A self-regulating phase change aggregate coupled with moisture, heat and light, its preparation method and its application in phase change mortar
By introducing a humidity-responsive gel layer and a photothermal-responsive thermal conductivity control component into phase change aggregates, combined with an inorganic interface reinforcement layer, the problems of leakage resistance and thermal response of phase change aggregates under environmental changes are solved, achieving efficient thermal energy storage and crack protection of phase change mortar.
Patent Information
- Application Number
- CN202611603135.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing phase change aggregates and phase change mortars are prone to shell damage, pore connectivity, and phase change material migration under long-term thermal cycling, wet-dry cycling, and stirring shearing. Furthermore, they are difficult to automatically adjust the participation of phase change materials and heat conduction paths according to changes in ambient humidity, solar radiation intensity, and temperature, resulting in insufficient anti-leakage performance, thermal response efficiency, and interfacial bonding performance.
A self-regulating phase change aggregate using moisture-heat and light coupling is formed by loading phase change materials in a porous carrier and coating it with a humidity-responsive gel layer and a photothermal-responsive thermal conductivity regulating component, combined with an inorganic interface reinforcement layer, thereby achieving dynamic adjustment of pore connectivity and heat conduction path.
It improves the anti-leakage performance, thermal response efficiency, and interfacial bonding performance of phase change materials, reduces the risk of phase change material migration, and achieves the synergistic effect of thermal regulation, crack protection, and humidity response of phase change mortar, making it suitable for building exterior walls, roofs, and floors.
Smart Images

Figure CN123106053A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building energy-saving materials technology, and in particular relates to a self-regulating phase change aggregate coupled with moisture, heat and light, its preparation method and its application in phase change mortar. Background Technology
[0002] Phase change materials can absorb or release latent heat during the phase change process. Introducing them into the mortar system can enable the mortar to have functions of enclosure, plastering, leveling and heat storage.
[0003] Currently, microcapsule phase change materials or porous carrier-loaded phase change materials are commonly used as phase change aggregates added to mortar. However, the existing phase change aggregates rely on fixed shells or fixed pore structures to encapsulate the phase change materials. Under long-term thermal cycling, wet-dry cycling, and mortar mixing and shearing, problems such as shell damage, pore connectivity, and phase change material migration are prone to occur.
[0004] Meanwhile, in existing phase change mortars, phase change aggregates are usually uniformly dispersed in the mortar matrix. When the amount of phase change aggregates is high, the mortar strength and interfacial bonding performance decrease. When the amount of phase change aggregates is low, the thermal energy storage effect is insufficient. Therefore, existing phase change mortars with uniformly mixed phase change aggregates cannot simultaneously achieve the functions of surface crack resistance and wear resistance, intermediate high-efficiency heat storage, and bottom heat flow regulation.
[0005] In addition, most existing phase change aggregates and phase change mortars are passive heat storage and release materials. They cannot automatically adjust the degree of phase change material participation, heat conduction path and pore connectivity according to changes in ambient humidity, solar radiation intensity and temperature. They are difficult to adapt to complex service conditions such as strong radiation in summer, low temperature in winter, high humidity environment and day-night temperature difference.
[0006] Therefore, it is necessary to develop a new type of phase change aggregate that combines humidity response, photothermal response, thermal conductivity regulation, impermeability and interface enhancement functions, and further construct a phase change mortar system with functional gradients in the thickness direction to take into account the surface crack resistance and wear resistance, the middle efficient heat storage and the bottom heat flow regulation functions. Summary of the Invention
[0007] To address the aforementioned shortcomings of existing phase change aggregates and phase change mortars, this invention provides a self-regulating phase change aggregate coupled with moisture, heat, and light, its preparation method, and its application in phase change mortars. This phase change aggregate can automatically adjust pore connectivity and heat conduction paths according to environmental humidity, temperature, and solar radiation conditions, thereby improving the anti-leakage performance, thermal response efficiency, interfacial bonding performance, and thermal cycling stability of phase change materials. It can be applied to the preparation of gradient phase change mortars, enabling the mortar to form a photothermal response protective mortar layer, a phase change heat storage mortar layer, and a humidity-controlled mortar layer along the thickness direction, achieving synergistic effects of thermal regulation, crack protection, thermal conductivity regulation, and humidity response.
[0008] This invention provides a self-regulating phase change aggregate coupled with humidity, heat, and light, comprising a porous carrier, a phase change material, a humidity-responsive gel layer, a photothermal-responsive thermal conductivity regulating component, and an inorganic interface reinforcement layer. The phase change material is loaded in the pores of the porous carrier, the humidity-responsive gel layer continuously or semi-continuously coats the outside of the porous carrier, the photothermal-responsive thermal conductivity regulating component is dispersed in the humidity-responsive gel layer, and the inorganic interface reinforcement layer coats the outside of the humidity-responsive gel layer. The porous carrier is selected from one or more of expanded perlite, diatomaceous earth, and ceramsite, and the phase change material is selected from stone... The component comprises one or more of wax, stearic acid, methyl laurate and polyethylene glycol; the humidity-responsive gel layer is selected from any one of calcium alginate gel, chitosan and silica sol composite gel, and bentonite and polyacrylate composite gel; the photothermal response thermal conductivity regulating component is selected from any one or more of carbon black, expanded graphite and MXene; and the inorganic interface reinforcement layer is selected from any one of nano-SiO2 layer, calcium silicate hydrate layer formed by the reaction of sodium metasilicate and calcium salt, and aluminosilicate gel layer formed by the reaction of metakaolin, alkali activator and silica sol.
[0009] In some embodiments, the components are proportioned as follows by weight: 40-50 parts of porous carrier, 35-45 parts of phase change material, 8-12 parts of humidity-responsive gel layer, 1-3 parts of photothermal-responsive thermal conductivity regulating component, and 4-5 parts of inorganic interface reinforcement layer.
[0010] In some embodiments, the phase change material is a low-temperature phase change material composed of polyethylene glycol and methyl laurate with a phase change temperature of 18~22°C, or a medium-temperature phase change material composed of paraffin and stearic acid with a phase change temperature of 24~28°C, or a high-temperature phase change material composed of paraffin and stearic acid with a phase change temperature of 32~38°C.
[0011] This invention also provides a method for preparing self-regulating phase change aggregates through hydrothermal and optical coupling, used to prepare the self-regulating phase change aggregates through hydrothermal and optical coupling described in any of the above technical solutions, comprising the following steps: S1. Heat and melt the phase change material to obtain molten phase change material; S2. Place the porous carrier in the molten phase change material, and under vacuum conditions, allow the molten phase change material to enter the pores of the porous carrier to obtain primary phase change aggregate; S3. Disperse the photothermal response thermal conductivity regulating component in the precursor solution of the humidity response gel layer, coat the precursor solution of the humidity response gel layer containing the photothermal response thermal conductivity regulating component on the surface of the primary phase change aggregate, and induce the precursor cross-linking to form a humidity response gel layer with the photothermal response thermal conductivity regulating component embedded in the internal or external surface on the surface of the primary phase change aggregate to obtain the secondary phase change aggregate. S4. The slurry of the inorganic interface reinforcement layer is coated on the outer surface of the secondary phase change aggregate in multiple layers. After each layer of slurry is surface dry, the next layer is coated. The inorganic interface reinforcement layer is formed by drying and curing, and the phase change aggregate with wet heat and light coupling is obtained.
