A reverse hydrogen reduction method for ultrafine tungsten carbide powder and its preparation process

By combining reverse hydrogen reduction and multi-stage high-temperature carbonization with airflow classification, the problems of uneven particle size and grain growth in traditional ultrafine tungsten carbide powder were solved, and ultrafine tungsten carbide powder with uniform particle size was prepared, thus improving the performance of the alloy.

CN123105641APending Publication Date: 2026-11-17CHONGQING KANCIRON IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611439897.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional ultrafine tungsten carbide preparation processes suffer from uneven tungsten powder particle size distribution and the retention of some grains during the carbide process, leading to a decrease in alloy performance.

Method used

Ultrafine tungsten powder was prepared by reverse hydrogen reduction method, and then subjected to multi-stage high-temperature carbonization and airflow classification treatment, combined with grain inhibitors, to control the particle size distribution of tungsten powder and inhibit grain growth, resulting in ultrafine tungsten carbide powder with uniform particle size.

Benefits of technology

This resulted in finer and more uniform particle size distribution of ultrafine tungsten carbide powder, avoiding abnormal grain growth and improving the overall performance of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105641A_ABST
    Figure CN123105641A_ABST
Patent Text Reader

Abstract

This invention relates to the field of powder metallurgy technology, specifically to an ultrafine tungsten carbide powder prepared by reverse hydrogen reduction and its preparation process. Blue tungsten is loaded into a boat and placed in a reduction furnace, hydrogen is introduced, and a reduction reaction is carried out using reverse hydrogen reduction to obtain ultrafine tungsten powder. The ultrafine tungsten powder is then mixed uniformly with a carbon source and grain inhibitor in a specific ratio to obtain a mixture. The mixture is placed in a carbonization furnace and subjected to multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks. The tungsten carbide blocks are pre-crushed and then subjected to airflow classification to obtain ultrafine tungsten carbide powder. In the reverse hydrogen reduction process, the hydrogen flow direction is opposite to the material propulsion direction, allowing fresh hydrogen to first contact the partially reduced material, effectively removing the water vapor generated during reduction and ensuring a consistent reducing atmosphere. This prevents abnormal particle growth in the tungsten powder. The airflow classification process removes a small amount of agglomerated particles that may form during carbonization, resulting in ultrafine tungsten carbide powder with an extremely narrow particle size distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of powder metallurgy technology, and in particular to an ultrafine tungsten carbide powder prepared by reverse hydrogen reduction and its preparation process. Background Technology

[0002] Ultrafine cemented carbide, due to its combined properties of high hardness, high strength, and good toughness, is widely used in high-efficiency precision cutting tools, micro-drills, micro-milling machines, and precision molds. One of the key technical challenges in preparing ultrafine cemented carbide lies in how to improve the uniformity of the alloy grain size and avoid the formation of abnormally large grains during sintering. These abnormally large grains are often the source of fracture in ultrafine cemented carbide products.

[0003] Currently, the mainstream method for mass production of tungsten carbide both domestically and internationally is the tungsten oxide hydrogen reduction-carbide method. This method uses tungsten oxide as raw material, reduces it to tungsten powder with hydrogen, and then mixes the tungsten powder with carbon black before high-temperature carbide processing.

[0004] However, the traditional hydrogen reduction process has many limitations in the large-scale production of ultrafine tungsten powder. For example, when using coarse-grained raw materials such as tungsten dioxide, due to the coarse grain size (generally between 10 and 50 μm), some agglomerates are retained during the reduction and carbonization process, forming agglomerates (with a particle size between 1 and 10 μm) in ultrafine tungsten carbide. Even if physical crushing is subsequently used, the crushing effect is limited due to the extreme hardness of tungsten carbide, and the poor crystal integrity of the agglomerates will preferentially dissolve and precipitate on the coarser grains during the subsequent liquid-phase sintering stage, forming abnormally large grains that seriously affect the alloy properties. Summary of the Invention

[0005] The purpose of this invention is to provide an ultrafine tungsten carbide powder prepared by reverse hydrogen reduction and its preparation process, which aims to solve the problems of uneven particle size distribution of tungsten powder and the retention of some crystals to form agglomerates during the carbonization process in traditional ultrafine tungsten carbide preparation processes.

