosslinked framework and the confined volatilization process to form and stably retain open cavities with annular pore edges.
The initial cross-linked framework is formed by the first oxidative cross-linking and the migratable volatile components are retained. The migratable volatile components are redistributed by thermal migration treatment under an inert atmosphere. The spatial distribution is fixed by the second oxidative cross-linking and the primary pores are formed by the confined volatilization treatment. Subsequently, carbonization and activation treatments are used to form open pores with annular pore edges.
This method achieves stable retention of the annular pore edges of open cavities in pitch-based porous carbon, forming a continuous carbon framework and secondary pore structure. This provides mass transfer channels and adsorption sites for pollutant adsorption, thereby improving the performance of the adsorption material.
Smart Images

Figure CN123105635A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon material preparation technology, specifically to a pitch-based porous carbon with annular pore edges and its preparation method. Background Technology
[0002] Asphalt, with its high carbon content and abundant aromatic structure, can serve as a carbon source for porous carbon materials. Existing asphalt-based porous carbon is typically prepared through oxidative crosslinking, carbonization, and activation. Oxidative crosslinking enhances the structural stability of the asphalt precursor during subsequent heat treatment, carbonization forms a continuous carbon framework, and activation further develops the pore structure. The resulting asphalt-based porous carbon can then be used as an adsorbent for pollutant adsorption.
[0003] However, the oxidative crosslinking in the existing asphalt-based porous carbon preparation process usually aims to improve the overall crosslinking degree of asphalt, so that the migratable volatile components are sufficiently fixed before subsequent carbonization. The subsequent pore structure mainly depends on the activation treatment to form. Therefore, it is difficult to utilize the redistribution of migratable volatile components in the initial crosslinking skeleton and the subsequent restricted volatilization process to form and stably retain open pores with annular pore edges. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a pitch-based porous carbon with annular pore edges and its preparation method, solving the problem that it is difficult to utilize the redistribution of migratable volatile components in the initial crosslinked framework and the restricted volatilization process to form and stably retain open cavities with annular pore edges in the existing pitch-based porous carbon preparation process.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A method for preparing pitch-based porous carbon with annular pore edges, comprising:
[0007] The asphalt raw material is subjected to a first oxidative crosslinking to obtain a first crosslinking precursor, which includes an initial crosslinking backbone and a migratable volatile component distributed in the initial crosslinking backbone.
[0008] The first crosslinking precursor is subjected to thermal migration treatment under an inert atmosphere to redistribute the migratable volatile components in the initial crosslinking backbone, thereby obtaining a thermally migratable precursor.
[0009] The thermally migrating precursor is subjected to a second oxidative crosslinking to fix the spatial distribution of the redistributed migratable volatile components, thereby obtaining a crosslinked precursor.
[0010] The crosslinking precursor is subjected to restricted volatilization treatment under an inert atmosphere, so that the migratable volatile components are thermally decomposed and discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0011] The cavity-forming precursor is subjected to carbonization treatment to obtain carbonized material.
[0012] The carbonized material is activated to obtain the pitch-based porous carbon with annular pore edges.
[0013] Preferably, the asphalt raw material is petroleum asphalt or coal tar pitch.
[0014] Preferably, the temperature of the first oxidative crosslinking is 200-280°C, the time is 20-120 min, and the heating rate is 0.5-3°C / min.
[0015] Preferably, the first oxidative crosslinking is carried out in an air atmosphere, the mass of the asphalt raw material in a single treatment is 5-10g, and the air flow rate of the first oxidative crosslinking is 300-2200mL / min.
[0016] Preferably, the thermal migration treatment uses nitrogen or argon as the inert atmosphere, and the temperature of the thermal migration treatment is 220-310°C, and the time is 15-90 min.
[0017] Preferably, the second oxidative crosslinking uses air or a mixture of oxygen and nitrogen.
[0018] Preferably, when the second oxidative crosslinking uses a mixture of oxygen and nitrogen, the oxygen volume content is 5% to 21%.
[0019] Preferably, the temperature of the second oxidative crosslinking is 250–340°C, the time is 20–120 min, and the heating rate is 0.5–3°C / min.
[0020] Preferably, the restricted volatilization treatment includes heating the crosslinking precursor to 320–550°C at a heating rate of 0.3–2.5°C / min under the inert atmosphere, and holding it at 380–480°C for 20–120 min.
[0021] Preferably, the carbonization process includes heating the cavity-forming precursor to 750–1000°C in the inert atmosphere at a heating rate of 2–8°C / min, and holding it at that temperature for 60–180 min.
[0022] Preferably, the activation treatment uses potassium hydroxide as the activator, the mass ratio of the carbonized material to the potassium hydroxide is 1:1 to 1:3, the activation temperature is 700 to 850°C, and the activation time is 30 to 120 min.
[0023] The present invention also provides a pitch-based porous carbon, the pitch-based porous carbon comprising a continuous carbon skeleton, wherein a plurality of open cavities are formed in the continuous carbon skeleton opening to the surface of the continuous carbon skeleton, at least a portion of the cavities having annular pore edges around their openings, and secondary pores being formed on the pore walls of the cavities, the diameter of the secondary pores being smaller than the equivalent diameter of the pore openings of the cavities.
[0024] Preferably, the asphalt-based porous carbon is prepared by sequentially subjecting asphalt raw materials to a first oxidative crosslinking, thermal migration treatment, a second oxidative crosslinking, restricted volatilization treatment, carbonization treatment, and activation treatment.
[0025] Preferably, the annular rim extends circumferentially along the opening of the corresponding cavity, and at least some adjacent cavities are interconnected.
[0026] The present invention also provides an adsorbent material comprising the pitch-based porous carbon.
[0027] The present invention also provides the application of the adsorbent material in the adsorption of pollutants.
