A mechanical activation method for preparing ultrafine high-purity alumina
By using mechanical activation and low-temperature inert carbon activation treatment, combined with PEG and HEC to form a dual carbon framework template, the problem of particle size control and agglomeration of ultrafine α-Al2O3 particles at high temperature was solved, achieving high dispersion stability and excellent polishing performance.
Patent Information
- Application Number
- CN202611613078.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to prepare small-diameter ultrafine α-Al2O3 particles under high-temperature conditions, and these particles tend to agglomerate in aqueous media, affecting dispersion stability and polishing performance.
Ultrafine high-purity alumina was prepared by mechanical activation. The process involved three-stage wet mechanical activation and low-temperature inert carbon activation, combined with PEG and HEC to form a dual-carbon framework template, which inhibited grain coarsening and agglomeration and improved dispersion stability.
Stable control of ultrafine high-purity α-Al2O3 particles with a particle size of 100-130 nm was achieved, improving their dispersibility and polishing performance in aqueous systems and reducing micro-scratches and surface roughness.
Smart Images

Figure CN123105696A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ultrafine alumina material preparation technology, and in particular to a mechanical activation method for preparing ultrafine high-purity alumina. Background Technology
[0002] Ultrafine α-phase alumina possesses high hardness and a high polishing removal rate, making it a common core abrasive for CMP polishing of semiconductor silicon carbide, sapphire, and memory wafers. Among these, alumina polishing slurries with a particle size of 100–130 nm offer a good balance between polishing rate and surface quality. With the development of advanced polishing technologies, higher requirements are being placed on the particle size and distribution, purity, water dispersibility, polished surface quality, and batch stability of alumina abrasives.
[0003] In existing technologies, the Bayer process for preparing α-Al₂O₃ in industry typically employs calcination of aluminum hydroxide (AH), requiring high-temperature calcination above 1200–1300 °C to achieve the α-phase transformation. However, under these high-temperature conditions, nanoscale precursors are prone to Ostwald ripening and hard agglomeration, leading to a rapid increase in the original crystal size to 1–5 μm, making it difficult to obtain small-particle-size products. While existing methods such as α-seed induction, mineralizer assistance, and improved drying methods can reduce the phase transformation temperature or agglomeration to some extent, they still struggle to simultaneously achieve both sufficient α-phase transformation and small-particle-size control.
[0004] On the other hand, nano-α-Al2O3 particles have a large specific surface area and high surface energy, making them prone to aggregation and affecting their dispersion stability in aqueous media. Current stabilization methods for α-Al2O3 polishing abrasives and polishing slurries mainly include two approaches: adding dispersants to the polishing slurry and using a separating phase at the powder end.
[0005] For example, CN111548738A and CN116515401B achieve particle suspension by adding dispersants such as polyacrylic acid, PVP, and BYK after grinding α-Al2O3 powder, utilizing electrostatic effects and steric hindrance. However, the added dispersants mainly bind to the particle surface through physical adsorption, and are prone to desorption during storage aging, pH shift, or polishing shearing, leading to particle flocculation. CN1546381A uses nano-carbon black to coat the precursor and completely decarburizes and removes the carbon layer with air after calcination and phase inversion. Although this can reduce dry powder agglomeration to some extent, the isolation effect disappears after complete decarburization, and the high surface energy α-Al2O3 particles are still prone to re-agglomeration during subsequent pulping.
[0006] Therefore, a mechanical activation method for preparing ultrafine high-purity alumina is proposed. Summary of the Invention
[0007] To address the problems in existing technologies for preparing α-Al₂O₃, such as high phase transformation temperature, abnormal grain growth, large particle size, and easy formation of hard agglomerates, this invention provides a mechanical activation method for preparing ultrafine high-purity alumina. This method controls the particle size of α-Al₂O₃ and suppresses grain coarsening and particle sintering agglomeration during the high-temperature phase transformation process. Furthermore, by subjecting the powder after high-temperature calcination to low-temperature inert carbon activation treatment, the dispersion stability of the obtained α-Al₂O₃ powder in an aqueous system is improved.
