A low-temperature melting and crystal phase control process for a high-toughness jade crystal material
By using a multi-source fluxing component synergistic formulation and self-exothermic reaction-assisted low-temperature melting, combined with stepwise crystallization heat treatment, the problem of high melting temperature of jade crystal material was solved, realizing the production of jade crystal material with low energy consumption and high performance, improving bending strength and fracture toughness, and realizing the efficient utilization of industrial solid waste.
Patent Information
- Application Number
- CN202611359682.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for reducing the melting temperature of jade crystal materials suffer from problems such as increased melt viscosity, slowed component diffusion, increased chemical inhomogeneity, increased porosity, and decreased mechanical properties. Furthermore, the lack of precise control over the crystal phase leads to high production costs and poor performance.
A multi-source fluxing component synergistic formulation design is adopted, combined with self-exothermic reaction-assisted low-temperature melting and stepwise crystallization heat treatment. The crystal phase is controlled by differential scanning calorimetry to form a multi-scale toughened structure, including the combination of basic components and three types of fluxes. The self-exothermic reaction is triggered to achieve viscosity control of glass melt at low temperature, and columnar/fibrous grains are formed through stepwise crystallization.
It achieves a reduction in low-temperature melting temperature by 100-400℃, a reduction in energy consumption by 20%-30%, a reduction in porosity to 0.22%-0.28%, and an increase in flexural strength and fracture toughness by 17%-53%. It also enables the efficient utilization of industrial solid waste and green, low-carbon production.
Smart Images

Figure CN123105997A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic non-metallic materials and microcrystalline glass preparation technology, and in particular to a low-temperature melting and crystal phase control process for a high-toughness jade crystal material. Background Technology
[0002] Microcrystalline glass (also known as glass-ceramic) is a composite material formed by controlling the heat treatment of base glass to precipitate microcrystals. It combines the advantages of glass in forming and processing with the high strength, high hardness, and corrosion resistance of ceramics, making it widely used in architectural decoration, electronic display cover plates, and other fields. Traditional microcrystalline glass typically requires melting temperatures above 1500℃, resulting in extremely high energy consumption, significant refractory material loss in the kiln, and high production costs.
[0003] To lower the melting temperature, several technologies have been explored. For example, adding slag can reduce the melting temperature by 50–100°C, or combining high-sodium, low-silicon waste slag with high-silicon, low-calcium gasification slag can lower the melting temperature to 1100–1400°C. Furthermore, silicate polymerization and exothermic melting technology can initiate a solid-phase exothermic reaction at a relatively low external trigger temperature, utilizing the heat released by the reaction itself to reach the melting temperature.
[0004] However, the existing technology still has the following shortcomings: (1) There is a contradiction between low temperature melting and high densification. The lower melting temperature leads to increased melt viscosity, slower component diffusion, increased chemical inhomogeneity of glass melt, increased porosity and decreased mechanical properties in the subsequent crystallization stage; (2) There is a lack of systematic research on the synergistic effect of multi-source fluxing components, and the fluxing effect is not fully utilized; (3) There is a lack of process synergy in the whole chain of melting-crystallization. The crystallization system design does not consider the influence of melting history on glass structure, that is, there is a lack of fine control over the crystal phase; (4) The influence mechanism of thermal history on crystallization behavior is unclear.
[0005] Therefore, developing a low-temperature melting and crystal phase control process for high-toughness jadeite materials that systematically and synergistically matches composition design and melting process, and can effectively control crystal phase, has become an urgent technical problem to be solved in this field. Summary of the Invention
[0006] The purpose of this invention is to provide a low-temperature melting and crystal phase control process for high-toughness jade crystal materials to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] 1. Synergistic formulation design of multi-source fluxing components
[0009] The basic components are mainly industrial solid waste (slag, fly ash, red mud, coal gangue, etc.), with the following weight percentages: SiO2: 45%–60%, CaO: 15%–25%, Al2O3: 5%–12%, MgO: 2%–8%, Fe2O3 / FeO: 0.5%–5%. Three types of fluxing agents are added:
[0010] Type A (Na2O / K2O): 2%–8%, introduced by carbonates or nitrates, its function is to “open” the network structure;
[0011] Type B (MgO / ZnO): 3%–10%, introduced as oxides, serving as a “flexible” network;
[0012] Type C (CaF2 / B2O3): 1%–4%, its function is to improve interfacial wettability.