[0006] To achieve the above objectives, in a first aspect, the present invention provides a reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder, comprising the following steps: Blue tungsten was loaded into a boat and placed in a reduction furnace. Hydrogen was introduced, and a reduction reaction was carried out using the reverse hydrogen reduction method to obtain ultrafine tungsten powder. The ultrafine tungsten powder is mixed evenly with a carbon source and a grain inhibitor in a certain proportion to obtain a mixture. The mixture is placed in a carbonization furnace and subjected to multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks. The tungsten carbide block material is pre-crushed and then subjected to air classification to obtain ultrafine tungsten carbide powder.

[0007] The specific method for placing blue tungsten in a boat in a reduction furnace, introducing hydrogen gas, and carrying out a reduction reaction using a reverse hydrogen reduction method to obtain ultrafine tungsten powder is as follows: Blue tungsten is loaded into a boat-shaped dish and placed in a single-layer arrangement inside the reduction furnace; Hydrogen gas is introduced, and the reduction reaction is carried out using the reverse hydrogen reduction method. After the reduction reaction is completed, the furnace is cooled to room temperature under a hydrogen protective atmosphere.

[0008] The process parameters for the reverse hydrogen reduction method are as follows: reduction temperature 650~850℃, boat loading 1.5~2.5kg / boat, and hydrogen flow rate 5~12 m³ / min. 3 / h, hydrogen dew point is -60℃ to -80℃, reduction time is 4 to 10 h.

[0009] The carbon source is carbon black, graphite powder, or a mixture of both, and the particle size of the carbon source is ≤1μm. The grain inhibitor is selected from one or more of vanadium carbide, chromium carbide, tantalum carbide, and niobium carbide.

[0010] The specific method for placing the mixture in a carbonization furnace and performing multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks is as follows: The mixture is placed in a carbonization furnace and heated to 900-1050°C at a rate of 5-10°C / min for a low-temperature carbonization stage, and held at that temperature for 1-3 hours. The mixture after low-temperature carbonization is heated to 1100-1300℃ at a rate of 2-5℃ / min for high-temperature carbonization and held for 2-5 hours. After carbonization, the tungsten carbide blocks are cooled to room temperature in a hydrogen protective atmosphere to obtain tungsten carbide blocks.

[0011] The specific method for pre-crushing the tungsten carbide ingot and then subjecting it to airflow classification to obtain ultrafine tungsten carbide powder is as follows: The tungsten carbide block material is fed into a jaw crusher or hammer crusher and crushed to a particle size ≤ 5 mm. The pre-crushed tungsten carbide powder is fed into an air classifier for air classification, and the fine powder is collected to obtain ultrafine tungsten carbide powder. The collected coarse powder is returned to the crushing process for reprocessing.

[0012] Secondly, the present invention also provides an ultrafine tungsten carbide powder prepared by reverse hydrogen reduction, which is prepared using the reverse hydrogen reduction ultrafine tungsten carbide powder preparation process described in the first aspect above.

