Methods for manufacturing porous silicon, porous silicon and secondary batteries

By preparing porous silicon with Si crystal phase and CaxMg2-xSi2O6 crystal phase, the problem of insufficient pressure resistance of porous silicon was solved, and high porosity and stable battery performance were maintained under pressure.

CN123105644APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511999451.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2025-12-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing porous silicon has insufficient resistance to compression, which causes the volume of the negative electrode active material layer to expand during charging, affecting battery performance.

Method used

Porous silicon with Si and CaxMg2-xSi2O6 crystal phases was prepared by contacting raw materials containing CaSiO3 with alkaline earth metal gas and acid, thereby improving its pressure resistance.

Benefits of technology

The prepared porous silicon is not easily collapsed under pressure, maintains high porosity, suppresses the volume expansion of the negative electrode active material layer, and maintains stable battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention provides a method for manufacturing porous silicon capable of producing porous silicon with excellent pressure resistance. The method comprises the following steps: contacting a raw material containing CaSiO3 with an alkaline earth metal gas; and contacting the raw material in contact with the alkaline earth metal gas with an acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing porous silicon, porous silicon, and a secondary battery. Background Technology

[0002] Silicon is known to have a high theoretical capacity, which is effective for achieving high energy density in batteries. On the other hand, silicon is known to expand in volume easily during battery charging.

[0003] Patent Document 1 discloses a method for manufacturing porous silicon. This method includes a reduction step and a cleaning step. In the reduction step, Mg vapor is contacted with a raw material containing SiO2 under specific conditions, thereby obtaining an intermediate product containing Si and MgO. In the cleaning step, MgO is removed from the intermediate product. Thus, porous silicon is obtained.

[0004] Patent Document 1: Japanese Patent Application Publication No. 2023-76283 Summary of the Invention

[0005] However, the fine pores of porous silicon obtained by conventional manufacturing methods are easily collapsed by pressure (e.g., the pressing pressure during the fabrication of the active material layer), and the porosity of the porous silicon may decrease due to pressure. That is, the pressure resistance of the porous silicon may be insufficient. When the negative electrode active material layer of a secondary battery contains porous silicon with low porosity, it may be difficult to suppress the volume expansion of the negative electrode active material layer during charging. As a result, the battery performance of the secondary battery may deteriorate.

[0006] The present invention was made in view of the above circumstances.

[0007] One embodiment of the present invention aims to solve the problem of providing a method for manufacturing porous silicon that can produce porous silicon with excellent pressure resistance.

[0008] Another embodiment of the present invention aims to solve the problem of providing a porous silicon and a secondary battery with excellent pressure resistance.

[0009] The means to solve the above problems include the following implementation methods.

[0010] <1> A method for manufacturing porous silicon includes the following steps: contacting a raw material containing CaSiO3 with an alkaline earth metal gas; and contacting the raw material in contact with the alkaline earth metal gas with an acid.

[0011] <2> A porous silicon having a Si crystal phase as the main phase and a Ca phase as the secondary phase. x Mg 2-x The crystal phase of Si2O6 (0≤x≤1).

[0012] <3> The porous silicon according to <2>, wherein the pore volume measured by the Barrett-Joyner-Halenda method is 0.2 cm³. 3 / g or more.

[0013] <4> The porous silicon according to <2> or <3>, wherein the BET specific surface area is 70 m². 2 / g or more.

[0014] <5> A secondary battery comprising: a negative electrode layer; a positive electrode layer; and an electrolyte layer disposed between the negative electrode layer and the positive electrode layer.

[0015] The negative electrode layer has a negative electrode current collector and a negative electrode active material layer disposed on one or two surfaces of the negative electrode current collector.

[0016] The negative electrode active material layer comprises porous silicon as described in any one of <2> to <4>.

[0017] Invention Effects

[0018] According to one embodiment of the present invention, a method for manufacturing porous silicon capable of producing porous silicon with excellent pressure resistance is provided.

[0019] According to another embodiment of the present invention, a porous silicon with excellent pressure resistance and a secondary battery are provided. Attached Figure Description

[0020] Figure 1 This is a cross-sectional view of a secondary battery according to an embodiment of the present invention.