[0013] The three types of fluxes form a synergistic chain of "opening-flexibility-lubrication", which makes the viscosity of the glass melt η≤100Pa·s at 1100~1400℃.
[0014] 2. Self-exothermic reaction-assisted low-temperature melting
[0015] The self-exothermic reaction system is added at 10%–30% of the total mass of the base components and consists of activated coal gangue, red mud, and a boron-containing mineralizer (borax or boric acid). The mass ratio of activated coal gangue to red mud is 4:3–2:1, and the boron-containing mineralizer accounts for 2%–8% of the mass of the self-exothermic reaction system. The exothermic reaction of silicate polymerization is triggered at 700℃±50℃, with an exothermic enthalpy of… Self-sustaining melting can be achieved at ≥200 J / g.
[0016] 3. Synergistic matching and crystal phase control of the entire melting-crystallization process chain
[0017] The properties of glass at different melting temperatures were determined by differential scanning calorimetry (DSC). The activation energy for crystallization was calculated using the Kissinger equation. :
[0018]
[0019] In the formula, β is the heating rate (K / min). R is the crystallization peak temperature (K), R is the gas constant (8.314 J / (mol·K)), and C is a constant.
[0020] Establish and The association model: when At ≤1250℃, the nucleation time is 30–60 min, and the nucleation temperature tends to be... +50℃; when At ≥1400℃, the nucleation time is 90–150 min, and the nucleation temperature tends to be... -50℃.
[0021] 4. Stepwise crystallization heat treatment (core of crystal phase control)
[0022] Nucleation stage: Heating at 2-5℃ / min to Keep warm for 30–150 minutes;
[0023] First step crystallization: Increase the temperature by 1-3℃ / min to Hold at this temperature for 60–120 minutes to generate equiaxed primary grains;
[0024] Second step crystallization: Increase the temperature by 1-3℃ / min to... Hold at a temperature of 90–180 min to induce directional growth of columnar / fibrous grains, forming a multi-scale toughened structure with interlaced columnar crystals and filled granular crystals (columnar crystal aspect ratio ≥ 5).
[0025] Annealing stage: Cool to room temperature at 1-2℃ / min.
[0026] Compared with the prior art, the beneficial effects of the present invention are:
[0027] (1) The melting temperature is reduced by 100-400℃, and energy consumption is reduced by 20%-30%;
[0028] (2) The porosity of the finished product is as low as 0.22% to 0.28%, which is lower than the 0.35% of the traditional high-temperature melting method;
[0029] (3) The flexural strength reaches 138.5~152.6MPa, and the fracture toughness reaches 3.92~4.35MPa·m^{1 / 2}, which are 17%~29% and 38%~53% higher than those of the traditional high-temperature melting method, respectively;
[0030] (4) Using industrial solid waste as the main raw material, the solid waste utilization rate is ≥60%, achieving green and low-carbon production;
[0031] (5) Through composition-process synergistic design and step-by-step crystallization phase control, the process adaptability is strong and the development cycle is short. Attached Figure Description
[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0033] Figure 1 This is a flow chart of a low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to the present invention.
[0034] Figure 2 The above are the performance test results for Embodiment 1 of the present invention;
[0035] Figure 3 The above are the performance test results for Embodiment 2 of the present invention;
[0036] Figure 4 The results are the performance test results of Comparative Example 1 of this invention. Detailed Implementation
[0037] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0038] Please see Figures 1 to 4 The technical solution provided by this invention:
[0039] Example 1
[0040] (1) Raw material preparation
[0041] Basic components: 35% activated coal gangue, 25% red mud, 20% fly ash, 10% quartz sand, 10% limestone. Added fluxes: Type A (Na2O) 5%, Type B (MgO) 4%, Type C (CaF2) 2%. Self-exothermic reaction system: 8% activated coal gangue, 6% red mud, 2% borax (by mass of basic components).
[0042] (2) Low-temperature melting
[0043] Melting temperature 1250℃, time 2.5h. An exothermic reaction is triggered at 700℃, and the system self-heats to approximately 1150℃. Melt viscosity was measured. (1350℃). DSC: , , (10℃ / min). Calculated using the Kissinger equation. .
[0044] (3) Calendering: to make a 10mm thick glass plate.