[0013] This invention discloses a reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder. A blue tungsten boat is placed in a reduction furnace, hydrogen gas is introduced, and a reduction reaction is carried out using a reverse hydrogen reduction method to obtain ultrafine tungsten powder. The ultrafine tungsten powder is then mixed uniformly with a carbon source and a grain inhibitor in a specific ratio to obtain a mixture. This mixture is placed in a carbonization furnace and subjected to multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks. The tungsten carbide blocks are pre-crushed and then subjected to airflow classification to obtain ultrafine tungsten carbide powder. In this method, the hydrogen flow direction is opposite to the material propulsion direction during reverse hydrogen reduction. Fresh hydrogen first contacts the partially reduced material, which helps to fully remove the water vapor generated during reduction, ensuring the consistency of the reducing atmosphere. This effectively inhibits abnormal growth of tungsten powder particles, resulting in ultrafine tungsten powder with finer particle size and more uniform distribution. Furthermore, the segmented control of pre-reaction in a low-temperature stage and full carbonization in a high-temperature stage avoids the problems of local overheating and abnormal grain growth caused by the intense reaction in traditional one-step high-temperature carbonization. The low-temperature stage allows tungsten powder to initially react with the carbon source to form low-order carbides, while the high-temperature stage ensures complete carbonization and promotes perfect grain development. Simultaneously, because the carbonization reaction proceeds in steps, it effectively inhibits rapid grain growth. The inhibitors agglomerate at the tungsten carbide grain boundaries during carbonization, effectively pinning grain boundary migration and further suppressing grain growth, ensuring ultra-fine grains in the final product. Airflow classification effectively removes any small agglomerates that may form during carbonization, resulting in ultra-fine tungsten carbide powder with an extremely narrow particle size distribution. This solves the problems of uneven tungsten powder particle size distribution and the retention of some grains during carbonization, forming agglomerates, present in traditional ultra-fine tungsten carbide preparation processes. Attached Figure Description

[0014] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.

[0015] Figure 1 This is a flowchart of a reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder provided by the present invention.

[0016] Figure 2 This is a flowchart of step S1 of a reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder provided by the present invention.

[0017] Figure 3 This is a flowchart of step S3 in the reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder provided by the present invention.

[0018] Figure 4 This is a flowchart of step S4 in the reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder provided by the present invention. Detailed Implementation

[0019] The embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.

[0020] Please see Figures 1 to 4 In a first aspect, the present invention provides a process for preparing ultrafine tungsten carbide powder by reverse hydrogen reduction, comprising the following steps: S1 Place the blue tungsten boat in a reduction furnace, introduce hydrogen gas, and carry out a reduction reaction using the reverse hydrogen reduction method to obtain ultrafine tungsten powder; Specific methods: S11 The blue tungsten is loaded into a boat dish and placed in the reduction furnace in a single-layer arrangement; Hydrogen gas is introduced into S12, and the reduction reaction is carried out by reverse hydrogen reduction. After the reduction reaction is completed, the furnace is cooled to room temperature under a hydrogen protective atmosphere.

[0021] In this embodiment of the invention, the process parameters of the reverse hydrogen reduction method are: reduction temperature of 650~850℃, boat loading of 1.5~2.5 kg / boat, and hydrogen flow rate of 5~12 m³ / kg. 3 / h, hydrogen dew point is -60℃ to -80℃, reduction time is 4 to 10 h.

[0022] S2. The ultrafine tungsten powder is mixed evenly with a carbon source and a grain inhibitor in a certain proportion to obtain a mixture. In this embodiment of the invention, the amount of carbon source added is calculated as 6.0%~6.4% of the mass of ultrafine tungsten powder, and the amount of grain inhibitor added is 0.2%~1.0% of the mass of ultrafine tungsten powder. The ultrafine tungsten powder, carbon source, and grain inhibitor are placed together in a three-dimensional mixer or a V-type mixer and mixed at a speed of 20~60 r / min for 4~10 h; the carbon source is carbon black, graphite powder, or a mixture of both, and the particle size of the carbon source is ≤1 μm; the grain inhibitor is selected from at least one of vanadium carbide (VC), chromium carbide (Cr3C2), tantalum carbide (TaC), and niobium carbide (NbC). S3 The mixture is placed in a carbonization furnace and subjected to multi-stage high-temperature carbonization under hydrogen atmosphere protection to obtain tungsten carbide blocks. Specific methods: S31 The mixture is placed in a carbonization furnace and heated to 900-1050°C at a rate of 5-10°C / min for a low-temperature carbonization stage, and held at that temperature for 1-3 hours. In this embodiment of the invention, blue tungsten is loaded into boats and arranged in a single layer inside the reduction furnace. The spacing between the boats is 10-30 mm, and the thickness of the boats is 8-15 mm. The single-layer arrangement combined with the appropriate boat spacing facilitates the uniform distribution and sufficient flow of hydrogen among the materials, promptly carrying away the water vapor generated by the reduction reaction. This prevents excessively high local water vapor partial pressure, which could lead to abnormal growth of tungsten powder particles. The rapid heating rate in the low-temperature section helps to quickly pass through the carbonization reaction initiation temperature range, avoiding uneven local reactions caused by prolonged material residence in this temperature range.

