A modified fly ash, its preparation method and application
By using alkali activation, biomineralization, and mechanical ball milling to synergistically treat fly ash, multiple immobilization barriers are formed, solving the problem of low removal efficiency of oxyacid radical-type heavy metals in fly ash and achieving efficient and low-cost heavy metal immobilization.
Patent Information
- Application Number
- CN202611306794.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for removing heavy metals from fly ash have low efficiency in treating oxyanion-type heavy metals (such as Cr(VI) and As), require large amounts of reagents, and are prone to causing secondary pollution.
Alkali activation treatment was used to expose heavy metals, combined with Bacillus subtilis-mediated phosphate biomineralization and mechanical ball milling, and zero-valent iron reduction was used to form multiple fixed barriers, generating insoluble phosphate mineral precipitates and geopolymer gels, thereby increasing the specific surface area.
It significantly improves the removal rate of chromium and arsenic, reduces the amount of reagents used, has low treatment costs, is environmentally friendly, greatly reduces the risk of heavy metal leaching, and meets environmental protection standards.
Smart Images

Figure FT_1 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste harmless treatment and resource utilization technology, specifically relating to a modified fly ash, its preparation method and application. Background Technology
[0002] Fly ash is a major solid waste generated by coal-fired power plants. Although fly ash has broad prospects for resource utilization in building materials, soil improvement, and mine backfilling, it is usually enriched with various heavy metals such as lead, cadmium, chromium, arsenic, copper, zinc, nickel, and mercury. Direct utilization poses a serious risk of environmental leaching. Therefore, pre-treatment of fly ash to reduce its heavy metal leaching toxicity before resource utilization is of significant environmental and engineering value.
[0003] Currently, the main methods for removing heavy metals from fly ash include physical sorting, chemical elution, and mechanochemical methods. Physical sorting methods (such as grading, magnetic separation, and gravity separation) are simple to operate and produce no secondary pollution, but their removal efficiency for heavy metals contained in the glassy crystal lattice is limited. Chemical elution methods (such as acid leaching and complexation) have good treatment effects, but acid leaching or complexation treatments require large amounts of reagents, are costly, and generate large amounts of acidic wastewater. Mechanochemical methods (such as ball milling) can break the glassy coating of fly ash particles through mechanical force, increasing the specific surface area and promoting the release and transformation of heavy metals, but ball milling alone still has room for improvement in removing oxyanion-type heavy metals (such as Cr(VI) and As).
[0004] In summary, existing methods for removing heavy metals from fly ash are inefficient for treating oxyacid radical-type heavy metals (chromium, arsenic), require large amounts of reagents, and are prone to causing secondary pollution. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a modified fly ash, its preparation method, and its application. The method of this invention effectively improves the treatment efficiency for oxyanion-type heavy metals (chromium, arsenic) and reduces the amount of reagents used, while also making the generated wastewater easier to treat.
[0006] To achieve the above objectives, the present invention employs the following technical solution: A method for preparing modified fly ash, characterized by comprising the following steps: Raw fly ash and an alkaline solution are mixed evenly at 60℃~80℃ for alkaline activation treatment to obtain an alkaline fly ash solution; the concentration of the alkaline solution is 0.5mol / L~2mol / L. The concentration of the alkaline solution is 0.5mol / L~2mol / L, which is within the low concentration range of alkali, and can carry out the alkaline activation reaction, while reducing the cost of subsequent washing wastewater.
[0007] The alkaline fly ash solution is cooled to 30℃~40℃, and Bacillus subtilis and organophosphate monoester salts are added for mineralization treatment, so that heavy metal ions form precipitates, and alkaline pretreated fly ash is obtained.
[0008] Alkali-pretreated fly ash, zero-valent iron, and water are mixed evenly and then ball-milled to obtain modified fly ash.
[0009] This invention first employs an alkaline activation treatment. During this process, the alkaline solution erodes the vitreous coating on the surface of the fly ash particles, exposing the heavy metals sealed within. Simultaneously, the alkaline solution reacts with the active SiO2 and Al2O3 in the fly ash to generate a geopolymer gel (hydrated sodium aluminosilicate or hydrated calcium aluminosilicate) with a three-dimensional network structure. This gel, through a triple process of physical encapsulation, chemical bonding, and ion exchange, firmly immobilizes heavy metal ions within its gel framework, achieving highly efficient removal of these ions.