[0045] (4) Stepwise crystallization heat treatment (crystal phase control)
[0046] Nucleation: 3℃ / min to 690℃, hold for 90min; First step crystallization: 2℃ / min to 840℃, hold for 90min; Second step crystallization: 2℃ / min to 890℃, hold for 150min; Annealing: 1.5℃ / min cooling.
[0047] (5) Post-processing: coarse grinding, fine grinding, polishing.
[0048] Properties: Porosity 0.28%, density 2.71 g / cm³ 3 It has a flexural strength of 138.5 MPa, a fracture toughness of 3.92 MPa·m^{1 / 2}, a water absorption rate of 0.06%, and a Vickers hardness of 7.8 GPa. The main crystalline phases are diopside and anorthite; the microstructure consists of columnar crystals with an aspect ratio of 5–10 and equiaxed nanocrystals of approximately 200 nm.
[0049] Example 2
[0050] (1) Raw material preparation
[0051] Basic components: 40% activated coal gangue, 20% red mud, 15% fly ash, 15% quartz sand, 10% limestone. Fluxes: Type A (K2O) 4%, Type B (MgO+ZnO 1:1) 6%, Type C (B2O3) 2.5%. Self-exothermic reaction system: 10% activated coal gangue, 8% red mud, 2.5% borax.
[0052] (2) Low-temperature melting
[0053] Melting temperature 1300℃, time 2 hours. An exothermic reaction is triggered at 710℃, self-heating to 1180℃. Melt viscosity... DSC: .
[0054] (3) Calendering: Same as in Example 1.
[0055] (4) Stepwise crystallization heat treatment (crystal phase control)
[0056] Nucleation: 3℃ / min to 700℃, hold for 80min; First step crystallization: 2℃ / min to 855℃, hold for 100min; Second step crystallization: 2℃ / min to 910℃, hold for 180min; Annealing: 1.5℃ / min cooling.
[0057] (5) Post-processing: Same as in Example 1.
[0058] Properties: Porosity 0.22%, density 2.73 g / cm³, flexural strength 152.6 MPa, fracture toughness 4.35 MPa·m^{1 / 2}, water absorption 0.04%, Vickers hardness 8.1 GPa. Main crystalline phases: diopside + enstatite; columnar crystals with an aspect ratio of 6–12, equiaxed nanocrystals approximately 150 nm.
[0059] Comparative Example 1 (Traditional High-Temperature Melting Process)
[0060] Same basic components as in Example 1 (no flux, no self-exothermic reaction), melting temperature 1550℃, one-step crystallization (650℃ / 60min + 900℃ / 180min). Properties: porosity 0.35%, flexural strength 118.2MPa, fracture toughness 2.85MPa·m^{1 / 2}.
[0061] Comparative Example 2 (Low-temperature melting without synergistic process)
[0062] Same flux as in Example 1, no self-exothermic reaction, melting temperature 1250℃, one-step crystallization (same as Comparative Example 1). Properties: porosity 1.2%, flexural strength 85.4MPa, fracture toughness 2.31MPa·m^{1 / 2}.
[0063] Results Analysis
[0064] Examples 1 and 2, at temperatures 250–300°C lower than conventional high-temperature melting processes, exhibited lower porosity and significantly improved flexural strength and fracture toughness (the flexural strength of Example 2 was increased by 29.1% and the fracture toughness by 52.6% compared to Comparative Example 1), verifying the effectiveness of the composition-process synergistic design and crystal phase control strategy of the present invention.
[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-temperature melting and crystal phase control process for a high-toughness jade crystal material, characterized in that, Includes the following steps: (1) Raw material preparation: The basic components are prepared using industrial solid waste as the main raw material, and three types of fluxing agents and a self-exothermic reaction system are added and mixed evenly; the three types of fluxing agents include A-type network modified fluxing agent, B-type intermediate fluxing agent and C-type interfacial active fluxing agent; the A-type fluxing agent is Na2O and / or K2O, introduced in the form of carbonate or nitrate; the B-type fluxing agent is MgO and / or ZnO, introduced in the form of oxide; the C-type fluxing agent is CaF2 and / or B2O3; the self-exothermic reaction system includes activated coal gangue, red mud and boron-containing mineralizer; (2) Low temperature melting: The mixture prepared in step (1) is melted at a temperature of 1100℃~1400℃. During the melting process, the self-exothermic reaction is triggered at 700℃±50℃. The heat released by the reaction is used to assist the melting of the material. After clarification and homogenization, glass melt is obtained. (3) Calendering: The glass melt obtained in step (2) is calendered to form a glass plate of a predetermined thickness; (4) Stepwise crystallization heat treatment: The glass plate obtained in step (3) is subjected to crystallization heat treatment, including nucleation stage, first crystallization stage, second crystallization stage and annealing stage; wherein, the first crystallization temperature is The second step crystallization temperature , This is the crystallization initiation temperature of the glass; (5) Post-processing: The jade crystal blank slab after heat treatment in step (4) is coarsely ground, finely ground and polished to obtain the finished product.
2. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, The weight percentages of the basic components are as follows: SiO2: 45%–60%, CaO: 15%–25%, Al2O3: 5%–12%, MgO: 2%–8%, Fe2O3 / FeO: 0.5%–5%; the amount of the type A flux added is 2%–8% based on the mass of the oxides; the amount of the type B flux added is 3%–10%; and the amount of the type C flux added is 1%–4%.
3. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, The amount of the self-exothermic reaction system added is 10% to 30% of the total mass of the basic components, wherein the mass ratio of activated coal gangue to red mud is 4:3 to 2:1, and the amount of boron-containing mineralizer added is 2% to 8% of the mass of the self-exothermic reaction system.
4. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, During the low-temperature melting process in step (2), the area enthalpy of the exothermic peak of the self-exothermic reaction is determined by differential scanning calorimetry. ,when Self-sustaining melting is achieved at ≥200 J / g. Increase the amount of boron-containing mineralizer when the concentration is <200 J / g.
5. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, The process also includes a crystallization kinetics analysis step: using differential scanning calorimetry to determine the glass transition temperature of the base glass at different melting temperatures. Crystallization initiation temperature and crystallization peak temperature The activation energy for crystallization was calculated using the Kissinger equation. The Kissinger equation is: In the formula, β is the heating rate, with units of K / min; The crystallization peak temperature is given in K; R is the gas constant, taken as 8.314 J / (mol·K); C is a constant. Establish melting temperature With crystallization activation energy The relationship model between them; when The nucleation time is 30–60 min, and the nucleation temperature is biased towards +50℃; when For temperatures ≥1400℃, nucleation time is 90–150 min, with nucleation temperature biased towards… -50℃.
6. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, The specific conditions for the stepwise crystallization heat treatment are as follows: Nucleation stage: Heat at a rate of 2–5 °C / min until… +50℃ -50℃, keep warm for 30-150 minutes, uniform temperature field; First step crystallization: Heat at a rate of 1–3 °C / min to Keep warm for 60–120 minutes; The second step is crystallization: heating at a rate of 1–3 °C / min until… Keep warm for 90–180 minutes; Annealing stage: Cool to room temperature at a cooling rate of 1-2℃ / min.
7. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, In the stepwise crystallization heat treatment, the first step crystallization generates equiaxed primary grains, and the second step crystallization induces the directional growth of columnar or fibrous grains on the basis of the primary grains, forming a multi-scale toughened microstructure with interlaced columnar crystals and filled granular crystals, wherein the aspect ratio of the columnar crystals is ≥5.
8. The low-temperature melting and crystal phase control process for a high-toughness jade crystal material according to claim 1, characterized in that, The viscosity of the glass melt in the low-temperature melting process at 1100℃~1400℃ The porosity of the finished jade crystal product is less than 0.5%, the flexural strength is ≥120MPa, and the fracture toughness is ≥3.5MPa, with a pressure of ≤100Pa·s. .
9. A high-toughness jade crystal material prepared by a low-temperature melting and crystal phase control process according to any one of claims 1 to 8, characterized in that, The jade crystal material is composed of one or more of the following main crystalline phases: diopside, anorthite, and enstatite. Its microstructure consists of columnar crystals with an aspect ratio ≥ 5 and equiaxed nanocrystals with a size ≤ 300 nm. The columnar crystals interweave to form a framework, and the equiaxed nanocrystals fill the gaps between the columnar crystals.
10. The high-toughness jade crystal material according to claim 9, characterized in that, The flexural strength of the jade crystal material is 138.5–152.6 MPa, and the fracture toughness is 3.92–4.35 MPa. Bulk density ≥ 2.69 g / cm³ 3 .