[0012] In some embodiments, in step S3, when the humidity-responsive gel layer is calcium alginate gel, sodium alginate solution is used as a precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing photothermal response and thermal conductivity regulating components is coated onto the surface of the primary phase change aggregate in several stages. After each coating, atomized calcium salt solution is sprayed to induce sodium alginate ion crosslinking to form calcium alginate gel. When the humidity-responsive gel layer is a chitosan and silica sol composite gel, a chitosan and silica sol composite solution is used as a precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, a precursor solution containing photothermal response and thermal conductivity regulating components is sprayed onto the surface of the primary phase change aggregate in several stages. The precursor solution of the photothermal response thermal conductivity regulating component is coated onto the surface of the primary phase change aggregate in stages. After each coating, chitosan gelation is induced by an alkaline environment, and silica sol condensation is induced to form a chitosan-silica sol composite gel. When the humidity-responsive gel layer is a bentonite-polyacrylate composite gel, the bentonite-polyacrylate composite solution is used as the precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing the photothermal response thermal conductivity regulating component is coated onto the surface of the primary phase change aggregate in stages. After each coating, a crosslinking agent is sprayed to induce gelation and form a bentonite-polyacrylate composite gel.
[0013] This invention further provides the application of the self-regulating phase change aggregate coupled with moisture and light as described in any of the above technical solutions in phase change mortar. The phase change mortar, along its thickness direction from the surface to the bottom layer, sequentially includes a photothermal response protective mortar layer, a phase change heat storage mortar layer, and a moisture-releasing controlled mortar layer. Each mortar layer includes cementitious materials and self-regulating phase change aggregate coupled with moisture and light. In the photothermal response protective mortar layer, the mass ratio of phase change aggregate to cementitious materials is 1:(3.0~3.5). In the phase change aggregate, high-temperature phase change materials with a phase change temperature of 32~38℃ are used; in the phase change thermal storage mortar layer, the mass ratio of phase change aggregate to cementitious material is 1:(1.2~1.5), and medium-temperature phase change materials with a phase change temperature of 24~28℃ are used in the phase change aggregate; in the humidity slow-release regulating mortar layer, the mass ratio of phase change aggregate to cementitious material is 1:(2.5~3.1), and low-temperature phase change materials with a phase change temperature of 18~22℃ are used in the phase change aggregate.
[0014] In some embodiments, the photothermal responsive protective mortar layer further includes reinforcing fillers selected from one or more of silica fume, polyethylene fibers, and basalt fibers.
[0015] In some embodiments, the humidity-controlled mortar layer further includes a thermally conductive filler selected from one or both of expanded graphite and boron nitride.
[0016] In some embodiments, the phase change mortar has a photothermal response protective mortar layer with a thickness of 3 mm, a phase change thermal storage mortar layer with a thickness of 16-18 mm, and a humidity slow-release regulating mortar layer with a thickness of 5-8 mm.
[0017] In some embodiments, the preparation method of phase change mortar is as follows: photothermal response protective mortar, phase change heat storage mortar and humidity slow-release regulating mortar are prepared respectively; humidity slow-release regulating mortar is applied to the surface of the base layer to form a humidity slow-release regulating mortar layer; phase change heat storage mortar is applied to the surface of the humidity slow-release regulating mortar layer to form a phase change heat storage mortar layer; and photothermal response protective mortar is applied to the surface of the phase change heat storage mortar layer to form a photothermal response protective mortar layer.
[0018] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: 1. The moisture-heat and light-coupled self-regulating phase change aggregate provided by the present invention encapsulates the phase change material by adding a humidity-responsive gel layer and regulates the pore connectivity by humidity response, so that the phase change aggregate has the ability to dynamically adjust the anti-leakage capability according to the change of environmental humidity, instead of relying solely on fixed pore adsorption or ordinary microcapsule encapsulation of phase change material. 2. The moisture-heat and light-coupled self-regulating phase change aggregate provided by the present invention introduces photothermal response thermal conductivity regulating components into the humidity-responsive gel layer, enabling the phase change aggregate to enhance heat absorption and heat conduction under strong solar radiation or high temperature and low humidity conditions, thereby improving the thermal response rate of the phase change material. 3. The moisture-heat and light-coupled self-regulating phase change aggregate provided by the present invention forms a synergistic effect through the reversible swelling and shrinkage of the humidity-responsive gel layer and the reconstruction of the heat conduction path of the photothermal-responsive thermally conductive component, thereby reducing the risk of phase change material migration under high humidity conditions and improving the thermal response efficiency of phase change material under low humidity and strong light conditions. 4. The wet heat and light coupling self-regulating phase change aggregate provided by the present invention improves the interfacial bonding between the phase change aggregate and the inorganic mortar matrix by setting an inorganic interface reinforcement layer; at the same time, when the inorganic mortar matrix is a strongly alkaline cementitious system, the risk of hydroxide ions migrating inward can be reduced by the outermost inorganic interface reinforcement layer. 5. The preparation method of the self-regulating phase change aggregate coupled with wet heat and light provided by the present invention has simple preparation steps, which is conducive to large-scale industrial production. At the same time, its inorganic interface reinforcement layer is formed by multi-layer coating, which can reduce the possibility of forming through defects in a single coating film. When applied to a strongly alkaline gelling system, it prolongs the migration path of hydroxide ions inward and reduces the risk of strong alkaline solution contacting the internal humidity-responsive gel layer. 6. The phase change mortar prepared using the self-regulating phase change aggregate with moisture and light coupling provided by this invention, through the synergistic cooperation of the photothermal response protective mortar layer, the phase change heat storage mortar layer, and the moisture slow-release regulating mortar layer set from the surface to the bottom layer, can avoid the problems of strength reduction, insufficient interfacial bonding force, or insufficient heat storage efficiency caused by the uniform addition of phase change materials in traditional mortars. It achieves a synergistic improvement in mechanical properties, thermal energy storage performance, and service durability, and is especially suitable for building exterior walls, roofs, floors, and prefabricated energy-saving enclosure components. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the structure of the self-regulating phase change aggregate based on the coupling of moisture, heat and light provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of a gradient phase change mortar using self-regulating phase change aggregates coupled with wet heat and light, provided in an embodiment of the present invention. Figure 3 SEM images of the secondary intermediate-temperature phase change aggregate prepared in Example 3 of the present invention are shown, wherein (a) is an SEM image of a single secondary intermediate-temperature phase change aggregate, and (b) and (c) are high-magnification magnified images of local areas on the surface of the secondary intermediate-temperature phase change aggregate. Figure 4 The images shown are cross-sectional SEM images of the medium-temperature self-regulating phase change aggregate-3 prepared in Example 3 of the present invention, wherein (a) is a cross-sectional SEM image of a single medium-temperature self-regulating phase change aggregate-3, and (b) is a magnified view of a portion of the medium-temperature self-regulating phase change aggregate-3. Detailed Implementation
[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] like Figure 1As shown, this embodiment of the invention provides a self-regulating phase change aggregate coupled with humidity, heat, and light, comprising a porous carrier, a phase change material, a humidity-responsive gel layer, a photothermal-responsive thermal conductivity regulating component, and an inorganic interface reinforcement layer. The phase change material is loaded in the pores of the porous carrier, the humidity-responsive gel layer continuously or semi-continuously coats the outside of the porous carrier, the photothermal-responsive thermal conductivity regulating component is dispersed in the humidity-responsive gel layer, and the inorganic interface reinforcement layer coats the outside of the humidity-responsive gel layer. The porous carrier is selected from one or more of expanded perlite, diatomaceous earth, and ceramsite, and the phase change material... The components are selected from one or more of paraffin wax, stearic acid, methyl laurate, and polyethylene glycol; the humidity-responsive gel layer is selected from any one of calcium alginate gel, chitosan and silica sol composite gel, and bentonite and polyacrylate composite gel; the photothermal response thermal conductivity regulating component is selected from any one or more of carbon black, expanded graphite, and MXene; and the inorganic interface reinforcement layer is selected from any one of nano-SiO2 layer, calcium silicate hydrate layer formed by the reaction of sodium metasilicate and calcium salt, and aluminosilicate gel layer formed by the reaction of metakaolin, alkali activator, and silica sol.