[0008] The technical solution of this invention is achieved as follows: A method for preparing ultrafine high-purity alumina by mechanical activation includes the following steps: High-purity boehmite powder was added to a PEG / HEC dual carbon framework dispersion prepared from PEG and hydroxyethyl cellulose (HEC) to form a slurry. The slurry is subjected to three-stage wet mechanical activation, which enables the high-purity boehmite powder to achieve particle dispersion, lattice activation and surface activation in stages, and allows PEG and HEC to be adsorbed and coated on the particle surface in situ to construct a pre-formed dual carbon skeleton network. The mechanically activated slurry was dried and then subjected to gradient heating carbonization under nitrogen protection to pre-carbonize and solidify PEG and HEC, forming a three-dimensional carbon skeleton template. High-temperature calcination under a nitrogen atmosphere dehydrates boehmite and completes the crystal phase transformation from γ-Al2O3 to α-Al2O3. The spatial confinement effect of the three-dimensional carbon framework template inhibits grain coarsening and agglomeration, forming α-Al2O3 particles.
[0009] Furthermore, the purity of the high-purity boehmite powder is 99.995%; the high-purity boehmite powder is circulated and washed three times with ultrapure water to remove surface-adsorbed inorganic salts and soluble impurities, and then vacuum dried at 105°C for later use.
[0010] The term "high purity" in this invention refers to the use of 99.995% pure boehmite powder as raw material, and the reduction of surface impurities and the introduction of impurities during mechanical activation through ultrapure water circulation cleaning, the use of 99.99% pure α-phase alumina grinding balls, and a silicon carbide ball mill jar. The total heavy metal impurities in the resulting α-Al₂O₃ powder are controlled below 30 ppm.
[0011] Further, the PEG is selected from PEG-2000 to 8000; PEG and hydroxyethyl cellulose (HEC) are added to ultrapure water and stirred at 40 to 50°C for 30 minutes until completely dissolved to obtain a uniform and transparent PEG / HEC dual carbon framework dispersion; the amount of PEG added is 1.5% to 3.0% and the amount of HEC added is 0.8% to 1.8% based on the mass of boehmite powder.
[0012] Furthermore, the high-purity boehmite powder is added to the PEG / HEC dual carbon framework dispersion to prepare a uniform slurry with a solid content of 20% to 30%; the three-stage wet mechanical activation uses α-phase alumina grinding balls with a purity of 99.99%, the particle size of the grinding balls is 0.2 to 0.6 mm, the ball-to-material ratio is 3:1 to 5:1, and the grinding jar is made of silicon carbide.
[0013] Furthermore, the three-stage wet mechanical activation preferably includes: a first-stage coarse activation, using 600 r / min for 1 h; a second-stage medium-refining activation, using 900 r / min for 1.5 h; and a third-stage ultra-micro surface activation, using 1200 r / min for 0.5–1 h.
[0014] Furthermore, after the three-stage wet mechanical activation is completed, the resulting slurry is homogenized by high-speed shearing at 3000-4000 r / min for 15-25 min, and then allowed to stand and mature at room temperature for 1.5 h.
[0015] Further, the matured slurry is filtered and dried at 110°C to obtain precursor composite powder; the precursor composite powder is placed under nitrogen protection, heated to 280°C at 4°C / min and held for 1 hour, then heated to 380°C at 3°C / min and held for 2 hours to pre-carbonize and solidify the PEG and HEC system, forming a three-dimensional carbon skeleton template.
[0016] Furthermore, after the gradient heating carbonization is completed, the nitrogen inert atmosphere is maintained, the temperature is raised to 1000-1180℃ and held for 2-3 hours to dehydrate the boehmite and complete the crystal phase transformation from γ-Al2O3 to α-Al2O3.
[0017] Furthermore, after high-temperature calcination, the temperature is lowered to 450–520°C, and the temperature is maintained at this temperature for 1.0–1.5 hours under a nitrogen atmosphere for low-temperature inert carbon activation treatment, which does not oxidize or decarbonize throughout the process and retains the carbon skeleton.
[0018] Furthermore, after the low-temperature inert carbon activation treatment is completed, the furnace is cooled in a sealed manner under nitrogen conditions. The soft agglomerates are dispersed by airflow and the trace ultra-large particulate impurities are removed by 3500 mesh sieve to obtain ultrafine high-purity α-Al2O3 particles with a particle size of 100-130 nm.
