A cloisonné enamel painting base glaze based on natural desert sand and its preparation process

By using natural desert sand and food-grade environmentally friendly additives to prepare the base glaze for cloisonné enamel paintings, the problems of high dependence on the industrial colored sand base glaze industry chain, poor mechanical properties, lack of mildew resistance, and poor environmental protection have been solved. This has achieved low-cost, safe, and environmentally friendly base glaze preparation and suitability for all age groups, making it suitable for independent creation in grassroots education and small cultural and creative studios.

CN123105986APending Publication Date: 2026-11-17NAIMAN BANNER NO 1 PRIMARY SCHOOL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611322160.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing industrial colored sand base glaze supply chain is highly dependent, has poor mechanical properties, lacks mildew resistance, has weak adaptability and poor environmental performance, and has a complex production process, making it difficult to meet the low-cost and stable supply needs of grassroots educational institutions and small cultural and creative studios.

Method used

Using natural desert sand as the core raw material, and combined with food-grade environmentally friendly auxiliary materials to modify and prepare cloisonné enamel painting base glaze, it is prepared through a room temperature process, including steps such as collection, washing, drying, sieving and room temperature stirring, forming a dual protection system and particle size differentiation ratio to meet the needs of handmade creations of different age groups.

Benefits of technology

It achieves low-cost, safe, and environmentally friendly preparation of base glaze without high-temperature calcination, with a 0% cracking rate, a 4-level abrasion fastness, a 0-level mildew resistance, and a waste material reuse rate of over 92%. It is suitable for manual operation by all age groups, reducing the operation threshold and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1787822904261-000001
    Figure REF-OBJ-1787822904261-000001
Patent Text Reader

Abstract

This application relates to the technical field of cloisonné enamel painting materials, specifically disclosing a cloisonné enamel painting base glaze based on natural desert sand and its preparation process. The cloisonné enamel painting base glaze comprises the following raw materials in parts by weight: 70-90 parts natural desert sand, 5-15 parts water-based environmentally friendly plant dyes, 10-30 parts purified water, 1-5 parts water-soluble environmentally friendly color-fixing adhesive, and 0.1-0.5 parts natural anti-mildew and antibacterial agent. This application uses natural desert sand to replace traditional industrial colored sand, which can significantly reduce costs, achieve a 0% cracking rate after 72 hours of curing, a friction fastness grade of 4, a mildew resistance grade of 0, zero detection of heavy metals, a waste reuse rate of over 92%, a 96% reduction in carbon emissions, and an 89% reduction in the production cycle. It can be widely used in primary and secondary school art education, club training, cultural and creative pendants, home decoration, and other fields, realizing the independent controllability of the cloisonné enamel painting base glaze industrial chain, its suitability for all ages, its safety and non-toxicity, and its green recycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of cloisonné enamel painting materials, and in particular to a cloisonné enamel painting base glaze based on natural desert sand and its preparation process. Background Technology

[0002] Cloisonné enamel (Jingtai Blue) is a national intangible cultural heritage of my country, and its application in recent years has become increasingly widespread in areas such as characteristic art education in primary and secondary schools, intangible cultural heritage-based school courses, popular cultural and creative products, and home decoration. In the creation of cloisonné enamel paintings, the base glaze and colored sand are indispensable core consumables. Currently, commercially available cloisonné enamel glazes are all made from industrial quartz sand as the base material, undergoing multiple processes including ore mining, high-temperature firing at over 1200℃, dyeing with chemical pigments, and blending with chemical additives, resulting in a very high degree of industrial dependence.

[0003] The existing technology has the following main defects and shortcomings: (1) High dependence on the industrial chain and unstable supply chain: Industrial colored sand production relies on heavy chemical processes such as quartz mining and high-temperature calcination. Raw material and energy costs fluctuate greatly, and long-distance transportation increases supply chain risks, making it difficult to meet the low-cost and stable supply needs of grassroots educational institutions and small cultural and creative studios.

[0004] (2) Poor overall mechanical properties and low finished product qualification rate: Industrial quartz sand particles have sharp edges and weak interfacial bonding with the curing adhesive. After the finished product is cured, it is easy to crack, fall off, and powder fall off. At the same time, the particle porosity is low and the dye adsorption is poor, which easily leads to color fading and color bleeding.

[0005] (3) Lack of anti-mold and antibacterial properties: Industrial colored sand and its chemical additives are prone to mold growth, especially in humid southern regions. Mold spots will appear on the finished products after 3 to 6 months of storage, which seriously affects the appearance and preservation value of the works.