[0021] Figure 2 The XRD diffraction patterns of porous silicon in Example 1 and Comparative Example 1 are shown (horizontal axis: diffraction angle 2θ, vertical axis: intensity).

[0022] Figure 3 This is a graph showing the porosity of porous silicon in Example 1 and Comparative Example 1 after pressing at 60 kN / cm2. Detailed Implementation

[0023] Hereinafter, embodiments of the present invention will be described. These descriptions are illustrative of the embodiments and do not limit the scope of the present invention.

[0024] In this specification, the numerical range indicated by “~” represents the range to which the values ​​before and after “~” are included, respectively, as the minimum and maximum values.

[0025] In the numerical ranges described in this specification, the upper or lower limit of a numerical range can be replaced by the upper or lower limit of other numerical ranges described in other stages. Furthermore, the upper or lower limit of the numerical ranges described in this specification can be replaced by the values ​​shown in the embodiments.

[0026] In this specification, the term "process" includes not only independent processes, but also processes that can be clearly distinguished from other processes, as long as they achieve the intended purpose of the process.

[0027] In this specification, when describing embodiments with reference to the accompanying drawings, the structure of these embodiments is not limited to the structure shown in the drawings. Furthermore, the sizes of the components in the figures are conceptual, and the relative sizes of the components are not limited thereto.

[0028] In this specification, each component may contain multiple corresponding substances. When the amount of each component in the composition is mentioned in this embodiment, if multiple substances corresponding to each component are present in the composition, it indicates the total amount of the multiple substances present in the composition, unless otherwise stated.

[0029] (1) Method for manufacturing porous silicon

[0030] The method for manufacturing porous silicon according to the present invention includes the following steps: contacting a raw material containing CaSiO3 with an alkaline earth metal gas (hereinafter also referred to as the "reduction step"); and contacting the raw material in contact with the alkaline earth metal gas with an acid (hereinafter also referred to as the "acid treatment step"). The reduction step and the acid treatment step are performed in this order.

[0031] "Porous silicon" refers to an aggregate (i.e., powder) of Si particles having multiple fine pores. "Si particles" refers to particles containing Si as the main component, and also containing Mg and Ca elements. Specifically, the proportion of Si in the total elements contained in the Si particles can be, for example, 50% or more by mass, 90% or more by mass, 95% or more by mass, less than 98% by mass, or less than 97% by mass. Si particles can contain elements different from Si, Mg, and Ca (e.g., Li, Sn, Fe, Co, Ni, Ti, Cr, B, and P). Si particles can contain impurities (e.g., oxides). The elemental Si contained in the Si particles can be amorphous Si or crystalline Si.

[0032] The porous silicon manufacturing method of the present invention has the above-described structure, and therefore can manufacture porous silicon with excellent pressure resistance.

[0033] This effect is inferred based on the following reasons, but is not limited to them.

[0034] In this invention, it is believed that an intermediate with a sea-island structure is synthesized by reacting a raw material containing CaSiO3 with an alkaline earth metal gas through a reduction process. It is believed that the sea-island phase of the intermediate's sea-island structure contains Si. It is believed that the island phase of the intermediate's sea-island structure contains MgO, CaO, MgSi2, and Ca. x Mg 2-x The Si₂O₆ component (0≤x≤1) has the property of being insoluble in acids. The MgO and CaO components are readily soluble in acids. The MgSi₂ component exhibits the property of easily separating Mg upon contact with acids. Ca... x Mg 2-x The Si2O6 (0≤x≤1) component has the property of not readily reacting with acids.