[0028] This invention provides a pitch-based porous carbon with annular pore edges and a method for its preparation. It has the following beneficial effects:
[0029] 1. This invention forms an initial cross-linked framework from asphalt raw materials through a first oxidative cross-linking process while retaining migratable volatile components. Thermal migration treatment under an inert atmosphere redistributes these migratable volatile components within the initial cross-linked framework. A second oxidative cross-linking process fixes the spatial distribution of the redistributed migratable volatile components. A restricted volatilization treatment causes the migratable volatile components to be thermally decomposed and discharged, thereby forming primary pores. This enables the formation and stable retention of annular pore edges in the subsequently obtained asphalt-based porous carbon, solving the problem of difficulty in forming and stably retaining open pores with annular pore edges in existing preparation processes.
[0030] 2. The present invention first forms primary pores through restricted volatilization treatment, then obtains carbonized material with open pores through carbonization treatment, and further forms secondary pores on the pore walls of the open pores through activation treatment, so that the obtained pitch-based porous carbon forms a pore structure of different scales composed of open pores and secondary pores, avoiding the need to rely solely on activation treatment to form pores.
[0031] 3. The asphalt-based porous carbon obtained by the present invention includes a continuous carbon skeleton and a plurality of open cavities formed in the continuous carbon skeleton. At least some of the adjacent open cavities are interconnected, which can provide a mass transfer channel for pollutants to enter the interior of the continuous carbon skeleton. At the same time, secondary pores are formed on the pore walls of the open cavities, which can further provide adsorption sites, thus making it suitable for pollutant adsorption.
[0032] 4. The present invention includes a first oxidative crosslinking, thermal migration treatment, a second oxidative crosslinking, a restricted volatilization treatment, a carbonization treatment, and an activation treatment, so that the initial crosslinking framework formation, the redistribution of migratable and volatile components, the fixation of spatial distribution, the formation of primary pores, and the formation of secondary pores are completed in different treatment stages. The pore structure of the obtained asphalt-based porous carbon can be adjusted by the temperature, time, and heating rate of each stage. Attached Figure Description
[0033] Figure 1 This is a scanning electron microscope image of a pitch-based porous carbon sample at 10,000x magnification.
[0034] Figure 2 This is a scanning electron microscope image of a pitch-based porous carbon sample at 50,000x magnification.
[0035] Figure 3 This is a scanning electron microscope image of a pitch-based porous carbon sample at 100,000x magnification.
[0036] Figure 4 This is a scanning electron microscope image of a pitch-based porous carbon sample at 10,000x magnification in another observation area.
[0037] Figure 5 This is a scanning electron microscope image of a pitch-based porous carbon sample at 50,000x magnification in another observation area.
[0038] Figure 6 This is a scanning electron microscope image of a pitch-based porous carbon sample at 100,000x magnification in another observation area. Detailed Implementation
[0039] The present application will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the embodiments are only for illustrating the present application and are not intended to limit the scope of protection of the present application.
[0040] Asphalt has a high carbon content and can form asphalt-based porous carbon after oxidative crosslinking, carbonization, and activation treatment. Current preparation processes typically involve increasing the degree of oxidative crosslinking of the asphalt raw material to maintain structural stability during subsequent heating, followed by carbonization to form a carbon skeleton, and primarily relying on activation treatment to develop the pore structure. However, when oxidative crosslinking mainly aims to increase the overall degree of crosslinking, the migratable and volatile components in the asphalt raw material are easily and sufficiently fixed before subsequent carbonization. The migration and volatilization processes of these migratable and volatile components themselves are difficult to utilize to form a pore structure with a specific pore morphology.
[0041] During the observation of the microstructure of pitch-based porous carbon, the applicant discovered that, for example... Figures 1-6 As shown, multiple open cavities can be formed in the continuous carbon skeleton of asphalt-based porous carbon, opening to the surface of the continuous carbon skeleton. Some of the open cavities have relatively obvious annular pore edges around their openings, and small pore structures can also be observed on the pore walls of the open cavities. Based on the above morphological characteristics, the applicant further studied the structural evolution of asphalt raw materials during crosslinking, temperature-induced volatilization, and activation processes. It was found that if a certain initial crosslinked skeleton is formed while retaining the migratable volatilizable components, and if the migratable volatilizable components are redistributed and fixed before subsequent volatilization, then the restricted volatilization of the migratable volatilizable components can be used to form primary cavities, and further open cavities with annular pore edges can be obtained.
[0042] Based on the above findings, this application first performs a first oxidative crosslinking on the asphalt raw material to form a first crosslinking precursor. The first crosslinking precursor includes an initial crosslinking framework and migratable volatile components distributed within the initial crosslinking framework. The first oxidative crosslinking does not fully crosslink all components in the asphalt raw material, but rather retains migratable volatile components that can migrate and volatilize during subsequent heating while forming the initial crosslinking framework.
[0043] Subsequently, the first crosslinking precursor is subjected to thermal migration treatment under an inert atmosphere, which redistributes the migratable volatile components within the initial crosslinking backbone, resulting in a thermally migratable precursor. Because the thermal migration treatment is performed under an inert atmosphere, while redistributing the migratable volatile components, it reduces the extent to which oxidative crosslinking occurs further in this stage, preventing premature fixation of the migratable volatile components.
[0044] The thermally migrated precursor is further subjected to a second oxidative crosslinking process to fix the spatial distribution of the redistributed migratory volatile components, resulting in a crosslinked precursor. Thus, the first oxidative crosslinking is used to form the initial crosslinked framework, the thermal migration treatment is used to redistribute the migratory volatile components, and the second oxidative crosslinking is used to fix the spatial distribution of the redistributed migratory volatile components. The three treatment stages play different roles.
