A liquid precursor slurry for hydrophobic silica aerogel and its preparation method

By using a phase-separation formulation of composite surfactants and slow-release catalysts and a single-stage alcohol washing process, the problems of stable storage and atmospheric pressure drying of silica aerogel precursor slurry were solved, achieving efficient and low-cost production of hydrophobic aerogels.

CN123105665APending Publication Date: 2026-11-17HUAMIN TIANYU (HENGQIN GUANGDONG PROVINCE) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611432081.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silica aerogel precursor slurries suffer from several problems, including short shelf life at room temperature (prone to premature gelation), pore shrinkage and collapse during atmospheric pressure drying leading to cracking, the use of strong acids and alkalis to corrode equipment during production, and high production costs.

Method used

A hydrophobic silica aerogel liquid precursor slurry was prepared by using a composite surfactant system and a slow-release catalyst through phase separation formulation and a single-stage closed-loop alcohol washing process. Combined with a step-by-step drying process from atmospheric pressure to reduced pressure, stable storage and efficient production were achieved.

Benefits of technology

Stable storage of liquid precursor slurry at room temperature for up to 240 hours was achieved, reducing equipment corrosion and waste liquid treatment costs, improving material turnover efficiency in the production line, avoiding pore collapse, and preparing high-performance hydrophobic aerogel materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105665A_ABST
    Figure CN123105665A_ABST
Patent Text Reader

Abstract

This invention discloses a liquid precursor slurry for hydrophobic silica aerogel and its preparation method. The precursor slurry raw materials, by weight, include: 30.0-35.0 parts methyltrimethoxysilane, 35.0-45.0 parts deionized water, 1.0-3.0 parts glacial acetic acid, 12.0-16.0 parts urea, and 8.0-15.0 parts a composite surfactant system. During preparation, an acidic silane premix and a urea coagulation buffer are prepared separately and mixed at room temperature. In the system, the surfactant self-assembles to form mixed micelles that encapsulate the silica oligomers, significantly delaying the polycondensation reaction and achieving stable storage of the slurry at room temperature. Upon heating, the urea slowly releases ammonia gas to drive homogeneous polycondensation in the system. The wet gel is dehydrated by a single-stage closed-ring alcohol washing, and the residual ammonia gas catalyzes in-situ hydrophobic modification of the framework. Finally, the finished product is obtained through step-by-step atmospheric pressure dehydration and drying. This invention solves the problems of premature gelation of slurry and easy collapse and cracking during normal pressure drying, simplifies the production process, and eliminates the dependence on high-pressure equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanoporous thermal insulation materials technology, specifically to a liquid precursor slurry for hydrophobic silica aerogel and its preparation method. Background Technology

[0002] Due to its high porosity and extremely low thermal conductivity, silica aerogel has a wide range of applications in industrial pipeline insulation, building energy conservation and new energy thermal protection. At present, the sol-gel method is commonly used in the industrial preparation of silica aerogel. This method involves hydrolyzing and polycondensing siloxane precursors under the action of a catalyst to form a three-dimensional silica gel network, followed by solvent replacement and drying to obtain the finished product.

[0003] In existing conventional preparation systems, precursor slurries are usually prepared by directly adding highly active catalysts (such as strong acids, strong bases, or high-concentration acid-base salts). This process makes it difficult to control the hydrolysis and condensation reactions of silanes at room temperature. The precursor slurry is prone to cross-linking and solidification in a short time after preparation, making it impossible to achieve stable storage and transportation at room temperature. This forces the production line to adopt a fresh-for-use mode, which limits the time window for construction operations and the flexibility of material allocation. At the same time, strong acid and strong base environments will cause serious corrosion to conventional production equipment and metal pipelines, which will significantly increase the depreciation and maintenance costs of equipment. In addition, the treatment of reaction waste liquid also faces environmental pressure.

[0004] On the other hand, during the conventional atmospheric pressure drying stage of wet gels, the evaporation of solvent within the pores generates a huge capillary contraction force at the gas-liquid-solid interface. This stress causes severe collapse of the gel's nanopores, drastic shrinkage of the skeleton volume, and macroscopic cracking. To overcome the cracking problem, the industry usually relies on supercritical drying technology. However, this technology requires operation under high pressure and harsh conditions, resulting in large equipment investment, high energy consumption, and limited production cycles, which directly increases the manufacturing cost of aerogels. Although there are improved processes based on atmospheric pressure drying, they often require long-term, multi-level gradient static solvent replacement and surface modification of the wet gel. The overall production process is cumbersome and time-consuming, with large solvent consumption, making it difficult to meet the industrial demand for low-cost and continuous large-scale production. Summary of the Invention

[0005] The purpose of this invention is to provide a liquid precursor slurry for hydrophobic silica aerogel and its preparation method, so as to solve the technical problems of existing aerogel precursor slurries, such as short storage period at room temperature and easy premature gelation, pore shrinkage and collapse during normal pressure drying process leading to cracking, use of strong acid and strong alkali to corrode equipment in the production process, and high production cost.

[0006] To address the problems mentioned in the background art, the first aspect of the present invention provides a liquid precursor slurry for hydrophobic silica aerogels. By weight, its raw material components include: 30.0-35.0 parts of methyltrimethoxysilane; 35.0-45.0 parts of deionized water; 1.0-3.0 parts of glacial acetic acid; 12.0-16.0 parts of urea; and 8.0-15.0 parts of a composite surfactant system.