[0006] (4) Poor adaptability to teaching and potential safety hazards: Commercial industrial colored sand particles have fixed and single specifications, and cannot be adjusted according to the hands-on ability of different age groups; at the same time, they contain heavy metal chemical dyes and corrosive curing agents, and long-term direct contact poses potential health risks, making them unsuitable for teaching scenarios for minors.

[0007] (5) Low resource utilization and insufficient environmental protection: Industrial colored sand cannot be decolorized and reused for secondary color adjustment, and the waste colored sand generated during production and use is difficult to degrade naturally; at the same time, the high-temperature calcination process emits a large amount of carbon dioxide, which does not conform to the concept of green and low-carbon development.

[0008] (6) The production process is complex and the threshold for implementation is high: Industrial colored sand production requires large-scale equipment such as professional high-temperature kilns and chemical reaction kettles. The initial investment is large and there are safety production risks. It is impossible to realize on-site preparation and student participation in teaching scenarios.

[0009] Currently, only a small number of enamel glaze preparation technologies exist that use ordinary river sand and quartz sand as raw materials. Among related technologies, Chinese patent CN109650848A discloses a self-generating enamel porcelain clay, whose body material contains 45-55% sand particles taken from the desert, combined with various mineral raw materials such as pyrophyllite, purple wood knot, coal gangue, magnesium-based bentonite, potassium feldspar, sodium feldspar, micron-sized spodumene, zirconium silicate, and wollastonite. This technology belongs to the field of enamel porcelain (ceramics) preparation and employs a high-temperature firing process. In addition, CN111114185A relates to a method for producing cloisonné enamel paintings, the core of which lies in the painting production process and does not involve the formulation design or preparation process innovation of the base glaze raw materials; CN109177626A relates to a cloisonné enamel production process, whose glaze is a traditional enamel mineral glaze, not a desert sand-based material.

[0010] To date, there are no publicly available technical solutions, patents, or documents that disclose a technical solution for preparing cloisonné enamel painting base glaze using pristine desert sand as the core raw material and employing an all-room-temperature environmentally friendly process, indicating a significant technological gap in this field. Summary of the Invention

[0011] This application aims to overcome the core shortcomings of existing industrial colored sand base glazes, such as high dependence on the industrial chain, poor mechanical properties, lack of mildew resistance, weak adaptability, and poor environmental protection. It provides a cloisonné enamel painting base glaze based on natural desert sand and its preparation process. This application uses pristine natural desert sand as the core raw material, combined with food-grade environmentally friendly auxiliary materials to modify and prepare a special base glaze, replacing traditional industrial colored sand. It balances the self-controllability of the industrial chain, the comprehensive performance of materials, safety, and environmental protection, making it suitable for handicraft creation and large-scale teaching for all ages.

[0012] Firstly, this application provides a cloisonné enamel painting base glaze based on natural desert sand, employing the following technical solution: A cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials in parts by weight: 70-90 parts natural desert sand, 5-15 parts water-based environmentally friendly plant dyes, 10-30 parts purified water, 1-5 parts water-soluble environmentally friendly color-fixing glue, and 0.1-0.5 parts natural anti-mildew and antibacterial agent.

[0013] In one specific feasible implementation, the natural desert sand is the fine sand on the surface of the sunny slope of the original desert, ranging from 0 to 20 cm.

[0014] In one specific implementation scheme, the cloisonné enamel painting base glaze based on natural desert sand also includes the following raw materials in parts by weight: 0.05 to 0.2 parts of food-grade rheology modifier.

[0015] In one specific implementation, the water-soluble environmentally friendly color-fixing adhesive is food-grade polyvinyl alcohol.