[0019] The embodiments of the present invention have the following advantages due to the adoption of the above technical solutions: I. This invention achieves particle dispersion, refinement and lattice activation through a three-stage wet mechanical activation process. Combined with the confinement effect of the dual carbon framework, it can suppress abnormal grain growth during high-temperature phase transformation, thereby ensuring that the particle size of the obtained α-Al2O3 particles is stably controlled within 100-130 nm.
[0020] II. This invention forms a dual carbon framework system by compounding PEG and HEC, and constructs a three-dimensional carbon framework template after gradient heating carbonization. During high-temperature calcination, it forms spatial isolation for particles, reducing grain contact, sintering and hard agglomeration.
[0021] Third, the present invention further employs low-temperature inert carbon activation treatment after high-temperature calcination, and does not perform oxidation and decarburization during the treatment process to retain the carbon skeleton, which is beneficial to improving the dispersion stability of the obtained α-Al2O3 powder in the aqueous system and reducing the amount of dispersant used in CMP polishing fluid.
[0022] IV. This invention utilizes ultrapure water circulation for cleaning high-purity boehmite powder, and employs 99.99% pure α-phase alumina grinding balls and a silicon carbide ball mill jar, which helps reduce impurities on the raw material surface and introduced during mechanical activation. The total heavy metal impurities in the obtained α-Al₂O₃ powder can be controlled below 30 ppm; the total heavy metal impurities in the powder obtained in Example 1 were 3.2 ppm. When the obtained powder is used for CMP polishing, it helps reduce micro-scratches and surface roughness while maintaining a high material removal rate. Attached Figure Description
[0023] Figure 1 This is a flowchart of the mechanical activation method for preparing ultrafine high-purity alumina according to the present invention. Detailed Implementation
[0024] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0025] This invention provides a mechanical activation method for preparing ultrafine high-purity alumina, mainly comprising four steps: First, high-purity boehmite powder is added to a PEG / HEC dual-carbon framework dispersion prepared by PEG and hydroxyethyl cellulose (HEC) to form a slurry; second, the slurry is subjected to a three-stage wet mechanical activation process, which enables the high-purity boehmite powder to achieve particle dispersion, lattice activation, and surface activation stepwise, and allows PEG and HEC to be adsorbed and coated in situ on the particle surface, constructing a pre-formed dual-carbon framework network; third, the mechanically activated slurry is dried and subjected to gradient heating carbonization under nitrogen protection, which pre-carbonizes and solidifies PEG and HEC to form a three-dimensional carbon framework template; finally, high-temperature calcination is performed under a nitrogen atmosphere to dehydrate the boehmite and complete the crystal phase transformation from γ-Al2O3 to α-Al2O3. The spatial confinement effect of the three-dimensional carbon framework template inhibits grain coarsening and agglomeration, forming α-Al2O3 particles; Based on the above technical solution, the high-purity boehmite powder can be further pretreated by ultrapure water circulation cleaning and vacuum drying; after three-stage wet mechanical activation, the slurry is subjected to high-speed shear homogenization and room temperature aging; after high-temperature calcination, it is further subjected to low-temperature inert carbon activation treatment to improve the dispersion stability of the obtained powder in the aqueous system; and after low-temperature inert carbon activation, it is subjected to closed furnace cooling under nitrogen conditions, airflow powder dispersion and 3500 mesh sieving to obtain ultrafine high-purity α-Al2O3 particles with a particle size of 100-130nm.
[0026] like Figure 1 As shown, the present invention provides a mechanical activation method for preparing ultrafine high-purity alumina, comprising the following steps: Step 1: Preparation of slurry containing high-purity boehmite powder and PEG / HEC dual-carbon framework dispersion High-purity boehmite powder with a purity of 99.995% was selected as the raw material.
[0027] Preferably, the high-purity boehmite powder is circulated and washed three times with ultrapure water to remove inorganic salts and soluble impurities adsorbed on the particle surface; after washing, it is vacuum dried at 105°C for later use.
[0028] When preparing the PEG / HEC dual-carbon framework dispersion, PEG-2000 to 8000 is selected, with PEG-4000 being preferred. PEG and hydroxyethyl cellulose (HEC) are added to ultrapure water and stirred at a constant temperature of 40–50°C for 30 minutes until completely dissolved, resulting in a uniform and transparent PEG / HEC dual-carbon framework dispersion.