[0007] Furthermore, the composite surfactant system is composed of a combination of cationic surfactants and nonionic block copolymers. By weight, the specific composition and proportions of the composite surfactant system are: 6.0-10.0 parts of hexadecyltrimethylammonium chloride, and 2.0-5.0 parts of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer.

[0008] Furthermore, the polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer is poloxamer 407, with a number-average molecular weight between 9840 and 14600, and a polyoxyethylene fraction between 71.5% and 74.9% by mass.

[0009] Furthermore, the composite surfactant system is a pre-prepared assembly, and its preparation method includes the following steps: hexadecyltrimethylammonium chloride and polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer are added to a reaction vessel, and 10.0-15.0 parts of deionized water are added; mechanical stirring is turned on at 20-25℃, the stirring speed is set to 150-400 rpm, and stirring is continued for 45-90 min to carry out physical self-assembly, and a transparent mixed micelle dispersion is obtained, which is the composite surfactant pre-assembly.

[0010] A second aspect of the present invention provides a method for preparing a liquid precursor slurry for hydrophobic silica aerogels, comprising the following steps:

[0011] Step S1, Preparation of acidic silane premix A: Mix and stir a portion of deionized water, glacial acetic acid and the composite surfactant system, then add methyltrimethoxysilane dropwise at a uniform rate and continue stirring to obtain premix A;

[0012] Step S2, Preparation of sustained-release coagulation buffer B: Mix the remaining deionized water with urea and stir until completely dissolved to obtain coagulation buffer B;

[0013] Step S3, Homogenization and Storage: At room temperature, premixed solution A and buffer solution B are simultaneously injected into a mixing tank and mixed and stirred to form a homogeneous and stable liquid precursor slurry.

[0014] Step S4, isothermal triggering and gel curing: Inject the liquid precursor slurry into a sealed mold or immerse it in a hydrophilic fiber substrate, move it into a temperature control device, heat it to the isothermal triggering zone and keep it at that temperature to complete the wet gel curing.

[0015] Step S5, Single-stage closed-loop alcohol washing and skeleton consolidation: Connect the container containing the wet gel to the closed solvent circulation washing device, inject anhydrous methanol or anhydrous ethanol as the circulation replacement medium, and perform continuous single-stage closed-loop rinsing.

[0016] Step S6, Gradient Dehydration and Drying at Normal Pressure: The washed wet gel is transferred into an adjustable vacuum drying oven at normal pressure and dried in a stepwise manner from normal pressure to reduced pressure. After cooling, pure blocky hydrophobic silica aerogel body or aerogel composite insulation product is obtained.

[0017] Furthermore, in step S1, the temperature is controlled in the range of 20-25℃, and the pH value of the system is controlled in the range of 2.5-3.5. The addition method of methyltrimethoxysilane is as follows: it is added dropwise at a rate of 1.0-2.0 parts / min using a constant flow pump. After the addition is completed, the speed is increased to 300-400 rpm and stirring is continued for 30-45 min.

[0018] Furthermore, in step S3, the mixing speed is set to 200-350 rpm and the mixing time is 30-40 min; the resulting liquid precursor slurry is sealed and stored in an environment of 15-25℃, and its stable storage period can reach 240 h.

[0019] Furthermore, in step S4, the heating rate is controlled at 1.5-2.5℃ / min, the temperature of the isothermal triggering zone is 65-75℃, and the holding time is 10-16 h; the hydrophilic fiber substrate is high silica glass fiber cloth or ceramic fiber cotton.

[0020] Furthermore, in step S5, the temperature of the circulating solvent is controlled to be constant at 45-55℃, the pressure of the system pipeline is controlled at 0.1-0.2 MPa, the solvent circulation flow rate is set to 180-220 L / min, the cross-sectional flow velocity of the circulation pipeline is controlled at 0.5-1.5 m / s, and the total duration of continuous single-stage circulation rinsing is 8-12 h.

[0021] Further, in step S6, the specific implementation of the step-by-step drying process from atmospheric pressure to reduced pressure is as follows: the first stage is atmospheric pressure desolventizing, where the chamber temperature is raised to 60-70℃ under an ambient pressure of 0.1 MPa, and the drying is carried out at a constant temperature for 120-180 min; the second stage is low vacuum deep drying, where the vacuum pump is turned on to slowly reduce the absolute pressure to 3000-5000 Pa, and then the drying temperature is raised to 80-100℃, and the drying is carried out at a constant temperature for 90-150 min.

[0022] The present invention, by adopting the above technical solution, can bring the following beneficial effects:

[0023] 1. This invention constructs a composite surfactant system using hexadecyltrimethylammonium chloride and poloxamer 407, combined with a slow-release catalytic system composed of glacial acetic acid and urea. This allows the precursor slurry to maintain stable storage for up to 240 hours in a sealed environment at 15-25℃ without premature gelation. The phase separation preparation and the gentle hydrolysis of urea avoid local pH changes and internal stress concentration caused by the instantaneous neutralization of strong acids and bases, thus reducing the wet gel cracking rate. At the same time, the weak acid and slow-release weak base system reduces the corrosiveness of the reaction waste liquid. Conventional stainless steel equipment resistant to weak acid corrosion (such as 316L) can meet the production requirements, reducing equipment investment and waste liquid treatment costs.

