A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization
By using triethanolamine-enhanced sodium carbonate recycling mineralization, the problem of low mineralization efficiency of calcium and magnesium components in steel slag and red mud in existing technologies has been solved. This method achieves efficient CO2 mineralization and rapid slurry reaction of backfill materials with low sodium carbonate content, thereby improving the carbon fixation potential and mechanical properties of backfill materials. It is suitable for green backfill mining in coal mines.
Patent Information
- Application Number
- CN202611484287.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing coal-based solid waste cemented backfill materials have limited effective calcium and magnesium content in CO2 mineralization reactions, resulting in insufficient CO2 fixation capacity per unit backfill material. This makes it difficult to achieve efficient carbon fixation simultaneously during backfill preparation and curing. Furthermore, the high energy consumption of pretreatment or high sodium carbonate content in existing technologies can lead to increased costs, salt accumulation, and unstable hydration reactions.
A triethanolamine-enhanced sodium carbonate recycling mineralization method is adopted. By adding sodium carbonate and triethanolamine to steel slag and red mud, CO2 mineralization reaction is promoted to form carbon-fixing backfill material suitable for different coal-based solid waste cemented backfill material ratios. The mineralization efficiency and mechanical properties of the backfill material are improved by utilizing the chelating effect of triethanolamine and the recycling mechanism of sodium carbonate.
Under low-alkali conditions, it achieved efficient CO2 mineralization fixation and synergistic improvement of backfill performance, shortened reaction time, increased carbon fixation and mechanical properties of backfill materials, is suitable for continuous mining operations, and reduced cost risks.
Smart Images

Figure CN123106091A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of green backfilling mining technology in coal mines, specifically a method for preparing carbon-fixing backfill materials by triethanolamine-enhanced sodium carbonate recycling mineralization. Background Technology
[0002] Coal mining, coal-fired power generation, steel smelting, and coal chemical processes generate large amounts of CO2, along with bulk solid waste such as coal gangue, fly ash, coal gasification slag, steel slag, and red mud. How to achieve synergistic CO2 emission reduction, solid waste disposal, and goaf remediation within mining areas is a pressing issue that needs to be addressed in the green and low-carbon transformation of the coal and related energy-intensive industries. Preparing solid waste containing alkaline minerals into mine backfill materials, and allowing CO2 to undergo a mineralization reaction with the calcium and magnesium components during the backfilling process to form stable carbonates, is a technological approach that combines CO2 fixation, solid waste resource utilization, and goaf remediation.
[0003] Existing coal-based solid waste cemented backfill materials typically use coal gangue, fly ash, coal slime, and coal gasification slag as main raw materials, relying primarily on cement, slag, and other cementing components to form hydration products to achieve backfill strength. While these materials can meet the backfilling requirements of goaf areas, the effective calcium and magnesium components that can directly participate in CO2 mineralization reactions are limited in their system, resulting in insufficient CO2 fixation capacity per unit backfill material. This makes it difficult to achieve efficient carbon fixation simultaneously during backfill preparation and curing.
[0004] Alkaline industrial solid wastes such as steel slag and red mud contain a high proportion of calcium and magnesium components, theoretically possessing high CO2 mineralization potential. However, the calcium and magnesium elements in these solid wastes do not all exist in highly reactive forms such as free CaO and free MgO. Most of them are encapsulated or solidified in calcium silicate, calcium aluminoferrite, calcium aluminum silicate, and other mineral phases with relatively stable crystal structures. The low dissolution rate and weak migration ability of these calcium and magnesium components limit the actual carbon fixation efficiency of steel slag and red mud in the filling system.
[0005] To improve the efficiency of solid waste mineralization, existing technologies typically employ methods such as increasing reaction temperature, increasing CO2 pressure, extending carbonization time, increasing mechanical grinding intensity, and adding admixtures. However, mine backfill materials must simultaneously meet engineering requirements such as continuous slurry preparation, pipeline transportation, goaf filling, setting and hardening, and subsequent load-bearing capacity. Simply relying on high-energy-consuming pretreatment or prolonged carbonization processes to enhance the mineralization reaction not only increases process complexity and operating costs, making it difficult to adapt to continuous mine backfill operations, but also affects the working and mechanical properties of the backfill material, leading to failure to meet engineering requirements. Conversely, simply increasing the dosage of carbonate admixtures such as sodium carbonate may cause problems such as salt accumulation in the system, deterioration of slurry rheological properties, disruption of hydration reactions, unstable early strength development, and increased material costs.