[0045] Then, the crosslinking precursor is subjected to restricted volatilization treatment under an inert atmosphere. The migratable volatile components decompose during heating and are expelled from the crosslinking precursor. Under the structural constraints of the initial crosslinking backbone and the structure formed by the second oxidative crosslinking, primary cavities are formed in the crosslinking precursor, resulting in a cavity-forming precursor. The cavity-forming precursor is then subjected to carbonization treatment to further fix the primary cavities and form a continuous carbon backbone, yielding a carbonized material.
[0046] Finally, the carbonized material undergoes an activation treatment. This activation treatment further develops the pore structure based on the existing primary pores, resulting in pitch-based porous carbon comprising a continuous carbon skeleton. Multiple open pores opening to the surface of the continuous carbon skeleton are formed within this skeleton. At least some of the open pores have annular pore edges around their openings, and secondary pores are formed on the pore walls of these open pores. The diameter of these secondary pores is smaller than the equivalent diameter of the openings of the open pores. This application thus integrates the initial crosslinking skeleton formation, the redistribution of migratable volatile components, the fixation of the spatial distribution of migratable volatile components, the formation of primary pores, and the formation of secondary pores into different processing stages to achieve the preparation of pitch-based porous carbon with annular pore edges.
[0047] Unless otherwise specified, the raw materials used in the following examples are all commercially available, as detailed below.
[0048] Petroleum asphalt, CAS No. 8052-42-4, used as asphalt raw material; coal tar pitch, CAS No. 65996-93-2, used as asphalt raw material; potassium hydroxide, CAS No. 1310-58-3, analytical grade, used as an activator; hydrochloric acid, CAS No. 7647-01-0, analytical grade, used for washing after activation treatment; nitrogen, CAS No. 7727-37-9, high-purity nitrogen, used as an inert atmosphere; argon, CAS No. 7440-37-1, high-purity argon, used as an inert atmosphere; oxygen, CAS No. 7782-44-7, used to prepare a mixture of oxygen and nitrogen; deionized water, CAS No. 7732-18-5, used for washing.
[0049] In the embodiments, ambient air or compressed air is used; when a mixture of oxygen and nitrogen is used, it is prepared according to the oxygen volume content described in the corresponding embodiments.
[0050] In the embodiment where the first oxidative crosslinking is performed using an air atmosphere, the mass of the asphalt raw material processed in a single step is 5–10 g, and the air flow rate for the first oxidative crosslinking is 300–2200 mL / min. The air flow rate refers to the volume of air introduced per unit time, expressed in mL / min.
[0051] Example 1
[0052] This embodiment provides a method for preparing pitch-based porous carbon with annular pore edges, as detailed below.
[0053] Petroleum asphalt was selected as the asphalt raw material. The asphalt raw material was crushed and screened to remove obvious impurities and set aside for later use.
[0054] The asphalt raw material undergoes its first oxidative crosslinking. The asphalt raw material is placed in a tube furnace and heated to 200°C at a rate of 0.5°C / min under air atmosphere. It is then held at 200°C for 20 min to induce oxidative crosslinking, yielding the first crosslinking precursor. The first crosslinking precursor comprises an initial crosslinking backbone and migratable volatile components distributed within the initial crosslinking backbone.
[0055] After the first oxidative crosslinking is completed, the air supply is stopped, and nitrogen is continuously introduced into the tube furnace as an inert atmosphere to perform thermal migration treatment on the first crosslinking precursor. The first crosslinking precursor is heated to 220°C under an inert atmosphere and held at 220°C for 15 minutes to allow the migratable volatile components to redistribute in the initial crosslinking backbone, thus obtaining the thermally migratable precursor.
[0056] After the thermal migration treatment, oxygen-containing gas is reintroduced to perform a second oxidative crosslinking on the thermal migration precursor. In this embodiment, a mixture of oxygen and nitrogen is used, with an oxygen volume content of 5%. The mixture is heated to 250°C at a heating rate of 0.5°C / min and held at 250°C for 20 min to fix the spatial distribution of the redistributed migratable volatile components, thus obtaining the crosslinked precursor.
[0057] After the second oxidative crosslinking is completed, the mixed gas flow is stopped, and nitrogen gas is introduced again to perform restricted volatilization treatment on the crosslinking precursor under an inert atmosphere. The restricted volatilization process is controlled starting from 320℃, and the temperature is continued to rise to 380℃ at a heating rate of 0.3℃ / min, and held at 380℃ for 20min. This allows the migratable volatile components to be thermally decomposed and discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0058] Subsequently, under an inert atmosphere, the cavity-forming precursor was carbonized by heating it to 750°C at a heating rate of 2°C / min, holding it at 750°C for 60 min, and then cooling it to obtain the carbonized material.
[0059] The carbon material was uniformly mixed with potassium hydroxide at a mass ratio of 1:1 to activate the carbon material. The temperature was raised to 700℃ under nitrogen protection and maintained at 700℃ for 30 minutes. After activation, the mixture was allowed to cool naturally. The resulting product was washed with hydrochloric acid solution, then with deionized water until the washing solution was neutral. It was then dried to obtain pitch-based porous carbon with annular pore edges.
[0060] The resulting pitch-based porous carbon with annular pore edges includes a continuous carbon skeleton, in which multiple open cavities are formed that open to the surface of the continuous carbon skeleton. At least some of the open cavities have annular pore edges around their openings, and secondary pores are formed on the pore walls of the open cavities. The diameter of the secondary pores is smaller than the equivalent diameter of the opening of the open cavities.
[0061] Example 2
[0062] This embodiment provides a method for preparing pitch-based porous carbon with annular pore edges, as detailed below.
[0063] Petroleum asphalt was selected as the asphalt raw material, and the asphalt raw material was crushed and screened.