[0016] In a specific feasible implementation scheme, by weight, in a teaching scenario for children aged 6-9, the cloisonné enamel painting base glaze based on natural desert sand comprises the following raw materials: 80-90 parts natural desert sand, 5-8 parts water-based environmentally friendly plant dyes, 10-15 parts purified water, 4-5 parts water-soluble environmentally friendly color-fixing adhesive, and 0.3-0.5 parts natural anti-mildew and antibacterial agent; in a general teaching and cultural and creative scenario for children aged 10-16, the cloisonné enamel painting base glaze based on natural desert sand comprises the following raw materials: natural desert sand, 80-90 parts water-based environmentally friendly plant dyes, 5-8 parts purified water, 10-15 parts purified water, 4-5 parts water-soluble environmentally friendly color-fixing adhesive, and 0.3-0.5 parts natural anti-mildew and antibacterial agent; The cloisonné enamel base glaze based on natural desert sand comprises the following raw materials in parts by weight: 70-75 parts natural desert sand, 12-15 parts water-based environmentally friendly plant dyes, 20-30 parts purified water, 1-3 parts water-soluble environmentally friendly color-fixing adhesive, and 0.1-0.2 parts natural anti-mildew and antibacterial agent. For professional creative settings for individuals aged 16 and above, the cloisonné enamel base glaze based on natural desert sand comprises the following raw materials in parts by weight: 70-75 parts natural desert sand, 12-15 parts water-based environmentally friendly plant dyes, 20-30 parts purified water, 1-3 parts water-soluble environmentally friendly color-fixing adhesive, and 0.1-0.2 parts natural anti-mildew and antibacterial agent.

[0017] Secondly, this application provides a preparation process for a cloisonné enamel painting base glaze based on natural desert sand, employing the following technical solution: A preparation process for a cloisonné enamel painting base glaze based on natural desert sand includes the following steps: S1. Collect fine sand from the pristine desert, manually remove impurities, soak in pure water for 8-15 minutes, and rinse 2-3 times to obtain clean sand. S2. Dry the washed sand in a ventilated environment at 20-35℃ until the moisture content is 2-3% to obtain ready-to-use natural desert sand. S3. According to the ratio, mix the prepared natural desert sand, water-based environmentally friendly plant dye, and purified water at room temperature for 10-15 minutes to obtain the dyeing material. Add water-soluble environmentally friendly color-fixing glue and natural anti-mildew and antibacterial agent to the dyeing material, stir and dry to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0018] In a specific feasible implementation, in step S2, the dried sand is graded and screened using three levels of standard sieves: 50 mesh, 80 mesh, and 120 mesh. The particles obtained by sieving through the 50 mesh sieve are used for professional creative scenarios for children aged 16 and above, the particles obtained by sieving through the 80 mesh sieve are used for general teaching and cultural and creative scenarios for children aged 10-16, and the particles obtained by sieving through the 120 mesh sieve are used for early childhood teaching scenarios for children aged 6-9.

[0019] In one specific implementation scheme, in step S2, the sand is spread out to a thickness of 1-3 cm and turned over evenly every 1 hour during the drying process.

[0020] In one specific implementation scheme, in step S3, after adding water-soluble environmentally friendly color-fixing adhesive and natural anti-mildew and antibacterial agent, stir at low speed for 5 minutes, spread the mixture to a thickness of 1-2 cm, and dry it in a ventilated environment at 20-35℃ for 2-4 hours.

[0021] In summary, this application has the following beneficial effects: 1. This application uses rounded, porous, naturally microporous desert sand as a physical framework to adsorb plant dyes. Pure water is used as a medium to achieve capillary penetration of the dye into the particles. A water-soluble, environmentally friendly fixing adhesive forms a coating film on the particle surface via hydrogen bonds to lock in the dye and antifungal agent. A dual protection system is constructed using natural antifungal and antibacterial agents and the fixing adhesive film. Food-grade rheology modifiers precisely control the slurry consistency to adapt to different operating scenarios, forming a complete functional closed loop. This is further enhanced by S1 directional collection and washing for impurity removal, S2 precise water control, and a three-stage sieve. The combined process of S3 room temperature dyeing and composite color fixing secondary drying enables the base glaze of this application to achieve excellent comprehensive performance with 0% cracking rate after 72 hours of curing, 4-level rubbing fastness, 0-level mildew resistance, zero detection of heavy metals lead and cadmium, a waste reuse rate of over 92%, and carbon emissions of only about 50 kg / ton per unit of production capacity. This solves the four core defects of the existing industrial colored sand industry chain from the source: high dependence, poor mechanical properties, lack of mildew resistance, and poor environmental protection.

[0022] 2. This application preferably uses a three-level standard sieve to classify and screen the sand, and combines it with three different weight ratios for coordinated operation. 120-mesh ultrafine particles with a high-fixation color glue ratio are used for teaching scenarios for children aged 6-9, which greatly reduces the operation threshold and eliminates flying sand and powdering; 80-mesh medium particles with a balanced ratio are used for general teaching and cultural and creative scenarios for children aged 10-16, taking into account both color laying and fine blue dotting; 50-mesh coarse particles with a low-fixation color glue ratio are used for professional creative scenarios for children aged 16 and above, which maximizes the preservation of the natural three-dimensional texture of the sand. Through the dual-dimensional fine adjustment of particle size and ratio, the same basic solution can fully cover the manual operation needs of all age groups from young children to professional creators, which significantly improves the teaching adaptability and scenario versatility of the base glaze.

