A wide-temperature-range, low-viscosity kiln-transformed crystalline glaze and its preparation method

By combining a composite crystal nucleus structure with a dispersant, the problems of easy thickening in the water-based glaze slurry stage and easy dissolution in the firing stage of zinc-silicon crystalline glaze are solved, achieving low viscosity stability of the glaze slurry and uniform precipitation of crystal flowers within a wide temperature range, thus improving the fluidity of glaze application and the stability of crystal flowers.

CN123105993APending Publication Date: 2026-11-17FOSHAN TAOYING NEW MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611409266.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing zinc-silicon crystalline glazes tend to thicken during the water-based glaze slurry stage and dissolve prematurely during the firing stage, making it difficult to simultaneously achieve high solids content glaze fluidity and wide temperature range crystallization stability.

Method used

A composite nucleus structure is adopted, including a wollastonite support activated by limited acid, a zinc-titanium composite oxide layer, and an aluminum-boron-silicon amorphous layer, forming a sequential mechanism of "slurry isolation - temperature-induced crystallization - multi-interface nucleation". Sodium polyacrylate and sodium hexametaphosphate provide steric hindrance and electrostatic repulsion, and sodium carboxymethyl cellulose forms a reversible weak network to reduce ion activity and particle bridging.

Benefits of technology

It achieves low viscosity stability of glaze slurry and uniform precipitation of crystals over a wide temperature range, avoiding the problems of glaze slurry thickening and uneven crystal formation, and improving the fluidity of glaze application and the stability of crystal formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze and its preparation method, belonging to the field of ceramic glaze technology. The crystalline glaze comprises frit, potassium feldspar, quartz, calcined kaolin, zinc oxide, wollastonite, dolomite, composite nuclei, colorant, water, sodium polyacrylate, sodium hexametaphosphate, and sodium carboxymethyl cellulose. The composite nuclei use wollastonite activated by limited acid as a carrier, and its surface sequentially has a zinc-titanium composite oxide layer and an amorphous coating layer containing aluminum borosilicate. The amorphous coating layer inhibits the dissolution of active ions and particle bridging in the aqueous glaze slurry, and gradually softens during firing, allowing the zinc-titanium composite oxide and the wollastonite carrier to form heterogeneous nucleation interfaces with different thermal stability. The composite nuclei, combined with a composite dispersion system, is beneficial for balancing the fluidity of high-solids-content glaze slurries with crystallization stability at different peak firing temperatures, making it suitable for daily-use ceramics, architectural ceramics, and decorative art ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of ceramic glaze technology, specifically relating to a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze and its preparation method. Background Technology

[0002] Kiln-transformed crystalline glazes are decorative glazes in which controlled crystallization occurs within the glaze layer during firing and cooling, resulting in radial, platy, star-shaped, or clustered crystal flowers. Zinc silicate crystalline glazes typically achieve crystal flowers by increasing the ZnO and SiO2 content and adding nucleating components such as TiO2, and by setting a crystallization holding zone after melting. The number, size, and boundaries of the crystal flowers are jointly influenced by the glaze composition, particle fineness, glaze layer thickness, peak temperature, cooling rate, and crystallization holding regime.

[0003] Patent application CN101481261A discloses the direct addition of titanium oxide and zinc oxide to a pyroxene-based glaze; patent application CN109809695A discloses a crystalline glaze composed of glass powder, zinc oxide, titanium dioxide, kaolin, and barite, utilizing the slow degassing of barite at high temperatures to control crystal size; patent application CN105565907A discloses a crystal-inducing glaze composed of zinc oxide, quartz, and titanium oxide, achieving kiln-transformed crystal patterns through targeted glazing. These methods primarily regulate crystallization through the basic formula, nucleating agent dosage, bubble formation, or glaze application location.

[0004] Under water-based glazing conditions, the surface hydration, ion dissolution, and high specific surface area of ​​zinc oxide, fine-grained TiO2, silicate minerals, and clay components enhance the electrostatic bridging and spatial network between particles. Especially when reducing water content and increasing solid content, the glaze slurry is prone to increased apparent viscosity, excessive thixotropy, uneven atomization in the spray gun, or hard sedimentation after storage. Simply increasing the dispersant may lead to a decrease in the drying strength of the glaze layer or adsorption competition on different mineral surfaces. On the other hand, directly added fine-grained nucleating agents tend to dissolve rapidly into the glass phase during heating; when the peak temperature or holding time changes, the number of effective crystal nuclei and supersaturation fluctuate accordingly, making it difficult to simultaneously achieve optimal crystal density, size, and glaze flow.

[0005] Therefore, there is a need for a crystallization promoting component that has low ionic activity and particle bridging tendency in water-based glaze slurry, and can gradually interact with the glaze melt during firing while retaining the heterogeneous nucleation interface, so as to alleviate the problem of difficulty in achieving both high solids content glaze fluidity and wide temperature range crystallization stability. Summary of the Invention

[0006] This invention addresses the problem that active nucleating components in existing zinc-silicon crystalline glazes tend to cause thickening in the aqueous glaze slurry stage and premature dissolution in the firing stage, making it difficult to simultaneously achieve high solids content glaze fluidity and crystallization stability over a wide peak temperature range. The invention provides a kiln-transformed crystalline glaze with a wide temperature range and low viscosity, and its preparation method.

[0007] The objective of this invention can be achieved through the following technical solutions: A wide-temperature-range, low-viscosity kiln-transformed crystalline glaze comprises, by weight, 35-45 parts frit, 10-16 parts potassium feldspar, 10-16 parts quartz, 3-6 parts calcined kaolin, 14-20 parts zinc oxide, 5-10 parts wollastonite, 2-5 parts dolomite, 3-6 parts composite crystal nuclei, 0.2-2.5 parts colorant, 38-48 parts water, 0.15-0.35 parts sodium polyacrylate, 0.05-0.20 parts sodium hexametaphosphate, and 0.08-0.20 parts sodium carboxymethyl cellulose; the composite crystal nuclei comprise a wollastonite carrier activated by limited acid, a zinc-titanium composite oxide layer anchored to the surface of the carrier, and an aluminum-boron-silicon amorphous layer coating the outer side of the zinc-titanium composite oxide layer.