[0006] A 2025 Chinese patent (CN 121377695 A) discloses a coal slime-based goaf backfill material and carbon fixation method. Sodium carbonate is used to activate the pozzolanic activity of the coal slime, creating favorable conditions for subsequent carbon dioxide mineralization reactions and making CO2 more soluble in water, thereby promoting the carbon fixation capacity of the backfill material. However, sodium carbonate does not directly participate in the chemical cycle mineralization reaction. Studies have shown that to achieve sufficient mineralization of calcium and magnesium components in steel slag and red mud, sodium carbonate and sodium hydroxide are usually added in a 1:1 ratio. However, high sodium carbonate content leads to increased backfill material costs, excessive salinity, disruption of the hydration process, unstable early strength development, and unsuitability for continuous backfilling operations in mines. In the field of CO2 capture, triethanolamine has been attempted for direct absorption of gaseous CO2. However, existing technologies have not applied triethanolamine to mineralized backfill systems containing steel slag and red mud. The reason for this is that triethanolamine, when used alone in filling materials, can only utilize its own ability to absorb CO2, but cannot stimulate the carbon fixation potential of the filling materials, thus failing to achieve large-capacity carbon fixation and making its addition largely meaningless. Therefore, there is an urgent need for a method to prepare filling materials that can still achieve efficient CO2 mineralization, rapid slurry reaction, and stable strength development in the later stages, even with low sodium carbonate content. Summary of the Invention
[0007] This invention overcomes the shortcomings of existing technologies by proposing a method for preparing carbon-fixing backfill materials through triethanolamine-enhanced sodium carbonate recycling mineralization. Based on the principle that amine promotes carbonate recycling to regulate the reactivity of calcium-magnesium solid wastes such as steel slag and red mud, this invention achieves a synergistic improvement in carbon dioxide mineralization and backfill performance under low-alkali conditions. It solves the problems of large sodium carbonate consumption, long reaction time, and unsuitability for backfill material preparation during the sodium carbonate mineralization process, while simultaneously stimulating the carbon fixation potential of the backfill materials.
[0008] This invention is achieved through the following technical solution: A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization includes the following steps: S1. Mixing raw materials: Steel slag, red mud and coal-based solid waste cementitious filling material are placed in a reaction vessel, water is added and stirred to make the solid particles uniformly dispersed in the liquid phase to obtain the initial filling slurry; S2. Adding sodium carbonate and triethanolamine: Add sodium carbonate and triethanolamine to the obtained initial filling slurry, and continue stirring until the two are evenly dispersed in the initial filling slurry to form a filling slurry to be carbonized containing sodium carbonate and triethanolamine; the amount of sodium carbonate is 2-5% of the total mass of steel slag and red mud; the amount of triethanolamine is 0.02-0.05% of the total mass of cementitious materials; S3. Introduce CO2: Introduce CO2 gas into the obtained carbonized filling slurry to obtain solid carbonized filling slurry; S4. Cast the specimen, demold and cure to obtain the carbon-fixed filling material.
[0009] Furthermore, the carbon injection pressure during the CO2 introduction process is 0.5~2.5 MPa.
[0010] Furthermore, in step S1, water is added after stirring for 5-10 minutes, and stirring is continued for another 5-10 minutes to ensure that the solid particles are uniformly dispersed in the liquid phase.
[0011] Furthermore, in step S2, continue stirring for 5-10 minutes until both are evenly dispersed in the filling slurry.
[0012] Furthermore, in step S3, during the introduction of CO2, the reaction is carried out by stirring at a speed of 300~1000 rpm for 20~30 minutes.
[0013] Furthermore, in step S3, the pressure inside the reactor is 1.0~1.5MPa, and the reaction temperature is 25~65℃.