[0023] 3. The method described in this application operates entirely at room temperature, requiring no high-temperature calcination or large-scale industrial equipment. Only basic teaching aids such as trays, sieves, and mixing containers are needed to complete all preparation processes. This allows students to participate independently in raw material preparation in a teaching setting, extending intangible cultural heritage education from simply using consumables to creating their own materials—a deeper teaching experience. It also meets the low-cost, on-demand, and green production needs of small cultural and creative studios. Furthermore, the waste base glaze, due to the physical adsorption of plant dyes, can be reused after soaking in water for decolorization, ultrasonic cleaning, drying, and sieving. This creates a green circular loop for sand resources in both teaching and production scenarios. Compared to the traditional linear production-waste model of industrial colored sand, this method represents a qualitative leap in resource utilization efficiency and environmental friendliness, providing a complete technical solution for the cloisonné enamel painting material field that is self-controllable across the entire industry chain, suitable for all ages, safe, non-toxic, and greenly circular. Detailed Implementation

[0024] Unless otherwise specified, all raw materials used in this application are commercially available. The natural desert sand is from a sunny slope in Naiman Banner, Tongliao City, Inner Mongolia Autonomous Region, with a surface layer of 0-20cm. The water-based environmentally friendly plant dye is a powdered plant extract dye made from the natural plant *Lithospermum erythrorhizon* through water extraction, alcohol precipitation, concentration, and spray drying. The water-soluble environmentally friendly fixing agent is food-grade polyvinyl alcohol, brand: Kuraray PVA205 (Japan). The natural antifungal and antibacterial agent is ε-polylysine hydrochloride, CAS number 25988-63-0, food grade. The food-grade rheology modifier is xanthan gum, CAS number 11138-66-2, purity ≥99%. The industrial colored sand is obtained by calcining industrial quartz sand at temperatures above 1200℃, particle size: 120 mesh. The chemically synthesized dye is 1,4-diaminoanthraquinone, CAS number 81-63-0, purity ≥99%. Chemical color-fixing adhesive, liquid modified polyvinyl alcohol, Wuhan Meiqilin New Materials Co., Ltd., density (20°C): 1.08 g / cm³, effective ingredient content 99%, viscosity (20°C): 1300 mPas.

[0025] The present application will be further described in detail below with reference to embodiments and comparative examples.

[0026] Example 1

[0027] This embodiment provides a cloisonné enamel painting base glaze based on natural desert sand, comprising the following raw materials: 85kg of natural desert sand, 6.5kg of water-based environmentally friendly plant dyes, 12.5kg of purified water, 4.5kg of water-soluble environmentally friendly color-fixing adhesive, and 0.4kg of natural anti-mildew and antibacterial agent.

[0028] This embodiment also provides a preparation process for a cloisonné enamel painting base glaze based on natural desert sand, including the following steps: S1. Select a sunny slope of the original desert and collect the top 0-20cm of original fine sand. Manually remove large particles such as stones, dead branches, and weeds. Then, soak it in pure water for 12 minutes and rinse it twice to remove dust, soil and soluble salts from the sand to obtain clean sand.

[0029] S2. Spread the washed sand evenly on a dustproof tray with a thickness of 2cm. Dry it in a ventilated environment at 20-35℃, turning it over evenly every 1 hour. Dry it until the moisture content is between 2-3%. Use a 120-mesh standard sieve to grade and screen the dried sand. After screening, seal and store it separately to obtain the natural desert sand for later use.

[0030] S3. According to the ratio, the prepared natural desert sand obtained by sieving through a 120-mesh sieve, water-based environmentally friendly plant dye, and purified water are stirred at room temperature for 12.5 minutes to obtain the dyeing material. Water-soluble environmentally friendly color-fixing glue and natural anti-mildew and antibacterial agent are added to the dyeing material. After stirring for 5 minutes, the mixture is spread out to a thickness of 1 cm and dried in a ventilated environment at 20-35℃ for 3 hours to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0031] Example 2

[0032] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 80kg of natural desert sand, 5kg of water-based environmentally friendly plant dye, 10kg of purified water, 4kg of water-soluble environmentally friendly color-fixing glue, and 0.3kg of natural anti-mildew and antibacterial agent.