[0022] The roles of each component in the above-mentioned self-regulating phase change aggregate based on the coupling of moisture, heat, and light are explained below: (1) Porous carriers have open pore structures and certain mechanical strength. On the one hand, they are used to adsorb and confine phase change materials. On the other hand, when phase change aggregates are used to make mortar, they maintain the morphological stability of phase change aggregate particles during mortar mixing and molding. The expanded perlite, diatomite and ceramsite listed above have suitable pore structures and mechanical strength, and are suitable as porous carriers. (2) Phase change materials are used to regulate temperature. They can absorb heat and melt when the ambient temperature exceeds the phase change temperature to prevent the ambient temperature from rising too quickly, and solidify and release heat when the ambient temperature decreases to slow down the decrease of the ambient temperature, thus making the temperature curve flatter. The paraffin, stearic acid, methyl laurate and polyethylene glycol listed above have different phase change temperatures. By combining them, phase change materials with different phase change temperatures can be obtained, which can ensure that the phase change temperature of the phase change material is adjustable, the latent heat is stable, and it has good wettability with porous carriers. (3) While encapsulating the phase change material, the humidity-responsive gel layer is mainly used to adjust the openness of the pores on the surface of the phase change aggregate under different humidity conditions. Specifically, when the relative humidity of the environment is high, the humidity-responsive gel layer absorbs water and swells, reducing the effective cross-section of the interconnected channels on the surface of the porous carrier; when the relative humidity of the environment is low and under high temperature or solar radiation conditions, the humidity-responsive gel layer loses water and shrinks, making the heat conduction path on the surface of the phase change aggregate more continuous. The calcium alginate gel, chitosan and silica sol composite gel, and bentonite and polyacrylate composite gel listed above can all provide humidity-responsive characteristics. (4) The photothermal response thermal conductivity control components are distributed in the humidity response gel layer. They can improve the absorption capacity of the phase change aggregate surface to light energy under solar radiation conditions and transfer the absorbed heat to the phase change material along the interface between the humidity response gel layer and the porous carrier. A coupled control relationship of "humidity triggering and thermal conduction path reconstruction" is formed between them and the humidity response gel layer. Specifically, when the humidity response gel layer is in a contracted state, the distance between the photothermal response thermal conductivity control components decreases, forming a continuous or semi-continuous thermal conduction network, thereby improving the heat absorption rate of the phase change material. When the humidity response gel layer is in a swollen state, the spacing between the photothermal response thermal conductivity control components increases, the thermal channel is weakened, and the humidity response gel layer seals the pores, improving the anti-leakage ability. The carbon black, expanded graphite and MXene listed above have good photothermal response capabilities and can absorb light energy under solar radiation conditions to transfer heat to the phase change material. (5) The inorganic interface reinforcement layer can reduce the interfacial incompatibility between the organic humidity-responsive gel layer and the inorganic mortar matrix, and improve the interfacial bonding between the phase change aggregate and the mortar matrix. At the same time, when the inorganic mortar matrix is a strongly alkaline cementitious system, the risk of hydroxide ions migrating inward can be reduced through the outermost inorganic interface reinforcement layer. The nano-SiO2 layer, calcium silicate hydrate layer and silica-alumina gel layer listed above can interact with the cement matrix interface region, and the silica-alumina gel layer can form a continuous silica-alumina gel network with the geopolymer matrix. Among them, when the humidity-responsive gel layer uses calcium alginate gel and the phase change aggregate is used in a strongly alkaline cementitious system, it is preferable to use a multi-layer coated silica-alumina gel layer as the inorganic interface reinforcement layer.
[0023] In summary, the aforementioned moisture-heat and light-coupled self-regulating phase change aggregate regulates pore connectivity through a moisture-responsive gel layer, improves heat transfer under heating conditions through photothermal response and thermal conductivity control of components, and enhances interfacial bonding with the mortar matrix through an inorganic interface reinforcement layer.
[0024] In a preferred embodiment, the components are proportioned as follows by weight: 40-50 parts porous carrier, 35-45 parts phase change material, 8-12 parts humidity-responsive gel layer, 1-3 parts photothermal-responsive thermal conductivity regulating component, and 4-5 parts inorganic interface reinforcement layer. When the components are within the above preferred proportions, the phase change aggregate can simultaneously achieve good latent heat, leakage control, thermal response, and mortar interface bonding performance.
[0025] In a preferred embodiment, the phase change material is a low-temperature phase change material composed of polyethylene glycol and methyl laurate, with a phase change temperature of 18-22°C; a medium-temperature phase change material composed of paraffin wax and stearic acid, with a phase change temperature of 24-28°C; or a high-temperature phase change material composed of paraffin wax, with a phase change temperature of 32-38°C. Using polyethylene glycol and methyl laurate composites is advantageous for obtaining low-temperature phase change materials with relatively low phase change temperatures, which can be used for low-temperature heat storage and indoor insulation in winter. Using paraffin wax and stearic acid composites is advantageous for obtaining medium-temperature phase change materials with moderate phase change temperatures, which can be used for temperature regulation within the human body's thermal comfort range. High-temperature paraffin wax with relatively high phase change temperatures can be used as a high-temperature phase change material, which can be used for heat buffering under high summer temperatures and solar radiation conditions.
[0026] This invention also provides a method for preparing self-regulated phase change aggregate through hydrothermal and optical coupling, comprising the following steps: S1. Heat and melt the phase change material to obtain molten phase change material; S2. Place the porous carrier in the molten phase change material, and under vacuum conditions, allow the molten phase change material to enter the pores of the porous carrier to obtain primary phase change aggregate; S3. Disperse the photothermal response thermal conductivity regulating component in the precursor solution of the humidity response gel layer, coat the precursor solution containing the photothermal response thermal conductivity regulating component on the surface of the primary phase change aggregate, and induce cross-linking of the precursor to form a humidity response gel layer with the photothermal response thermal conductivity regulating component embedded in the internal or external surface of the primary phase change aggregate to obtain the secondary phase change aggregate. S4. The slurry of the inorganic interface reinforcement layer is coated on the outer surface of the secondary phase change aggregate in multiple layers. After each layer of slurry is surface dry, the next layer is coated. The inorganic interface reinforcement layer is formed by drying and curing, and the phase change aggregate with wet heat and light coupling is obtained.
[0027] The aforementioned method for preparing self-regulated phase change aggregates through hydrothermal and photocoupled processes is simple, requiring no complex equipment or cumbersome procedures, thus reducing production costs and energy consumption. This facilitates large-scale industrial production and demonstrates good economic efficiency. Furthermore, in this method, the inorganic interface reinforcement layer is formed through multi-layer coating, reducing the possibility of through-hole defects formed in a single coating application. When applied to strongly alkaline gelling systems, this extends the inward migration path of hydroxide ions, reducing the risk of strong alkaline solutions contacting the internal humidity-responsive gel layer.