[0035] Next, if an acid treatment process is performed, the intermediate becomes porous. Specifically, if the acid treatment process is performed, a portion of the island phases in the intermediate (e.g., MgO and CaO components) dissolves, thereby obtaining porous silicon. This porous silicon is considered to have a Si crystalline phase as the main phase and a Ca secondary phase. x Mg 2-x The crystal phase of Si₂O₆ (0≤x≤1). Si and Ca x Mg 2-x Si₂O₆ (0≤x≤1) is relatively hard. Specifically, the bulk modulus of Si is 110 GPa, and that of Ca... x Mg 2-x The bulk modulus of Si2O6 (0≤x≤1) is 113.6 GPa. Therefore, the fine pores of the porous silicon obtained by the manufacturing method of the present invention are not easily collapsed by pressure (e.g., the pressing pressure during the fabrication of the active material layer). It is presumed that this method produces porous silicon with excellent pressure resistance.

[0036] (1.1) Reduction process

[0037] In the reduction process, the raw material containing CaSiO3 is brought into contact with an alkaline earth metal gas. This is considered to be the synthesis of the aforementioned intermediate.

[0038] The raw material containing CaSiO3 can be composed of CaSiO3, or it can contain components different from CaSiO3 within a range that does not impair the effects of the present invention. The raw material containing CaSiO3 can be a product.

[0039] The raw material containing CaSiO3 can be a powder. The shape of the particles constituting the raw material is not particularly limited, and examples include spherical (e.g., true spherical and ellipsoidal) particles. "Spherical" refers to particles with an aspect ratio of 0.1 to 10. The average primary particle size of the raw material containing CaSiO3 can be 10 nm or more, 50 nm or more, or 150 nm or more, or it can be less than 10 μm, less than 3 μm, or less than 1 μm. A portion of the raw material containing CaSiO3 can form secondary particles. The average primary particle size is the value of D50, which is the particle size (median particle size) at the 50% cumulative value of the particle size distribution on a volume basis determined by laser diffraction scattering.

[0040] The reduction process is not particularly limited and a vacuum furnace can be used. In a vacuum furnace, for example, the internal pressure is reduced, and the interior is heated to a temperature at which alkaline earth metals produce alkaline earth metal gases. The generated alkaline earth metal gases diffuse into the furnace, come into contact with the raw materials, and thereby carry out a reduction reaction to produce intermediates.

[0041] Examples of alkaline earth metal gases include beryllium, magnesium, calcium, strontium, barium, and radium. Alkaline earth metal gases can include magnesium gas or be magnesium gas alone.

[0042] There are no particular limitations on the methods for generating alkaline earth metal gases; for example, methods for heating alkaline earth metals or their alloys can be cited.

[0043] Examples of raw materials for magnesium gas include metallic magnesium (hereinafter, metallic Mg), Mg₂Si, MgCa alloy, MgCu₂, MgNi₂, and MgSn alloy. For example, magnesium gas is produced by heating the raw materials for magnesium gas to 600°C, 650°C, 700°C, or 800°C.

[0044] The temperature of the reduction reaction is not particularly limited; for example, it can be 500℃~900℃, 550℃~750℃, or 600℃~700℃. By setting the temperature of the reduction reaction to 600℃~700℃, the average pore diameter of the manufactured porous silicon can be made smaller.

[0045] The reaction time for the reduction reaction should be appropriately selected based on the pressure and temperature conditions described above. The reaction time for the reduction reaction can be 1 hour to 48 hours, 3 hours to 24 hours, or 5 hours to 18 hours.

[0046] (1.2) Acid treatment process

[0047] In the acid treatment process, the raw material, which has been in contact with the alkaline earth metal gas, is brought into contact with acid. As a result, a portion of the island phase of the aforementioned intermediate dissolves, and the intermediate becomes porous. That is, porous silicon is obtained.

[0048] There are no particular limitations on the type of acid used; examples include hydrochloric acid, nitric acid, and sulfuric acid. The concentration of the acid used in the acid treatment process is selected appropriately based on the type of acid.

[0049] In the acid treatment process, porous silicon can be cleaned with cleaning solutions (e.g., distilled water and alcohol) as needed, or it can be dried.

[0050] (2) Porous silicon

[0051] The porous silicon of the present invention has a Si crystal phase as the main phase and a Ca phase as the secondary phase. x Mg 2-x The crystal phase of Si2O6 (0≤x≤1).

[0052] "Main phase" refers to the phase to which the largest peak in the X-ray diffraction pattern of porous silicon belongs. "Secondary phase" refers to a crystalline phase that is not the main phase.