[0014] Furthermore, the steel slag is one of converter steel slag, open-hearth steel slag, and electric arc furnace steel slag. Steel slag is classified into converter steel slag, open-hearth steel slag, and electric arc furnace steel slag according to the steelmaking method. Among them, converter steel slag has a higher total CaO mass fraction, and the content of various calcium components is generally dominant, indicating that it has a significant calcium-rich characteristic. The main chemical components of the converter steel slag include calcium oxide (CaO) accounting for 35%~55%, and free calcium oxide (f-CaO) accounting for 5%~20%; in the main mineral phase composition, tricalcium silicate (C3S) accounts for 20%~30%, and dicalcium silicate (C2S) accounts for 15%~25%.
[0015] Furthermore, the red mud is one of the Bayer process red mud, sintering process red mud, and combined process red mud. Red mud is classified into Bayer process red mud, sintering process red mud, and combined process red mud according to the alumina production process. Among them, the combined process red mud has a higher total CaO mass fraction and a significant overall enrichment of calcium components, indicating that it has a significant calcium-rich characteristic. The combined process red mud has a CaO content of 40%–50% in its main chemical components and a C2S content of 25%–40% in its main mineral phase composition.
[0016] Furthermore, the mass ratio of steel slag to red mud is 9~4:1~6.
[0017] The principle of this invention is as follows: The raw materials for coal-based solid waste cemented backfill material adopt any proportion system that meets the requirements of backfill fluidity, cementation hardening performance and underground backfilling. In addition, a carbon fixation reaction component composed of steel slag and red mud is added to the proportion system, and sodium carbonate and triethanolamine are added as synergistic enhancers so that the carbon fixation reaction component undergoes a mineralization reaction under the condition of carbon dioxide introduction, forming a carbon fixation backfill material suitable for different proportions of coal-based solid waste cemented backfill materials.
[0018] Although the steel slag and red mud are rich in Ca / Mg, most of the Ca / Mg is bound in low-reactivity mineral phases such as calcium silicate. Conventional CO2 carbonization mainly consumes free Ca in the pore fluid. 2+ It is difficult to sustain the induction of calcium migration and release from the crystal lattice; sodium carbonate, as a carbonate donor, reacts with mineral phases such as dicalcium silicate and tricalcium silicate, causing the Ca bound by the mineral phase structure to... 2+ It is converted into CaCO3 precipitate, and Na2SiO3 and NaOH are generated simultaneously.
[0019] The triethanolamine is introduced into the carbon-fixing backfill slurry containing steel slag and red mud as a reinforcing agent of the sodium carbonate circulating mineralization system. It is used to promote the dissolution of CO2 in the liquid phase of the slurry and promote the in-situ regeneration of NaOH and Na2SiO3 generated during the circulating mineralization process into Na2CO3 under the action of CO2. This allows sodium carbonate to continuously participate in the carbonate precipitation reaction, thereby shortening the circulating mineralization reaction time and significantly improving the mineralization efficiency of the backfill material.
[0020] Sodium carbonate, which undergoes chemical recycling and carbon fixation during the mixing stage, remains in the pore fluid of the filling slurry, providing Na for the subsequent curing stage. + It participates in the formation of hydrated sodium aluminum silicate (NASH) gel, thereby achieving a continuous synergistic effect between the mixing and curing stages and improving the mechanical properties of its filling material.
[0021] During the curing phase, triethanolamine significantly reduced the free Ca2+ in the pore solution through chelation. 2+ And Al 3+ The concentration of fly ash was reduced, thus breaking the bottleneck of slow early dissolution and allowing more calcium and aluminum components to dissolve continuously, generating more nanoscale gel products. This significantly reduced the total porosity of the slurry, and the refinement of the pore structure directly contributed to the improvement of the compressive strength of the filling material.
[0022] In summary, incorporating sodium carbonate is the main way to increase carbon fixation, utilizing Na₂CO₃ to rapidly precipitate Ca in the solution. 2+ The generation of CaCO3 continuously disrupts the thermodynamic equilibrium of the calcium silicate phase in steel slag and red mud, creating a strong driving force. Subsequently, Na2CO3 is regenerated under the action of CO2, thus constructing a sustainable cycle process. The addition of triethanolamine is the main way to accelerate the mineralization reaction rate. Triethanolamine contains both amino groups and multiple hydroxyl groups, forming a unique "tripod" structure that can quickly capture CO2 molecules and react to generate alkyl bicarbonate. Under alkaline conditions, it can be further deprotonated and converted into CO3. 2- .