[0033] Example 3

[0034] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 90kg of natural desert sand, 8kg of water-based environmentally friendly plant dyes, 15kg of purified water, 5kg of water-soluble environmentally friendly color-fixing glue, and 0.5kg of natural anti-mildew and antibacterial agent.

[0035] Example 4

[0036] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 75kg of natural desert sand, 8kg of water-based environmentally friendly plant dyes, 15kg of purified water, 3kg of water-soluble environmentally friendly color-fixing glue, and 0.2kg of natural anti-mildew and antibacterial agent.

[0037] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using an 80-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 80-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0038] Example 5

[0039] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 78kg of natural desert sand, 10kg of water-based environmentally friendly plant dye, 18kg of purified water, 3.5kg of water-soluble environmentally friendly color-fixing glue, and 0.25kg of natural anti-mildew and antibacterial agent.

[0040] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using an 80-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 80-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0041] Example 6

[0042] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 80kg of natural desert sand, 12kg of water-based environmentally friendly plant dye, 20kg of purified water, 4kg of water-soluble environmentally friendly color-fixing glue, and 0.3kg of natural anti-mildew and antibacterial agent.

[0043] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using an 80-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 80-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0044] Example 7

[0045] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 70kg of natural desert sand, 12kg of water-based environmentally friendly plant dye, 20kg of purified water, 1kg of water-soluble environmentally friendly color-fixing glue, and 0.1kg of natural anti-mildew and antibacterial agent.

[0046] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using a 50-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 50-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0047] Example 8

[0048] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 73kg of natural desert sand, 14kg of water-based environmentally friendly plant dye, 25kg of purified water, 2kg of water-soluble environmentally friendly color-fixing glue, and 0.15kg of natural anti-mildew and antibacterial agent.

[0049] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using a 50-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 50-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0050] Example 9

[0051] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials: 75kg of natural desert sand, 15kg of water-based environmentally friendly plant dye, 30kg of purified water, 3kg of water-soluble environmentally friendly color-fixing glue, and 0.2kg of natural anti-mildew and antibacterial agent.

[0052] In step S2 of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand, the dried sand is graded and screened using a 50-mesh standard sieve. After screening, the sand is stored separately in sealed containers to obtain spare natural desert sand. In step S3, the spare natural desert sand obtained from the 50-mesh sieve, water-based environmentally friendly plant dye, and purified water are mixed according to the specified ratio and stirred at room temperature for 12.5 minutes to obtain the dyeing material.

[0053] Example 10

[0054] The only difference between this embodiment and Embodiment 1 is that the preparation process of the cloisonné enamel painting base glaze based on natural desert sand includes the following steps: S1. Select a sunny slope of the original desert and collect the top 0-20cm of original fine sand. Manually remove large particles such as stones, dead branches, and weeds. Then, soak it in pure water for 8 minutes and rinse it twice to remove dust, soil and soluble salts from the sand to obtain clean sand.

[0055] S2. Spread the washed sand evenly on a dustproof tray with a thickness of 2cm. Dry it in a ventilated environment at 20-35℃, turning it over evenly every 1 hour. Dry it until the moisture content is between 2-3%. Use a 120-mesh standard sieve to grade and screen the dried sand. After screening, seal and store it separately to obtain the natural desert sand for later use.

[0056] S3. According to the ratio, the prepared natural desert sand obtained by sieving through a 120-mesh sieve, water-based environmentally friendly plant dye, and purified water are stirred at room temperature for 10 minutes to obtain the dyeing material. Water-soluble environmentally friendly color-fixing glue and natural anti-mildew and antibacterial agent are added to the dyeing material. After stirring for 5 minutes, the mixture is spread out to a thickness of 2cm and dried in a ventilated environment at 20-35℃ for 2 hours to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0057] Example 11

[0058] The only difference between this embodiment and Embodiment 1 is that the preparation process of the cloisonné enamel painting base glaze based on natural desert sand includes the following steps: S1. Select a sunny slope of the original desert and collect the top 0-20cm of original fine sand. Manually remove large particles such as stones, dead branches, and weeds. Then, soak it in pure water for 15 minutes and rinse it 3 times to remove dust, soil and soluble salts from the sand to obtain clean sand.

[0059] S2. Spread the washed sand evenly on a dustproof tray with a thickness of 2cm. Dry it in a ventilated environment at 20-35℃, turning it over evenly every 1 hour. Dry it until the moisture content is between 2-3%. Use a 120-mesh standard sieve to grade and screen the dried sand. After screening, seal and store it separately to obtain the natural desert sand for later use.