[0023] S32 heats the mixture after low-temperature carbonization to 1100~1300℃ at a rate of 2~5℃ / min for high-temperature carbonization, and holds it at that temperature for 2~5 hours. In this embodiment of the invention, using a slower heating rate in the high-temperature section is beneficial for the carbonization reaction to proceed fully and uniformly, reducing local overheating caused by the exothermic reaction.

[0024] After S33 carbonization is completed, it is cooled to room temperature in a hydrogen protective atmosphere to obtain tungsten carbide blocks.

[0025] In this embodiment of the invention, after the reduction reaction is completed, the furnace is cooled to room temperature under a hydrogen protective atmosphere, with the hydrogen flow rate maintained at 3-6 m³ / h during the cooling process. 3 / h. Maintaining a hydrogen protective atmosphere during the cooling process can effectively prevent the oxidation of ultrafine tungsten powder, while avoiding thermal stress and particle adhesion caused by excessively rapid cooling.

[0026] S4 pre-crushes the tungsten carbide block material and then processes it through airflow classification to obtain ultrafine tungsten carbide powder.

[0027] Specific methods: S41 The tungsten carbide block material is fed into a jaw crusher or hammer crusher and crushed to a particle size ≤ 5 mm. S42 feeds the pre-crushed tungsten carbide powder into an air classifier for air classification, collects the fine powder to obtain ultrafine tungsten carbide powder, and returns the collected coarse powder to the crushing process for reprocessing.

[0028] In this embodiment of the invention, the pre-crushed tungsten carbide powder is fed into an air classifier. The classifier wheel rotates at 3000-6000 rpm, and the induced draft fan frequency is 30-50 Hz. The collected fine powder is the ultrafine tungsten carbide powder, while the collected coarse powder is returned to the crushing process for reprocessing. Specifically, the air classification process employs a series two-stage air classification. The first stage removes coarse particles, and the second stage collects ultrafine powder. The classifier wheel in the first stage rotates at 2000-3500 rpm, and the classifier wheel in the second stage rotates at 4000-6500 rpm. This two-stage classification allows for more precise control of the product's particle size distribution range, improving the accuracy and efficiency of the classification.

[0029] Secondly, the present invention also provides an ultrafine tungsten carbide powder prepared by reverse hydrogen reduction, which is prepared using the reverse hydrogen reduction ultrafine tungsten carbide powder preparation process described in the first aspect above.

[0030] To better understand this technical solution, the following embodiments are provided for further explanation: Example 1

[0031] The process for preparing ultrafine tungsten carbide powder by reverse hydrogen reduction in this embodiment includes the following steps: (11) Reverse hydrogen reduction Blue tungsten with an average particle size of 10 μm was packed into boats with a spacing of 20 mm between them. The boats weighed 2.0 kg per boat, with a thickness of 12 mm, and were arranged in a single layer in the reduction furnace. Hydrogen gas was introduced, and a reverse hydrogen reduction reaction was carried out at a flow rate of 9 m³ / h. 3 The hydrogen dew point was -70℃, the reduction temperature was 750℃, and the reduction time was 7 hours. After reduction, the furnace was cooled to room temperature under a hydrogen protective atmosphere, with the hydrogen flow rate maintained at 4.5 m³ / h. 3 / h, to obtain ultrafine tungsten powder.