[0008] This invention uses wollastonite activated by limited acid as a carrier, forming a silicon-rich hydroxyl anchoring interface while maintaining the wollastonite framework. This allows the zinc-titanium precursor to preferentially deposit on the carrier surface, reducing the agglomeration of zinc-titanium components as free fine particles. The zinc-titanium composite oxide layer provides a heterogeneous nucleation interface with compositional correlation to the zinc silicate crystalline phase. The wollastonite carrier and the zinc-titanium layer have different dissolution and reaction rates, forming nucleation sources with staggered formation times during the heating and crystallization holding stages, which helps reduce the dependence of the number of effective crystal nuclei on a single peak temperature. The aluminum borosilicate amorphous layer isolates the inner active surface during the aqueous glaze stage, reducing Zn²⁺. + Ca² + The rapid dissolution of plasma and the resulting particle bridging occur during the firing stage. The amorphous layer first becomes compatible with the base glaze melt and gradually softens, reducing its shielding effect on the zinc-titanium layer, thus achieving a phased division of labor between slurry stabilization and firing crystallization. Sodium polyacrylate and sodium hexametaphosphate provide steric hindrance-electrostatic repulsion and complexation of multivalent ions, respectively, and, in combination with a low amount of sodium carboxymethyl cellulose, reduce the structural thickening of high-solids glaze slurry while maintaining glaze adhesion.

[0009] Furthermore, the D50 of the composite crystal nucleus is 3–10 μm. When the D50 is too small, the particle specific surface area is too large, which easily consumes dispersant and increases the risk of agglomeration. When the D50 is too large, the uniformity of glazing decreases and the effective heterogeneous interface per unit mass is reduced.

[0010] Furthermore, the limited acid activation includes: mixing 100 parts by weight of wollastonite, 20-80 parts by weight of citric acid, and 800-1500 parts by weight of water, treating at 40-65°C for 1-3 hours, and obtaining surface-activated wollastonite through solid-liquid separation, washing, and drying. Citric acid performs limited complexation leaching of the surface Ca, making the surface relatively silica-rich and increasing Si-OH anchoring points; the specified proportions and treatment conditions are used to avoid excessive acid degradation of the wollastonite framework.

[0011] Furthermore, the zinc-titanium composite oxide layer is formed by the following method: 100 parts by weight of surface-activated wollastonite are dispersed in 350-650 parts by weight of water and 250-500 parts by weight of ethanol; 20-45 parts by weight of zinc acetate dihydrate, 15-35 parts by weight of tetrabutyl titanate, 5-15 parts by weight of citric acid, and 1-12 parts by weight of ammonia water with a mass fraction of 10-25% are added to adjust the pH to 7.5-8.5; the reaction is carried out at 50-70°C for 2-5 hours; after drying, it is calcined at 700-850°C for 1-3 hours. The water-ethanol mixed medium regulates the hydrolysis rate of tetrabutyl titanate, the citric acid complexation further mitigates local hydrolysis, and the activated wollastonite surface provides a preferred deposition site; calcination transforms the precursor into a zinc-titanium composite oxide layer attached to the carrier.

[0012] Furthermore, the amorphous aluminum borosilicate layer is formed by the following method: 100 parts by weight of wollastonite with a zinc-titanium composite oxide layer are dispersed in 350-700 parts by weight of water; 20-45 parts by weight of silica sol with a solid content of 30%, 2-6 parts by weight of boric acid, 4-12 parts by weight of aluminum nitrate nonahydrate, and 1-10 parts by weight of nitric acid aqueous solution with a mass fraction of 5-10% are added sequentially to adjust the pH to 4.0-5.5; the mixture is aged at 40-60°C for 1-4 hours; after drying, it is heat-treated at 450-600°C for 1-2 hours. The silica sol forms a continuous framework compatible with the glaze phase, the boron component regulates the softening behavior of the outer layer, the aluminum component improves the stability of the outer layer in the aqueous phase, and the heat treatment causes the three components to form an isolation layer mainly composed of an amorphous morphology.

[0013] Furthermore, the frit comprises, by mass percentage, 55-62% SiO2, 6-10% B2O3, 12-18% Na2O and K2O combined, 6-10% CaO, 4-8% ZnO, and 3-6% Al2O3, with the balance being MgO and unavoidable impurities. This composition enables the frit to form a glassy phase with appropriate viscosity and zinc silicate crystallization ability within the stated firing temperature, and is compatible with the outer layer of the composite crystal nucleus.

[0014] A method for preparing a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze includes the following steps: Surface-activated wollastonite, wollastonite with a zinc-titanium composite oxide layer, and composite crystal nuclei were prepared sequentially. Fused material, potassium feldspar, quartz, calcined kaolin, zinc oxide, wollastonite, dolomite, and composite crystal nuclei were dry-mixed, then water, sodium polyacrylate, and sodium hexametaphosphate were added and the mixture was wet-milled. Sodium carboxymethyl cellulose and a colorant were then added for further dispersion. The mixture was sieved and iron was removed to obtain a kiln-transformed crystalline glaze slurry. Dispersing before adding sodium carboxymethyl cellulose avoids prematurely increasing the viscosity of the continuous phase and reducing the ball milling dispersion efficiency.

[0015] Furthermore, during the wet ball milling process, the mass ratio of glaze to grinding balls is 1:(1.5~2.5), and the ball milling is performed until the D90 is no greater than 45μm. The grinding ball loading and the final particle size jointly control the collision efficiency and particle specific surface area, avoiding coarse particle sedimentation caused by insufficient grinding, and also avoiding surface energy increase and secondary agglomeration caused by over-grinding.

[0016] Furthermore, after adding sodium carboxymethyl cellulose and colorant, continue dispersing for 20-60 minutes, pass through a 250-325 mesh sieve to remove iron, and let stand at 20-30℃ for 12-24 hours. This subsequent dispersion ensures uniform distribution of sodium carboxymethyl cellulose and colorant, while sieving removes coarse particles and iron impurities. Standing allows the dispersant to adsorb and achieve a reproducible thixotropic structure with the glaze slurry.