[0064] The asphalt raw material was placed in a tube furnace and subjected to the first oxidative crosslinking in an air atmosphere. The temperature was increased to 280°C at a rate of 3°C / min and held at 280°C for 120 min to obtain the first crosslinking precursor. The first crosslinking precursor includes an initial crosslinking backbone and a migratable volatile component distributed in the initial crosslinking backbone.
[0065] After the first oxidative crosslinking is completed, the air supply is stopped, and argon gas is introduced as an inert atmosphere to perform thermal migration treatment on the first crosslinking precursor. The first crosslinking precursor is heated to 310°C and held at 310°C for 90 min to allow the migratable volatile components to redistribute in the initial crosslinking backbone, thus obtaining the thermally migratable precursor.
[0066] Air was then reintroduced to perform a second oxidative crosslinking of the thermally migrating precursor. The oxygen volume content of the air was 21%, and the temperature was increased to 340°C at a rate of 3°C / min. The temperature was then maintained at 340°C for 120 min to fix the spatial distribution of the redistributed migratable volatile components, thus obtaining the crosslinked precursor.
[0067] After the second oxidation crosslinking is completed, the air supply is stopped and argon gas is reintroduced to perform confined volatilization treatment on the crosslinking precursor under an inert atmosphere. The crosslinking precursor is heated at a rate of 2.5 °C / min, and held at 480 °C for 120 min. Then, the temperature is further increased to 550 °C, causing the migratable volatile components to decompose thermally and be discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0068] The cavity-forming precursor was carbonized under an inert atmosphere by heating it to 1000°C at a rate of 8°C / min and holding it at 1000°C for 180 min. After cooling, the carbonized material was obtained.
[0069] The carbon material was mixed with potassium hydroxide at a mass ratio of 1:3 to activate the carbon material by heating to 850℃ under nitrogen protection and holding at 850℃ for 120 min. After activation and cooling, the product was washed with hydrochloric acid solution and then with deionized water until the washing solution was neutral. After drying, pitch-based porous carbon with annular pore edges was obtained.
[0070] The resulting pitch-based porous carbon with annular pore edges includes a continuous carbon skeleton, in which multiple open pores are formed that open to the surface of the continuous carbon skeleton, and at least some of the open pores have annular pore edges around their openings, and secondary pores are formed on the pore walls of the open pores.
[0071] Example 3
[0072] Petroleum asphalt was selected as the asphalt raw material. The asphalt raw material was crushed and screened and then placed in a tubular furnace.
[0073] First, the asphalt raw material underwent a first oxidative crosslinking process. The temperature was increased to 245°C at a rate of 1.5°C / min in air and held at 245°C for 60 min to obtain the first crosslinking precursor. During this first oxidative crosslinking process, a portion of the asphalt raw material underwent oxidative crosslinking and formed an initial crosslinking backbone, while migratable and volatile components were retained within this backbone.
[0074] After the first oxidative crosslinking is completed, the air supply is stopped and nitrogen is introduced as an inert atmosphere. Under the inert atmosphere, the temperature is increased to 275°C at a rate of 1°C / min and held at 275°C for 45 min to perform thermal migration treatment on the first crosslinking precursor, so that the migratable volatile components are redistributed in the initial crosslinking backbone, thus obtaining the thermally migrated precursor.
[0075] Air was then reintroduced to perform a second oxidative crosslinking on the thermally migrating precursor. The temperature was increased to 315°C at a rate of 1°C / min and held at 315°C for 60 min to fix the spatial distribution of the redistributed migratable and volatile components, thus obtaining the crosslinked precursor.
[0076] After the second oxidative crosslinking is completed, the air supply is stopped, and nitrogen is introduced again. The crosslinking precursor is subjected to confined volatilization treatment under an inert atmosphere, with the temperature increased to 430℃ at a rate of 0.8℃ / min and held at 430℃ for 60 min, then increased to 520℃ at a rate of 1.5℃ / min and held for 30 min. During the confined volatilization treatment, the migratable volatile components are thermally decomposed, and the resulting volatile components are discharged from the crosslinking precursor, forming primary cavities within the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0077] Subsequently, under a nitrogen atmosphere, the cavity-forming precursor was carbonized by heating it to 900°C at a rate of 4°C / min and holding it at 900°C for 120 min to convert the cavity-forming precursor into a stable carbon skeleton. After cooling, the carbonized material was obtained.
[0078] The carbon material was thoroughly mixed with potassium hydroxide at a mass ratio of 1:2 to activate the carbon material. The temperature was raised to 780℃ under nitrogen protection and maintained at 780℃ for 60 minutes. After activation, the material was allowed to cool naturally. The residual inorganic components were removed with hydrochloric acid solution, and then the material was repeatedly washed with deionized water until the washing solution was neutral. After drying, pitch-based porous carbon with annular pore edges was obtained.
[0079] The resulting pitch-based porous carbon with annular pore edges includes a continuous carbon skeleton, in which multiple open cavities are formed that open to the surface of the continuous carbon skeleton. At least some of the open cavities have annular pore edges around their openings, and secondary pores are formed on the pore walls of the open cavities. The diameter of the secondary pores is smaller than the equivalent diameter of the opening of the open cavities.
[0080] Example 4
[0081] The main difference between this embodiment and Embodiment 3 is that coal tar pitch is used as the asphalt raw material, and a mixture of oxygen and nitrogen is used for the second oxidation crosslinking.
[0082] Coal tar pitch was selected as the asphalt raw material. The asphalt raw material was crushed and screened and then placed in a tubular furnace.
[0083] The asphalt raw material was subjected to a first oxidative crosslinking under an air atmosphere by heating to 225°C at a rate of 1°C / min and holding at 225°C for 90 min to obtain the first crosslinking precursor. The first crosslinking precursor includes an initial crosslinking backbone and a migratable volatile component distributed in the initial crosslinking backbone.