[0024] 2. This invention employs a single-stage closed-loop alcohol circulation rinsing process. Warm alcohol washing solution removes free water from the pores of the wet gel, while urea decomposes residual trace amounts of ammonia in the pores to create a slightly alkaline environment. This promotes secondary condensation of unreacted silanol groups on the skeleton surface, consolidating the hydrophobic structure of the skeleton. Compared to traditional multi-stage gradient static immersion replacement, this process combines solvent replacement with in-situ hydrophobic modification, eliminating the need for multi-stage disassembly and transport steps. This shortens the replacement and cleaning cycle to 8-12 hours, improving production line material turnover efficiency and reducing solvent evaporation loss.

[0025] 3. This invention imparts high-density methyl groups to the framework through in-situ hydrophobic modification, combined with a step-by-step drying process from atmospheric pressure to reduced pressure. This increases the interfacial contact angle during the solvent evaporation process, significantly reduces capillary shrinkage stress, and avoids pore collapse and volume shrinkage during atmospheric pressure drying. It eliminates the need for supercritical high-pressure drying equipment. The pure aerogel body and composite insulation products obtained by atmospheric pressure drying retain the complete nanoporous structure, with a room temperature thermal conductivity of 0.018-0.020 W / (m·K) and a hydrophobicity greater than 99%. This enables the large-scale preparation of high-performance hydrophobic aerogel materials under low-cost atmospheric pressure conditions. Attached Figure Description

[0026] Figure 1 This is a process flow diagram for preparing the liquid precursor slurry for hydrophobic silica aerogel of the present invention;

[0027] Figure 2 This is a schematic diagram of the microstructure of the liquid precursor slurry and the gel phase transition mechanism of the present invention;

[0028] Figure 3 The graphs show the dynamic viscosity of the slurry as a function of time in the various embodiments and comparative examples of this invention.

[0029] Figure 4 This is a bar chart comparing the wet gel cracking rates of various embodiments and comparative examples of the present invention;

[0030] Figure 5 This is a bar chart comparing the room temperature thermal conductivity of various embodiments and comparative examples of the present invention;

[0031] Figure 6 This is a comparison chart of the bulk density of the aerogel products of various embodiments and comparative examples of the present invention;

[0032] Figure 7 This is a comparison chart of the hydrophobicity of the aerogel products in various embodiments and comparative examples of the present invention. Detailed Implementation

[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] Please see the appendix Figure 1-7 This invention provides a liquid precursor slurry for hydrophobic silica aerogel and its preparation method.

[0035] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.

[0036] Methyltrimethoxysilane, CAS No. 1185-55-3, molecular formula Purity ≥ 98%;

[0037] Glacial acetic acid, CAS No. 64-19-7, molecular formula Purity ≥ 99%;

[0038] Urea, CAS No. 57-13-6, molecular formula Analytical grade, purity ≥ 99%;

[0039] Hexadecyltrimethylammonium chloride, CAS No. 112-02-7, molecular formula Purity ≥ 99%;

[0040] Poloxamer 407, also known as polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer, CAS number 9003-11-6, is a nonionic polymeric surfactant with the general structural formula [insert structural formula here]. Where a is approximately 101, b is approximately 56, the average molecular weight is distributed between 9840 and 14600, and the mass fraction of polyoxyethylene is approximately 71.5% to 74.9%;

[0041] Anhydrous methanol, CAS No. 67-56-1, molecular formula Analytical grade, purity ≥ 99.5%;

[0042] Anhydrous ethanol, CAS No. 64-17-5, molecular formula Analytical grade, purity ≥ 99.5%;

[0043] Deionized water, prepared in the laboratory, conductivity ≤0.1μS / cm;

[0044] High-silica fiberglass cloth, commercially available industrial grade, 3mm thick, 300g / L areal density. ;

[0045] Ceramic fiber cotton, commercially available industrial grade, 10mm thick, density 128kg / m³ .

[0046] Preparation Example

[0047] Preparation Example 1:

[0048] This preparation example provides a pre-assembled composite surfactant, comprising the following steps:

[0049] Add 8.0 parts of hexadecyltrimethylammonium chloride and 3.5 parts of poloxamer 407 to a stainless steel mixing tank resistant to weak acid corrosion, and add 13.0 parts of deionized water;

[0050] At room temperature (20-25℃), turn on the mechanical stirrer and set the stirring speed to 300 rpm;

[0051] After stirring continuously for 60 minutes, the cationic and nonionic surfactants are fully dissociated in the aqueous phase by high shear force, and the water and molecules undergo physical self-assembly to obtain a homogeneous and transparent mixed micelle dispersion with high viscosity but fluidity, which is the pre-assembled composite surfactant for later use.

[0052] Preparation Example 2:

[0053] This preparation example provides a pre-assembled composite surfactant, comprising the following steps:

[0054] Add 6.0 parts of hexadecyltrimethylammonium chloride and 2.0 parts of poloxamer 407 to a stainless steel mixing tank resistant to weak acid corrosion, and add 10.0 parts of deionized water;

[0055] At room temperature (20-25℃), turn on the mechanical stirrer and set the stirring speed to 250 rpm;

[0056] Stir continuously for 45 minutes to allow the cationic and nonionic surfactants to fully dissociate in the aqueous phase and undergo physical self-assembly, resulting in a homogeneous and transparent mixed micelle dispersion with flowability, i.e., a pre-assembled composite surfactant for later use.