[0023] Furthermore, the sodium carbonate can still participate in the activation and reconstruction of aluminosilicate components in solid waste during the curing stage. Under a highly alkaline environment, the amorphous or low-crystallinity Si-O and Al-O networks in solid wastes such as fly ash gradually depolymerize, and the released silicate and aluminate ions can react with Na+. + Together they participate in the formation of hydrated sodium aluminum silicate gel or together with calcium to form a composite hydrated aluminum silicate gel. This type of gel product can fill the pores between particles and encapsulate unreacted particles, thereby organically linking the mineralization and carbon fixation process in the stirring stage with the gelation and hardening process in the curing stage, and achieving a synergistic improvement in carbon fixation reaction and mechanical property development.
[0024] Furthermore, during the curing stage, the triethanolamine reduces the instantaneous saturation of some free metal ions through chelation, promoting the continuous dissolution of the surface of particles such as fly ash, steel slag, and red mud. This allows components such as calcium, aluminum, and silicon to continuously enter the pore liquid and participate in hydration and polymerization reactions. This effect helps to overcome the problem of insufficient early dissolution rate of glassy phase or low-activity mineral phase in coal-based solid waste, increases the generation of hydrated calcium silicate gel (CSH), hydrated calcium aluminum silicate gel (CASH), NASH, and their composite gels, and gradually transforms the pores of the slurry from interconnected macropores to fine gel pores and capillaries, thereby improving the structural density and compressive strength of the filling body.
[0025] The main reaction mechanisms and chemical reactions involved in the mineralization and carbon fixation process of this invention are as follows: Reaction Mechanism 1: Due to Ca 2+ It is a divalent cation and can react with CO3. 2- A strong electrostatic reaction occurs, forming a CaCO3 precipitate with extremely low solubility; in contrast, Na... + It is a monovalent cation, reacting with CO3. 2- The formed Na₂CO₃ has high solubility and mainly remains in the liquid phase in ionic form; therefore, under the action of sodium carbonate, the Ca released from steel slag and red mud... 2+ Priority for CO3 2- It is fixed as CaCO3, while Na + It mainly serves to balance charge and maintain an alkaline environment.
[0026] 3 Na2CO3+Ca3SiO5+ H2O→Na2SiO3+ 3CaCO3↓+ 4NaOH Reaction 2: 2 Na2CO3+Ca2SiO4+ H2O→Na2SiO3+ 2CaCO3↓+ 2NaOH Reaction 3: Na2CO3+ CaO + H2O→CaCO3↓+ 2NaOH Reaction 4: CO2+ Na2SiO3+ H2O→H2SiO3+ Na2CO3 Reaction 5: CO2 + 2NaOH → H2O + Na2CO3 Reaction Mechanism 2: The chelation, dispersion, and solubilization effects of triethanolamine on active calcium-silicon phases and free calcium oxide in steel slag and red mud accelerate the migration of calcium components into the liquid phase, while simultaneously promoting the conversion of CO2 to CO3. 2- The conversion increases the effective CO3 in the system. 2- The supply of sodium carbonate is beneficial for the Na2SiO3 and NaOH generated in the reaction to be further converted and regenerated under the action of CO2, thereby improving the recycling efficiency with a lower sodium carbonate content, shortening the reaction time, and avoiding the limitations of high sodium carbonate dosage and long cycle treatment on the adaptability of filling material preparation process.
[0027] Reaction 6: TEA + H2O TEAH + + OH − Reaction 7: CO2 + H2O + 2TEA CO3 2- + 2TEAH + The beneficial effects of this invention compared to the prior art are as follows: 1. This invention uses multi-source industrial solid waste such as steel slag, red mud, coal gangue, and fly ash as main raw materials to construct a triethanolamine-regulated sodium carbonate recycling and mineralization carbon fixation filling material system. Unlike existing technologies that mainly use sodium carbonate as an alkaline activator or pH adjuster, this invention uses sodium carbonate as a carbonate recycling carrier and mineralization reaction medium, enabling it to undergo dynamic regeneration and recycling during the calcium-magnesium mineral phase carbonation, carbon dioxide-water phase conversion, and silicate phase reaction, thereby continuously promoting the mineralization and carbon fixation of calcium-magnesium components in steel slag and red mud.