[0053] The porous silicon of the present invention has the above-described structure, and therefore exhibits excellent pressure resistance.

[0054] This effect is inferred based on the same reasoning as that for manufacturing the aforementioned porous silicon, but is not limited thereto.

[0055] Porous silicon can be in the form of powder. The shape of the particles constituting porous silicon is not particularly limited, and examples include spherical (e.g., true spherical and ellipsoidal) shapes. The average primary particle size of porous silicon is the same as the average primary particle size exemplified as that of a raw material containing CaSiO3.

[0056] The mass ratio of the Si crystal phase to porous silicon can be above 80% by mass, above 90% by mass, above 95% by mass, below 99% by mass, or below 98% by mass.

[0057] Ca x Mg 2-x In Si2O6, x ranges from 0 to 1, and can be 0.60 to 0.90 or 0.89.

[0058] The residual Ca content in the porous silicon of the present invention is not particularly limited, and can be 0.5% to 3.0% by mass or 1.0% to 2.0% by mass relative to the total amount of porous silicon. The residual Mg content in the porous silicon of the present invention is not particularly limited, and can be 0.2% to 2.0% by mass or 0.5% to 1.0% by mass relative to the total amount of porous silicon. The methods for determining the residual Ca and residual Mg content are the same as those described in the examples.

[0059] The porous silicon of the present invention preferably has a pore volume of 0.2 cm³, as determined by the Barrett-Joyner-Halenda method (hereinafter also referred to as the "BJH method"). 3 / g or more, preferably 0.3cm 3 / g or more, can be 1.0cm 3 Below / g, it can also be 0.5cm 3 / g or less. The pore volume of porous silicon is 0.2cm³. 3 Porosity of porous silicon increases with a volume of / g or more. The method for determining the fine pore volume is the same as that described in the examples.

[0060] The preferred BET specific surface area of ​​the porous silicon of the present invention is 70 m². 2 / g or more, preferably 100m 2 / g or more, can be 200m 2 Below / g, it can also be 150m 2 / g or less. The BET specific surface area of ​​porous silicon is 70m². 2 With a porosity of 6g or higher, a negative electrode layer exhibiting excellent resistance to pressure applied during the manufacturing process of secondary batteries can be formed. That is, in a negative electrode layer using this porous silicon as the negative electrode active material, a high porosity can be maintained even when pressed under specified pressure during the manufacturing process of secondary batteries.

[0061] The porous silicon of the present invention is preferably used as the negative electrode active material in secondary batteries such as lithium-ion batteries. The fine pores of the porous silicon of the present invention are not easily collapsed by pressure (e.g., the pressing pressure during the fabrication of the active material layer). Therefore, the volume expansion of the negative electrode layer using this porous silicon as the negative electrode active material is suppressed during charging and discharging. Therefore, by using the porous silicon of the present invention, stable battery characteristics can be maintained.

[0062] (3) Secondary battery

[0063] The secondary battery of the present invention comprises: a negative electrode layer; a positive electrode layer; and an electrolyte layer disposed between the negative electrode layer and the positive electrode layer. The negative electrode layer has a negative electrode current collector and a negative electrode active material layer disposed on one or both sides of the negative electrode current collector. The negative electrode active material layer comprises the porous silicon of the present invention.

[0064] The secondary battery of the present invention has the above-described structure, thus suppressing the expansion of the negative electrode active material layer during charging. Therefore, even with repeated alternating charging and discharging, the battery performance of the solid-state battery of the present invention is not easily degraded.

[0065] The electrolyte layer is typically located between the positive and negative electrode layers and contains an ion conductor that carries carrier ions (e.g., lithium ions and sodium ions). Examples of ion-conducting media include solid electrolytes, non-aqueous electrolytes, non-aqueous gel electrolytes, solid ion-conducting polymers, and inorganic solid electrolytes.

[0066] The following describes a secondary battery that uses a solid electrolyte as an ion-conducting medium.