[0032] (12) Carbon mixing The ultrafine tungsten powder obtained in step (11) was mixed with carbon black (particle size ≤ 0.8 μm) at a mass ratio of 1:0.062, and 0.5% VC by mass of the ultrafine tungsten powder was added as a grain inhibitor. The above materials were placed in a three-dimensional mixer and mixed at a speed of 45 r / min for 6 h to obtain a uniformly mixed material.

[0033] (13) Multi-stage high-temperature carbonization The mixture obtained in step (12) is placed in a graphite boat and placed in a carbonization furnace under a hydrogen atmosphere (hydrogen flow rate 5 m³ / h). 3 The mixture undergoes multi-stage high-temperature carbonization ( / h). First, the temperature is increased to 950℃ at a rate of 8℃ / min and held for 1.5h; then, it is increased to 1200℃ at a rate of 3℃ / min and held for 2.5h. After carbonization, the mixture is cooled to room temperature in a hydrogen protective atmosphere, maintaining a hydrogen flow rate of 3.5m³ / min during cooling. 3 / h, to obtain tungsten carbide ingots.

[0034] (14) Breaking and airflow classification The tungsten carbide blocks obtained in step (13) are pre-crushed using a jaw crusher. The discharge port width is adjusted to 5mm, and the material is crushed to a particle size of ≤3mm. Then, the material is sent to an air classifier for classification. The classifier wheel speed is 4500rpm, and the blower frequency is 40Hz. The collected fine powder is ultrafine tungsten carbide powder.

[0035] The particle size of the ultrafine tungsten carbide powder obtained in this embodiment was measured using a laser particle size analyzer. The results were: D10 = 0.38 μm, D50 = 0.58 μm, D90 = 0.92 μm, (D90-D10) / D50 = 0.93. The total carbon content was 6.14%, with combined carbon ≥ 6.10% and free carbon ≤ 0.05%.

[0036] Example 2

[0037] The process for preparing ultrafine tungsten carbide powder by reverse hydrogen reduction in this embodiment includes the following steps: (21) Reverse hydrogen reduction Blue tungsten with an average particle size of 8 μm was packed into boats with a spacing of 15 mm between them. Each boat weighed 1.8 kg, and the boat thickness was 10 mm. These boats were arranged in a single layer in the reduction furnace. Hydrogen gas was introduced, and a reverse hydrogen reduction reaction was carried out at a flow rate of 8 m³ / h. 3 The hydrogen dew point was -65℃, the reduction temperature was 720℃, and the reduction time was 8 hours. After reduction, the furnace was cooled to room temperature under a hydrogen protective atmosphere, with the hydrogen flow rate maintained at 4 m³ / h. 3 / h, to obtain ultrafine tungsten powder.

[0038] (22) Carbon mixing The ultrafine tungsten powder obtained in step (21) was mixed with carbon black (particle size ≤ 0.8 μm) at a mass ratio of 1:0.063. At the same time, 0.3% Cr3C2 and 0.2% TaC by mass of the ultrafine tungsten powder were added as grain inhibitors. The above materials were placed in a V-type mixer and mixed at a speed of 35 r / min for 8 hours to obtain a uniformly mixed material.

[0039] (23) Multi-stage high-temperature carbonization The mixture obtained in step (22) is placed in a graphite boat and placed in a carbonization furnace under a hydrogen atmosphere (hydrogen flow rate 4 m³ / h). 3 The process involves three stages of high-temperature carbonization. The first stage involves heating to 920℃ at a rate of 8℃ / min and holding for 2 hours. The second stage involves heating to 1020℃ at a rate of 4℃ / min and holding for 2 hours. The third stage involves heating to 1150℃ at a rate of 3℃ / min and holding for 3 hours. After carbonization, the furnace is cooled to room temperature under a hydrogen protective atmosphere, maintaining a hydrogen flow rate of 3 m³ / min throughout the cooling process. 3 / h, to obtain tungsten carbide ingots.

[0040] (24) Breaking and airflow classification The tungsten carbide blocks obtained in step (23) are pre-crushed using a hammer crusher. The gap between the hammer and the impact plate is adjusted to 4mm. The blocks are crushed to a particle size of ≤4mm and then sent to an air classifier for classification. The classifier wheel speed is 5000rpm and the blower frequency is 45Hz. The collected fine powder is ultrafine tungsten carbide powder.