[0028] 2. This invention further enhances the above-mentioned cyclic mineralization process by introducing triethanolamine. Triethanolamine helps promote the absorption and conversion of CO2 in the alkaline aqueous phase and increases CO3 concentration. 2- / HCO3 - / OH -The dynamic conversion efficiency between these processes is improved, thereby accelerating the sodium carbonate recycling efficiency and avoiding the risks of salt accumulation, increased cost, decreased fluidity, and later-stage stability in the filling material caused by solely relying on large amounts of sodium carbonate to supply carbonate ions. From a chemical reaction mechanism perspective, introducing triethanolamine into the chemical recycling mineralization of sodium carbonate not only overcomes the shortcomings of large dosage, long reaction time, and unsuitability for filling material preparation in the sodium carbonate mineralization process, but also stimulates the carbon fixation potential of the filling material, resulting in a significant increase in carbon fixation compared to using triethanolamine or sodium carbonate alone.
[0029] 3. This invention achieves synergistic coupling between the CO2 mineralization and carbon fixation process and the hydration and hardening process of the backfill material. On the one hand, the carbonate products generated by the mineralization reaction can fill the pores of the slurry, optimize the microstructure, and improve the density of the backfill. On the other hand, the active silica-alumina-calcium components in steel slag, red mud, fly ash, and coal gangue further participate in the hydration reaction under the alkaline environment and the regulation of triethanolamine, generating CSH gel, CASH gel, and AFt-type hydration products, forming a composite cemented structure in which carbonate crystals and hydration gels interlock, thereby improving the early strength, later strength, and long-term stability of the backfill.
[0030] During the curing stage, sodium carbonate promotes the dissolution of aluminosilicate components such as fly ash and participates in the formation of NASH gel, while triethanolamine can regulate Ca2+ through chelation. 2+ Al 3+ The dissolution and migration of plasma coordinate the carbonate precipitation and hydration gel formation processes, alleviating the problem of delayed early hydration that may occur when sodium carbonate acts alone. The two work together to improve the working performance and mechanical properties of the filling body, which is of great significance for realizing carbon dioxide fixation, multi-source solid waste resource utilization and goaf filling and treatment.
[0031] 4. The raw materials of this invention are widely available, the preparation process is simple and the cost is low, making it suitable for industrial application and promotion. It has positive significance for promoting the collaborative treatment of multi-source solid waste, carbon dioxide emission reduction and green and low-carbon mining. Attached Figure Description
[0032] Figure 1 This is a flowchart of the method described in this invention. Detailed Implementation
[0033] To make the technical problems to be solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail with reference to the embodiments and accompanying drawings. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention. The technical solutions of this invention are described in detail below with reference to the embodiments and accompanying drawings, but the scope of protection is not limited thereto. Example 1
[0034] A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization includes the following steps: S1, Raw material mixing 1. The cementitious material is composed of fly ash and cement. Based on the total mass of the cementitious material, the fly ash content is 80% and the cement content is 20%; the water-cement ratio of the cementitious material is 0.54. 2. The aggregate consists of fine aggregate, medium aggregate, and coarse aggregate. Based on the total mass of the aggregate, fine aggregate accounts for 30%, and medium and coarse aggregate each account for 35%. 3. The water-reducing agent is an external admixture, with the admixture dosage based on the total mass of the cementitious materials at 3%. 4. Converter steel slag and combined process red mud are used as high Ca / Mg auxiliary materials with a mass ratio of 6:4. This compound auxiliary material is an external admixture, and the external admixture basis is the total mass of the matrix of cementitious materials and aggregates, with an external admixture amount of 20%.