[0084] After the first oxidative crosslinking is completed, switch to argon gas and heat the first crosslinking precursor to 265°C and hold for 60 min under an inert atmosphere to perform thermal migration treatment on the first crosslinking precursor, so that the migratable volatile components are redistributed in the initial crosslinking backbone to obtain the thermally migrated precursor.
[0085] Subsequently, a mixture of oxygen and nitrogen gas with an oxygen volume content of 10% was introduced into the tube furnace. The temperature was increased to 300°C at a heating rate of 1.2°C / min and held at 300°C for 80 min to perform a second oxidative crosslinking on the thermal migration precursor, thereby obtaining the crosslinked precursor.
[0086] After the second oxidation crosslinking is completed, the temperature is switched back to argon gas and heated to 420°C at a heating rate of 1°C / min under an inert atmosphere. The temperature is held at 420°C for 80 min, and then heated to 500°C at a heating rate of 2°C / min and held for 40 min to perform restricted volatilization treatment on the crosslinking precursor. This allows the migratable volatile components to be thermally decomposed and discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0087] Maintaining an inert atmosphere, the cavity-forming precursor is heated to 850°C at a heating rate of 5°C / min, and carbonized at 850°C for 90 min to obtain carbonized material.
[0088] The carbonized material was mixed with potassium hydroxide at a mass ratio of 1:1.5, and the mixture was heated to 750℃ under nitrogen protection and maintained at 750℃ for 90 minutes for activation treatment. After activation treatment, the material was washed with hydrochloric acid solution, deionized water, and dried to obtain pitch-based porous carbon with annular pore edges.
[0089] Example 5
[0090] This embodiment provides a method for preparing pitch-based porous carbon with annular pore edges, as detailed below.
[0091] Petroleum asphalt was selected as the asphalt raw material. The asphalt raw material was crushed and screened and then placed in a tubular furnace.
[0092] The asphalt raw material was heated to 260°C at a heating rate of 2°C / min in air and held at 260°C for 45 min to undergo the first oxidative crosslinking, yielding the first crosslinking precursor. The first crosslinking precursor includes an initial crosslinking backbone and migratable volatile components distributed within the initial crosslinking backbone.
[0093] Then, nitrogen was switched to be used as an inert atmosphere to heat the first crosslinking precursor to 290°C and hold it at 290°C for 60 minutes to perform thermal migration treatment on the first crosslinking precursor, so that the migratable volatile components are redistributed in the initial crosslinking backbone to obtain the thermally migrated precursor.
[0094] After the thermal migration treatment, air was introduced again, and the temperature was increased to 330°C at a rate of 1°C / min. The temperature was maintained at 330°C for 75 min to perform a second oxidative crosslinking on the thermal migration precursor, thereby fixing the spatial distribution of the redistributed migratable volatile components and obtaining the crosslinked precursor.
[0095] The temperature was switched back to nitrogen and increased to 400°C at a rate of 0.6°C / min under an inert atmosphere. The temperature was held at 400°C for 40 min, then increased to 480°C at a rate of 1.2°C / min and held at 480°C for 60 min. This process was used to restrict the volatilization of the crosslinking precursor, causing the migratable volatile components to decompose under heat and be discharged from the crosslinking precursor. This process formed primary cavities in the crosslinking precursor, resulting in a cavity-forming precursor.
[0096] Subsequently, the temperature was increased to 920°C at a rate of 3°C / min under a nitrogen atmosphere, and held at 920°C for 100 min to carbonize the cavity-forming precursor, thus obtaining carbonized material.
[0097] The carbon material was mixed with potassium hydroxide at a mass ratio of 1:1.5 and heated to 730℃ under nitrogen protection. The mixture was then held at 730℃ for 45 minutes to activate the carbon material. After activation and cooling, the resulting product was washed sequentially with hydrochloric acid solution and deionized water until the washing solution was neutral. Finally, it was dried to obtain pitch-based porous carbon with annular pore edges.
[0098] The resulting pitch-based porous carbon with annular pore edges includes a continuous carbon skeleton, in which multiple open pores are formed that open to the surface of the continuous carbon skeleton, and at least some of the open pores have annular pore edges around their openings, and secondary pores are formed on the pore walls of the open pores.
[0099] Example 6
[0100] This embodiment provides a method for preparing pitch-based porous carbon with annular pore edges, as detailed below.
[0101] Petroleum asphalt was selected as the asphalt raw material. The asphalt raw material was crushed and screened and then placed in a tubular furnace.
[0102] The asphalt raw material was heated to 235°C at a heating rate of 1°C / min in air and held at 235°C for 75 min to undergo the first oxidative crosslinking, yielding the first crosslinking precursor. The first crosslinking precursor includes an initial crosslinking backbone and migratable volatile components distributed within the initial crosslinking backbone.
[0103] Switch to nitrogen gas as an inert atmosphere, heat the first crosslinking precursor to 280°C, and maintain it at 280°C for 90 minutes to perform thermal migration treatment on the first crosslinking precursor, so that the migratable volatile components are redistributed in the initial crosslinking backbone to obtain the thermally migrated precursor.
[0104] A mixture of oxygen and nitrogen is reintroduced, with an oxygen volume content of 15%. The temperature is increased to 320°C at a rate of 2°C / min and held at 320°C for 45 min to perform a second oxidative crosslinking on the thermal migration precursor, thus obtaining the crosslinked precursor.
[0105] Then, nitrogen gas was switched to the inert atmosphere and the temperature was increased to 450°C at a rate of 1.5°C / min. The temperature was held at 450°C for 45 min and then increased to 530°C to perform restricted volatilization treatment on the crosslinking precursor. This allowed the migratable volatile components to be thermally decomposed and discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor, thus obtaining a cavity-forming precursor.
[0106] Maintaining a nitrogen atmosphere, the temperature is increased to 800℃ at a rate of 6℃ / min, and held at 800℃ for 150min to carbonize the cavity precursor, thus obtaining carbonized material.