[0067] (3.1) Negative electrode layer

[0068] The negative electrode layer has a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector comprises the porous silicon (negative electrode active material) of the present invention, and may further comprise at least one of a solid electrolyte, a conductive material, and a binder, if desired.

[0069] The solid electrolyte can be any known solid electrolyte. Examples of solid electrolytes include, for example, sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes. Sulfide solid electrolytes may contain Li and S elements. Preferably, sulfide solid electrolytes contain at least one of P, Ge, Sn, and Si elements. Sulfide solid electrolytes may contain at least one of O and halogen elements (e.g., F, Cl, Br, and I elements). The solid electrolyte can be glass, glass-ceramic, or a crystalline material. Glass is obtained by amorphous treatment of the raw material composition (e.g., a mixture of Li₂S and P₂S₅). Examples of amorphous treatment include, for example, mechanical grinding. Glass-ceramic is obtained by heat treatment of glass. Crystalline materials are obtained, for example, by solid-phase reaction treatment of the raw material composition. The proportion of solid electrolyte in the negative electrode active material layer can be 20% to 80% by mass.

[0070] Examples of conductive materials include carbon materials, metal particles, and conductive polymers. Examples of carbon materials include acetylene black (AB), Ketjen black (KB), carbon fibers, carbon nanotubes (CNTs), and carbon nanofibers (VGCF). The volume ratio of the binder to the negative electrode active material layer can be 5% to 10% by volume.

[0071] Examples of adhesives include fluoride-based adhesives (e.g., polyvinylidene fluoride (PVDF)), polyimide-based adhesives, and rubber-based adhesives. The volume ratio of the adhesive to the negative electrode active material layer can be 2% to 5% by volume.

[0072] The negative current collector is the layer that collects current from the negative electrode active material layer. Examples of negative current collectors include aluminum, SUS (Steel Use Stainless), copper, nickel, and carbon. Examples of the shape of the negative current collector include, for example, a foil.

[0073] (3.2) Electrolyte layer

[0074] The electrolyte layer contains a solid electrolyte and may further contain a binder if necessary. The thickness of the solid electrolyte layer can range from 0.1 μm to 300 μm.

[0075] As a solid electrolyte, an example of a solid electrolyte that can be included in the negative electrode active material layer can be cited. The content of the solid electrolyte in the solid electrolyte layer can be 70% to 100% by mass, or 90% to 100% by mass. As a binder, an example of a binder that can be included in the negative electrode active material layer can be cited.

[0076] (3.3) Positive electrode

[0077] The positive electrode typically has a positive current collector and a layer of positive active material disposed on one or both sides of the positive current collector. The positive active material layer contains a positive active material, and may further contain at least one of a solid electrolyte, a conductive material, and a binder, if required.

[0078] Examples of positive electrode active materials include oxide active materials. Examples of oxide active materials include layered rock salt active materials (e.g., LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and LiCoO2, etc.), spinel-type active materials (e.g., LiMn2O4 and Li4Ti5O4, etc.). 12 And olivine-type active substances (e.g., LiFePO4 and LiMnPO4, etc.).

[0079] As a solid electrolyte, an example of a solid electrolyte that can be included in the negative electrode active material layer can be cited. The proportion of the solid electrolyte in the positive electrode active material layer is not particularly limited and can be 20% to 80% by mass. As a conductive material, an example of a conductive material that can be included in the negative electrode active material can be cited. The volume ratio of the binder to the positive electrode active material layer can be 5% to 10% by volume. As a binder, an example of a binder that can be included in the negative electrode active material can be cited. The volume ratio of the binder to the positive electrode active material layer can be 5% to 10% by volume.

[0080] The positive current collector is the layer that collects current from the positive electrode active material layer. Examples of positive current collectors include SUS, aluminum, nickel, iron, titanium, and carbon. Examples of the shape of the positive current collector include, for example, a foil.

[0081] (3.4) Exterior body

[0082] The secondary battery of the present invention typically includes an outer casing. The outer casing houses the positive electrode, the electrolyte layer, and the negative electrode. There are no particular limitations on the outer casing; for example, laminated outer casings and metal cans can be used.