[0029] Based on the mass of boehmite powder, the PEG content is 1.5%–3.0% and the HEC content is 0.8%–1.8%; preferably, the PEG content is 2.2 wt% and the HEC content is 1.2 wt%.
[0030] PEG is used to rapidly penetrate the interparticle spaces and improve the dispersion state of particles during mechanical activation, inhibiting secondary soft agglomeration of newly formed ultrafine particles; HEC forms a continuous network structure and a carbon skeleton during subsequent carbonization. The combination of PEG and HEC forms a dual carbon skeleton system.
[0031] Pretreated high-purity boehmite powder was added to the PEG / HEC dual carbon framework dispersion to prepare a uniform slurry with a solid content of 20% to 30%.
[0032] Step Two: Three-stage wet mechanical activation and in-situ coating The slurry obtained in step one is subjected to three-stage wet mechanical activation.
[0033] Preferably, α-phase alumina grinding balls with a purity of 99.99% are used, and the particle size of the grinding balls is 0.2 to 0.6 mm, preferably 0.3 mm; the ball-to-material ratio is 3:1 to 5:1, preferably 4:1; the grinding jar is made of silicon carbide.
[0034] In a preferred embodiment, the three-stage wet mechanical activation includes: The first stage is primary coarse activation, which involves grinding at 600 r / min for 1 hour to break up the original agglomerates of high-purity boehmite powder and remove impurities from the particle surface. The second stage is secondary refining and activation, which involves grinding at 900 r / min for 1.5 h to further break down coarse particles and introduce lattice defects; The third stage is three-level ultrafine surface activation, which involves grinding at 1200 r / min for 0.5 to 1 h to further modify the particle surface, so that PEG and HEC can be adsorbed and coated in situ on the particle surface, and a pre-formed dual carbon framework network can be constructed.
[0035] Through a three-stage wet mechanical activation process, high-purity boehmite powder is first deagglomerated and uniformly dispersed at a lower intensity, and then the mechanical action intensity is gradually increased to achieve particle refinement, lattice activation and surface activation, thereby improving the problems of uneven activation and particle size differentiation that are prone to occur during constant parameter mechanical activation.
[0036] During the mechanical activation process, PEG and HEC come into full contact with the high-purity boehmite particles and gradually form an in-situ adsorption and coating structure on the particle surface, providing a basis for the subsequent gradient heating carbonization to form a three-dimensional carbon framework template.
[0037] Furthermore, after the three-stage wet mechanical activation is completed, the resulting slurry is homogenized by high-speed shearing at 3000-4000 r / min for 15-25 min to eliminate local micro-flocculation; then it is allowed to stand and mature at room temperature for 1.5 h to further improve the double carbon skeleton coating structure on the particle surface and improve the coating uniformity.
[0038] Step 3: Gradient heating carbonization to form a three-dimensional carbon skeleton template The mechanically activated slurry is then dried.
[0039] Preferably, the homogenized and aged slurry is filtered and dried at 110°C to obtain precursor composite powder.
[0040] The precursor composite powder was subjected to gradient temperature carbonization under nitrogen protection.
[0041] Preferably, the temperature is increased to 280°C at a heating rate of 4°C / min and held for 1 hour, and then increased to 380°C at a heating rate of 3°C / min and held for 2 hours.
[0042] During the gradient heating carbonization process, the PEG and HEC system is gradually pre-carbonized and solidified, forming a rigid and stable three-dimensional carbon skeleton template between the particles, which keeps the particles spatially isolated during the subsequent high-temperature calcination process.
[0043] Step 4: High-temperature calcination in a nitrogen atmosphere for crystal phase transformation After the gradient heating carbonization is completed, the high-temperature calcination continues under a nitrogen inert atmosphere.
[0044] Preferably, the temperature is raised to 1000-1180℃ and held for 2-3 hours to dehydrate the high-purity boehmite and complete the crystal phase transformation from γ-Al2O3 to high-purity α-Al2O3.
[0045] During the high-temperature crystalline phase transformation process, the three-dimensional carbon skeleton template formed in step three provides spatial isolation and confinement for the particles, reducing direct contact between grains and thus inhibiting grain coarsening and particle agglomeration.
[0046] Furthermore, after high-temperature calcination, the resulting powder can be subjected to low-temperature inert carbon activation treatment.