[0010] After the alkaline activation treatment, Bacillus subtilis and organophosphate monoester salts were added to the alkaline fly ash solution. In the alkaline environment, Bacillus subtilis secreted alkaline phosphatase (ALP), which hydrolyzed and broke the phosphate ester bonds in the organophosphate monoester salts, releasing PO4. 3- Ions, released PO4 3- Pb leached from fly ash 2+ Cd 2+ Cu 2+ Ni 2+ Zn 2+ Heavy metal cations rapidly combine to form insoluble phosphate mineral precipitates (such as Pb3(PO4)2, whose solubility product constant Ksp≈10). -44 This process fixes heavy metal ions from the liquid phase into solid minerals. The resulting phosphate mineral particles adhere to the surface of fly ash particles and the geopolymer gel network, forming a triple removal barrier together with the physical encapsulation of the geopolymer and the reduction products of zero-valent iron.
[0011] During subsequent ball milling, mechanical ball milling further refines the fly ash particles, significantly increasing their specific surface area and generating numerous fresh broken bonds and defect sites on the particle surface. These active sites facilitate the penetration of alkaline solutions and the dispersion of zero-valent iron. Simultaneously, the mechanical force of ball milling transforms unstable forms of heavy metals in fly ash (water-soluble, acid-soluble, and reducible forms) into stable residual forms, significantly reducing the risk of environmental leaching. Zero-valent iron is also added during ball milling. Under the mechanical force of ball milling, the zero-valent iron is uniformly dispersed and activated, reducing highly toxic and highly mobile Cr(VI) to less toxic and less mobile Cr(III); and it is itself oxidized to Fe. 2+ Fe 2+ Further oxidized to Fe 3+Subsequently, it reacts with arsenate ions to form insoluble ferric arsenate precipitate, thereby achieving the fixation of arsenic. In addition, zero-valent iron also has good reducing and adsorption removal capabilities for mercury, and also has a displacement deposition effect on heavy metals such as lead, copper, and nickel.
[0012] In a preferred embodiment of the present invention, the amount of Bacillus subtilis added is 0.5% to 5% of the mass of fly ash.
[0013] The amount of organic phosphate monoester salt added is 0.1% to 2% of the mass of fly ash.
[0014] If the amount of Bacillus subtilis and organophosphate monoester salt added is too small, the biomineralization reaction cannot be carried out effectively, resulting in poor precipitation. If the amount added is too large, there will be problems such as excess phosphate.
[0015] In a preferred embodiment of the present invention, the mineralization treatment time is 60 min to 180 min.
[0016] A temperature range of 30℃ to 40℃ is suitable for Bacillus subtilis to secrete alkaline phosphatase, ensuring the activity of alkaline phosphatase and thus efficiently hydrolyzing organophosphate monoesters to release phosphate. The mineralization treatment time can be adaptively adjusted according to the amount of Bacillus subtilis added.
[0017] In a preferred embodiment of the present invention, the mass ratio of raw fly ash to zero-valent iron is 20:1~4.
[0018] If the ratio of raw fly ash to zero-valent iron exceeds the above parameter range, too little zero-valent iron will result in insufficient reduction capacity, while excessive zero-valent iron will cause agglomeration problems.
[0019] In a preferred embodiment of the present invention, the ratio of raw fly ash to alkaline solution is 1g: 3mL~5mL.
[0020] A ratio of 1g of raw fly ash to 3-5mL of alkaline solution can form a solution system of suitable concentration, allowing the fly ash and alkaline solution to react effectively. In a preferred embodiment of the present invention, the alkaline activation treatment time is 10 min to 30 min.
[0021] The present invention involves alkaline activation treatment within a temperature range of 60℃ to 80℃ for 10 min to 30 min. This temperature and time range can significantly promote the erosion of the fly ash vitreous structure by the alkaline solution during alkaline activation treatment, and at the same time promote the rapid formation of geopolymer gel.