[0041] The particle size of the ultrafine tungsten carbide powder prepared in this embodiment was measured, and the results were: D10=0.35μm, D50=0.52μm, D90=0.85μm, (D90-D10) / D50=0.96.

[0042] Example 3

[0043] The process for preparing ultrafine tungsten carbide powder by reverse hydrogen reduction in this embodiment includes the following steps: (31) Reverse hydrogen reduction Blue tungsten with an average particle size of 12 μm was loaded into boats with a spacing of 25 mm between them. The boats weighed 2.2 kg per boat, with a thickness of 14 mm, and were arranged in a single layer in the reduction furnace. Hydrogen gas was introduced, and a reverse hydrogen reduction reaction was carried out at a flow rate of 10 m³ / h. 3 The hydrogen dew point was -75℃, the reduction temperature was 780℃, and the reduction time was 6 hours. After reduction, the furnace was cooled to room temperature under a hydrogen protective atmosphere, maintaining a hydrogen flow rate of 5 m³ / h during the cooling process. 3 / h, to obtain ultrafine tungsten powder.

[0044] (32) Carbon mixing The ultrafine tungsten powder obtained in step (31) was mixed with carbon black (particle size ≤ 0.8 μm) at a mass ratio of 1:0.061, and 0.4% NbC by mass of the ultrafine tungsten powder was added as a grain inhibitor. The above materials were placed in a three-dimensional mixer and mixed at a speed of 50 r / min for 5 h to obtain a uniformly mixed material.

[0045] (33) Multi-stage high-temperature carbonization The mixture obtained in step (32) is placed in a graphite boat and placed in a carbonization furnace under a hydrogen atmosphere (hydrogen flow rate 6m). 3 The process involves three stages of high-temperature carbonization. The first stage involves heating to 980℃ at a rate of 7℃ / min and holding for 1 hour. The second stage involves heating to 1080℃ at a rate of 3℃ / min and holding for 1 hour. The third stage involves heating to 1250℃ at a rate of 2℃ / min and holding for 2 hours. After carbonization, the furnace is cooled to room temperature under a hydrogen protective atmosphere, maintaining a hydrogen flow rate of 4 m³ / min throughout the cooling process. 3 / h, to obtain tungsten carbide ingots.

[0046] (34) Breaking and airflow classification The tungsten carbide blocks obtained in step (33) are pre-crushed using a jaw crusher. The discharge port width is adjusted to 6mm, and the material is crushed to a particle size of ≤3mm. Then, it is fed into a series two-stage air classifier for classification. The first stage classifier rotates at 3000rpm, the second stage classifier rotates at 5500rpm, and the blower frequency is 40Hz. The collected second-stage fine powder is ultrafine tungsten carbide powder.

[0047] The particle size of the ultrafine tungsten carbide powder prepared in this embodiment was measured, and the results were: D10=0.41μm, D50=0.62μm, D90=0.98μm, (D90-D10) / D50=0.92.

[0048] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the reverse hydrogen reduction method is replaced by the forward hydrogen reduction method (the direction of hydrogen flow is the same as the direction of material propulsion), while the remaining steps and parameters are the same as in Example 1.

[0049] The particle size distribution of the ultrafine tungsten carbide powder prepared in Comparative Example 1 was as follows: D10 = 0.42 μm, D50 = 0.75 μm, D90 = 1.68 μm, (D90-D10) / D50 = 1.68. It is evident that the tungsten powder prepared by the cis-hydrogen reduction method has a significantly coarser particle size and a wider distribution, resulting in a significantly less uniform particle size in the final tungsten carbide product compared to the embodiment of this invention.

[0050] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that a one-step high-temperature carbonization (direct heat treatment at 1200℃ for 5 hours) is used instead of multi-stage high-temperature carbonization, while the remaining steps and parameters are the same as in Example 1.