[0047] Specifically, the temperature is lowered to 450–520°C, and the nitrogen atmosphere is maintained for 1.0–1.5 hours. Preferably, the temperature is maintained at 480°C for 1.2 hours.
[0048] No oxidative decarburization is performed during the low-temperature inert carbon activation process to preserve the carbon skeleton. This treatment helps reduce the tendency of the resulting α-Al₂O₃ particles to agglomerate and settle in aqueous systems, thereby improving the dispersion stability of the powder.
[0049] Furthermore, after low-temperature inert carbon activation, the particles are cooled in a sealed furnace under nitrogen conditions. The soft agglomerates are dispersed by airflow and removed by a 3500-mesh sieve to obtain ultrafine high-purity α-Al2O3 particles with a particle size of 100–130 nm.
[0050] Example 1 This embodiment is a preferred embodiment.
[0051] High-purity boehmite powder with a purity of 99.995% was selected, washed three times with ultrapure water, and then vacuum dried at 105℃ for later use.
[0052] PEG-4000 and HEC were added to ultrapure water, with PEG-4000 added at 2.2 wt% and HEC added at 1.2 wt% based on the mass of boehmite powder. The mixture was stirred at 45°C for 30 min until completely transparent to obtain a PEG / HEC dual carbon framework dispersion.
[0053] Pretreated high-purity boehmite powder was added to the PEG / HEC dual carbon framework dispersion to prepare a slurry with a solid content of 25% and a ball-to-particle ratio of 4:1.
[0054] The slurry is subjected to a three-stage wet mechanical activation process, in the following order: Primary coarse activation: Grind at 600 r / min for 1 hour; Secondary refining and activation: grinding at 900 r / min for 1.5 h; Level 3 ultrafine surface activation: grinding at 1200 r / min for 0.5 h.
[0055] After mechanical activation, the material was homogenized by high-speed shearing at 3500 r / min for 20 min and then allowed to stand at room temperature for 1.5 h to mature.
[0056] The matured slurry was filtered and dried, and then subjected to gradient heating carbonization under a nitrogen atmosphere: the temperature was raised to 280℃ and held for 1 hour, and then raised to 380℃ and held for 2 hours, so that the PEG and HEC system was pre-carbonized and a three-dimensional carbon skeleton template was formed.
[0057] The nitrogen atmosphere was then maintained, and the temperature was raised to 1150℃ and held for 2.5 hours to complete the α-phase crystal phase transformation.
[0058] After high-temperature calcination, the temperature is lowered to 480℃ and held at that temperature for 1.2 hours under a nitrogen atmosphere for low-temperature inert carbon activation treatment. No oxidation or decarburization is performed throughout the process.
[0059] After processing, the powder was cooled in a sealed furnace under nitrogen conditions, dispersed by airflow, and sieved through a 3500-mesh sieve to obtain ultrafine high-purity α-Al2O3 particles.
[0060] The obtained powder had a D50 of 115 nm and a total heavy metal impurity content of 3.2 ppm. The above total heavy metal impurity data were used to characterize the impurity control level of the α-Al₂O₃ powder obtained in this embodiment.
[0061] To verify the application performance of the obtained α-Al2O3 particles, they were further formulated into a CMP polishing slurry.
[0062] The CMP polishing solution contains 5.5 wt% α-Al2O3 powder, 0.2 wt% alkaline regulator, 0.08 wt% dispersant, 0.05 wt% wetting agent, and the remainder is ultrapure water, with the pH adjusted to 8.5.
[0063] The obtained CMP polishing slurry was completely stable after standing for 72 hours, with no stratification or sedimentation. When used for sapphire polishing, the surface roughness Ra was 0.44 nm, the number of micro-scratches larger than 0.5 μm was 0, the material removal rate MRR was 82.3 nm / min, and the polished surface was defect-free.
[0064] Example 2 The basic preparation process in this embodiment is the same as in Example 1, except that some process parameters are different.
[0065] Based on the mass of boehmite powder, the PEG addition was 1.5wt% and the HEC addition was 0.8wt%; the three-stage mechanical activation speed was adjusted to 1000 r / min; the high-temperature calcination temperature was 1120℃ and the holding time was 2.5h.