[0017] Furthermore, the process includes applying glaze slurry to the surface of the ceramic body to form a dry glaze layer of 0.5–1.2 mm thickness and firing it in an oxidizing atmosphere; raising the temperature to 1160–1240 °C at 3–5 °C / min and holding it for 15–40 min; lowering the temperature to 1050–1120 °C at 2–5 °C / min and holding it for crystallization for 40–100 min; and then lowering the temperature to 900 °C at 1–3 °C / min before cooling it in the furnace. The glaze layer thickness provides space for crystal growth, the peak temperature phase homogenizes the glass phase and softens the outer layer, the controlled cooling and crystallization holding exposes the zinc-titanium layer and wollastonite interface sequentially and promotes the nucleation and growth of zinc silicates, and the slow cooling stage reduces the thermal stress of the glaze layer.

[0018] The beneficial effects of this invention are: (1) The basic glass network in this invention consists of 35-45 parts of frit, 10-16 parts of potassium feldspar, 10-16 parts of quartz, and 3-6 parts of calcined kaolin: the frit provides the pre-melted borosilicate glass phase and the low-temperature liquid phase, reducing the heat load required for complete melting; potassium feldspar supplements alkali metal oxides and Al2O3, adjusting the melt viscosity and thermal expansion; quartz continuously provides SiO2, enabling the melt to reach the silicon supersaturation state required for zinc silicate crystallization during cooling; calcined kaolin supplements Al2O3 and improves the suspension of the glaze slurry and the high-temperature viscosity of the melt. 14-20 parts of zinc oxide are both a fluxing component and the main zinc source for zinc silicate crystals; 5-10 parts of wollastonite provide CaO and SiO2, and 2-5 parts of dolomite provide Ca²⁺. + Mg²+ At high temperatures, these components act as network-modifying ions to reduce the initial melt viscosity. During the cooling stage, they regulate crystal nucleation and growth by altering the local diffusion rate and interfacial energy. The proportions of these components ensure that the glaze melts fully at 1160–1240℃ without excessive fluxing and severe glaze flow. A balance is achieved between high crystallization driving force and melt support capacity, reducing the three opposing risks of insufficient crystallization, crystal coarsening, and glaze flow. Colorant, at 0.2–2.5 parts within a specified dosage, imparts a kiln-transformed base color and creates a color difference with the crystallization. Simultaneously, it avoids excessive transition metal oxides altering the melt's redox state or disturbing crystallization. Its addition after the composite crystal nuclei and continued dispersion help reduce localized color patches and non-target nucleation points.

[0019] (2) The composite nuclei used in this invention, in parts 3 to 6, adopt a three-level structure of “wollastonite carrier activated by limited acid – zinc-titanium composite oxide layer – aluminum borosilicate amorphous layer”. Limited acid activation removes part of the surface Ca and forms a silicon-rich hydroxyl layer without destroying the main skeleton of wollastonite, increasing the subsequent anchoring points; the zinc-titanium composite oxide layer is confined and fixed on the carrier surface, and its Zn / Ti related interface reduces the nucleation barrier of zinc silicate heterogeneous phase; the aluminum borosilicate amorphous layer isolates the active surfaces of Zn and Ca in the aqueous glaze slurry stage, inhibiting ion dissolution and particle bridging, and in the heating stage, it is compatible with the basic borosilicate melt and gradually softens. This forms a time sequence mechanism of “slurry isolation – heating crystal release – multi-interface nucleation”, avoiding the thickening, agglomeration and early complete dissolution of the aqueous phase caused by directly adding fine ZnO or TiO2.

[0020] (3) The water used in this invention provides a continuous phase for wet ball milling, dispersant migration and adsorption, and spraying; sodium polyacrylate (0.15-0.35 parts) is adsorbed on the particle surface through carboxylate groups, providing electrostatic repulsion and steric hindrance; sodium hexametaphosphate (0.05-0.20 parts) is adsorbed at the mineral edge and complexes with the aqueous phase Ca². + Mg² + First, the two components reduce the yield structure and high shear viscosity. Sodium carboxymethyl cellulose (0.08–0.20 parts) is added after ball milling to form a reversible weak network at a lower dosage, restoring the low-shear suspension structure and improving the glaze's water retention and drying adhesion strength. Together, these three components create a shear-thinning behavior suitable for glazing. The aforementioned base glaze provides a glassy matrix phase that can crystallize without excessive flow. The tertiary composite nuclei reduce ion activity in the aqueous phase and release their nucleation ability during firing in the order of outer layer softening, zinc-titanium layer exposure, and continuous interface provision by the wollastonite carrier. The composite dispersion system keeps the nuclei and the high-zinc base material homogeneous in water. Because the effective nuclei do not rely entirely on instantaneous formation at a single temperature point, this simultaneously reduces glaze viscosity, avoids hard settling, and maintains stable visible crystals over a wide peak temperature range. Detailed Implementation

[0021] The specific embodiments of the present invention will be described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments.

[0022] Raw materials and general conditions: Wollastonite is selected as powder with a chemical purity of not less than 95% and a D50 of 3–8 μm; zinc oxide, quartz, calcined kaolin, potassium feldspar, and dolomite are ceramic-grade raw materials. The zinc source is zinc acetate dihydrate, the titanium source is tetrabutyl titanate, and the aluminum source is aluminum nitrate nonahydrate. Water is deionized water, and ethanol is anhydrous ethanol. All proportions in each step are by mass.

[0023] The frit used contains, by mass percentage, 58.5% SiO2, 8.0% B2O3, 7.5% Na2O, 5.5% K2O, 8.0% CaO, 7.0% ZnO, 4.5% Al2O3, and 1.0% MgO. After weighing according to the formula, it is melted at 1350–1450℃ until homogeneous, then water-quenched, dried, and pulverized.

[0024] Example 1: Take 100 parts of wollastonite with a D50 of 5.2 μm, 58 parts of citric acid and 1000 parts of water and mix them. Stir at 50℃ and 400 r / min for 2 h. Filter, wash with water until the pH of the last washing solution is 6.5, and dry at 95℃ for 8 h to obtain surface-activated wollastonite M1-1.