[0060] S3. According to the ratio, the prepared natural desert sand obtained by sieving through a 120-mesh sieve, water-based environmentally friendly plant dye, and purified water are stirred at room temperature for 15 minutes to obtain the dyeing material. Water-soluble environmentally friendly color-fixing glue and natural anti-mildew and antibacterial agent are added to the dyeing material. After stirring for 5 minutes, the mixture is spread out to a thickness of 2cm and dried in a ventilated environment at 20-35℃ for 4 hours to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0061] Example 12

[0062] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand in this embodiment includes the following raw materials: 85kg of natural desert sand, 6.5kg of water-based environmentally friendly plant dye, 12.5kg of purified water, 4.5kg of water-soluble environmentally friendly color-fixing glue, 0.4kg of natural anti-mildew and antibacterial agent, and 0.05kg of food-grade rheology modifier.

[0063] The S3 step of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand is as follows: According to the formula, the prepared natural desert sand obtained by sieving through a 120-mesh sieve, water-based environmentally friendly plant dyes, and purified water are stirred at room temperature for 12.5 minutes to obtain the dyeing material. Water-soluble environmentally friendly color-fixing glue, natural anti-mildew and antibacterial agent, and food-grade rheology modifier are added to the dyeing material. After stirring for 5 minutes, the mixture is spread out to a thickness of 1 cm and dried in a ventilated environment at 20-35℃ for 3 hours to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0064] Example 13

[0065] The only difference between this embodiment and Embodiment 1 is that the cloisonné enamel painting base glaze based on natural desert sand in this embodiment includes the following raw materials: 85kg of natural desert sand, 6.5kg of water-based environmentally friendly plant dye, 12.5kg of purified water, 4.5kg of water-soluble environmentally friendly color-fixing glue, 0.4kg of natural anti-mildew and antibacterial agent, and 0.2kg of food-grade rheology modifier.

[0066] The S3 step of the preparation process of the cloisonné enamel painting base glaze based on natural desert sand is as follows: According to the formula, the prepared natural desert sand obtained by sieving through a 120-mesh sieve, water-based environmentally friendly plant dyes, and purified water are stirred at room temperature for 12.5 minutes to obtain the dyeing material. Water-soluble environmentally friendly color-fixing glue, natural anti-mildew and antibacterial agent, and food-grade rheology modifier are added to the dyeing material. After stirring for 5 minutes, the mixture is spread out to a thickness of 1 cm and dried in a ventilated environment at 20-35℃ for 3 hours to obtain the cloisonné enamel painting base glaze based on natural desert sand.

[0067] Comparative Example 1 The only difference between this comparative example and Example 1 is that, in the raw materials and preparation process of the cloisonné enamel painting base glaze based on natural desert sand, an equal amount of natural desert sand is used to replace the natural anti-mildew and antibacterial agent.

[0068] Comparative Example 2 The only difference between this comparative example and Example 1 is that, in the raw materials and preparation process of the cloisonné enamel painting base glaze based on natural desert sand, an equal amount of industrial colored sand is used to replace the natural desert sand.

[0069] Comparative Example 3 The only difference between this comparative example and Example 1 is that, in the raw materials and preparation process of the cloisonné enamel painting base glaze based on natural desert sand, an equal amount of chemical dyeing auxiliaries are used to replace the water-based environmentally friendly plant dyes.

[0070] Comparative Example 4 The only difference between this comparative example and Example 1 is that, in the raw materials and preparation process of the cloisonné enamel painting base glaze based on natural desert sand, an equal amount of chemical color-fixing adhesive is used to replace the water-soluble environmentally friendly color-fixing adhesive.

[0071] Performance testing The following performance tests were conducted on Examples 1-13 and Comparative Examples 1-4: Cracking rate after 72 hours of curing: Referring to the initial drying crack resistance test method in GB / T 9779-2015 "Multi-layer architectural coatings", the cracking rate of the cloisonné enamel painting base glaze based on natural desert sand prepared in each example and comparative example was tested after 72 hours of curing.

[0072] Abrasion fastness (grade): Referring to GB / T 3920-2008 "Textiles - Tests for color fastness - Color fastness to rubbing", the abrasion fastness (grade) of the cloisonné enamel painting base glazes based on natural desert sand prepared in each example and comparative example was tested.

[0073] Mildew resistance rating: Referring to GB / T 24128-2018 "Test Method for Mildew Resistance of Plastics", the mildew resistance rating of the cloisonné enamel painting base glaze based on natural desert sand prepared in each example and comparative example was tested.