[0066] The remaining high-purity boehmite powder pretreatment, PEG / HEC dual carbon framework dispersion preparation, slurry preparation, first two stages of mechanical activation, homogenization and aging, gradient carbonization, low-temperature inert carbon activation and powder posttreatment were carried out in accordance with Example 1.
[0067] The obtained ultrafine high-purity α-Al2O3 powder has a D50 of 128 nm and a PDI of 0.18.
[0068] The obtained powder was used to prepare a CMP polishing slurry and its performance was tested. When the obtained CMP polishing slurry was used for polishing, the surface roughness Ra was 0.47 nm, the material removal rate MRR was 80.5 nm / min, the number of micro-scratches was 0, and the polishing quality was excellent. After standing for 72 hours, there was no stratification, but there was slight suspension unevenness.
[0069] Example 3 The basic preparation process in this embodiment is the same as in Example 1, except that some process parameters are different.
[0070] Based on the mass of boehmite powder, the PEG addition was 3.0 wt% and the HEC addition was 1.8 wt%; the three-stage mechanical activation was carried out by grinding at 1200 r / min for 1 h; the high-temperature calcination temperature was 1180℃ and the holding time was 2.5 h.
[0071] The remaining steps are performed in accordance with Example 1.
[0072] The obtained ultrafine high-purity α-Al2O3 powder has a D50 of 103 nm, with uniform particle size and no obvious agglomeration; the CMP polishing slurry prepared using the obtained powder has good static stability.
[0073] The obtained powder was used to prepare a CMP polishing slurry and its performance was tested. When the obtained CMP polishing slurry was used for polishing, the surface roughness Ra was 0.42 nm, the material removal rate MRR was 79.6 nm / min, the number of micro-scratches was 0, and there were no defects on the polished surface. After standing for 72 hours, it was completely stable and there were no abnormalities.
[0074] Comparative Example 1 This comparative example is used to verify the effect of the three-stage wet mechanical activation method on the particle size and application performance of the obtained α-Al2O3 powder.
[0075] This comparative example does not use the three-stage wet mechanical activation method, but instead uses a single-stage grinding process of 1000 r / min for 3 hours; the remaining auxiliary agent system, gradient carbonization, high-temperature calcination, low-temperature inert carbon activation and post-treatment process are the same as in Example 1.
[0076] Test results show that after single-stage grinding, the grain activation is insufficient, and the α-Al2O3 powder obtained after calcination has a D50 of 156 nm and a wide particle size distribution.
[0077] After the obtained powder was used to prepare CMP polishing slurry, obvious sedimentation and bottom agglomeration occurred after standing for 24 hours. When used for sapphire polishing, the surface roughness Ra was 1.18 nm, the material removal rate MRR was 60.2 nm / min, and the number of micro-scratches was 26 to 32, indicating dense scratches.
[0078] Comparative Example 2 This comparative example is used to verify the role of HEC in the PEG / HEC dual carbon framework system.
[0079] This comparative example only added PEG and did not add HEC, and used a PEG single carbon template system; the other three stages of wet mechanical activation, gradient carbonization, high temperature calcination, low temperature inert carbon activation and powder post-processing were the same as in Example 1.
[0080] Test results show that when PEG is used alone, the continuity of carbon skeleton film formation is poor and the high-temperature confinement ability is weak. The D50 of the α-Al2O3 powder obtained after calcination is 142 nm.
[0081] After preparing CMP polishing slurry using the obtained powder, slight stratification and a small amount of sedimentation occurred; when used for polishing, the surface roughness Ra was 0.89 nm, the material removal rate MRR was 68.5 nm / min, the number of micro-scratches was 14 to 18, there were obvious scratches and poor polishing uniformity.
[0082] Comparative Example 3 This comparative example is used to verify the role of PEG in the PEG / HEC dual carbon framework system.
[0083] This comparative example only added HEC and did not add PEG, and used the HEC single carbon template system; the other three stages of wet mechanical activation, gradient carbonization, high temperature calcination, low temperature inert carbon activation and powder post-processing were the same as in Example 1.
[0084] Test results show that during the mechanical activation process, the slurry exhibits localized viscosity and flocculation, and the particle coating thickness is uneven. The D50 of the α-Al2O3 powder obtained after calcination is 136 nm.