[0028] It should be noted that in step S1, to ensure the phase change material melts, it is preferable to heat and stir at a temperature 10-20°C higher than the melting point of the component with the highest melting point in the phase change material to form a homogeneous melt. Specifically: for low-temperature phase change materials composed of polyethylene glycol and methyl laurate, a melting temperature of 65-75°C is used; for medium-temperature phase change materials composed of paraffin wax and stearic acid, a melting temperature of 75-85°C is used; and for high-temperature phase change materials composed of high-temperature paraffin wax, a melting temperature of 80-90°C is used.
[0029] It should be noted that in step S2, the vacuum treatment pressure is -0.07 to -0.08 MPa, the vacuum treatment time is 25 to 30 minutes, and after returning to normal pressure, the temperature is maintained for another 5 to 15 minutes. Treating under vacuum conditions of -0.07 to -0.08 MPa for 25 to 30 minutes allows most of the molten phase change material to enter the pores inside the porous carrier. After returning to normal pressure, the temperature is maintained for another 5 to 15 minutes, which uses the pressure difference to further fill the pores of the porous carrier with the remaining molten phase change material. This treatment avoids the energy waste caused by excessively long vacuum treatment time and ensures the adsorption amount of molten phase change material.
[0030] It should be noted that in step S3, when the humidity-responsive gel layer is calcium alginate gel, sodium alginate solution is used as the precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing photothermal response thermal conductivity regulating components is coated onto the surface of the primary phase change aggregate in several times. After each coating, atomized calcium salt solution is sprayed to induce sodium alginate ion cross-linking to form calcium alginate gel. After each spraying, agitation continues until there is no obvious free liquid on the particle surface and no continuous adhesion and agglomeration between particles. Then, the next coating of precursor solution and spraying of calcium salt solution are carried out to allow the cross-linking reaction to proceed gradually. When the humidity-responsive gel layer is a chitosan and silica sol composite gel, the chitosan and silica sol composite solution is used as the precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing photothermal response and thermal conductivity regulating components is coated onto the surface of the primary phase change aggregate in stages. After each coating, the chitosan gels and silica sols are condensed to form a chitosan and silica sol composite gel by the weakly alkaline environment generated by the atomization of sodium bicarbonate solution with pH adjusted to 8.5. After each induction, the agitation continues until there is no obvious free liquid on the particle surface and no continuous adhesion and agglomeration between particles, and then the next coating and induction of the precursor solution is carried out. When the humidity-responsive gel layer is a bentonite-polyacrylate composite gel, a bentonite-polyacrylate composite solution is used as the precursor solution. Under continuous agitation of the primary phase change aggregate, the precursor solution containing photothermal response and thermal conductivity regulating components is coated onto the surface of the primary phase change aggregate in stages. After each coating, calcium chloride solution is sprayed to induce gelation and form the bentonite-polyacrylate composite gel. After each spray, agitation continues until there is no obvious free liquid on the particle surface and no continuous adhesion or agglomeration between particles, before the next coating of the precursor solution and spraying of the calcium chloride solution are performed. In this embodiment, the precursor solution is coated in stages and cross-linking is induced in stages, which facilitates control according to the particle dispersion state.
[0031] It should be noted that in step S3, after the photothermal response thermal conductivity regulating component is added to the precursor solution of the humidity-responsive gel layer, it needs to be ultrasonically dispersed for 5 to 20 minutes to avoid agglomeration of the photothermal response thermal conductivity regulating component and improve the uniformity of the distribution of the photothermal response thermal conductivity regulating component in the humidity-responsive gel layer.
[0032] It should be noted that in step S4, the slurry of the inorganic interface reinforcement layer is applied in multiple layers to the outer surface of the continuously agitated secondary phase change aggregate. Each layer of slurry is allowed to dry completely before the next layer is applied. Before applying the next layer, the particle agitation direction or coating path is changed. Finally, the aggregate is dried at 40-50℃ for 12-24 hours. This multi-layer coating reduces local defects in the inorganic interface reinforcement layer and avoids the formation of defects that penetrate the entire inorganic interface reinforcement layer in the thickness direction.
[0033] like Figure 2As shown, this embodiment of the invention further provides the application of the above-mentioned self-regulating phase change aggregate coupled with moisture and light in phase change mortar. The phase change mortar, from the surface to the bottom layer along its thickness direction, sequentially includes a photothermal response protective mortar layer, a phase change heat storage mortar layer, and a moisture-releasing controlled mortar layer. Each mortar layer includes cementitious materials and self-regulating phase change aggregate coupled with moisture and light. In the photothermal response protective mortar layer, the mass ratio of phase change aggregate to cementitious materials is 1:(3.0~3.5). The phase change aggregate uses high-temperature phase change materials with a phase change temperature of 32~38℃; in the phase change thermal storage mortar layer, the mass ratio of phase change aggregate to cementitious material is 1:(1.2~1.5), and the phase change aggregate uses medium-temperature phase change materials with a phase change temperature of 24~28℃; in the humidity slow-release regulating mortar layer, the mass ratio of phase change aggregate to cementitious material is 1:(2.5~3.1), and the phase change aggregate uses low-temperature phase change materials with a phase change temperature of 18~22℃. In this phase change mortar, the surface photothermal response protective mortar layer contains a relatively small amount of phase change aggregate, which is a high-temperature phase change material. This allows the surface photothermal response protective mortar layer to primarily absorb solar radiation heat and rapidly transfer it to the phase change material. Simultaneously, the small amount of phase change aggregate avoids the problem of decreased surface mechanical strength caused by excessive aggregate addition. The middle phase change thermal storage mortar layer contains a relatively larger amount of phase change aggregate, which is a medium-temperature phase change material. This allows the middle phase change thermal storage mortar layer to primarily bear the load of latent heat. This phase change mortar features a heat storage and release function, absorbing or releasing heat within a comfortable temperature range to reduce ambient temperature fluctuations. Simultaneously, the abundant phase change aggregate ensures effective heat storage. A relatively small amount of low-temperature phase change material is added to the bottom layer of the humidity-controlled mortar, which primarily buffers changes in substrate humidity, regulates internal heat transfer, and provides heat storage in low-temperature environments. The small amount of phase change aggregate also prevents the degradation of interfacial bonding performance caused by excessive aggregate addition. In summary, this phase change mortar, through the synergistic combination of a photothermal response protective mortar layer, a phase change heat storage mortar layer, and a humidity-controlled mortar layer arranged in a gradient from the surface to the bottom, avoids the strength reduction, insufficient interfacial bonding, or insufficient heat storage efficiency problems caused by the uniform addition of phase change materials in traditional mortars. It achieves a synergistic improvement in mechanical properties, heat storage performance, and service durability, making it particularly suitable for building exterior walls, roofs, floors, and prefabricated energy-saving enclosure components.
[0034] In a preferred embodiment, the photothermal responsive protective mortar layer further includes reinforcing filler selected from one or more of silica fume, polyethylene fiber, and basalt fiber. By adding reinforcing filler to the surface photothermal responsive protective mortar layer, the crack resistance, wear resistance, and impact resistance of the mortar surface can be improved.
[0035] In a preferred embodiment, the humidity-controlled mortar layer further includes a thermally conductive filler selected from one or both of expanded graphite and boron nitride. By adding a thermally conductive filler to the bottom layer of the humidity-controlled mortar layer, the interfacial thermal resistance between the humidity-controlled mortar layer and the base layer can be reduced, promoting uniform heat transfer along the thickness direction. This allows the added low-temperature self-regulating phase change aggregate (i.e., the moisture-heat and light-coupled self-regulating phase change aggregate obtained using low-temperature phase change materials) to participate in heat storage and release in a timely manner, and reduces local heat accumulation and interlayer temperature gradients.