[0022] In a preferred embodiment of the present invention, the ball milling process is as follows: under the conditions of a ball-to-material ratio of 8 to 15:1 and a rotation speed of 300 rpm to 600 rpm, the ball milling process is carried out for 60 min to 150 min.
[0023] During ball milling, if the ball-to-material ratio is too small, the number of grinding balls is insufficient, the collision frequency is low, and the impact force is insufficient, the fly ash particles will not be ground finely, reducing the active sites on the surface of the fly ash particles.
[0024] When the ball-to-material ratio is too high, the space inside the tank is filled with grinding balls, leaving the material with insufficient space to tumble, which leads to overheating of the machine and agglomeration of the material.
[0025] Sufficient mechanical force can be generated at a rotation speed of 300 rpm to 600 rpm and a ball milling time of 60 min to 150 min to refine fly ash particles and activate zero-valent iron.
[0026] In a preferred embodiment of the present invention, the organophosphate monoester salt is one or more of the sodium salt and potassium salt of organophosphate monoester, the alkaline solution is one or more of the sodium hydroxide solution, potassium hydroxide solution and sodium silicate solution, and the zero-valent iron is one or more of the nano zero-valent iron powder, submicron zero-valent iron powder and micron zero-valent iron powder.
[0027] The present invention also provides modified fly ash prepared by the above preparation method.
[0028] This invention also provides the application of the above-mentioned modified fly ash in the preparation of building material admixtures, saline-alkali land improvement materials, mine filling materials, or soil remediation materials.
[0029] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention employs a four-effect synergistic method. First, heavy metals in fly ash are exposed through alkaline activation treatment, and then fixed by a geopolymer gel generated by the reaction of an alkaline solution with the active components of fly ash. Then, through Bacillus subtilis-mediated phosphate biomineralization, alkaline phosphatase secreted by Bacillus subtilis hydrolyzes organic phosphate monoester salt substrates to produce PO4. 3- The process involves the addition of zero-valent iron (ZVFe) to form phosphate precipitates with very low solubility in the heavy metal ions of fly ash. Further addition of ZVFe, followed by mechanical ball milling, further refines the fly ash particles, significantly increasing their specific surface area and creating numerous fresh broken bonds and defect sites on the particle surface. These active sites facilitate the penetration of alkaline solutions and the dispersion of ZVFe. ZVFe reduces highly toxic Cr(VI) to less toxic Cr(III), while simultaneously forming insoluble ferric arsenate precipitates with arsenate ions. These products are then removed by the encapsulation of geopolymer gels. Simultaneously, the mechanical action of ball milling transforms unstable forms of heavy metals in fly ash (water-soluble, acid-soluble, and reducible) into stable residual states, significantly reducing the risk of environmental leaching. This invention employs a four-pronged synergistic mechanism of alkali activation, Bacillus subtilis-mediated phosphate biomineralization, mechanical ball milling, and ZVFe. The synergistic effect of each step significantly enhances the removal of chromium and arsenic from fly ash compared to single-treatment methods.
[0030] (2) This invention employs four methods in synergy: alkali activation treatment, Bacillus subtilis-mediated phosphate biomineralization, zero-valent iron, and mechanical ball milling, to form multiple fixed barriers and achieve efficient locking of various heavy metals. At the same time, the microbial mineralization process does not require a large amount of chemical precipitants, resulting in low processing costs and environmental friendliness.
[0031] (3) The modification method of the present invention has a broad-spectrum removal capability for multiple metals. It can remove not only chromium and arsenic, but also other typical heavy metals such as lead, cadmium, copper, zinc, nickel, and mercury. The removal rate of Pb can reach 62%, the removal rate of Cr can reach 50%, the removal rate of As can reach 58%, and the removal rate of Cd can reach 56%.
[0032] (4) The alkaline solution used in this invention has a low concentration (0.5-2 mol / L), uses a small amount of zero-valent iron (5%-20%), and can be biodegraded or treated harmlessly. The washing wastewater has a simple composition and is easy to treat to meet discharge standards.