[0083] (3.5) Implementation Method

[0084] The following is for reference. Figure 1 An example of the secondary battery of the present invention will be described below. The secondary battery 1 includes a positive electrode layer 2, a negative electrode layer 3, and an electrolyte layer 4 disposed between the positive electrode layer 2 and the negative electrode layer 3. The positive electrode layer 2 includes a positive current collector 5 and a positive active material layer 6. The negative electrode layer 3 includes a negative current collector 7 and a negative active material layer 8.

[0085] Example

[0086] The present invention will be described in more detail below using examples, but the technical scope of the present invention is not limited to the following examples.

[0087] [1] Porous silicon

[0088] [1.1] Example 1

[0089] [1.1.1] Reduction process

[0090] In a glove box filled with argon atmosphere, calcium silicate (CaSiO3, manufactured by Angene, AG00A4W0) was pulverized in a mortar for 5 minutes. Then, 0.97 g of the pulverized calcium silicate (CaSiO3) was weighed and placed in a vacuum reactor. Furthermore, 1.28 g of magnesium silicide (Mg2Si, manufactured by KOSUICHI CORPORATION) was placed below the position of the calcium silicate (CaSiO3) in the vacuum reactor. The vacuum reactor was removed from the glove box and calcined at 850°C under vacuum conditions (approximately 80 Pa) for 12 hours. This brought the calcium silicate (CaSiO3) into contact with the magnesium gas. The heating rate in the vacuum reactor was set to 10°C / minute.

[0091] [1.1.2] Acid treatment process

[0092] Next, the powder was allowed to cool naturally after the reaction. One g of the powder was mixed with 88.5 ml of a 6% (w / w) HCl aqueous solution and stirred for 1 hour, undergoing acid treatment. This brought calcium silicate (CaSiO3), which had been in contact with magnesium gas, into contact with hydrochloric acid. This operation was carried out in a simple glove box filled with argon gas. Afterward, the powder was dried in a vacuum dryer at 120°C for 12 hours in an argon-filled glove box. Thus, porous silicon powder was obtained.

[0093] [1.2] Comparative Example 1

[0094] Powdered porous silicon was obtained in the same manner as in Example 1, except that 1g of SiO2 (Kishida Chemical Co., Ltd., product code: 010-70255) was used instead of 0.97g of calcium silicate (CaSiO3) and 2.55g of magnesium silicide (Mg2Si) was used instead of 1.28g of magnesium silicide (Mg2Si).

[0095] [2] Determination method

[0096] [2.1] BET specific surface area

[0097] Nitrogen adsorption on porous silicon was measured using a Micromeritics BELSORP MAX X instrument. Adsorption isotherms were analyzed using the BET method within the range of 0.1 < P / P0 < 0.25, and the specific surface area of ​​the porous silicon (i.e., BET specific surface area) was calculated. The results are shown in Table 1.

[0098] [2.2] Fine pore volume Vp

[0099] Based on mesoporous analysis using the BJH method with gas adsorption measurements (adsorption side), the pore volume Vp of porous silicon was calculated. The results are shown in Table 1.

[0100] [2.3] Residual Ca and Residual Mg content

[0101] The porous silica was dissolved, and the residual Ca and Mg contents were quantified using ICP-AES analysis with a Shimadzu ICPS-8100. The samples were dissolved by acid treatment with nitric acid and hydrofluoric acid. The Ca concentration was calculated by comparing it with a Ca calibration curve, and the Mg concentration was calculated by comparing it with a Mg calibration curve. The results are shown in Table 1.

[0102] [2.4] X-ray crystal structure analysis

[0103] X-ray diffraction (XRD) was performed on porous silicon using an X-ray diffraction apparatus. The results are shown in Table 1 and... Figure 2 .like Figure 2 As shown, in the porous silicon of Example 1, there exists a Si crystalline phase as the main phase and a Ca phase as the secondary phase. x Mg 2-x The crystal phase of Si2O6 (x=0.89). For example... Figure 2 As shown, in the porous silicon of Comparative Example 1, the Si crystalline phase exists, but the Ca phase does not. x Mg 2- x The crystal phase of Si2O6 (0≤x≤1).