[0051] The particle size distribution of the ultrafine tungsten carbide powder prepared in Comparative Example 2 was as follows: D10 = 0.45 μm, D50 = 0.72 μm, D90 = 1.85 μm, and (D90-D10) / D50 = 1.94. Furthermore, some abnormally grown coarse grains were visible in the SEM images. This indicates that abnormal grain growth is prone to occur during the one-step high-temperature carbonization process, resulting in poor product uniformity.

[0052] The above-disclosed embodiments are merely preferred examples of the reverse hydrogen reduction method for ultrafine tungsten carbide powder and its preparation process, and should not be construed as limiting the scope of the present application. Those skilled in the art can understand that implementing all or part of the above-described embodiments and making equivalent changes in accordance with the claims of the present application are still within the scope of the present application.

Claims

1. A process for preparing ultrafine tungsten carbide powder by reverse hydrogen reduction, characterized in that, Includes the following steps: Blue tungsten was loaded into a boat and placed in a reduction furnace. Hydrogen was introduced, and a reduction reaction was carried out using the reverse hydrogen reduction method to obtain ultrafine tungsten powder. The ultrafine tungsten powder is mixed evenly with a carbon source and a grain inhibitor in a certain proportion to obtain a mixture. The mixture is placed in a carbonization furnace and subjected to multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks. The tungsten carbide block material is pre-crushed and then subjected to air classification to obtain ultrafine tungsten carbide powder.

2. The reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in claim 1, characterized in that, The specific method for placing blue tungsten in a boat in a reduction furnace, introducing hydrogen gas, and carrying out a reduction reaction using the reverse hydrogen reduction method to obtain ultrafine tungsten powder is as follows: Blue tungsten is loaded into a boat-shaped dish and placed in a single-layer arrangement inside the reduction furnace; Hydrogen gas is introduced, and the reduction reaction is carried out using the reverse hydrogen reduction method. After the reduction reaction is completed, the furnace is cooled to room temperature under a hydrogen protective atmosphere.

3. The reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in claim 1, characterized in that, The process parameters for the reverse hydrogen reduction method are: reduction temperature of 650~850℃, boat loading of 1.5~2.5 kg / boat, and hydrogen flow rate of 5~12 m³ / kg. 3 / h, hydrogen dew point is -60℃ to -80℃, reduction time is 4 to 10 h.

4. The reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in claim 1, characterized in that, The carbon source is carbon black, graphite powder, or a mixture of both, with a particle size ≤1μm. The grain inhibitor is selected from one or more of vanadium carbide, chromium carbide, tantalum carbide, and niobium carbide.

5. The reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in claim 1, characterized in that, The specific method for placing the mixture in a carbonization furnace and performing multi-stage high-temperature carbonization under a hydrogen atmosphere to obtain tungsten carbide blocks is as follows: The mixture is placed in a carbonization furnace and heated to 900-1050°C at a rate of 5-10°C / min for a low-temperature carbonization stage, and held at that temperature for 1-3 hours. The mixture after low-temperature carbonization is heated to 1100-1300℃ at a rate of 2-5℃ / min for high-temperature carbonization and held for 2-5 hours. After carbonization, the tungsten carbide blocks are cooled to room temperature in a hydrogen protective atmosphere to obtain tungsten carbide blocks.

6. The reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in claim 1, characterized in that, The specific method for pre-crushing the tungsten carbide ingot and then subjecting it to airflow classification to obtain ultrafine tungsten carbide powder is as follows: The tungsten carbide block material is fed into a jaw crusher or hammer crusher and crushed to a particle size ≤ 5 mm. The pre-crushed tungsten carbide powder is fed into an air classifier for air classification, and the fine powder is collected to obtain ultrafine tungsten carbide powder. The collected coarse powder is returned to the crushing process for reprocessing.

7. A reverse hydrogen reduction method for ultrafine tungsten carbide powder, characterized in that, It is prepared using the reverse hydrogen reduction method for preparing ultrafine tungsten carbide powder as described in any one of claims 1-6.