[0085] After using the obtained powder to prepare CMP polishing slurry, local flocculation and poor light transmittance occurred; when used for polishing, the surface roughness Ra was 0.76 nm, the material removal rate MRR was 71.3 nm / min, the number of micro-scratches was 9 to 13, and sporadic carbon black spots and fine scratches appeared.
[0086] Comparative Example 4 This comparative example is used to verify the effect of low-temperature inert carbon activation treatment on the dispersion stability and polishing performance of the obtained α-Al2O3 powder.
[0087] In this comparative example, the low-temperature inert carbon activation treatment was omitted, and the carbon layer was completely removed in an air atmosphere at 700°C after high-temperature calcination. The remaining processes, including high-purity boehmite powder pretreatment, PEG / HEC dual carbon framework system, three-stage wet mechanical activation, gradient carbonization, and high-temperature calcination, were the same as in Example 1.
[0088] Test results show that after complete decarburization, the surface of the powder no longer retains a carbon layer, and the particles are prone to agglomeration. The D50 of the obtained α-Al2O3 powder is 148 nm. When using this powder to prepare CMP polishing slurry, the amount of dispersant needs to be doubled, and the obtained CMP polishing slurry shows a large amount of sedimentation and obvious agglomeration after standing for 48 hours, indicating that its dispersion stability has decreased significantly.
[0089] When used for polishing, the surface roughness Ra is 1.05 nm, the material removal rate MRR is 63.8 nm / min, the number of micro-scratches is 21 to 25, and obvious polishing lines and surface defects appear.
[0090] Performance test results The performance of the α-Al2O3 powders and corresponding CMP polishing solutions obtained in Examples 1-3 and Comparative Examples 1-4 was compared, and the test results are shown in the table below.
[0091]
[0092] The test results above show that the D50 of the α-Al2O3 powders obtained in Examples 1 to 3 are 115nm, 128nm and 103nm respectively, all within the range of 100 to 130nm; the D50 of the powders obtained in Comparative Examples 1 to 4 are 156nm, 142nm, 136nm and 148nm respectively, all higher than those in Examples 1 to 3.
[0093] Regarding the polished surface quality, the Ra values of Examples 1-3 were 0.44 nm, 0.47 nm, and 0.42 nm, respectively, with zero micro-scratches in each example; while the Ra values of Comparative Examples 1-4 were 1.18 nm, 0.89 nm, 0.76 nm, and 1.05 nm, respectively, with varying numbers of micro-scratches in each example.
[0094] Regarding the material removal rate, the MRR of Examples 1-3 were 82.3 nm / min, 80.5 nm / min and 79.6 nm / min, respectively, which were higher than those of the comparative examples.
[0095] Regarding the stability of the slurry, both Example 1 and Example 3 remained completely stable after standing for 72 hours. Example 2 did not show stratification, but only slight uneven suspension. The comparative examples, on the other hand, showed sedimentation, stratification, local flocculation, or severe agglomeration.
[0096] The above results indicate that the three-stage wet mechanical activation, the PEG / HEC dual carbon framework system, and the three-dimensional carbon framework template formed by gradient heating carbonization work together to control particle size and suppress sintering agglomeration during the α-Al2O3 crystal phase transformation. Further low-temperature inert carbon activation treatment is beneficial to improving the dispersion stability of the obtained powder in an aqueous system.
[0097] Therefore, the present invention can obtain ultrafine high-purity α-Al2O3 particles with a particle size of 100-130 nm, and make the obtained α-Al2O3 suitable for CMP polishing while taking into account material removal rate, surface roughness and micro-scratching control.
[0098] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various variations or substitutions within the technical scope disclosed in the present invention, and these should all be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing ultrafine high-purity alumina by mechanical activation, characterized in that, Includes the following steps: Step 1: Add high-purity boehmite powder to a PEG / HEC dual-carbon framework dispersion prepared from PEG and hydroxyethyl cellulose (HEC) to form a slurry; Step 2: Perform three-stage wet mechanical activation on the slurry to achieve particle dispersion, lattice activation and surface activation of the high-purity boehmite powder in stages, and to adsorb and coat PEG and HEC in situ on the particle surface to construct a pre-formed double carbon framework network. Step 3: Dry the mechanically activated slurry and perform gradient temperature carbonization under nitrogen protection to pre-carbonize and solidify PEG and HEC, forming a three-dimensional carbon skeleton template. Step 4: High-temperature calcination is carried out under a nitrogen atmosphere to dehydrate the boehmite and complete the crystal phase transformation from γ-Al2O3 to α-Al2O3. The spatial confinement effect of the three-dimensional carbon framework template inhibits grain coarsening and agglomeration, forming α-Al2O3 particles.
2. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 1, characterized in that: The purity of the high-purity boehmite powder is 99.995%; The high-purity boehmite powder was circulated and washed three times with ultrapure water to remove adsorbed inorganic salts and soluble impurities from the surface, and then vacuum dried at 105°C for later use.
3. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 1, characterized in that: The PEG used is PEG-2000 to 8000; The PEG and hydroxyethyl cellulose (HEC) were added to ultrapure water and stirred at 40–50 °C for 30 min until completely dissolved to obtain a uniform and transparent PEG / HEC dual carbon skeleton dispersion. The amount of PEG added is 1.5% to 3.0% and the amount of HEC added is 0.8% to 1.8% based on the mass of boehmite powder.
4. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 1, characterized in that: The high-purity boehmite powder was added to the PEG / HEC dual carbon framework dispersion to prepare a uniform slurry with a solid content of 20% to 30%. The three-stage wet mechanical activation uses α-phase alumina grinding balls with a purity of 99.99%, the particle size of the grinding balls is 0.2-0.6 mm, the ball-to-material ratio is 3:1-5:1, and the grinding jar is made of silicon carbide.
5. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 4, characterized in that: The three-stage wet mechanical activation includes: First-stage coarse activation involves grinding at 600 r / min for 1 hour to break up native agglomerates and remove surface impurities; Secondary refining and activation involves grinding at 900 r / min for 1.5 h to break up coarse grains and introduce lattice defects; Three-stage ultrafine surface activation was performed by grinding at 1200 r / min for 0.5–1 h to modify the particle surface, allowing PEG and HEC to be adsorbed and coated in situ on the particle surface, thus constructing a pre-formed dual carbon framework network.
6. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 1, characterized in that: After the three-stage wet mechanical activation is completed, the resulting slurry is homogenized by high-speed shearing at 3000-4000 r / min for 15-25 min to eliminate local micro-flocculation. After high-speed shearing homogenization, the slurry is left to stand at room temperature for 1.5 hours to mature, so as to improve the double carbon skeleton coating structure on the particle surface.
7. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 6, characterized in that: The matured slurry was filtered and dried at 110°C to obtain the precursor composite powder. The precursor composite powder was subjected to gradient heating carbonization under nitrogen protection. Specifically, the temperature was increased to 280°C at 4°C / min and held for 1 hour, and then increased to 380°C at 3°C / min and held for 2 hours to pre-carbonize and solidify the PEG and HEC system, forming a rigid and stable three-dimensional carbon skeleton template.
8. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 1, characterized in that: After gradient heating carbonization is completed, a nitrogen inert atmosphere is maintained, the temperature is raised to 1000-1180℃ and held for 2-3 hours to dehydrate the boehmite and complete the crystal phase transformation from γ-Al2O3 to α-Al2O3. The spatial confinement effect of the three-dimensional carbon skeleton template is used to suppress grain coarsening and agglomeration.
9. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 8, characterized in that: After high-temperature calcination, the temperature is lowered to 450–520℃ and held at that temperature for 1.0–1.5 hours under a nitrogen atmosphere for low-temperature inert carbon activation treatment. The entire process involves non-oxidative decarburization and preservation of the carbon skeleton.
10. The method for preparing ultrafine high-purity alumina by mechanical activation according to claim 9, characterized in that: After the low-temperature inert carbon activation treatment is completed, the furnace is cooled in a closed manner under nitrogen conditions. The soft agglomerates are dispersed by airflow and the trace ultra-large particle impurities are removed by 3500 mesh sieve to obtain ultrafine high-purity α-Al2O3 particles with a particle size of 100-130nm.
Citation Information
Patent Citations
Alumina polishing solution and preparation method thereof
CN111548738A
Alumina polishing liquid and preparation method thereof
CN116515401B
Method for preparing conglobate-free nano alpha-Al2O3 powders
CN1546381A