[0057] Preparation Example 3:

[0058] This preparation example provides a pre-assembled composite surfactant, comprising the following steps:

[0059] Add 10.0 parts of hexadecyltrimethylammonium chloride and 5.0 parts of poloxamer 407 to a stainless steel mixing tank resistant to weak acid corrosion, and add 15.0 parts of deionized water;

[0060] At room temperature (20-25℃), turn on the mechanical stirrer and set the stirring speed to 400 rpm;

[0061] Stir continuously for 90 minutes to allow the cationic and nonionic surfactants to fully dissociate in the aqueous phase, and the water and molecules to undergo physical self-assembly, resulting in a homogeneous and transparent mixed micelle dispersion with high viscosity but good flowability, which is the pre-assembled composite surfactant for later use.

[0062] Example

[0063] Example 1:

[0064] This embodiment provides a method for preparing a pure bulk hydrophobic silica aerogel and its liquid precursor slurry, using intermediate parameters, and includes the following steps:

[0065] Step S1: Preparation of acidic silane premix A: At 25°C, the composite surfactant pre-assembly obtained in Preparation Example 1 was added to a stainless steel mixing tank resistant to weak acid corrosion. 2.0 parts of glacial acetic acid were added, and mechanical stirring was started at 150 rpm for 20 min. At this time, the pH value of the system was in the range of 2.5 to 3.5. Then, 32.5 parts of methyltrimethoxysilane were added dropwise at a rate of 1.5 parts / min using a constant flow pump. After the addition was completed, the speed was increased to 350 rpm, and stirring was continued at 25°C for 40 min to obtain a homogeneous and stable premix A.

[0066] Step S2, Preparation of sustained-release coagulation buffer B: In another 25°C stainless steel container resistant to weak acid corrosion, add 27.0 parts of deionized water, then add 14.0 parts of urea at a uniform rate, turn on the mechanical stirrer, set the speed to 200 rpm, and continue stirring for 25 minutes until the urea is completely dissolved to obtain coagulation buffer B.

[0067] Step S3, Homogenization and Stabilization of Slurry: At 25°C, premixed solution A and buffer solution B are simultaneously injected into a homogenization mixing tank and mixed at 300 rpm for 35 min to form a homogenized and stable liquid precursor silica sol slurry. The slurry is then sealed and stored in an environment of 20°C to 25°C, maintaining the liquid mobile phase structure.

[0068] Step S4, isothermal triggering and gel curing: The above liquid precursor slurry is directly injected into a sealed mold, moved into a programmable temperature control device, and the ambient temperature is raised to 70°C at a heating rate of 2.0°C / min. The mixture is kept at a constant temperature for 12 hours to trigger homogeneous curing of the system and obtain a three-dimensional silica wet gel.

[0069] Step S5, Single-stage closed-loop alcohol washing and skeleton consolidation: Connect the container containing the wet gel to a closed solvent circulation washing device, inject anhydrous methanol as the circulation replacement medium, control the temperature of the circulating solvent to be constant at 50℃, control the pressure of the system pipeline to be controlled at 0.15MPa, set the solvent circulation flow rate to 200L / min, control the cross-sectional flow velocity to 1.0m / s, and continuously perform single-stage circulation washing for 10h;

[0070] Step S6, Gradient Dehydration and Drying at Normal Pressure: The washed wet gel is transferred into an adjustable vacuum drying oven at normal pressure. The temperature of the oven is raised to 65°C under an ambient pressure of 0.1 MPa and dried at a constant temperature for 150 min. Then, the vacuum pump is turned on to slowly reduce the absolute pressure to 4000 Pa and raise the drying temperature to 90°C. The drying is continued at a constant temperature for 120 min. After drying, the oven is allowed to cool naturally to 25°C to obtain a pure blocky hydrophobic silica aerogel body.

[0071] Example 2:

[0072] This embodiment provides a method for preparing an aerogel composite glass fiber insulation product and its liquid precursor slurry, using lower limit parameters, and includes the following steps:

[0073] Step S1: Preparation of acidic silane premix A: At 20°C, the composite surfactant pre-assembly obtained in Preparation Example 2 was added to a stainless steel mixing tank resistant to weak acid corrosion. 1.0 part of glacial acetic acid was added, and mechanical stirring was started at 100 rpm for 30 min. Then, 30.0 parts of methyltrimethoxysilane were added dropwise at a rate of 1.0 part / min using a constant flow pump. After the addition was completed, the speed was increased to 300 rpm, and stirring was continued at 20°C for 45 min to obtain a homogeneous and stable premix A.

[0074] Step S2, Preparation of sustained-release coagulation buffer B: In another stainless steel container resistant to weak acid corrosion at 20°C, add 25.0 parts of deionized water, then add 12.0 parts of urea at a uniform rate, turn on the mechanical stirrer, set the speed to 150 rpm, and continue stirring for 30 minutes until the urea is completely dissolved to obtain coagulation buffer B.