[0025] 100 parts of M1-1 were dispersed in 463 parts of water and 338 parts of ethanol. 30 parts of zinc acetate dihydrate were dissolved in 150 parts of water, and 23 parts of tetrabutyl titanate and 10 parts of citric acid were dissolved in 150 parts of ethanol. These solutions were added dropwise to the M1-1 dispersion over 60 minutes. 6 parts of 20% ammonia solution were added to adjust the pH to 8.0, and the reaction was carried out at 60°C for 3 hours. The mixture was concentrated under reduced pressure and spray-dried. The temperature was then increased to 780°C at 3°C / min in air and maintained for 2 hours. After cooling, slight depolymerization was observed to obtain M2-1.

[0026] 100 parts of M2-1 were dispersed in 500 parts of water. Then, 30 parts of silica sol (30% solids content), 4 parts of boric acid, 7.4 parts of aluminum nitrate nonahydrate, and 4 parts of nitric acid aqueous solution (8% by mass) were added sequentially to adjust the pH to 4.8. The mixture was stirred at 50℃ for 1 hour and aged for 2 hours. After spray drying, the temperature was increased to 520℃ at a rate of 2℃ / min and held for 1.5 hours. The mixture was then depolymerized using an air jet mill until the D50 was 5–8 μm, yielding the composite crystal nucleus M3-1.

[0027] Weigh out 40 parts by weight of frit, 12 parts of potassium feldspar, 12 parts of quartz, 5 parts of calcined kaolin, 16 parts of zinc oxide, 7 parts of wollastonite, 3 parts of dolomite, 4 parts of M3-1, and 1 part of Fe2O3, totaling 100 parts of dry materials. Mix the dry materials except Fe2O3 for 10 min, add 42 parts of water, 0.25 parts of sodium polyacrylate, and 0.10 parts of sodium hexametaphosphate, and wet ball mill at a glaze to grinding ball mass ratio of 1:2.0 until D90 is no greater than 45 μm; add 0.12 parts of sodium carboxymethyl cellulose (prepared as a 2% aqueous solution) and Fe2O3, continue to disperse for 40 min, pass through a 325 mesh sieve to remove iron, and let stand at 25℃ for 18 h to obtain glaze slurry S1.

[0028] S1 was sprayed onto the surface of ceramic test pieces from the same batch that had been bisque-fired at 900℃, and the dried glaze thickness was 0.8±0.1mm. The temperature was increased to 600℃ at 3℃ / min in an oxidizing atmosphere, then increased to 1200℃ at 5℃ / min and held for 25min; the temperature was then decreased to 1080℃ at 3℃ / min and held for 70min, then decreased to 900℃ at 2℃ / min and cooled in the furnace.

[0029] Example 2: M1-2 was obtained by treating 100 parts by weight of wollastonite, 20 parts by weight of citric acid, and 1500 parts by weight of water at 40°C for 3 hours, washing, and drying at 80°C. M2-2 was obtained by taking 100 parts by weight of M1-2, 20 parts by weight of zinc acetate dihydrate, 15 parts by weight of tetrabutyl titanate, 5 parts by weight of citric acid, 650 parts by weight of water, 500 parts by weight of ethanol, and 10 parts by weight of 10% ammonia solution, adjusting the pH to 7.5, reacting at 50°C for 5 hours, drying, and calcining at 700°C for 3 hours. M2-2 was obtained by taking 100 parts by weight of M2-2, 20 parts by weight of silica sol with a solid content of 30%, 2 parts by weight of boric acid, 4 parts by weight of aluminum nitrate nonahydrate, 700 parts by weight of water, and 8 parts by weight of 5% nitric acid aqueous solution, adjusting the pH to 4.0, aging at 40°C for 4 hours, drying, and heat-treating at 450°C for 2 hours.

[0030] Weigh out 44 parts by weight of frit, 10 parts of potassium feldspar, 10 parts of quartz, 4 parts of calcined kaolin, 14 parts of zinc oxide, 7 parts of wollastonite, 4 parts of dolomite, 6 parts of M3-2, and 1 part of Fe2O3. Add 38 parts of water, 0.35 parts of sodium polyacrylate, 0.05 parts of sodium hexametaphosphate, and 0.08 parts of sodium carboxymethyl cellulose. Prepare the slurry according to the feeding sequence of Example 1, with a pellet-to-material mass ratio of 1:1.5. Disperse for 20 minutes, pass through a 250-mesh sieve, and let stand at 20°C for 12 hours. After glazing, raise the temperature to 1160°C at 3°C / min and hold for 40 minutes, lower the temperature to 1050°C at 2°C / min and hold for 100 minutes, then lower the temperature to 900°C at 1°C / min and cool with the furnace.

[0031] Example 3: M1-3 was obtained by treating 100 parts by weight of wollastonite, 80 parts by weight of citric acid, and 800 parts by weight of water at 65°C for 1 hour, washing, and drying at 110°C. M2-3 was obtained by taking 100 parts by weight of M1-3, 45 parts by weight of zinc acetate dihydrate, 35 parts by weight of tetrabutyl titanate, 15 parts by weight of citric acid, 350 parts by weight of water, 250 parts by weight of ethanol, and 3 parts by weight of 25% ammonia solution, adjusting the pH to 8.5, reacting at 70°C for 2 hours, drying, and calcining at 850°C for 1 hour. M2-3 was obtained by taking 100 parts by weight of M2-3, 45 parts by weight of silica sol with a solid content of 30%, 6 parts by weight of boric acid, 12 parts by weight of aluminum nitrate nonahydrate, 350 parts by weight of water, and 2 parts by weight of 10% nitric acid aqueous solution, adjusting the pH to 5.5, aging at 60°C for 1 hour, drying, and heat-treating at 600°C for 1 hour.

[0032] Weigh out 42 parts by weight of frit, 11 parts by weight of potassium feldspar, 12 parts by weight of quartz, 4 parts by weight of calcined kaolin, 16 parts by weight of zinc oxide, 7 parts by weight of wollastonite, 3 parts by weight of dolomite, 4 parts by weight of M3-3, and 1 part by weight of Fe2O3. Add 40 parts by weight of water, 0.30 parts by weight of sodium polyacrylate, 0.10 parts by weight of sodium hexametaphosphate, and 0.10 parts by weight of sodium carboxymethyl cellulose. Prepare the slurry according to the feeding sequence of Example 1, with a ball-to-material mass ratio of 1:2.5. Disperse for 60 minutes, pass through a 325-mesh sieve, and let stand at 30°C for 24 hours. After glazing, raise the temperature to 1180°C at 5°C / min and hold for 15 minutes, lower the temperature to 1070°C at 5°C / min and hold for 80 minutes, then lower the temperature to 900°C at 3°C / min and cool with the furnace.