[0033] (5) The modified fly ash treated by the present invention has high safety, and the leaching concentration of various heavy metals can meet the requirements of relevant national environmental protection standards (such as GB 5085.3-2007). It can be directly used in building material admixtures, soil improvement and other resource utilization pathways. Attached Figure Description
[0034] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0035] Figure 1 The process flow diagram of the modified fly ash provided by the present invention. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0037] In existing technologies, physical sorting, chemical elution, or mechanochemical methods are commonly used for heavy metal ion removal from fly ash. However, single-method treatments suffer from low removal rates or high chemical reagent consumption. Therefore, this invention creatively combines four methods—alkali activation pretreatment, biomineralization treatment, mechanical ball milling treatment, and zero-valent iron reduction—in a synergistic manner for heavy metal removal from fly ash. Figure 1 As shown. Specifically, this invention mixes fly ash with an alkaline solution and adds Bacillus subtilis and organophosphate substrates for alkaline activation treatment and biomineralization pretreatment. Through the erosive effect of the alkaline solution on the fly ash, the vitreous coating on the surface of the fly ash particles is eroded and destroyed, exposing the internal heavy metals. The geopolymer gel generated by the reaction of the alkaline solution and the active components of the fly ash can fix the heavy metals. At the same time, the alkaline phosphatase secreted by Bacillus subtilis hydrolyzes the organophosphate into phosphate ions, which react with the dissolved heavy metal ions to form insoluble phosphate mineral precipitates.
[0038] After the alkali activation treatment and biomineralization pretreatment, the obtained alkali pretreated fly ash is mixed with zero-valent iron and then subjected to mechanochemical ball milling. The mechanochemical action is used to further refine the particles, increase the specific surface area, and promote the reduction and removal of heavy metals by zero-valent iron. Finally, solid-liquid separation, washing, and drying are performed to obtain modified fly ash with low leaching toxicity.
[0039] This invention achieves efficient removal of multiple metals from fly ash through multiple mechanisms that promote each other and work synergistically.
[0040] In this invention, zirconium balls are used for mechanical ball milling. The ball-to-material ratio is the mass ratio of the grinding balls to the material being ground. Taking Example 1 as an example, the ball-to-material ratio refers to the ratio of the mass of the zirconium balls to the total mass of the alkali-pretreated fly ash and nano-zero-valent iron powder. Moisture content refers to the percentage of water by mass of the wet material. Taking Example 1 as an example, the alkali-pretreated fly ash and nano-zero-valent iron powder are the dry material, which is then mixed with deionized water to form the wet material. The moisture content is 20%, with water accounting for 20% of the total mass of the wet material, and the remaining 80% being the total mass of the alkali-pretreated fly ash and nano-zero-valent iron powder.
[0041] The original fly ash used in this invention was taken from a coal-fired power plant. The heavy metal contents in the original fly ash were: Pb 160 mg / kg, Cr 85.2 mg / kg, As 25.8 mg / kg, and Cd 4.5 mg / kg.
[0042] The nano-zero-valent iron powder used in this invention was purchased from Qinhuangdao Taiji Ring Nano Products Co., Ltd., with a particle size of 80 nm. The Bacillus subtilis used in this invention was purchased from Shandong Dexing Biotechnology Co., Ltd., model UJSW01, with a viable count of 10⁻⁶. 11 CFU / mL. In the following examples, Bacillus subtilis bacterial suspension was prepared by dispersing 1g of Bacillus subtilis in 10mL of water for use.
[0043] Since the Bacillus subtilis purchased in this invention is in powder form, the mass of Bacillus subtilis can be directly weighed and then prepared into a bacterial solution for use. If the purchased Bacillus subtilis is in bacterial solution, the amount to be added should be determined according to the dry weight of the bacterial solution.
[0044] Example 1 Step 1: Mix 100g of fly ash with 400mL of 1mol / L NaOH solution at a ratio of 1g:4mL. Stir at 200rpm for 30 minutes in a 70℃ water bath to activate the alkali-containing fly ash solution. Then, cool the solution to 35℃ and add 20mL of Bacillus subtilis bacterial solution (i.e., Bacillus subtilis accounts for 2% of the mass of fly ash) and 0.5% of sodium monododecyl phosphate (sodium dodecyl phosphate) at 200rpm for 120 minutes at 35℃. After the reaction is complete, filter to obtain the first solid product. Wash the first solid product with deionized water until pH≈7, and dry at 105℃ for 4 hours to obtain alkali-pretreated fly ash.