[0075] Step S3, Homogenization and Stabilization of Slurry: At 20°C, premixed solution A and buffer solution B are simultaneously injected into a homogenization mixing tank and mixed at 200 rpm for 40 min to form a homogenized and stable liquid precursor silica sol slurry.

[0076] Step S4, isothermal triggering and gel curing: Keep the slurry in liquid state and directly immerse it in the high silica glass fiber cloth substrate under normal pressure to make the slurry completely penetrate the fiber pores. Transfer it to a sealed container and move it into a programmable temperature control device to raise the ambient temperature to 65°C at a heating rate of 1.5°C / min. Keep it at a constant temperature for 15 hours to trigger the homogeneous curing of the system and obtain aerogel composite glass fiber wet gel.

[0077] Step S5, Single-stage closed-loop alcohol washing and skeleton consolidation: Connect the container containing the composite wet gel to a closed solvent circulation flushing device, inject anhydrous ethanol as the circulation replacement medium, control the temperature of the circulating solvent to be constant at 45℃, control the pressure of the system pipeline to be controlled at 0.1MPa, set the solvent circulation flow rate to 180L / min, control the cross-sectional flow velocity to 0.8m / s, and continuously perform single-stage circulation flushing for 12h;

[0078] Step S6, Gradient Dehydration and Drying at Normal Pressure: The washed composite wet gel is transferred into an adjustable vacuum drying oven at normal pressure. The temperature of the oven is raised to 60°C under an ambient pressure of 0.1 MPa and dried at a constant temperature for 180 min. Then, the vacuum pump is turned on to slowly reduce the absolute pressure to 3000 Pa and raise the drying temperature to 80°C. The drying is continued at a constant temperature for 150 min. After drying, the oven is allowed to cool naturally to 20°C to obtain the aerogel composite glass fiber insulation product.

[0079] Example 3:

[0080] This embodiment provides a method for preparing a pure bulk hydrophobic silica aerogel and its liquid precursor slurry, using upper limit parameters, and includes the following steps:

[0081] Step S1: Preparation of acidic silane premix A: At 25°C, the composite surfactant pre-assembly obtained in Preparation Example 3 was added to a stainless steel mixing tank resistant to weak acid corrosion. 3.0 parts of glacial acetic acid were added, and mechanical stirring was started at 200 rpm for 20 min. Then, 35.0 parts of methyltrimethoxysilane were added dropwise at a rate of 2.0 parts / min using a constant flow pump. After the addition was completed, the speed was increased to 400 rpm, and stirring was continued at 25°C for 30 min to obtain a homogeneous and stable premix A.

[0082] Step S2, Preparation of sustained-release coagulation buffer B: In another 25°C stainless steel container resistant to weak acid corrosion, add 30.0 parts of deionized water, then add 16.0 parts of urea at a uniform rate, turn on the mechanical stirrer, set the speed to 250 rpm, and continue stirring for 20 minutes until the urea is completely dissolved to obtain coagulation buffer B.

[0083] Step S3, Homogenization and Stabilization of Slurry: At 25°C, premixed solution A and buffer solution B are simultaneously injected into a homogenization mixing tank and mixed at 350 rpm for 30 min to form a homogenized and stable liquid precursor silica sol slurry.

[0084] Step S4, isothermal triggering and gel curing: The above liquid precursor slurry is directly injected into a sealed mold, moved into a programmable temperature control device, and the ambient temperature is raised to 75°C at a heating rate of 2.5°C / min. The mixture is kept at a constant temperature for 10 hours to trigger homogeneous curing of the system and obtain a three-dimensional silica wet gel.

[0085] Step S5, Single-stage closed-loop alcohol washing and skeleton consolidation: Connect the container containing the wet gel to the closed solvent circulation washing device, inject anhydrous methanol as the circulation replacement medium, control the temperature of the circulating solvent to be constant at 55℃, control the pressure of the system pipeline to be controlled at 0.2MPa, set the solvent circulation flow rate to 220L / min, control the cross-sectional flow velocity to 1.2m / s, and continuously perform single-stage circulation washing for 8 hours;

[0086] Step S6, Gradient Dehydration and Drying at Normal Pressure: The washed wet gel is transferred into an adjustable vacuum drying oven at normal pressure. The temperature of the oven is raised to 70°C under an ambient pressure of 0.1 MPa and dried at a constant temperature for 120 min. Then, the vacuum pump is turned on to slowly reduce the absolute pressure to 5000 Pa and raise the drying temperature to 100°C. The drying is continued at a constant temperature for 90 min. After drying, the oven is allowed to cool naturally to 25°C to obtain a pure blocky hydrophobic silica aerogel body.

[0087] Example 4:

[0088] This embodiment provides a method for preparing an aerogel composite ceramic fiber thermal insulation product and its liquid precursor slurry, and uses intermediate mixing parameters to test its broad rheological applicability, including the following steps:

[0089] Step S1, Preparation of acidic silane premix A: At 25°C, the composite surfactant pre-assembly obtained in Preparation Example 1 was added to a stainless steel mixing tank resistant to weak acid corrosion. 2.0 parts of glacial acetic acid were added, and mechanical stirring was started at 150 rpm for 20 min. Then, 33.0 parts of methyltrimethoxysilane were added dropwise at a rate of 1.5 parts / min using a constant flow pump. After the addition was completed, the stirring speed was increased to 350 rpm, and stirring was continued at 25°C for 40 min to obtain premix A.