[0033] Example 4: M1-4 was obtained by treating 100 parts by weight of wollastonite, 35 parts by weight of citric acid, and 1200 parts by weight of water at 45°C for 2.5 h. M2-4 was obtained by taking 100 parts by weight of M1-4, 25 parts by weight of zinc acetate dihydrate, 19 parts by weight of tetrabutyl titanate, 8 parts by weight of citric acid, 550 parts by weight of water, 400 parts by weight of ethanol, and 7 parts by weight of 15% ammonia solution, adjusting the pH to 7.8, reacting at 55°C for 4 h, drying, and then calcining at 740°C for 2.5 h. M3-4 was obtained by taking 100 parts by weight of M2-4, 25 parts by weight of silica sol with a solid content of 30%, 3 parts by weight of boric acid, 6 parts by weight of aluminum nitrate nonahydrate, 600 parts by weight of water, and 5 parts by weight of 6% nitric acid aqueous solution, adjusting the pH to 4.4, aging at 45°C for 3 h, drying, and then heat-treating at 480°C for 2 h.

[0034] Weigh out 38 parts by weight of frit, 14 parts of potassium feldspar, 14 parts of quartz, 5 parts of calcined kaolin, 17 parts of zinc oxide, 6 parts of wollastonite, 2 parts of dolomite, 3 parts of M3-4, and 1 part of Fe2O3. Add 45 parts of water, 0.20 parts of sodium polyacrylate, 0.15 parts of sodium hexametaphosphate, and 0.15 parts of sodium carboxymethyl cellulose. Prepare the slurry and glaze according to Example 1. Hold at a peak temperature of 1220℃ for 25 minutes, then reduce to 1100℃ and hold for 60 minutes for crystallization. The remaining temperature fluctuation conditions are the same as in Example 1.

[0035] Example 5: M1-5 was obtained by treating 100 parts by weight of wollastonite, 70 parts by weight of citric acid, and 900 parts by weight of water at 60℃ for 1.5 h. M2-5 was obtained by taking 100 parts by weight of M1-5, 40 parts by weight of zinc acetate dihydrate, 30 parts by weight of tetrabutyl titanate, 12 parts by weight of citric acid, 400 parts by weight of water, 300 parts by weight of ethanol, and 4 parts by weight of 22% ammonia solution, adjusting the pH to 8.2, reacting at 65℃ for 2.5 h, drying, and then calcining at 820℃ for 1.5 h. M3-5 was obtained by taking 100 parts by weight of M2-5, 40 parts by weight of silica sol with a solid content of 30%, 5 parts by weight of boric acid, 10 parts by weight of aluminum nitrate nonahydrate, 400 parts by weight of water, and 3 parts by weight of 9% nitric acid aqueous solution, adjusting the pH to 5.2, aging at 55℃ for 1.5 h, drying, and then heat-treating at 560℃ for 1 h.

[0036] Weigh out 35 parts by weight of frit, 16 parts of potassium feldspar, 14.5 parts of quartz, 6 parts of calcined kaolin, 18 parts of zinc oxide, 5 parts of wollastonite, 2 parts of dolomite, 3 parts of M3-5, and 0.5 parts of Fe2O3. Add 48 parts of water, 0.15 parts of sodium polyacrylate, 0.20 parts of sodium hexametaphosphate, and 0.20 parts of sodium carboxymethyl cellulose. Prepare the slurry and glaze according to Example 1. Hold at a peak temperature of 1240℃ for 20 minutes, then reduce to 1120℃ and hold for 40 minutes for crystallization. The remaining temperature fluctuation conditions are the same as in Example 1.

[0037] Example 6: Endpoint frit A was prepared, with oxides comprising 55% SiO2, 10% B2O3, 18% Na2O and K2O combined, 10% CaO, 4% ZnO, and 3% Al2O3 by mass percentage. It was prepared according to the melting, water quenching, and pulverizing methods described in Example 1. M3-1 was prepared according to Example 1, and the composite nucleus D50 was reduced to 3.0 μm by air jet milling, designated as M3-6.

[0038] Weigh out 45 parts by weight of frit A, 10 parts by weight of potassium feldspar, 16 parts by weight of quartz, 3 parts by weight of calcined kaolin, 14 parts by weight of zinc oxide, 5 parts by weight of wollastonite, 2 parts by weight of dolomite, 4 parts by weight of M3-6, and 1 part by weight of Fe2O3. Add 43 parts by weight of water, 0.28 parts by weight of sodium polyacrylate, 0.12 parts by weight of sodium hexametaphosphate, and 0.10 parts by weight of sodium carboxymethyl cellulose. Prepare a slurry according to the feeding sequence of Example 1, with a pellet-to-material mass ratio of 1:2.0. Disperse for 35 minutes, pass through a 325-mesh sieve, and let stand at 25°C for 18 hours. After forming a dry glaze layer of 0.5 ± 0.05 mm, raise the temperature to 1200°C at 4°C / min and hold for 25 minutes. Lower the temperature to 1080°C at 3°C / min and hold for crystallization for 70 minutes. Then lower the temperature to 900°C at 2°C / min and cool with the furnace. The resulting sample is designated S6.

[0039] Example 7: Endpoint frit B was prepared with oxides comprising 62% SiO2, 36% B2O, 12% Na2O and K2O combined, 6% CaO, 8% ZnO, and 36% Al2O by mass percentage. It was prepared according to the melting, water quenching, and pulverizing methods described in Example 1. M3-5 was prepared according to Example 5, and the composite nucleus D50 was reduced to 10.0 μm by air jet milling, designated as M3-7.