[0107] The carbon material was mixed with potassium hydroxide at a mass ratio of 1:2.5, and heated to 820℃ under nitrogen protection. The mixture was then held at 820℃ for 75 minutes to activate the carbon material. After activation, the mixture was washed with hydrochloric acid solution and deionized water, and then dried to obtain pitch-based porous carbon with annular pore edges.
[0108] The resulting pitch-based porous carbon with annular pore edges includes a continuous carbon skeleton, in which multiple open cavities are formed that open to the surface of the continuous carbon skeleton. At least some of the open cavities have annular pore edges around their openings, and secondary pores are formed on the pore walls of the open cavities. The diameter of the secondary pores is smaller than the equivalent diameter of the opening of the open cavities.
[0109] Comparative Example 1
[0110] The difference between this comparative example and Example 3 is that no thermal migration treatment is performed.
[0111] After the first oxidative crosslinking is completed, the first crosslinking precursor is not placed in an inert atmosphere for thermal migration treatment, but is directly subjected to a second oxidative crosslinking.
[0112] Apart from the differences mentioned above, the remaining steps and process conditions are the same as in Example 3.
[0113] Comparative Example 2
[0114] The difference between this comparative example and Example 3 is that the thermal migration treatment uses an air atmosphere instead of an inert atmosphere.
[0115] After the first oxidative crosslinking is completed, the temperature is increased to 275°C at a rate of 1°C / min while maintaining an air atmosphere. The temperature is then maintained at 275°C for 45 min to perform thermal migration treatment on the first crosslinking precursor. The remaining thermal migration treatment conditions remain unchanged.
[0116] Apart from the differences mentioned above, the remaining steps and process conditions are the same as in Example 3.
[0117] Comparative Example 3
[0118] The difference between this comparative example and Example 3 is that a second oxidative crosslinking is not performed.
[0119] After the thermal migration treatment is completed, the thermal migration precursor is not subjected to a second oxidative crosslinking. Instead, the thermal migration precursor is directly subjected to a restricted volatilization treatment under an inert atmosphere.
[0120] Apart from the differences mentioned above, the remaining steps and process conditions are the same as in Example 3.
[0121] Comparative Example 4
[0122] The difference between this comparative example and Example 3 is that no restricted volatilization treatment is performed.
[0123] After the second oxidation crosslinking is completed, the crosslinking precursor is not subjected to restricted volatilization treatment. Instead, it is directly heated to 900°C at a heating rate of 4°C / min under a nitrogen atmosphere and held at 900°C for 120min to carbonize the crosslinking precursor and obtain carbonized material.
[0124] Apart from the differences mentioned above, the remaining steps and process conditions are the same as in Example 3.
[0125] Comparative Example 5
[0126] The difference between this comparative example and Example 3 is that no activation treatment is performed.
[0127] Following the method in Example 3, the first oxidative crosslinking, thermal migration treatment, second oxidative crosslinking, restricted volatilization treatment, and carbonization treatment were completed sequentially. After obtaining the carbonized material, potassium hydroxide was no longer used to activate the carbonized material. Instead, the carbonized material was cooled and then washed and dried.
[0128] Apart from the differences mentioned above, the remaining steps and process conditions are the same as in Example 3.
[0129] Test Example 1: Crosslinking Precursor State and Restricted Volatilization Capacity Test
[0130] To verify the effects of the first oxidative crosslinking, thermal migration treatment, and the second oxidative crosslinking on the state of the migratable volatile components, the toluene insoluble content and thermogravimetric analysis were performed on the samples obtained in the corresponding stages of Examples 1-6 and Comparative Examples 1-5.
[0131] The toluene-insoluble content was calculated using samples of equal mass that were dissolved, filtered, washed, and dried. The first crosslinking precursor, the thermal migration precursor, and the crosslinking precursor were determined separately.
[0132] Thermogravimetric analysis was conducted in a nitrogen atmosphere. The sample was heated from room temperature to 700°C, and the mass loss rate was recorded in the range of 320–550°C to characterize the retention of migratable volatile components in the sample before entering the restricted volatilization treatment.
[0133] Comparative Example 3 did not undergo a second oxidative crosslinking, and its mass loss rate at 320–550 °C was tested using the thermal migration precursor; the other samples were tested using the crosslinking precursor.
[0134] sample Toluene-insoluble content of the first crosslinking precursor (wt%) Toluene insoluble content (wt%), a precursor for thermal migration Toluene-insoluble content (wt%) of crosslinking precursor Mass loss rate (wt%) at 320–550℃ Example 1 46.8 47.5 67.9 28.4 Example 2 69.4 70.1 92.6 11.7 Example 3 57.6 58.3 80.7 21.6 Example 4 52.9 53.5 77.8 23.4 Example 5 61.8 62.4 88.1 14.6 Example 6 55.3 56.1 83.5 18.8 Comparative Example 1 57.6 — 81.2 20.9 Comparative Example 2 57.6 73.4 86.9 15.2 Comparative Example 3 57.6 58.3 — 30.7 Comparative Example 4 57.6 58.3 80.7 21.6 Comparative Example 5 57.6 58.3 80.7 21.6
[0135] The results above show that after the first oxidative crosslinking, Examples 1 to 6 all formed an initial crosslinking framework to a certain extent, while retaining a certain proportion of migratable volatile components. When thermal migration treatment was carried out under an inert atmosphere, the content of toluene insolubles changed little, indicating that the thermal migration treatment mainly caused the redistribution of migratable volatile components in the initial crosslinking framework, rather than further significant oxidative crosslinking.
[0136] After the second oxidative crosslinking, the toluene-insoluble content of the crosslinking precursor further increased, while still maintaining a certain mass loss rate of 320-550℃. This indicates that the spatial distribution of the redistributed migratory volatile components was fixed, but the migratory volatile components required for subsequent restricted volatilization treatment were still retained.