[0045] Step 2: Weigh 10g of nano zero-valent iron powder according to the mass ratio of original fly ash to nano zero-valent iron powder of 100:10. Mix the alkali pretreated fly ash obtained in Step 1 with nano zero-valent iron powder evenly, add deionized water to make the moisture content of the material about 20%, and obtain a mixed liquid.
[0046] The mixture was placed in a ball mill and milled for 90 minutes at a ball-to-material ratio of 10:1 and a rotation speed of 500 rpm. The milled solution was obtained after the milling process. The material was kept sealed during the milling process to prevent moisture evaporation.
[0047] Step 3: Filter the ball-milled solution to obtain a second solid product. Wash the second solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0048] Testing revealed that, compared to the original fly ash, the leaching concentrations of typical heavy metals in the modified fly ash obtained in this embodiment were significantly reduced. The removal effects on chromium and arsenic were particularly outstanding, while the leaching rates of heavy metals such as lead, cadmium, copper, and zinc also decreased substantially. Leaching test results showed that the leaching concentrations of various heavy metals were all below the limits specified in GB 5085.3-2007.
[0049] Example 2 Step 1: Mix 100g of fly ash with 500mL of 0.5mol / L NaOH solution at a ratio of 1g:5mL. Stir at 200rpm for 20 minutes in a 60℃ water bath to activate the alkali and obtain an alkali-containing fly ash solution. Then, cool the solution to 30℃ and add 5mL of Bacillus subtilis bacterial solution (i.e., Bacillus subtilis accounts for 0.5% of the mass of fly ash) and 0.1% of sodium monododecyl phosphate (sodium dodecyl phosphate) at 200rpm for 180 minutes at 30℃. After the reaction is complete, filter to obtain the first solid product. Wash the first solid product with deionized water until pH≈7 and dry at 105℃ for 4 hours to obtain alkali-pretreated fly ash.
[0050] Step 2: Weigh 5g of nano zero-valent iron powder according to the mass ratio of original fly ash to nano zero-valent iron powder of 100:5. Mix the alkali pretreated fly ash obtained in Step 1 with nano zero-valent iron powder evenly, add deionized water to make the moisture content of the material about 30%, and obtain a mixed liquid.
[0051] The mixture was placed in a ball mill and milled for 150 minutes at a ball-to-material ratio of 8:1 and a rotation speed of 300 rpm. The milled solution was obtained after the milling process. The material was kept sealed during the milling process to prevent moisture evaporation.
[0052] Step 3: Filter the ball-milled solution to obtain a second solid product. Wash the second solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0053] Example 3 Step 1: Mix 100g of fly ash with 300mL of 2mol / L NaOH solution at a ratio of 1g:3mL. Stir at 200rpm for 10 minutes in an 80℃ water bath to activate the alkali and obtain an alkali-containing fly ash solution. Then, cool the solution to 40℃ and add 50mL of Bacillus subtilis bacterial solution (i.e., Bacillus subtilis accounts for 5% of the mass of fly ash) and 2% of sodium monododecyl phosphate (2% of the mass of fly ash). Continue stirring at 200rpm for 60 minutes at 40℃. After the reaction is complete, filter to obtain the first solid product. Wash the first solid product with deionized water until pH≈7 and dry at 105℃ for 4 hours to obtain alkali-pretreated fly ash.
[0054] Step 2: Weigh 20g of nano-zero-valent iron powder according to the mass ratio of original fly ash to nano-zero-valent iron powder of 100:20. Mix the alkali-pretreated fly ash obtained in Step 1 with nano-zero-valent iron powder evenly, add deionized water to make the moisture content of the material about 15%, and obtain a mixed liquid.
[0055] The mixture was placed in a ball mill and milled for 60 minutes at a ball-to-material ratio of 15:1 and a rotation speed of 600 rpm. The milled solution was obtained after the milling process. The material was kept sealed during the milling process to prevent moisture evaporation.