[0040] Weigh out 35 parts by weight of frit B, 10 parts by weight of potassium feldspar, 10 parts by weight of quartz, 3.5 parts by weight of calcined kaolin, 20 parts by weight of zinc oxide, 10 parts by weight of wollastonite, 5 parts by weight of dolomite, 4 parts by weight of M3-7, and 2.5 parts by weight of Fe2O3. Add 46 parts by weight of water, 0.22 parts by weight of sodium polyacrylate, 0.18 parts by weight of sodium hexametaphosphate, and 0.18 parts by weight of sodium carboxymethyl cellulose. Prepare a slurry according to the feeding sequence of Example 1, with a pellet-to-material mass ratio of 1:2.2. Disperse for 50 min, pass through a 250-mesh sieve, and let stand at 25°C for 20 h. After forming a dry glaze layer of 1.2 ± 0.05 mm, raise the temperature to 1220°C at 4°C / min and hold for 30 min, lower the temperature to 1100°C at 4°C / min and hold for crystallization for 60 min, then lower the temperature to 900°C at 2°C / min and cool with the furnace. The resulting sample is designated S7.

[0041] Comparative Example 1: Similar to Example 1, except that 4 parts of M3-1 were replaced with 4 parts of a mechanical mixture consisting of 3.08 parts of unmodified wollastonite, 0.37 parts of ZnO, 0.18 parts of anatase TiO2, 0.24 parts of SiO2, 0.06 parts of B2O3 and 0.07 parts of Al2O3. The rest of the formulation, slurry preparation and firing conditions remained unchanged. The resulting sample was denoted as D1.

[0042] Comparative Example 2: Similar to Example 1, except that 4 parts of M3-1 were replaced with 4 parts of M1-1, and no zinc-titanium layer was constructed or aluminum borosilicate outer layer was applied. The resulting sample was designated as D2.

[0043] Comparative Example 3: Similar to Example 1, except that 4 parts of M3-1 were replaced with 4 parts of M2-1, and no aluminum borosilicate outer coating was applied. The resulting sample was designated as D3.

[0044] Comparative Example 4: The limited acid activation step of Example 1 was omitted. Instead, 100 parts of unmodified wollastonite were directly used to deposit zinc-titanium precursors and coat the outer layer according to the mass ratio of Example 1. The remaining slurry preparation and firing conditions were the same as in Example 1. The resulting sample was denoted as D4.

[0045] Comparative Example 5: Similar to Example 1, except that 4 parts of M3-1 were replaced with 4 parts of anatase TiO2, while the rest of the formulation, slurry preparation and firing conditions remained unchanged. The resulting sample was denoted as D5.

[0046] Comparative Example 6: Same as Example 1, except that 0.25 parts of sodium polyacrylate and 0.10 parts of sodium hexametaphosphate were not added, while 0.12 parts of sodium carboxymethyl cellulose were retained, and the other conditions remained unchanged. The resulting sample was denoted as D6.

[0047] Comparative Example 7: The composite crystal nucleus was prepared according to Example 1, except that 30 parts of 30% silica sol, 4 parts of boric acid, and 7.4 parts of aluminum nitrate nonahydrate were increased to 62 parts, 8 parts, and 15 parts, respectively, so that the coating layer was significantly thickened; the rest of the formulation, slurry preparation, and firing conditions were the same as in Example 1, and the resulting sample was denoted as D7.

[0048] Comparative Example 8: Similar to Example 1, the only difference is that M3-1 is reduced from 4 parts to 2 parts, and the frit is increased from 40 parts to 42 parts to keep the total dry material amount at 100 parts; the rest of the formulation, pulping and firing conditions remain unchanged, and the resulting low-volume boundary sample of composite nuclei is denoted as D8.

[0049] Comparative Example 9: Similar to Example 1, the only difference is that M3-1 is increased from 4 parts to 7 parts, and the frit is reduced from 40 parts to 37 parts to keep the total dry material amount at 100 parts; the rest of the formula, pulping and firing conditions remain unchanged, and the resulting high-volume composite nucleus boundary sample is denoted as D9.

[0050] Performance testing: 1. Particle size distribution test The D50 and D90 of the glaze slurry and composite crystal nuclei were determined using a laser diffractometer, following the test method specified in GB / T19077-2024 "Particle Size Analysis by Laser Diffraction". The glaze slurry was diluted with deionized water before injection, and the composite crystal nuclei were ultrasonically dispersed in an aqueous solution containing 0.05% sodium hexametaphosphate before injection. Each sample was tested in triplicate.

[0051] 2. Aqueous phase ion dissolution test The powder to be tested was mixed with water at a mass ratio of 1:20, shaken at 25℃ for 24 hours, and then filtered through a 0.22μm filter membrane. The concentrations of Zn and Ca in the filtrate were determined by inductively coupled plasma optical emission spectrometry (ICP-OES) in accordance with GB / T 30902-2014 "Determination of Impurity Elements in Inorganic Chemical Products by Inductively Coupled Plasma Optical Emission Spectrometry (ICP-OES)". Each sample was tested in triplicate.

[0052] 3. Glaze slurry rheological property test The glaze slurry was equilibrated at 25.0±0.5℃ for 30 min, and the shear rate was adjusted from 0.1 s⁻¹ to 0.1 s⁻¹ using a rotational rheometer. - ¹Logarithmic increase to 100s - ¹Reduced back to 0.1s - ¹, Record for 100 seconds - ¹ Apparent viscosity. Each sample was prepared in triplicate, and the mean and standard deviation were reported.

[0053] 4. Static stability test of glaze slurry 100 mL of glaze slurry was placed into a stoppered graduated cylinder and allowed to stand at 25°C for 24 hours. The height of the supernatant was recorded as the proportion of the total liquid column height. After standing for 7 days, the mixture was stirred at the same speed for 5 minutes to observe whether the sediment could be redispersed.

[0054] 5. Characterization of glaze crystal phase and crystal flowers The crystal phase of the glaze layer on the surface of the fired sample was determined by XRD; no less than 5 fields of view were photographed under the same illumination conditions, and the area fraction of crystal flowers, the number of crystal flowers per unit area, the equivalent diameter and its coefficient of variation were calculated using image analysis software.

[0055] 6. Wide-temperature-range firing adaptability test Using the same batch of S1 glaze slurry and body, the samples were fired at peak temperatures of 1160℃, 1180℃, 1200℃, 1220℃ and 1240℃ respectively, with a peak holding time of 25 min, and then cooled to 1080℃ for crystallization holding time of 70 min, with the other conditions being the same; the crystal phase, crystal flower morphology and defects such as glaze flow, pinholes, glaze shrinkage, cracking and glaze peeling were recorded.

[0056] Table 1. Particle size, rheology, static stability, and flower area for each embodiment and comparative example.