[0137] After thermal migration treatment in air atmosphere, the content of toluene insoluble matter in Comparative Example 2 increased significantly, indicating that significant oxidative cross-linking occurred at the same stage, which was not conducive to the full redistribution of the migratable volatile components.
[0138] Test Example 2: Morphology Test of Opening Cavity and Annular Pore Edge
[0139] The products obtained in Examples 1-6 and Comparative Examples 1-5 were observed using a scanning electron microscope.
[0140] At the same magnification, no fewer than 5 observation areas were randomly selected, and the number of open cavities, the equivalent diameter of the orifice, and the annular orifice edge were statistically analyzed.
[0141] The equivalent diameter of the orifice is calculated according to the following formula:
[0142] ;
[0143] in, Let A be the equivalent diameter of the orifice, and let A be the projected area of the orifice.
[0144] The continuity of the annular aperture edge is calculated according to the following formula:
[0145] ;
[0146] Where R is the continuity of the annular pore edge. P represents the length of the continuously identifiable annular rim surrounding the opening of the cavity, and P is the perimeter of the opening profile of the cavity.
[0147] An opening cavity with a continuous annular aperture edge of not less than 50% is considered to have an annular aperture edge.
[0148] Figures 1 to 6 The microstructure of the open pores, annular pore edges, and pore walls in the pitch-based porous carbon sample is shown, and its microstructure can be used to describe the morphology of the open pores and annular pore edges.
[0149] sample <![CDATA[Number of open pore cavities per 1000μm 2 > Median equivalent diameter of orifice (μm) The percentage of opening cavities with annular pore edges Average percentage of annular aperture continuity Example 1 31 0.74 43.8 61.2 Example 2 36 0.59 47.6 66.5 Example 3 52 0.86 68.7 77.4 Example 4 45 0.79 60.8 72.1 Example 5 41 0.65 63.5 80.2 Example 6 49 0.82 65.1 75.8 Comparative Example 1 27 0.58 28.4 51.6 Comparative Example 2 24 0.51 22.7 48.3 Comparative Example 3 34 1.12 19.5 39.8 Comparative Example 4 16 0.47 15.2 42.1 Comparative Example 5 46 0.78 66.2 78.1
[0150] As can be seen from the table, Examples 1 to 6 all yielded a relatively large number of open cavities, with Examples 3, 4, and 6 having a higher number of open cavities and a higher proportion of open cavities with annular rims.
[0151] Comparative Example 1, which was not subjected to thermal migration treatment, was still able to form some open cavities, but the proportion of open cavities with annular pore edges decreased significantly, indicating that thermal migration treatment is beneficial to the redistribution of migratable volatile components in the initial crosslinked backbone.
[0152] Comparative Example 3 did not undergo a second oxidative crosslinking, and its pore equivalent diameter was larger, but the continuity of the annular pore edge was significantly reduced. This indicates that the second oxidative crosslinking is beneficial for fixing the spatial distribution of the redistributed migratable volatile components and maintaining the structural integrity around the pores during the restricted volatilization treatment.
[0153] Comparative Example 4, which did not undergo restricted volatilization treatment, had the lowest number of open pores, indicating that restricted volatilization treatment is the main stage for the formation of primary pores.
[0154] Comparative Example 5 was not activated, but a high proportion of annular pore edges could still be observed, indicating that the annular pore edges are mainly formed during the restricted volatilization and carbonization processes, and that activation treatment is not the only source of annular pore edge formation.
[0155] Test Example 3: Pore Structure Test
[0156] The pore structure of the products obtained in Examples 1-6 and Comparative Examples 1-5 was tested using a nitrogen adsorption-desorption method.
[0157] Before testing, the sample was degassed under vacuum at 120℃ for 6 hours. The nitrogen adsorption-desorption isotherm was tested at 77K. The specific surface area and total pore volume were calculated using the BET method. The main pore size distribution range of the secondary pores was obtained through pore size distribution analysis.
[0158] sample <![CDATA[BET specific surface area m 2 / g]]> Total pore volume cm³ / g Secondary pore main pore size distribution (nm) Example 1 1185 0.71 0.9~4.2 Example 2 2510 1.42 0.7~5.6 Example 3 2196 1.26 0.8~4.9 Example 4 1768 1.02 0.8~4.5 Example 5 1496 0.88 0.9~3.8 Example 6 2368 1.35 0.7~5.2 Comparative Example 1 1912 1.06 0.8~4.6 Comparative Example 2 1846 1.01 0.8~4.3 Comparative Example 3 2025 1.12 0.8~4.7 Comparative Example 4 1734 0.96 0.9~4.1 Comparative Example 5 286 0.18 2.8~11.6
[0159] It can be seen that after activation treatment, Examples 1 to 6 all have high BET specific surface area and total pore volume, and at the same time form nanoscale secondary pores.
[0160] Based on the equivalent diameter of the pore opening in Test Example 2, it can be seen that the diameter of the secondary pore is significantly smaller than the equivalent diameter of the pore opening, which corresponds to the structural relationship of "open pore - secondary pore on the pore wall" in pitch-based porous carbon with annular pore edges.
[0161] Comparative Example 5, which was not activated, had a significantly lower BET specific surface area and total pore volume than Example 3. However, it still retained a high proportion of open pores with annular pore edges, indicating that the activation treatment was mainly used to further form secondary pores and increase the pore structure on the pore walls of the open pores, rather than to form primary pores alone.
[0162] Test Example 4: Pollutant Adsorption Performance Test
[0163] Methylene blue was selected as the model pollutant. 100 mL of a 500 mg / L methylene blue aqueous solution was prepared, and 50 mg of the sample to be tested was added. The mixture was then shaken and adsorbed at 25 °C.