[0036] In a preferred embodiment, the phase change mortar has the following characteristics: the photothermal response protective mortar layer has a thickness of 3 mm, the phase change thermal storage mortar layer has a thickness of 16-18 mm, and the humidity-controlled mortar layer has a thickness of 5-8 mm. Using the above-mentioned preferred thickness ratios for each mortar layer better balances mechanical properties, thermal energy storage performance, and service durability.
[0037] It should be noted that the cementing materials used in each mortar layer of the aforementioned phase change mortar can be ordinary silicate cement, sulfoaluminate cement, slag cement, low-carbon composite cementitious materials, geopolymer cementitious materials, or alkali-activated slag cementitious materials. For phase change mortar used in interior and exterior wall plastering and roof leveling layers, ordinary silicate cement or low-carbon composite cementitious materials are preferred; for phase change mortar used in low-carbon prefabricated energy-saving components, geopolymer cementitious materials composed of slag, fly ash, and metakaolin are preferred. Furthermore, slag powder, quartz sand, metakaolin, cellulose ether, water-reducing agents, and water-retaining agents can also be added to the phase change mortar to adjust its workability, interfacial bonding performance, and crack resistance.
[0038] In a preferred embodiment, the preparation method of phase change mortar is as follows: Photothermal responsive protective mortar, phase change thermal storage mortar, and humidity-controlled slow-release mortar are prepared separately. A humidity-controlled slow-release mortar layer is formed on the surface of the base layer using the humidity-controlled slow-release mortar. A phase change thermal storage mortar layer is formed on the surface of the humidity-controlled slow-release mortar layer using the phase change thermal storage mortar. Finally, a photothermal responsive protective mortar layer is formed on the surface of the phase change thermal storage mortar layer using the photothermal responsive protective mortar. It should be noted that, regarding the construction interval between two adjacent mortar layers, the subsequent mortar layer should be constructed before the initial setting of the preceding mortar layer to ensure the continuity of the interface between mortar layers.
[0039] To more clearly and in detail introduce the self-regulating phase change aggregate with wet heat and light coupling provided in the embodiments of the present invention, its preparation method and its application in phase change mortar, the following will describe it in conjunction with specific embodiments.
[0040] I. Preparation of Self-Regulated Phase Change Aggregate by Hygrothermal and Photocoupled Processes Example 1 A self-regulating phase change aggregate coupled with moisture, heat, and light is prepared as follows: (1) The phase change material polyethylene glycol 600 and methyl laurate were mixed at a mass ratio of 1:1. The peak phase change temperature of the composite phase change material was measured to be 20℃ by differential scanning calorimetry, which is a low-temperature phase change material. (2) Take 50g of the low-temperature phase change material obtained in step (1) and heat it at 70°C until it is completely melted to obtain a low-temperature melt phase change material; (3) Take 45g of diatomaceous earth with an average particle size of 0.5mm as a porous carrier and place it in the low-temperature molten phase change material obtained in step (2). Adsorb it under a vacuum of -0.07MPa for 25min, then restore the normal pressure and continue to keep it warm for 10min so that the low-temperature molten phase change material can fully enter the pores of the diatomaceous earth. Filter and cool to obtain 85g of primary low-temperature phase change aggregate. It can be calculated that the adsorbed low-temperature molten phase change material is 40g. (4) Dissolve chitosan in a 1.0% acetic acid solution to prepare a 1.8% chitosan solution. Mix the chitosan solution with silica sol at a mass ratio of 3:1 to obtain a precursor solution of chitosan and silica sol composite. Take 1g MXene, as a photothermal response thermal conductivity regulating component, was added to 300g of the precursor solution of chitosan and silica sol composite and ultrasonically dispersed for 10min. The primary low-temperature phase change aggregate obtained in step (3) was placed in a continuously tumbling rolling coating device, and the precursor solution containing MXene was coated on the surface of the primary low-temperature phase change aggregate in several batches. After each coating, the chitosan was induced to gel and the silica sol was condensed by atomizing 0.5mol / L sodium bicarbonate solution with pH adjusted to 8.5. After each induction, the mixture was tumbled until there was no obvious free liquid on the particle surface and no continuous adhesion and agglomeration between particles, and then the precursor solution was coated and induced again. After filtration, it was dried at 40℃ to constant weight to obtain 96g of secondary low-temperature phase change aggregate. According to the mass increase after drying and deducting the mass of 1g MXene, the formed chitosan-silica sol composite humidity-responsive gel layer was 10g. (5) 20g of nano-SiO2 slurry was rolled onto the surface of the secondary low-temperature phase change aggregate obtained in step (4) in two separate roll coatings. The slurry was dried before the next roll coating was performed. Before the second roll coating, the particle turning direction was changed and the aggregate was dried at 40℃ for 12h to form a nano-SiO2 inorganic interface reinforcement layer, resulting in 100g of low-temperature self-regulating phase change aggregate-1. According to the mass increment after drying, the nano-SiO2 inorganic interface reinforcement layer was 4g.
[0041] Example 2 A self-regulating phase change aggregate coupled with moisture, heat, and light is prepared as follows: (1) Take 45g of high-temperature paraffin with a phase change temperature of 35℃ as a high-temperature phase change material, and heat it at 85℃ until it is completely melted to obtain a high-temperature molten phase change material; (2) Take 50g of ceramsite with an average particle size of 1.8mm and a compressive strength of 3.5 MPa as a porous carrier and place it in the high-temperature molten phase change material obtained in step (1). Adsorb it under a vacuum of -0.08MPa for 30min, then restore it to normal pressure and continue to keep it warm for 10min so that the high-temperature molten phase change material can fully enter the pores of the ceramsite. Filter and cool to obtain 85g of primary high-temperature phase change aggregate. It can be calculated that the adsorbed high-temperature molten phase change material is 35g. (3) Disperse 6g of sodium-based bentonite in 194g of deionized water and stir for 30min to obtain a bentonite suspension with a mass fraction of 3.0%; dissolve 6g of sodium polyacrylate in 294g of deionized water to obtain a sodium polyacrylate solution with a mass fraction of 2.0%; mix the bentonite suspension and the sodium polyacrylate solution evenly to obtain a 500g bentonite and polyacrylate composite precursor solution; take 3g of expanded graphite as a photothermal response thermal conductivity regulating component and add it to the 500g bentonite and polyacrylate composite precursor solution, and ultrasonically disperse for 10min; (2) The obtained primary high-temperature phase change aggregate was placed in a continuously tumbling rolling coating device. The precursor solution containing expanded graphite was coated on the surface of the primary high-temperature phase change aggregate in several times. After each coating, a calcium chloride solution with a mass fraction of 3.0% was sprayed as a crosslinking agent to induce gelation. After each spraying, the aggregate was tumbled until there was no obvious free liquid on the particle surface and no continuous adhesion and agglomeration between particles. Then the precursor solution was coated and the calcium chloride solution was sprayed again. After filtration, the aggregate was dried at 45°C to constant weight to obtain 100g of secondary high-temperature phase change aggregate. Based on the mass increase after drying and deducting the mass of 3g of expanded graphite, the humidity-responsive gel layer of bentonite and polyacrylate composite was calculated to be 12g. (4) Sodium metasilicate and calcium chloride were dissolved in deionized water to prepare a sodium metasilicate solution of 0.5 mol / L and a calcium chloride solution of 0.5 mol / L. The sodium metasilicate solution and calcium chloride solution were mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min. After filtration and washing with deionized water, water was added to prepare a calcium silicate hydrate slurry with a solid content of 20%. 25 g of calcium silicate hydrate slurry was rolled onto the surface of the secondary high-temperature phase change aggregate obtained in step (3) in two batches. The slurry was rolled and dried before the next roll was rolled. Before the second roll, the particle turning direction was changed and the aggregate was dried at 45°C for 24 h to obtain 105 g of high-temperature self-regulating phase change aggregate-2. According to the mass increment after drying, the calcium silicate inorganic interface reinforcement layer was 5 g.