[0074] Heavy metal content (lead, cadmium): The heavy metal content of the cloisonné enamel painting base glaze based on natural desert sand prepared in each example and comparative example was tested with reference to GB 6675.4-2014 "Toy Safety Part 4: Migration of Certain Elements".

[0075] Waste reuse rate: Referring to GB / T 20862-2007 "Guidelines for Calculation of Product Recyclability", the waste reuse rate of the cloisonné enamel painting base glaze based on natural desert sand prepared in each example and comparative example was tested.

[0076] Carbon emissions per unit of production capacity (kg / ton): In accordance with GB / T 32150-2015 "General Rules for Accounting and Reporting of Greenhouse Gas Emissions of Industrial Enterprises", the carbon emissions per unit of production capacity of the cloisonné enamel painting base glaze based on natural desert sand prepared in each example and comparative example were tested.

[0077] The test results are shown in Table 1.

[0078] Table 1

[0079] Combining Example 1 and Comparative Examples 1-4 with Table 1, it can be seen that compared to Example 1, the anti-mildew rating of Comparative Example 1 plummeted from level 0 to level 3, proving that the natural anti-mildew and antibacterial agent is the core component that imparts long-lasting anti-mildew performance to the base glaze and is indispensable. Comparative Example 2 showed comprehensive deterioration in all indicators: cracking rate 15%, rubbing fastness only level 2, anti-mildew level 3, detection of heavy metals, 0% reuse rate, cycle 72h, and carbon emissions 1200 kg / ton. This demonstrates the comprehensive superiority of the technical solution of this invention compared to existing industrial colored sand. The rubbing fastness of Comparative Example 3 dropped to level 3, and heavy metals were detected. This indicates that although chemical dyes can provide color, their adhesion and safety are far inferior to plant dyes. The rubbing fastness of Comparative Example 4 dropped to level 3, and heavy metals were detected. This indicates that food-grade environmentally friendly color-fixing adhesive, while ensuring safety, has better adhesion performance than chemical color-fixing adhesives. Comparative Examples 1–4 confirmed the synergistic necessity of antifungal and antibacterial agents, desert sand, plant dyes, and environmentally friendly color-fixing adhesives. The replacement or absence of any component would lead to a significant decrease in at least one core performance indicator.

[0080] Based on Examples 1-13 and Table 1, it can be seen that no cracking occurred in Examples 1-13 after 72 hours of curing; the abrasion resistance reached level 4; the mildew resistance reached level 0; the lead and cadmium content were "not detected"; after soaking in clean water for decolorization, ultrasonic cleaning, drying and sieving, the proportion of waste base glaze that can be reused for dyeing is as high as 90% or more; the whole process only requires six room temperature steps: collection, cleaning, drying, sieving, dyeing, and color fixing and drying, without the need for high-temperature calcination, and the production cycle of a single batch is controlled at about 8 hours; the entire process is carried out at room temperature, with no high-temperature kiln energy consumption.

[0081] This is likely because the smooth, porous desert sand forms the physical framework, while pure water acts as a medium, carrying plant dyes that penetrate the micropores of the sand for internal coloring. Food-grade polyvinyl alcohol (PVA) fixing agent forms a coating on the particle surface via hydrogen bonds, locking in the dye. Natural antifungal and antibacterial agents, together with the fixing agent film, construct a dual protective system of surface antibacterial and moisture barrier. Rheology modifiers precisely control the slurry consistency to adapt to different operating scenarios. These six components form a complete functional closed loop; the absence of any component or its replacement with industrial-grade raw materials will lead to a break in the synergistic chain and a comprehensive deterioration of performance.

[0082] S1 involves directional collection of surface sand from a sunny slope and washing to remove impurities, laying the foundation for precise water control in the subsequent process. S2 controls the moisture content within the optimal window of 2%–3%, ensuring that particles do not stick together for smooth sieving while maintaining surface activity for uniform dyeing. Three-stage sieving ensures uniform particle size within the same batch, fundamentally eliminating color differences. S3 involves room-temperature stirring to allow for full dye penetration, and composite color fixing allows the fixing adhesive and anti-mildew agent to form a film and lock in place in one step. Slow secondary drying prevents the coating film from cracking. The output quality of each step (S1, S2, S3) directly determines the input conditions for the next step. The entire process operates at room temperature, eliminating the need for high-temperature equipment, ensuring safety and low energy consumption from the outset.