[0164] The adsorption amount at 60 min and the equilibrium adsorption amount after reaching adsorption equilibrium were measured respectively.
[0165] The adsorption capacity is calculated according to the following formula:
[0166] ;
[0167] in, This refers to the adsorption capacity. This represents the initial methylene blue concentration. This corresponds to the methylene blue concentration at that time. This is the volume of the methylene blue aqueous solution. The mass of the sample to be tested.
[0168] sample Adsorption capacity (mg / g) over 60 minutes equilibrium adsorption capacity (mg / g) Example 1 296 418 Example 2 401 578 Example 3 498 624 Example 4 421 536 Example 5 367 489 Example 6 474 603 Comparative Example 1 292 468 Comparative Example 2 267 444 Comparative Example 3 281 451 Comparative Example 4 235 396 Comparative Example 5 108 171
[0169] The results showed that Examples 1 through 6 all exhibited good pollutant adsorption capacity.
[0170] While the BET specific surface area of Example 3 was not the highest among all examples, its 60-minute adsorption capacity and equilibrium adsorption capacity were both at a relatively high level. Combined with Test Example 2, it can be seen that Example 3 simultaneously exhibits a high number of open pores and a high proportion of open pores with annular pore edges, indicating that the open pores can provide mass transfer channels for pollutants to enter the continuous carbon framework, while the secondary pores on the pore walls of the open pores further provide adsorption sites.
[0171] Although Example 2 has a higher specific surface area of BET, the proportion of open pores with annular pore edges is lower than that of Example 3, so its adsorption capacity at 60 min is lower than that of Example 3.
[0172] Comparative Example 5, due to the lack of activation treatment, had a lower degree of secondary pore development, resulting in a significant decrease in both BET specific surface area and adsorption capacity. Comparative Example 4, without restricted volatilization treatment, had a smaller number of open pores, leading to a significant decrease in its adsorption capacity at 60 min.
[0173] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing pitch-based porous carbon with annular pore edges, characterized in that, include: The asphalt raw material is subjected to a first oxidative crosslinking to obtain a first crosslinking precursor, which includes an initial crosslinking backbone and a migratable volatile component distributed in the initial crosslinking backbone; The first crosslinking precursor is subjected to thermal migration treatment under an inert atmosphere to redistribute the migratable volatile components in the initial crosslinking backbone, thereby obtaining a thermally migratable precursor. The thermally migrating precursor is subjected to a second oxidative crosslinking to fix the spatial distribution of the redistributed migratable volatile components, thereby obtaining a crosslinked precursor. The crosslinking precursor is subjected to restricted volatilization treatment under an inert atmosphere, so that the migratable volatile components are thermally decomposed and discharged from the crosslinking precursor, forming primary cavities in the crosslinking precursor to obtain a cavity-forming precursor. The cavity-forming precursor is subjected to carbonization treatment to obtain carbonized material; The carbonized material is activated to obtain the pitch-based porous carbon with annular pore edges.
2. The method for preparing pitch-based porous carbon with annular pore edges according to claim 1, characterized in that, The asphalt raw material is petroleum asphalt or coal tar pitch; the temperature of the first oxidative crosslinking is 200–280℃, the time is 20–120 min, and the heating rate is 0.5–3℃ / min; the first oxidative crosslinking is carried out in an air atmosphere, the single treatment mass of the asphalt raw material is 5–10 g, and the air flow rate of the first oxidative crosslinking is 300–2200 mL / min; the thermal migration treatment uses nitrogen or argon as the inert atmosphere, the temperature of the thermal migration treatment is 220–310℃, and the time is 15–90 min.
3. The method for preparing pitch-based porous carbon with annular pore edges according to claim 1, characterized in that, The second oxidation crosslinking uses air or a mixture of oxygen and nitrogen. The oxygen volume content of the second oxidation crosslinking is 5% to 21%, the temperature is 250 to 340°C, the time is 20 to 120 min, and the heating rate is 0.5 to 3°C / min.
4. The method for preparing pitch-based porous carbon with annular pore edges according to claim 1, characterized in that, The restricted volatilization treatment includes heating the crosslinked precursor to 320–550°C at a heating rate of 0.3–2.5°C / min under an inert atmosphere, and holding it at 380–480°C for 20–120 min.
5. The method for preparing pitch-based porous carbon with annular pore edges according to claim 1, characterized in that, The carbonization process includes heating the cavity-forming precursor to 750–1000°C in an inert atmosphere at a heating rate of 2–8°C / min and holding it at that temperature for 60–180 min.
6. The method for preparing pitch-based porous carbon with annular pore edges according to claim 1, characterized in that, The activation treatment uses potassium hydroxide as the activating agent, the mass ratio of the carbonized material to the potassium hydroxide is 1:1 to 1:3, the activation temperature is 700 to 850°C, and the activation time is 30 to 120 minutes.
7. A pitch-based porous carbon, characterized in that, It includes a continuous carbon skeleton, in which a plurality of opening cavities are formed that open to the surface of the continuous carbon skeleton, at least some of the opening cavities have annular rims formed around their openings, and secondary pores are formed on the walls of the opening cavities, the diameter of the secondary pores being smaller than the equivalent diameter of the openings of the opening cavities.
8. The pitch-based porous carbon according to claim 7, characterized in that, The asphalt-based porous carbon is prepared by asphalt raw material through a first oxidation crosslinking, thermal migration treatment, a second oxidation crosslinking, restricted volatilization treatment, carbonization treatment and activation treatment in sequence. The annular pore edge extends circumferentially along the pore opening of the corresponding opening cavity, and at least some of the adjacent opening pore cavities are interconnected.
9. An adsorbent material, characterized in that, The adsorbent material comprises the pitch-based porous carbon as described in claim 7.
10. The application of the adsorbent material according to claim 9 in pollutant adsorption.