[0104] [2.5] Pore residue rate after pressing

[0105] [2.5.1] Porosity before pressing

[0106] The porosity of porous silicon (hereinafter also referred to as "porosity before pressing") was calculated using equation (a) below, based on the pore volume Vp obtained by analysis using the BJH method with gas adsorption determination results. In equation (a), the true density of Si was used as 2.33 g / cm³. 3 .

[0107] Equation (a): Porosity = Vp / (Vp + 1 / 2.33) × 100

[0108] [2.5.2] Porosity after pressing

[0109] 50 mg of porous silica was placed inside an alumina cylinder (diameter: 11.28 mm). A uniaxial press was used to press the porous silica from both above and below using pins (material: SKD11). The pressing load was 60 kN / cm². 2 .

[0110] The pore volume Vp of the pressed porous silicon was calculated in the same manner as the method for determining the "pore volume Vp" described above. Using the pore volume Vp of the pressed porous silicon, the porosity of the pressed porous silicon (hereinafter also referred to as "porosity after pressing") was calculated using the above formula (a).

[0111] [2.5.3] Calculation of porosity residual rate

[0112] Using the porosity before and after pressing, the porosity after pressing is calculated using the following formula (b). The results are shown in... Figure 3 And as shown in Table 1. The permissible porosity residue exceeds 77.09%.

[0113] Equation (b): Pore residual rate = [Pore density after pressing / Pore density before pressing] × 100

[0114] [3] Results

[0115] [Table 1]

[0116]

[0117] [3.1] Comparative Example 1

[0118] In Comparative Example 1, no raw material containing CaSiO3 was used. The porous silicon of Comparative Example 1 does not contain Ca. x Mg 2-x The crystalline phase of Si2O6 (0≤x≤1). Therefore, the porosity of porous silicon does not exceed 77.09%.

[0119] As a result, it can be seen that the manufacturing method of the porous silicon in Comparative Example 1 is not "a manufacturing method of porous silicon capable of producing porous silicon with excellent pressure resistance".

[0120] [3.2] Example 1

[0121] The method for manufacturing porous silicon in Example 1 includes the reduction step and the acid treatment step described above. The porous silicon in Example 1 has a Si crystalline phase as the main phase and a Ca secondary phase. x Mg 2-x The crystalline phase is Si2O6 (x=0.89). Therefore, the porosity of porous silicon exceeds 77.09%.

[0122] As a result, it can be seen that the manufacturing method of porous silicon in Example 1 is "a manufacturing method of porous silicon capable of producing porous silicon with excellent pressure resistance". It can be seen that the porous silicon in Example 1 is "porous silicon with excellent pressure resistance".

[0123] Symbol Explanation

[0124] 1-Secondary battery, 2-Positive electrode layer, 3-Negative electrode layer, 4-Electrolyte layer, 5-Positive current collector, 6-Positive active material layer, 7-Negative current collector, 8-Negative active material layer.

Claims

1. A method for manufacturing porous silicon, characterized in that, Includes the following steps: Contacting the raw material containing CaSiO3 with an alkaline earth metal gas; and The raw material, which is in contact with the alkaline earth metal gas, is then brought into contact with acid.

2. A porous silicon, characterized in that, It has a Si crystal phase as the main phase and Ca as the secondary phase. x Mg 2-x The crystal phase of Si2O6 (0≤x≤1).

3. The porous silicon according to claim 2, characterized in that, The pore volume, determined by the Barrett-Joyner-Halenda method, was 0.2 cm³. 3 / g or more.

4. The porous silicon according to claim 2, characterized in that, BET has a specific surface area of ​​70m². 2 / g or more.

5. A secondary battery, characterized in that, have: A negative electrode layer; a positive electrode layer; and an electrolyte layer, disposed between the negative electrode layer and the positive electrode layer. The negative electrode layer has a negative electrode current collector and a negative electrode active material layer disposed on one or two surfaces of the negative electrode current collector. The negative electrode active material layer comprises the porous silicon as described in claim 2.