[0090] Step S2, Preparation of sustained-release coagulation buffer B: Add 27.0 parts of deionized water and 14.0 parts of urea to another 25℃ weak acid corrosion resistant stainless steel container, and stir continuously at 200 rpm for 25 min to obtain coagulation buffer B.

[0091] Step S3, Homogenization and Stabilization of Slurry: At 25°C, premixed solution A and buffer solution B are simultaneously injected into a homogenization mixing tank and mixed at 300 rpm for 35 min to form a homogenized and stable liquid precursor silica sol slurry.

[0092] Step S4, isothermal triggering and gel curing: Keep the slurry in liquid state and directly impregnate it into the ceramic fiber cotton substrate under normal pressure. Utilize the fluidity of the slurry to completely penetrate the deep pores of the fiber substrate. Transfer it to a sealed container and then to a temperature control device. Increase the temperature to 70°C at 2.0°C / min and keep it at a constant temperature for 12 hours to obtain aerogel composite ceramic fiber wet gel.

[0093] Step S5, Single-stage closed-loop alcohol washing and skeleton consolidation: Connect the container containing the composite wet gel to the device, inject anhydrous methanol, control the temperature at 50℃, the pressure at 0.15MPa, the flow rate at 200L / min, control the cross-sectional flow velocity at 1.0 m / s, and continuously rinse for 10h.

[0094] Step S6, atmospheric pressure gradient dehydration and drying: The chamber is heated to 65℃ and dried for 150 min under an ambient pressure of 0.1 MPa; then vacuumed to 4000 Pa and heated to 90℃ for another 120 min. After cooling, the aerogel composite ceramic fiber insulation product is obtained.

[0095] The microscopic mechanism and physicochemical effects of the liquid precursor slurry of this invention are as follows:

[0096] Microscopic core-shell structure construction and room temperature stability mechanism: In an acidic aqueous environment (pH 2.5-3.5) regulated by glacial acetic acid, hexadecyltrimethylammonium chloride and poloxamer 407 self-assemble to form mixed micelles; the silicon oligomers generated by the hydrolysis of methyltrimethoxysilane are encapsulated by the mixed micelles to form a microscopic core-shell structure; the hydrophilic segments on the outer layer of the micelles isolate the silanol groups through steric hindrance, significantly delaying the collision and condensation reaction between the silanol groups, so that the slurry maintains a kinetic stable state in a closed environment at room temperature of 15-25℃, achieving stable storage for up to 240 hours while maintaining fluidity, without stratification or precipitation.

[0097] Thermally triggered phase transition and homogeneous polycondensation mechanism: When the system is heated to 65-75℃, urea undergoes a slow hydrolysis reaction and releases ammonia gas gradually within 10-16 hours of heat preservation, driving a steady increase in the pH value of the system. The increase in pH value disrupts the phase structure of the mixed micelles, causing the core-shell structure to demulsify, and the coated silanol groups are synchronously and uniformly exposed throughout the system. Under alkaline conditions, the silanol groups undergo dehydration condensation reactions and crosslink to form a three-dimensional silica network framework. Because the alkaline substances are generated gradually within the system rather than being suddenly added from the outside, the internal stress caused by local concentration differences and acid-base neutralization is avoided, reducing the probability of cracking of the wet gel.

[0098] Furthermore, using the above preparation method, the reaction mechanism during each step is as follows:

[0099] Phase-separated preparation and controlled hydrolysis reaction: Steps S1 and S2 are prepared independently in separate phases; in step S1, glacial acetic acid provides a weakly acidic environment to control the hydrolysis of methyltrimethoxysilane at a slow rate, generating silanetriol and oligomers; the urea solution prepared in step S2 does not undergo hydrolysis at room temperature and remains neutral; when solution A and solution B are mixed in step S3, the system does not undergo a violent neutralization reaction, avoiding disordered rapid gelation caused by drastic temperature rise and pH change.

[0100] In-situ autocatalysis and removal of bound water by the washing solution: In step S5, anhydrous methanol or anhydrous ethanol flows through the wet gel channels at 45-55℃ and 0.1-0.2 MPa, removing free water inside the pores and effectively extracting and removing the surfactant micelle template wrapped around the framework; at the same time, the trace amount of ammonia gas remaining in the wet gel channels after urea decomposition in step S4 dissolves in the circulating alcohol washing solution, forming a slightly alkaline environment; when the slightly alkaline alcohol washing solution flows through the framework interface, it acts as a catalyst to promote the dehydration and methanol condensation of the incompletely reacted silanol and methoxy groups on the framework surface, consolidating the hydrophobic structure of the framework and removing bound water inside the pores.

[0101] Low capillary force and anti-collapse drying: In the step-drying process of step S6, the first stage removes low-boiling-point alcohol solvents from the pores at 60-70℃ and atmospheric pressure; step S5 achieves sufficient replacement of water by low surface tension alcohols, and a high-density methyl hydrophobic layer is formed on the surface of the framework, increasing the liquid-solid interface contact angle and significantly reducing capillary shrinkage stress. In the second stage, residual solvents are desorbed at 80-100℃ and 3000-5000 Pa negative pressure. The gel framework is sufficient to resist capillary shrinkage stress, avoiding pore structure collapse and volume shrinkage during atmospheric pressure drying, and preserving the nanoporous structure.