[0042] Example 3 A self-regulating phase change aggregate coupled with moisture, heat, and light is prepared as follows: (1) The phase change material paraffin and stearic acid were mixed at a mass ratio of 7:3. The peak phase change temperature of the composite phase change material was measured to be 27℃ by differential scanning calorimetry, which is a medium-temperature phase change material. (2) Take 55g of the medium-temperature phase change material obtained in step (1) and heat it at 80°C until it is completely melted to obtain a medium-temperature melt phase change material; (3) Take 40g of expanded perlite with an average particle size of 0.9mm and a water absorption rate of 200% as a porous carrier and place it in the medium-temperature molten phase change material obtained in step (2). Adsorb it under a vacuum of -0.08MPa for 30min, then restore it to normal pressure and continue to keep it warm for 10min so that the medium-temperature molten phase change material can fully enter the pores of the expanded perlite. Filter and cool to obtain 85g of primary medium-temperature phase change aggregate. It can be calculated that the adsorbed medium-temperature molten phase change material is 45g. (4) Take 2g of carbon black as the photothermal response thermal conductivity control component and add it to 400g of sodium alginate solution with a mass fraction of 2.0% and ultrasonically disperse for 10min; place the primary medium-temperature phase change aggregate obtained in step (3) in a continuously turning rolling coating device, and coat the surface of the primary medium-temperature phase change aggregate with sodium alginate solution containing carbon black in several times. After each coating, spray calcium chloride solution with a mass fraction of 3.0% to induce sodium alginate ion crosslinking. After each spray, continue to turn until there is no obvious free liquid on the particle surface and no continuous adhesion and agglomeration between particles, and then perform the next coating of sodium alginate solution and spraying of calcium chloride solution; after filtration, dry at 40℃ to constant weight to obtain 95g of secondary medium-temperature phase change aggregate; according to the mass increase after drying and deducting the mass of 2g of carbon black, the formed calcium alginate humidity-responsive gel layer is 8g; (5) Water glass with a modulus of 1.5 and sodium hydroxide solution with a mass ratio of 4:1 were mixed and allowed to stand for 24 hours to obtain an alkali activator; metakaolin, alkali activator and silica sol with a solid content of 25% were mixed in a mass ratio of 5:3:2 and stirred for 10 minutes to obtain a uniform silica-alumina gel slurry; 7.5g of silica-alumina gel slurry was rolled onto the outer surface of the secondary medium-temperature phase change aggregate obtained in step (4) in two batches. The slurry was dried before the next roll was rolled. Before the second roll, the particle turning direction was changed and the aggregate was dried at 45℃ for 24 hours to form a silica-alumina gel inorganic interface reinforcement layer to obtain 100g of medium-temperature self-regulating phase change aggregate-3; the silica-alumina gel inorganic interface reinforcement layer was 5g according to the mass increment after drying.
[0043] Example 4 The only difference from Example 1 is that in step (5), the silicon-aluminum gel slurry prepared in the same way as in Example 3 is used instead of the nano-SiO2 slurry. The silicon-aluminum gel slurry is rolled onto the outer surface of the secondary low-temperature phase change aggregate in two separate applications. The slurry is rolled and dried before the next application. Before the second application, the direction of particle turning is changed and the aggregate is dried at 45°C for 24 hours to obtain 100g of low-temperature self-regulating phase change aggregate-4. According to the mass increment after drying, the silicon-aluminum gel inorganic interface reinforcement layer is 4g.
[0044] Example 5 The only difference from Example 2 is that in step (4), the silica-alumina gel slurry prepared in the same way as in Example 3 is used instead of the calcium silicate hydrate slurry. The silica-alumina gel slurry is rolled onto the outer surface of the secondary high-temperature phase change aggregate in two separate applications. The slurry is rolled and dried before the next application. Before the second application, the direction of particle turning is changed and the aggregate is dried at 45°C for 24 hours to obtain 105g of high-temperature self-regulating phase change aggregate-5. According to the mass increment after drying, the silica-alumina gel inorganic interface reinforcement layer is 5g.
[0045] Comparative Example 1 The only difference from Example 3 is that step (4) is omitted, and 2g of carbon black is dispersed in the silica-alumina gel slurry used in step (5), and then rolled onto the primary medium-temperature phase change aggregate obtained in step (3) together with the silica-alumina gel slurry, so that the amount of carbon black and silica-alumina gel inorganic interface reinforcement layer in the resulting comparative phase change aggregate-1 is the same as that in Example 3. This comparative example is used to investigate the effect of the lack of calcium alginate humidity-responsive gel layer on the encapsulation of phase change materials and mortar performance.
[0046] Comparative Example 2 The only difference from Example 3 is that carbon black, a photothermal response thermal conductivity regulating component, is not added in step (4), and a calcium alginate humidity-responsive gel layer without the photothermal response thermal conductivity regulating component is formed on the surface of the primary medium-temperature phase change aggregate. The phase change aggregate finally prepared in this comparative example is designated as comparative phase change aggregate-2.
[0047] Comparative Example 3 The only difference from Example 3 is that step (5) is not performed, and the secondary medium-temperature phase change aggregate prepared in step (4) is used as the comparative phase change aggregate-3.
[0048] Comparative Example 4 The primary medium-temperature phase change aggregate prepared in step (3) of Example 3 is used as the phase change aggregate. At the same time, it is used together with carbon black, calcium alginate gel and silica-alumina gel slurry prepared in the proportion of Example 3 as a mixed mortar admixture.
[0049] Performance Characterization 1. Morphological characteristics The secondary mesophilic phase change aggregate prepared in step (4) of Example 3 and the finally prepared mesophilic self-regulating phase change aggregate-3 were observed by scanning electron microscopy. The results are as follows: Figure 3 and Figure 4 As shown. By Figure 3 As can be seen, a continuous coating layer (i.e., a calcium alginate humidity-responsive gel layer) was formed on the outer surface of the porous carrier loaded with the phase change material through step (4). The surface of the coating layer is relatively dense, and no obvious through cracks were observed. Meanwhile, see also... Figure 3 In Figure (b), as indicated by the red arrow, carbon black particles are visible within the coating layer, indicating that the carbon black has been embedded in the calcium alginate humidity-responsive gel layer. Figure 4 It is evident that a filling phase exists within the pores of the porous carrier, indicating that the phase change material has entered the pores of the porous carrier. Meanwhile, a composite shell structure formed by the calcium alginate humidity-responsive gel layer and the silica-alumina gel inorganic interface reinforcement layer can be observed on the outside of the porous carrier.
[0050] 2. Applied to mortar performance testing Take 67.5g of the self-regulating phase change aggregates-1 to-3 prepared in Examples 1-3, the comparative phase change aggregates-1 to-3 prepared in Comparative Examples 1-3, and the mixed mortar admixture prepared in Comparative Example 4, respectively, and mix them with 450g of PO 42.5 ordinary Portland cement, 1350g of ISO standard sand, and 225g of mixing water. The amount of phase change aggregate or mixed mortar admixture is 15% of the mass of ordinary Portland cement, and the water-cement ratio is 0.50. Homogeneous mortar specimens are prepared according to the same mixing, molding, and curing regime, and the mortar properties are tested. The results are shown in Table 1.