[0056] Step 3: Filter the ball-milled solution to obtain a second solid product. Wash the second solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0057] Comparative Example 1 Step 1: Weigh 100g of original fly ash and 10g of nano zero-valent iron powder according to the mass ratio of original fly ash to nano zero-valent iron powder of 100:10. Mix the original fly ash and nano zero-valent iron powder evenly, add deionized water to make the moisture content of the material about 20%, and obtain a mixture.
[0058] The mixture was placed in a ball mill and milled for 90 minutes at a ball-to-material ratio of 10:1 and a rotation speed of 500 rpm. The milled solution was obtained after the milling process. The material was kept sealed during the milling process to prevent moisture evaporation.
[0059] Step 3: Filter the ball-milled solution to obtain a solid product. Wash the solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0060] Comparative Example 2 Step 1: Mix 100g of fly ash with 400mL of 1mol / L NaOH solution at a ratio of 1g:4mL. Stir at 200rpm for 30 minutes in a 70℃ water bath for alkali activation. Then cool to 35℃, add 20mL of Bacillus subtilis bacterial solution (i.e., Bacillus subtilis mass accounts for 2% of fly ash mass) and 0.5% of sodium monododecyl phosphate mass of fly ash. Continue stirring at 200rpm for 120 minutes at 35℃ to obtain alkali-pretreated fly ash.
[0061] Step 2: Add deionized water to the alkali-pretreated fly ash obtained in Step 1 to make the material moisture content about 20% to obtain a mixed liquid.
[0062] The mixture was placed in a ball mill and milled for 90 minutes at a ball-to-material ratio of 10:1 and a rotation speed of 500 rpm. The milled solution was obtained after the milling process. The material was kept sealed during the milling process to prevent moisture evaporation.
[0063] Step 3: Filter the ball-milled solution to obtain a solid product. Wash the solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0064] Comparative Example 3 Step 1: Mix 100g of fly ash with 400mL of 1mol / L NaOH solution at a ratio of 1g:4mL. Stir at 200rpm for 30 minutes in a 70℃ water bath for alkali activation. Then cool to 35℃, add 20mL of Bacillus subtilis bacterial solution (i.e., Bacillus subtilis mass accounts for 2% of fly ash mass) and 0.5% of sodium monododecyl phosphate mass of fly ash. Continue stirring at 200rpm for 120 minutes at 35℃. After the reaction is complete, filter to obtain a solid product. Wash the solid product with deionized water until pH≈7, and dry at 105℃ for 4 hours to obtain modified fly ash.
[0065] Comparative Example 4 Step 1: Mix 100g of fly ash with 400mL of 1mol / L NaOH solution at a ratio of 1g:4mL to obtain an alkaline fly ash solution.
[0066] Step 2: Add 10g of nano-zero-valent iron powder to the alkaline fly ash solution at a mass ratio of 100:10 for fly ash and nano-zero-valent iron powder. Mix well to obtain an iron powder mixture. Place the iron powder mixture in a ball mill and ball mill for 120 minutes at a ball-to-material ratio of 10:1 and a rotation speed of 500 rpm. After ball milling, obtain the ball-milled solution. Keep the material sealed during the ball milling process to prevent moisture evaporation.
[0067] Step 3: Filter the ball-milled solution to obtain a solid product. Wash the solid product with deionized water until pH≈7, and dry it at 105℃ for 4 hours to obtain modified fly ash.
[0068] Table 1 Removal rate of heavy metals
[0069] As can be seen from Table 1, the method provided in Example 1 of this invention can achieve a removal rate of 62% for Pb, 50% for Cr, 58% for As, and 56% for Cd. Comparative Example 1 omitted the alkaline activation pretreatment step, and the removal effect of chromium and arsenic in the obtained product was significantly lower than that in Example 1. This is because most of the heavy metals in the original fly ash are sealed by the glassy coating layer. When the alkaline activation treatment step is omitted, the heavy metals inside the original fly ash cannot be effectively exposed, thus limiting the removal effect of heavy metal ions.