[0083] Using desert sand as the main material significantly reduces costs and ensures independent control of the industrial chain; the rounded sand particles and the hydrogen bond of the color-fixing adhesive reduce the curing crack rate to 0% and the abrasion fastness to level 4; the anti-mildew and antibacterial agent and the PVA moisture-proof film work together to achieve a mildew resistance level of 0; all food-grade raw materials ensure zero detection of heavy metals; three-stage screening and three-level ratio linkage achieve suitability for all age groups over 6 years old; the physical adsorption properties of plant dyes enable the reuse rate of waste after washing and decolorization to exceed 90%.

[0084] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A cloisonné enamel painting base glaze based on natural desert sand, characterized in that, The raw materials include the following parts by weight: 70-90 parts natural desert sand, 5-15 parts water-based environmentally friendly plant dye, 10-30 parts purified water, 1-5 parts water-soluble environmentally friendly color-fixing glue, and 0.1-0.5 parts natural anti-mildew and antibacterial agent.

2. The cloisonné enamel painting base glaze based on natural desert sand as described in claim 1, characterized in that, The natural desert sand is the fine sand on the surface of the sunny slope of the original desert, ranging from 0 to 20 cm.

3. The cloisonné enamel painting base glaze based on natural desert sand as described in claim 1, characterized in that, It also includes the following raw materials in parts by weight: 0.05 to 0.2 parts of food-grade rheology modifier.

4. The cloisonné enamel painting base glaze based on natural desert sand as described in claim 1, characterized in that, The water-soluble, environmentally friendly color-fixing adhesive is food-grade polyvinyl alcohol.

5. The cloisonné enamel painting base glaze based on natural desert sand as described in claim 1, characterized in that, By weight, in a teaching setting for children aged 6-9, the cloisonné enamel painting base glaze based on natural desert sand includes the following raw materials in parts by weight: 80-90 parts natural desert sand, 5-8 parts water-based environmentally friendly plant dyes, 10-15 parts purified water, 4-5 parts water-soluble environmentally friendly color-fixing glue, and 0.3-0.5 parts natural anti-mildew and antibacterial agent. For general teaching and cultural and creative scenarios for children aged 10-16, the cloisonné enamel painting base glaze based on natural desert sand comprises the following raw materials in parts by weight: 75-80 parts natural desert sand, 8-12 parts water-based environmentally friendly plant dyes, 15-20 parts purified water, 3-4 parts water-soluble environmentally friendly color-fixing glue, and 0.2-0.3 parts natural anti-mildew and antibacterial agent. For professional creative scenarios for children aged 16 and above, the cloisonné enamel painting base glaze based on natural desert sand comprises the following raw materials in parts by weight: 70-75 parts natural desert sand, 12-15 parts water-based environmentally friendly plant dyes, 20-30 parts purified water, 1-3 parts water-soluble environmentally friendly color-fixing glue, and 0.1-0.2 parts natural anti-mildew and antibacterial agent.

6. A preparation process for a cloisonné enamel painting base glaze based on natural desert sand as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Collect fine sand from the pristine desert, manually remove impurities, soak in pure water for 8-15 minutes, and rinse 2-3 times to obtain clean sand. S2. Dry the washed sand in a ventilated environment at 20-35℃ until the moisture content is 2-3% to obtain ready-to-use natural desert sand. S3. According to the ratio, mix the prepared natural desert sand, water-based environmentally friendly plant dye, and pure water at room temperature for 10-15 minutes to obtain the dyeing material. Add water-soluble environmentally friendly color-fixing glue and natural anti-mildew and antibacterial agent to the dyeing material, stir and dry to obtain the cloisonné enamel painting base glaze based on natural desert sand.

7. The preparation process of the cloisonné enamel painting base glaze based on natural desert sand according to claim 6, characterized in that, In step S2, the sand is spread out to a thickness of 1-3 cm and turned over evenly every hour during the drying process.

8. The preparation process of the cloisonné enamel painting base glaze based on natural desert sand according to claim 6, characterized in that, In step S3, after adding water-soluble environmentally friendly color-fixing adhesive and natural anti-mildew and antibacterial agent, stir at low speed for 5 minutes, spread the mixture to a thickness of 1-2 cm, and dry it in a ventilated environment at 20-35℃ for 2-4 hours.

Citation Information

Patent Citations

  • Cloisonn production process

    CN109177626A

  • Self-generated glazed enamel porcelain mud and technology for preparing enamel porcelain by adopting the same

    CN109650848A