[0057] Note: The data is the average value ± standard deviation of three parallel tests; the crystal nucleus D50 corresponds to the composite crystal nucleus used in each sample (D6, D8, and D9 use M3-1, while the other comparative examples did not use the three-level composite crystal nucleus of this invention, so "—" indicates that they are not applicable); the crystal flower area fraction was determined under the uniform peak firing condition of 1200℃; although D9 has a higher crystal flower area, it also shows crystal flower crowding, increased size dispersion, and a small number of pinholes, so it cannot be judged as having superior overall performance based solely on the crystal flower area.

[0058] Table 2. Results of 24-hour aqueous phase ion dissolution of composite crystal nuclei and control powders

[0059] Note: Data are the average of three parallel tests ± standard deviation; the ICP-OES detection limits for Zn are 0.005 mg / L and for Ca are 0.003 mg / L.

[0060] Table 3 shows the wide-temperature-range firing results of S1 and D1 at different peak temperatures.

[0061] Note: The area, number, and equivalent diameter of S1 are the average value ± standard deviation of 5 fields of view; D1 is a mechanically mixed substitute sample, and only the temperature stability of the area of ​​the crystal flowers is compared. "—" indicates that this parameter was not statistically analyzed.

[0062] As shown in Tables 1 and 2, the apparent viscosity of S1 relative to the mechanically mixed substitute sample D1 decreased from 508 mPa·s to 283 mPa·s, a reduction of approximately 44.3%; the area fraction of crystal flowers increased from 23.6% to 42.7%, an increase of 19.1 percentage points; the proportion of the supernatant layer at 24 h decreased from 7.1% to 1.4%; and the 7-day sediment improved from "difficult to redisperse" to "redispersible". The mechanism is not a simple addition of the components in the mechanical mixture: limited acid activation causes the zinc-titanium precursor to preferentially anchor on the wollastonite surface, and the continuous aluminum-boron-silicon outer layer reduces the activity of Zn and Ca ions in the aqueous phase (the Zn dissolution of M3-1 in Table 2 is only 0.42 mg / L, far lower than the 3.57 mg / L of D1 powder), thereby reducing the bridging between polyvalent ions and polymers and mineral edges; the outer layer softens during firing, and the support-type zinc-titanium interface can still reduce the heterogeneous nucleation barrier.

[0063] Compared to D3 without an aluminum borosilicate outer layer, S1 showed a decrease in apparent viscosity from 457 mPa·s to 283 mPa·s, a reduction of approximately 38.1%; a decrease in Zn dissolution concentration from 2.76 mg / L to 0.42 mg / L, a reduction of approximately 84.8%; and an increase in the crystallization area from 34.7% to 42.7%. This indicates that the appropriate thickness of the outer layer simultaneously provides both aqueous phase isolation and controlled exposure during firing. When the amount of raw material added to the outer layer was increased and the coating layer became too thick in D7, the dissolution of Zn and Ca further decreased to 0.17 mg / L and 0.46 mg / L, respectively, but the crystallization area decreased to 18.7%. This is because an excessively thick aluminum borosilicate layer prolongs the exposure path of the inner layer and reduces the effective nucleus density during the initial stage of crystallization and heat preservation, proving that a thicker isolation layer is not necessarily better.

[0064] Compared to TiO2 substitute sample D5, S1 showed a decrease in apparent viscosity from 438 mPa·s to 283 mPa·s, a reduction of approximately 35.4%, while the crystal flower area increased from 29.6% to 42.7%, an increase of 13.1 percentage points. Compared to D6, which omits sodium polyacrylate and sodium hexametaphosphate, the viscosity decreased from 817 mPa·s to 283 mPa·s, a reduction of approximately 65.4%, while the crystal flower areas of the two were similar (40.8% and 42.7%, respectively). The former comparison supports the difference between supported tertiary crystal nuclei and conventional free TiO2; the latter comparison indicates that the composite crystal nuclei mainly maintain sintering crystallization, and the sodium polyacrylate-sodium hexametaphosphate-sodium carboxymethyl cellulose system mainly establishes a rheological structure of "high shear, low viscosity, and suspension upon standing." The combined use of these two technical characteristics is necessary to achieve the overall effect. Although D6 has a relatively high crystal flower area, its glaze viscosity is as high as 817 mPa·s and it forms a hard deposit after 7 days, lacking sprayability and storage stability.

[0065] When the composite nucleus content in D8 was reduced to 2 parts, the glaze slurry remained relatively fluid (263 mPa·s), but the flower area decreased to 24.8%, indicating insufficient effective heterogeneous interface density. When D9 was increased to 7 parts, although the flower area rose to 45.7%, the apparent viscosity increased to 408 mPa·s, and the supernatant ratio increased to 3.1%. After 7 days, it became "difficult to redisperse," and the glaze surface showed crowded flowers and a small number of pinholes. This is because the high specific surface area of ​​the nuclei consumes dispersant and increases particle collisions, while the excessive number of nucleation sites leads to competitive flower growth. S6 and S7 used composite nuclei with D50 of 3.0 μm and 10.0 μm, respectively, with glaze layer thicknesses of 0.5 mm and 1.2 mm, respectively. Actual measurements showed that both maintained redispersibility and formed a flower area of ​​33.8%–40.6%, demonstrating good overall performance.

[0066] The particle size data in Table 1 show that the D50 of the composite nuclei used in the seven examples is 3.0 to 10.0 μm, and the D90 of each glaze slurry after ball milling is 35.4 to 44.2 μm. The particle size distribution is concentrated and the batch uniformity is good. The appropriate particle size ensures the uniformity of glazing and the number of effective heterogeneous interfaces, which is consistent with the rheological and crystal flower results in Table 1.