[0070] Comparative Example 2, which omitted the addition of zero-valent iron, showed significantly lower removal efficiency of chromium and arsenic compared to Example 1, indicating that the addition of zero-valent iron plays a crucial role in the reduction of chromium and the fixation of arsenic. In the absence of the reducing and precipitation effects of zero-valent iron, the removal of oxyanion-type heavy metals (chromium and arsenic) solely through the physical encapsulation of the alkali-activated geopolymer gel and the precipitation of biomineralized phosphate is limited, thus confirming the unique function of zero-valent iron in the four-effect synergistic system.
[0071] Comparative Example 3 omitted the mechanical ball milling step and the addition of zero-valent iron. Although the concentration of heavy metals leaching in the resulting product was reduced, the effect was far less than that of Example 1. In particular, the removal effect on heavy metals contained within the glass lattice was limited. This is because for chromium and arsenic existing in the form of oxyacid anions, there was a lack of both the reducing effect of zero-valent iron and the lack of Fe. 3+ The fixation mechanism of forming ferric arsenate precipitate with arsenate indicates that mechanochemical ball milling is a key step in breaking down the coating and releasing heavy metals.
[0072] Comparative Example 4 employed a one-step modification process, omitting Bacillus subtilis and organophosphate monoesters. Although the removal rate of heavy metal ions decreased, the removal effect was still lower than in Example 1. This is because, without phosphate, the heavy metal cations cannot be fixed through the formation of phosphate minerals, indicating that the Bacillus subtilis-mediated phosphate biomineralization step plays a crucial role in heavy metal removal. This invention, through a four-effect synergistic mechanism of alkali activation + biomineralization + mechanical activation + zero-valent iron reduction, not only exhibits significant removal effects on chromium and arsenic but also demonstrates good removal capabilities for various heavy metals such as lead, cadmium, copper, zinc, nickel, and mercury.
[0073] The above-described embodiments are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various improvements and substitutions without departing from the principles of the present invention, and these improvements and substitutions should also be considered within the scope of protection of the present invention. Therefore, the scope of protection of this invention should be determined by the scope of the claims.
Claims
1. A method for preparing a modified fly ash, characterized by, The method comprises the following steps: mixing the raw fly ash and the alkaline solution at 60-80 DEG C to obtain an alkali-containing fly ash solution, wherein the concentration of the alkaline solution is 0.5-2 mol / L; cooling the alkali-containing fly ash solution to 30-40 DEG C, adding Bacillus subtilis and organic phosphoric acid monoester salt, and performing mineralization treatment to form heavy metal ion precipitate, thereby obtaining alkali pretreated fly ash; mixing the alkali pretreated fly ash, zero-valent iron and water, and performing ball milling treatment to obtain modified fly ash.
2. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The addition amount of the Bacillus subtilis is 0.5-5% of the mass of the fly ash. The addition amount of the organic phosphoric acid monoester salt is 0.1-2% of the mass of the fly ash.
3. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The mineralization treatment time is 60-180 min.
4. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The mass ratio of the raw fly ash to the zero-valent iron is 20:1-4.
5. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The mass ratio of the raw fly ash to the alkaline solution is 1g:3-5 mL, and the concentration of the alkaline solution is 0.5-2 mol / L.
6. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The alkali activation treatment time is 10-30 min.
7. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The ball milling treatment is performed under the following conditions: the ball-to-material ratio is 8-15:1, the rotation speed is 300-600 rpm, and the ball milling time is 60-150 min.
8. The method of claim 1, wherein the modified fly ash is prepared by the steps of: The organic phosphoric acid monoester salt is one or more of organic phosphoric acid monoester sodium salt and organic phosphoric acid monoester potassium salt; the alkaline solution is one or more of sodium hydroxide solution, potassium hydroxide solution and sodium silicate solution; The zero-valent iron is one or more of nano zero-valent iron powder, submicron zero-valent iron powder and micron zero-valent iron powder. 9.A modified fly ash prepared by the preparation method of any one of claims 1-8. 10.Use of the modified fly ash of claim 9 in preparing building material admixture, saline-alkali soil improvement material, mine filling material or soil remediation material.