[0102] Comparative Example

[0103] Comparative Example 1:

[0104] Compared with Example 1, the difference is that the phase separation preparation process of premixed solution A and buffer solution B is not used. Instead, a single-tank one-step feeding method is used, in which all raw materials and deionized water in the formula are added to the mixing tank at 25°C for mixing and stirring. The rest are the same.

[0105] Comparative Example 2:

[0106] Compared with Example 1, the difference is that urea was not added. Instead, after the liquid precursor slurry was prepared, concentrated ammonia was directly added to the system to adjust the pH value to weakly alkaline (pH 7.5-8.0) to trigger gelation. The constant temperature standing and heating step was not performed. All other steps were the same.

[0107] Comparative Example 3:

[0108] Compared with Example 1, the difference is that the pre-assembled composite surfactant obtained in Example 1 is not added to the formulation, but instead an equal weight of deionized water is added as a substitute; otherwise, they are the same.

[0109] Comparative Example 4:

[0110] Compared with Example 1, the difference is that step S5 does not use a single-stage closed-loop alcohol wash, but instead uses a conventional gradient static immersion method, that is, the wet gel is statically immersed and replaced at room temperature for 24 hours in turn with deionized water, 50% methanol aqueous solution, and 100% anhydrous methanol, while the rest are the same.

[0111] Test case

[0112] Test Example 1

[0113] This test case mainly verifies the rheological stability of the precursor slurry under normal temperature conditions and its controlled thermal response curing characteristics.

[0114] The liquid precursor slurries from Examples 1 to 3 and Comparative Examples 2 to 3 were used as test samples. The dynamic viscosity of the slurries was measured after 0 hours, 48 ​​hours, 120 hours and 240 hours of storage at a constant temperature of 25°C using an NDJ digital rotational viscometer. Equal amounts of each group of slurry samples were placed in a sealed mold and allowed to stand at 25°C and a set trigger temperature, respectively. The time it took for the system to lose its mobile phase characteristics and form a continuous solid network was recorded as the gel time.

[0115] Table 1. Test results of rheological stability and gel curing time of liquid precursor slurry

[0116]

[0117] Note: The viscosity data of Comparative Example 2 at 48h, 120h and 240h in Table 1 are marked as "-", indicating that the sample had completely cross-linked and cured and lost its fluidity before this time point, and was outside the testing range of the rotational viscometer.

[0118] As shown in Table 1, the dynamic viscosity of the example showed a small increase after being placed at 25°C for 240 hours, maintaining a liquid mobile phase. In the system, cationic and nonionic surfactants assembled in the aqueous phase to form mixed micelles, creating a steric hindrance effect on the silane hydrolysis oligomers and inhibiting the condensation reaction rate of silanol groups at room temperature. Comparative Example 2 used ammonia to adjust the pH, resulting in rapid crosslinking within minutes at room temperature. In Comparative Example 3, after removing the composite surfactant, the viscosity increased rapidly over time. When the example was heated to the set trigger temperature, urea hydrolysis released ammonia, increasing the pH of the system, disrupting the mixed micelle equilibrium, exposing and crosslinking the silanol groups, thus completing controlled curing.

[0119] Test Example 2

[0120] This test case primarily verifies the molding quality and core physical thermal insulation performance of the final product.

[0121] The physicochemical properties of the silica aerogel products or composite products prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were characterized. The number of macroscopic cracks during the demolding process of the wet gel was recorded, and the cracking rate of each batch of samples was calculated. The bulk density of the final product was determined by a tap density meter according to the national standard GB / T 5162. The thermal conductivity of the samples at room temperature (25℃) was tested using a transient planar heat source thermal conductivity meter. The volume hydrophobicity of the samples was calculated by immersion in water and weighing according to the standard GB / T 10299.

[0122] Table 2. Test results of physicochemical properties and molding quality of silica aerogel

[0123]

[0124] According to test data, Comparative Example 1, single-tank feeding caused local pH fluctuations, and the cross-linked network generated internal stress, leading to an increased cracking rate and decreased thermal insulation performance of the wet gel. The embodiment used a phase-separated formulation combined with urea slow release, resulting in uniform silica network growth, reduced residual stress in the skeleton, and improved molding integrity. Comparative Example 4 used a gradient static immersion method, where the solvent replacement within the pores exhibited gradient differences. During atmospheric pressure solvent removal, the micropores collapsed due to capillary forces, leading to increased material density and thermal conductivity. The embodiment used a single-stage circulating cleaning method, which not only efficiently removed free water but, more importantly, the dynamic circulating fluid uniformly dissolved and distributed the trace amounts of residual ammonia gas in the deep pores of the wet gel throughout the cleaning system, forming a stable slightly alkaline environment. This effectively catalyzed in-situ hydrophobic bonding of unreacted groups on the skeleton surface. The strong skeleton, combined with the dehydrated pore environment, resisted the shrinkage stress during atmospheric pressure drying. The finished product retained its porous structure and possessed both thermal insulation and hydrophobic properties.

Claims

1. A liquid precursor slurry for hydrophobic silica aerogel, characterized in that, The raw material components, by weight, include: 30.0-35.0 parts of methyltrimethoxysilane; 35.0-45.0 parts of deionized water; 1.0-3.0 parts of glacial acetic acid; Urea 12.0-16.0 parts; The composite surfactant system consists of 8.0-15.0 parts.