[0067] Table 3 compares the crystallization area of ​​S1 and the mechanically mixed substitute sample D1 at five peak temperatures. The crystallization area of ​​S1 ranged from 27.5% to 42.7%, maintaining 30.8% and 27.5% at 1160℃ and 1240℃ respectively, even at temperatures 40℃ below the optimal range, with no severe glaze defects. In contrast, the crystallization area of ​​D1 ranged only from 10.5% to 23.6%, with an optimal value of only 23.6% at 1200℃. At 1240℃, it dropped sharply to 10.5% and showed significant glaze flow, indicating a significant deterioration in crystallization stability with temperature fluctuations. Zn₂SiO₄ crystal phases were detected in S1 at all five temperature points, with equivalent diameters ranging from 1.98 to 2.47 mm. This trend aligns with the different thermal responses of the tertiary interface: the aluminum borosilicate outer layer softens first and interdiffused with the glass; the zinc-titanium layer is subsequently exposed, providing strong nucleation sites; and the wollastonite support and its reaction boundary continue to provide heterogeneous interfaces over a longer period, making the nucleation source not entirely dependent on a single peak temperature for instantaneous formation. At 1240℃, the viscosity of the glass phase decreases and the dissolution of crystal nuclei accelerates, resulting in a decrease in the area and number of S1 crystal flowers and an increase in size dispersion (the coefficient of variation rises to 21.8%). However, controlled cooling and crystallization holding still retain visible crystal flowers, which contrasts sharply with the sharp deterioration of D1. This indicates that the present invention exhibits good crystallization stability and wide-temperature-range firing adaptability within the test temperature range of 1160–1240℃.

[0068] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.

Claims

1. A kiln-transformed crystalline glaze with a wide temperature range and low viscosity, characterized in that, The composition by weight is as follows: 35-45 parts frit, 10-16 parts potassium feldspar, 10-16 parts quartz, 3-6 parts calcined kaolin, 14-20 parts zinc oxide, 5-10 parts wollastonite, 2-5 parts dolomite, 3-6 parts composite crystal nucleus, 0.2-2.5 parts colorant, 38-48 parts water, 0.15-0.35 parts sodium polyacrylate, 0.05-0.20 parts sodium hexametaphosphate, and 0.08-0.20 parts sodium carboxymethyl cellulose; the composite crystal nucleus comprises a wollastonite carrier activated by limited acid, a zinc-titanium composite oxide layer anchored to the surface of the wollastonite carrier, and an aluminum-boron-silicon amorphous layer covering the outside of the zinc-titanium composite oxide layer.

2. The wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 1, characterized in that, The D50 of the composite crystal nucleus is 3–10 μm.

3. The wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 1, characterized in that, The limited acid activation includes: mixing 100 parts by weight of wollastonite, 20-80 parts by weight of citric acid and 800-1500 parts by weight of water, and treating at 40-65°C for 1-3 hours; after solid-liquid separation, washing and drying, surface-activated wollastonite is obtained.

4. The wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 1, characterized in that, The zinc-titanium composite oxide layer is formed by the following method: 100 parts by weight of wollastonite carrier activated by limited acid are dispersed in a mixed medium of 350-650 parts water and 250-500 parts ethanol. 20-45 parts zinc acetate dihydrate, 15-35 parts tetrabutyl titanate, 5-15 parts citric acid, and 1-12 parts ammonia water with a mass fraction of 10-25% are added to adjust the pH of the system to 7.5-8.

5. The reaction is carried out at 50-70°C for 2-5 hours. After drying, the mixture is calcined at 700-850°C for 1-3 hours to obtain a wollastonite carrier with a zinc-titanium composite oxide layer anchored on its surface.

5. The wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 1, characterized in that, The aluminum borosilicate amorphous layer is formed by the following method: 100 parts by weight of wollastonite carrier with a zinc-titanium composite oxide layer anchored on the surface are dispersed in 350-700 parts by weight of water, and 20-45 parts by weight of silica sol with a solid content of 30%, 2-6 parts by weight of boric acid, 4-12 parts by weight of aluminum nitrate nonahydrate, and 1-10 parts by weight of nitric acid aqueous solution with a mass fraction of 5-10% are added sequentially to adjust the pH to 4.0-5.

5. The mixture is then aged at 40-60°C for 1-4 hours; after drying, it is heat-treated at 450-600°C for 1-2 hours.

6. The wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 1, characterized in that, The frit comprises, by mass percentage of oxides: 55-62% SiO2, 6-10% B2O3, 12-18% Na2O and K2O combined, 6-10% CaO, 4-8% ZnO, 3-6% Al2O3, with the balance being MgO and unavoidable impurities.

7. A method for preparing a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze as described in any one of claims 1 to 6, characterized in that, Includes the following steps: Surface-activated wollastonite, wollastonite with zinc-titanium composite oxide layer and composite crystal nucleus are prepared sequentially; frit, potassium feldspar, quartz, calcined kaolin, zinc oxide, wollastonite, dolomite and composite crystal nucleus are dry mixed, water, sodium polyacrylate and sodium hexametaphosphate are added and wet ball milling is performed, then sodium carboxymethyl cellulose and colorant are added to continue dispersion, sieve and remove iron to obtain kiln-transformed crystalline glaze slurry.

8. The method for preparing a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 7, characterized in that, During the wet ball milling process, the mass ratio of glaze to grinding balls is 1:(1.5~2.5), and the glaze particles are milled until the D90 is no greater than 45μm.

9. The method for preparing a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 7, characterized in that, After adding sodium carboxymethyl cellulose and colorant, continue dispersing for 20-60 minutes, pass through a 250-325 mesh sieve to remove iron, and let the resulting glaze slurry stand at 20-30℃ for 12-24 hours.

10. The method for preparing a wide-temperature-range, low-viscosity kiln-transformed crystalline glaze according to claim 7, characterized in that, The process also includes applying the kiln-transformed crystalline glaze slurry to the surface of the ceramic body, drying it to form a glaze layer with a thickness of 0.5 to 1.2 mm, and firing it in an oxidizing atmosphere; raising the temperature at 3 to 5 °C / min to the peak firing temperature of 1160 to 1240 °C and holding it at that temperature for 15 to 40 min, lowering the temperature at 2 to 5 °C / min to 1050 to 1120 °C and holding it at that temperature for 40 to 100 min for crystallization, and after the crystallization holding is completed, lowering the temperature at 1 to 3 °C / min to 900 °C and then cooling it in the furnace.

Citation Information

Patent Citations

  • Titanium, zinc and pyroxene crystal glaze and preparing method thereof

    CN101481261A

  • Production method of flambe crystal pattern seeding color-fixing ceramic tile

    CN105565907A

  • Crystalline glaze and preparation method thereof

    CN109809695A