[0051] Table 1. Performance test results of Examples 1-3 and Comparative Examples 1-4 applied to mortar
[0052] As shown in Table 1, the leakage rate of Example 3 was 0.7%, and the latent heat retention rate after 100 thermal cycles was 96.8%, while those of Comparative Example 1, which lacked a humidity-responsive gel layer, were 4.8% and 82.4%, respectively. This indicates that the humidity-responsive gel layer has a significant effect on inhibiting leakage of the phase change material and maintaining cycle stability. The photothermal response time of Comparative Example 2, which lacked carbon black, was 31.5 min, significantly longer than the 19.2 min of Example 3, indicating that carbon black is beneficial for improving the photothermal response rate. The 28-day compressive strength, flexural strength, and bond strength of Comparative Example 3, which lacked an inorganic interface reinforcement layer, were 29.4 MPa, 5.3 MPa, and 0.91 MPa, respectively, lower than the 38.6 MPa, 7.2 MPa, and 1.52 MPa of Example 3, indicating that the inorganic interface reinforcement layer is beneficial for improving the compressive strength, flexural strength, and bond strength of the mortar. The 28-day compressive strength of Comparative Example 4, in which all components are physically mixed, is 28.7 MPa, flexural strength is 5.1 MPa, bond strength is 0.82 MPa, leakage rate is 3.6%, photothermal response time is 27.2 min, and latent heat retention rate after 100 thermal cycles is 84.1%, all of which are lower than those of Example 3. This indicates that the multilayer composite structure of Example 3 is beneficial to leveraging the synergistic effect of each functional component.
[0053] II. Preparation of Phase Change Mortar Example 6 A cement-based gradient phase change mortar, comprising, from the surface to the bottom layer, a photothermal response protective mortar layer, a phase change heat storage mortar layer, and a humidity-controlled slow-release mortar layer along its thickness direction; wherein, the photothermal response protective mortar layer comprises, by weight, the following components: 30 parts ordinary Portland cement, 55 parts quartz sand, 10 parts high-temperature self-regulating phase change aggregate-2 prepared in Example 2, 5 parts silica fume, 0.3 parts polypropylene fiber, 0.5 parts water-reducing agent, and mixing water, wherein the water-cement ratio is 0.36; the phase change heat storage mortar layer comprises, by weight, the following components: The mortar layer comprises 30 parts ordinary silicate cement, 38 parts quartz sand, 25 parts of the medium-temperature self-regulating phase change aggregate-3 prepared in Example 3, 8 parts slag powder, 0.2 parts cellulose ether, 0.5 parts water-reducing agent, and mixing water, wherein the water-cement ratio is 0.38; the moisture-release regulated mortar layer comprises the following components by mass: 30 parts ordinary silicate cement, 48 parts quartz sand, 12 parts of the low-temperature self-regulating phase change aggregate-1 prepared in Example 1, 3 parts expanded graphite, 5 parts metakaolin, 0.5 parts water-reducing agent, and mixing water, wherein the water-cement ratio is 0.40.
[0054] During the construction of this cement-based gradient phase change mortar, photothermal response protective mortar, phase change heat storage mortar, and humidity-controlled slow-release mortar are prepared according to the above-mentioned component ratios. A 5mm thick humidity-controlled slow-release mortar layer is formed on the surface of the base layer using the humidity-controlled slow-release mortar. An 18mm thick phase change heat storage mortar layer is formed on the surface of the humidity-controlled slow-release mortar layer using the phase change heat storage mortar. A 3mm thick photothermal response protective mortar layer is formed on the surface of the phase change heat storage mortar layer using the photothermal response protective mortar. After molding, the mortar is covered with a polyethylene film and left to stand for 24 hours in an environment of 20±2℃. After demolding, it is cured for 28 days under standard curing conditions of 20±2℃ and relative humidity not less than 95%.
[0055] Example 7 A geopolymer-based gradient phase change mortar comprises, from the surface to the bottom layer, a photothermal response protective mortar layer, a phase change thermal storage mortar layer, and a humidity-controlled slow-release mortar layer, arranged sequentially along the thickness direction. The cementing material is a low-carbon geopolymer cementing system prepared from slag powder, fly ash, and metakaolin in a mass ratio of 5:3:2. The alkali activator is a composite solution of water glass and sodium hydroxide with a modulus of 1.3, and the liquid-to-solid ratio is 0.42. The photothermal response protective mortar layer comprises 35 parts of cementitious material, 55 parts of quartz sand, 10 parts of high-temperature self-regulating phase change aggregate-5 prepared in Example 5, 0.3 parts of basalt fiber, and 14.7 parts of alkali activator; the phase change thermal storage mortar layer comprises 37.5 parts of cementitious material, 45 parts of quartz sand, 25 parts of medium-temperature self-regulating phase change aggregate-3 prepared in Example 3, and 15.8 parts of alkali activator; the humidity slow-release regulating mortar layer comprises 37.2 parts of cementitious material, 55 parts of quartz sand, 12 parts of low-temperature self-regulating phase change aggregate-4 prepared in Example 4, 3 parts of boron nitride thermally conductive filler, and 15.6 parts of alkali activator.
[0056] During the construction of the polymer-based gradient phase change mortar, photothermal response protective mortar, phase change thermal storage mortar, and humidity-controlled slow-release mortar were prepared according to the above-mentioned component ratios. An 8mm thick humidity-controlled slow-release mortar layer was formed on the base surface, followed by a 16mm thick phase change thermal storage mortar layer on top of the humidity-controlled mortar layer, and finally a 3mm thick photothermal response protective mortar layer on top of the phase change thermal storage mortar layer. After molding, the mortar was covered with a polyethylene film and left to stand at 20±2℃ for 24 hours. After demolding, it was sealed and cured for 7 days, and then cured for 28 days at 20±2℃ and 65±5% relative humidity.
[0057] Comparative Example 5 The difference from Example 6 is that the gradient structure with layers along the thickness direction in Example 6 is not used. Instead, the same components as in Example 6 are directly and uniformly mixed in one go according to the principle of the same dosage to prepare a homogeneous phase change mortar.
[0058] Comparative Example 6 The difference from Example 6 is as follows: Paraffin wax with a phase change temperature of 35°C is used as a high-temperature phase change aggregate to replace the high-temperature self-regulating phase change aggregate-2 prepared in Example 2 added to the photothermal response protective mortar layer; expanded perlite is used as a composite phase change material of paraffin wax and stearic acid with a phase change temperature of 27°C as a medium-temperature phase change aggregate to replace the medium-temperature self-regulating phase change aggregate-3 prepared in Example 3 added to the phase change thermal storage mortar layer; diatomaceous earth is used as a composite phase change material of polyethylene glycol 600 and methyl laurate with a phase change temperature of 20°C as a low-temperature phase change aggregate to replace the low-temperature self-regulating phase change aggregate-1 prepared in Example 1 added to the humidity-controlled mortar layer; and a gradient phase change mortar containing ordinary phase change aggregate is prepared according to the same three-layer gradient preparation steps as in Example 6.
[0059] Performance testing The performance of the mortars prepared in Examples 6 and 7 and Comparative Examples 5 and 6 was tested, and the results are shown in Table 2.