2. The liquid precursor slurry for hydrophobic silica aerogel according to claim 1, characterized in that: The composite surfactant system is composed of cationic surfactants and nonionic block copolymers. By weight, the specific composition and ratio of the composite surfactant system are: 6.0-10.0 parts of hexadecyltrimethylammonium chloride and 2.0-5.0 parts of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer.

3. The liquid precursor slurry for hydrophobic silica aerogel according to claim 2, characterized in that: The polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer is poloxamer 407, with a number-average molecular weight between 9840 and 14600, and a polyoxyethylene fraction between 71.5% and 74.9% by mass. Its general structural formula is... .

4. The liquid precursor slurry for hydrophobic silica aerogel according to claim 2, characterized in that, The composite surfactant system is a pre-prepared assembly, and its specific preparation method includes the following steps: hexadecyltrimethylammonium chloride and polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer are put into a reaction vessel, and 10.0-15.0 parts of the deionized water are added; mechanical stirring is turned on at 20-25°C, the stirring speed is set to 150-400 rpm, and stirring is continued for 45-90 min to carry out physical self-assembly, and a transparent mixed micelle dispersion is obtained, which is the composite surfactant pre-assembly.

5. A method for preparing a liquid precursor slurry for hydrophobic silica aerogel as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Step S1, Preparation of acidic silane premix A: Mix and stir a portion of the deionized water, glacial acetic acid and the composite surfactant system, then add methyltrimethoxysilane dropwise at a uniform rate and continue stirring to obtain premix A; Step S2, Preparation of sustained-release coagulation buffer B: Mix the remaining deionized water with urea and stir until completely dissolved to obtain coagulation buffer B; Step S3, Homogenization and Stabilization of Slurry: At room temperature, the premixed liquid A and buffer solution B are simultaneously injected into a mixing tank and mixed and stirred to form a homogeneous and stable liquid precursor slurry. Step S4, isothermal triggering and gel curing: The liquid precursor slurry is injected into a sealed mold or immersed in a hydrophilic fiber substrate, moved into a temperature control device, heated to the isothermal triggering zone and kept at that temperature to complete wet gel curing. Step S5, Single-stage closed-loop alcohol washing and framework consolidation: Connect the container containing the wet gel to a closed solvent circulation washing device, inject anhydrous methanol or anhydrous ethanol as the circulation replacement medium, and use the urea decomposition products remaining in the wet gel channels to make the alcohol washing solution slightly alkaline, and perform continuous single-stage closed-loop rinsing to promote secondary condensation on the framework surface. Step S6, Gradient Dehydration and Drying at Normal Pressure: The washed wet gel is transferred into an adjustable vacuum drying oven at normal pressure and dried in a stepwise manner from normal pressure to reduced pressure. After cooling, pure blocky hydrophobic silica aerogel body or aerogel composite insulation product is obtained.

6. The method for preparing the liquid precursor slurry for hydrophobic silica aerogel according to claim 5, characterized in that, In step S1: the temperature is controlled in the range of 20-25℃, and the pH value of the system is controlled in the range of 2.5-3.5; The methyltrimethoxysilane is added by using a constant flow pump at a rate of 1.0-2.0 parts / min, and after the addition is complete, the speed is increased to 300-400 rpm and stirring is continued for 30-45 min.

7. The method for preparing the liquid precursor slurry for hydrophobic silica aerogel according to claim 5, characterized in that, In step S3: the mixing speed is set to 200-350 rpm, and the mixing time is 30-40 min; The resulting liquid precursor slurry is sealed and stored in an environment of 15-25℃, where it can be stably stored for up to 240 hours.

8. The method for preparing the liquid precursor slurry for hydrophobic silica aerogel according to claim 5, characterized in that, In step S4: the heating rate is controlled at 1.5-2.5℃ / min, the temperature of the constant temperature triggering zone is 65-75℃, and the holding time is 10-16 h; The hydrophilic fiber substrate is high-silica glass fiber cloth or ceramic fiber cotton.

9. The method for preparing the liquid precursor slurry for hydrophobic silica aerogel according to claim 5, characterized in that, In step S5, the process parameters for the continuous single-stage closed-loop rinsing are: controlling the temperature of the circulating solvent to be constant at 45-55℃, and controlling the pressure of the system pipeline at 0.1-0.2 MPa; The solvent circulation flow rate is set to 180-220 L / min, the cross-sectional flow velocity of the circulation pipeline is controlled at 0.5-1.5 m / s, and the total duration of continuous single-stage circulation flushing is 8-12 h.

10. The method for preparing the liquid precursor slurry for hydrophobic silica aerogel according to claim 5, characterized in that, In step S6, the specific implementation of the stepped drying process from atmospheric pressure to reduced pressure is as follows: First stage: atmospheric pressure desolventizing: under ambient pressure The chamber temperature is then raised to 60-70℃ and kept at a constant temperature for 120-180 minutes. The second stage is low-vacuum deep drying: turn on the vacuum pump to slowly reduce the absolute pressure to 3000-5000 Pa, then raise the drying temperature to 80-100℃ and continue to dry at a constant temperature for 90-150 min.