[0060] Table 2. Mortar performance test results of Examples 6 and 7 and Comparative Examples 5 and 6
[0061] As shown in Table 2, the 28-day compressive strength, flexural strength, and bond strength of Example 6 were 40.2 MPa, 7.5 MPa, and 1.58 MPa, respectively, which were higher than those of Comparative Example 5 (34.8 MPa, 6.1 MPa, and 1.10 MPa, respectively), indicating that the layered gradient structure is beneficial for balancing surface strength and interlayer bonding performance. Compared with Comparative Example 6, which used ordinary phase change aggregate, the leakage rate of Example 6 decreased from 4.1% to 0.8%, and the latent heat retention rate after 100 thermal cycles increased from 85.7% to 97.2%. The 28-day compressive strength of Example 7 was 38.5 MPa, the leakage rate was 0.9%, and the latent heat retention rate after 100 thermal cycles was 96.5%, indicating that the geopolymer-based gradient phase change mortar also has good mechanical properties, impermeability, and thermal cycling stability.
Claims
1. A self-regulating phase change aggregate coupled with moisture, heat, and light, characterized in that, The device comprises a porous carrier, a phase change material, a humidity-responsive gel layer, a photothermal-responsive thermal conductivity regulating component, and an inorganic interface reinforcement layer. The phase change material is loaded in the pores of the porous carrier, the humidity-responsive gel layer is continuously or semi-continuously coated on the outside of the porous carrier, the photothermal-responsive thermal conductivity regulating component is dispersed in the humidity-responsive gel layer, and the inorganic interface reinforcement layer is coated on the outside of the humidity-responsive gel layer. The porous carrier is selected from one or more of expanded perlite, diatomaceous earth, and ceramsite; the phase change material is selected from one or more of paraffin wax, stearic acid, methyl laurate, and polyethylene glycol; the humidity-responsive gel layer is selected from any one of calcium alginate gel, chitosan and silica sol composite gel, and bentonite and polyacrylate composite gel; the photothermal response thermal conductivity regulating component is selected from any one or more of carbon black, expanded graphite, and MXene; and the inorganic interface reinforcement layer is selected from any one of nano-SiO2 layer, calcium silicate hydrate layer formed by the reaction of sodium metasilicate and calcium salt, and aluminosilicate gel layer formed by the reaction of metakaolin, alkali activator, and silica sol.
2. The self-regulating phase change aggregate based on the coupling of moisture, heat, and light according to claim 1, characterized in that, The components are proportioned as follows by weight: 40-50 parts porous carrier, 35-45 parts phase change material, 8-12 parts humidity-responsive gel layer, 1-3 parts photothermal response thermal conductivity regulating component, and 4-5 parts inorganic interface reinforcement layer.
3. The self-regulating phase change aggregate based on the coupling of moisture, heat, and light according to claim 1, characterized in that, The phase change material is a low-temperature phase change material composed of polyethylene glycol and methyl laurate with a phase change temperature of 18~22℃, or a medium-temperature phase change material composed of paraffin and stearic acid with a phase change temperature of 24~28℃, or a high-temperature phase change material composed of paraffin and stearic acid with a phase change temperature of 32~38℃.
4. A method for preparing self-regulating phase change aggregate through hydrothermal and optical coupling, characterized in that, The method for preparing the self-regulating phase change aggregate based on the coupling of wet heat and light as described in any one of claims 1-3 includes the following steps: S1. Heat and melt the phase change material to obtain molten phase change material; S2. Place the porous carrier in the molten phase change material, and under vacuum conditions, allow the molten phase change material to enter the pores of the porous carrier to obtain primary phase change aggregate; S3. Disperse the photothermal response thermal conductivity regulating component in the precursor solution of the humidity response gel layer, coat the precursor solution containing the photothermal response thermal conductivity regulating component on the surface of the primary phase change aggregate, and induce cross-linking of the precursor to form a humidity response gel layer with the photothermal response thermal conductivity regulating component embedded in the internal or external surface of the primary phase change aggregate to obtain the secondary phase change aggregate. S4. The slurry of the inorganic interface reinforcement layer is coated on the outer surface of the secondary phase change aggregate in multiple layers. After each layer of slurry is surface dry, the next layer is coated. The inorganic interface reinforcement layer is formed by drying and curing, and the phase change aggregate with wet heat and light coupling is obtained.
5. The method for preparing self-regulating phase change aggregate by hydrothermal and optical coupling according to claim 4, characterized in that, In step S3, when the humidity-responsive gel layer is calcium alginate gel, sodium alginate solution is used as a precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing photothermal response and thermal conductivity regulating components is coated onto the surface of the primary phase change aggregate in several stages. After each coating, atomized calcium salt solution is sprayed to induce sodium alginate ion crosslinking to form calcium alginate gel. When the humidity-responsive gel layer is a chitosan and silica sol composite gel, a chitosan and silica sol composite solution is used as a precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, a precursor solution containing photothermal response and thermal conductivity regulating components is sprayed onto the surface of the primary phase change aggregate in several stages. The precursor solution of the control component is coated onto the surface of the primary phase change aggregate in multiple applications. After each application, chitosan gelation is induced by an alkaline environment, and silica sol is condensed to form a chitosan-silica sol composite gel. When the humidity-responsive gel layer is a bentonite-polyacrylate composite gel, a bentonite-polyacrylate composite solution is used as the precursor solution. Under the condition of continuous agitation of the primary phase change aggregate, the precursor solution containing the photothermal response thermal conductivity control component is coated onto the surface of the primary phase change aggregate in multiple applications. After each application, a crosslinking agent is sprayed to induce gelation and form a bentonite-polyacrylate composite gel.
6. The application of the self-regulating phase change aggregate based on the coupling of moisture, heat, and light as described in any one of claims 1-3 in phase change mortar, characterized in that, The phase change mortar, from the surface to the bottom layer along its thickness direction, comprises a photothermal response protective mortar layer, a phase change thermal storage mortar layer, and a humidity-controlled slow-release mortar layer. Each mortar layer includes a cementing material and the humidity-heat and light-coupled self-regulating phase change aggregate. Specifically, in the photothermal response protective mortar layer, the mass ratio of phase change aggregate to cementing material is 1:(3.0~3.5), and the phase change aggregate uses a high-temperature phase change material with a phase change temperature of 32~38℃. In the phase change thermal storage mortar layer, the mass ratio of phase change aggregate to cementing material is 1:(1.2~1.5), and the phase change aggregate uses a medium-temperature phase change material with a phase change temperature of 24~28℃. In the humidity-controlled slow-release mortar layer, the mass ratio of phase change aggregate to cementing material is 1:(2.5~3.1), and the phase change aggregate uses a low-temperature phase change material with a phase change temperature of 18~22℃.
7. The application according to claim 6, characterized in that, The photothermal responsive protective mortar layer also includes reinforcing fillers, which are selected from one or more of silica fume, polyethylene fiber, and basalt fiber.
8. The application according to claim 6, characterized in that, The humidity-controlled mortar layer also includes a thermally conductive filler, which is selected from one or both of expanded graphite and boron nitride.
9. The application according to claim 6, characterized in that, In the phase change mortar, the thickness of the photothermal response protective mortar layer is 3 mm, the thickness of the phase change heat storage mortar layer is 16~18 mm, and the thickness of the humidity slow-release regulating mortar layer is 5~8 mm.
10. The application according to any one of claims 6-9, characterized in that, The preparation method of the phase change mortar is as follows: photothermal response protective mortar, phase change heat storage mortar and humidity slow-release regulating mortar are prepared respectively; the humidity slow-release regulating mortar is applied to the surface of the base layer to form the humidity slow-release regulating mortar layer; the phase change heat storage mortar is applied to the surface of the humidity slow-release regulating mortar layer to form the phase change heat storage mortar layer; and the photothermal response protective mortar is applied to the surface of the phase change heat storage mortar layer to form the photothermal response protective mortar layer.