[0035] All the above raw materials were put into the reactor and mixed. The temperature inside the reactor was set to 25°C and the pressure was set to 0 MPa. The stirring speed of the stirring paddle inside the reactor was adjusted to 500 rpm and stirred for 10 minutes. After mixing evenly, a solid carbon filling base slurry was obtained. The overall mass concentration of the slurry was controlled to be 79%.
[0036] S2, Modification and regulation by adding sodium carbonate and triethanolamine Take the base slurry prepared by S1 and add the modifying and enhancing components sodium carbonate and triethanolamine. The amount of sodium carbonate added is 2% of the total mass of converter steel slag and combined process red mud, and the amount of triethanolamine is a 0.01 mol / L solution, added at 0.02% of the total mass of the cementitious materials. Adjust the system moisture content by adding an appropriate amount of water to ensure that the mass concentration of the modified slurry remains at 79%. Transfer the modified slurry to a reactor and stir for 10 minutes at 25℃, 0 MPa, and 500 rpm to ensure uniform compounding of the modifying components with the base slurry.
[0037] S3, Atmospheric-Pressure Coupled CO2 Mineralization Reaction After the modification and stirring were completed, the process parameters of the reactor were adjusted as follows: reaction temperature 30℃, stirring speed 700rpm, CO2 gas was introduced into the reactor, carbon injection pressure was controlled at 2MPa, the reaction pressure in the reactor was stabilized at 1MPa, and the mineralization reaction was carried out under constant temperature and pressure for 30min to obtain a carbon-fixed filling slurry synergistically enhanced by triethanolamine-sodium carbonate.
[0038] The mineralization reaction process was characterized by real-time testing. The maximum total carbon sequestration of the modified system was 68.08 kg CO2 / t, and the mineralization reaction rate was 0.46 kg CO2 / (t·min).
[0039] S4, Casting Specimens The carbon-fixing filler slurry, which has undergone S3 mineralization reaction, is rapidly injected into a molding mold. The air bubbles inside the slurry are eliminated by vibration and static venting. The slurry is then leveled and molded to obtain a preliminary specimen of the modified mineralized carbon-fixing filler material.
[0040] S5, Demolding and Curing After the specimens were allowed to set initially, they were demolded and placed in a standard curing chamber for constant temperature and humidity curing for 28 days. The final product was a triethanolamine-enhanced sodium carbonate circulating mineralization-enhanced carbon-fixing filling material. After curing, the uniaxial compressive strength of the specimens reached 13.11 MPa. Example 2
[0041] A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization includes the following steps: S1, Raw material mixing 1. The cementitious material is composed of fly ash and cement. Based on the total mass of the cementitious material, the fly ash content is 80% and the cement content is 20%; the water-cement ratio of the cementitious material is 0.54. 2. The aggregate consists of fine aggregate, medium aggregate, and coarse aggregate. Based on the total mass of the aggregate, fine aggregate accounts for 30%, and medium and coarse aggregate each account for 35%. 3. The water-reducing agent is an external admixture, with the admixture dosage based on the total mass of the cementitious materials at 3%. 4. Converter steel slag and combined process red mud are used as high Ca / Mg auxiliary materials, with a mass ratio of 6:4; this compound auxiliary material is an external admixture, and the external admixture basis is the total mass of the cementitious materials and aggregate matrix, with an external admixture amount of 20%; All the above raw materials were put into the reactor and mixed. The temperature inside the reactor was set to 25°C and the pressure was set to 0 MPa. The stirring speed of the stirring paddle inside the reactor was adjusted to 500 rpm and stirred for 10 minutes. After mixing evenly, a solid carbon filling base slurry was obtained. The overall mass concentration of the slurry was controlled to be 79%.
[0042] S2, with the addition of a small amount of sodium carbonate and triethanolamine Sodium carbonate and triethanolamine were added to the obtained slurry. The amount of sodium carbonate added was 3% of the total mass of converter steel slag and combined process red mud, and the amount of triethanolamine added was 0.02 mol / L solution, which was 0.03% of the total mass of cementitious materials. The moisture content of the system was adjusted by adding an appropriate amount of water to ensure that the mass concentration of the modified slurry remained at 79%. The above materials were poured into a reactor, the temperature of which was set to 25℃ and the pressure to 0 MPa. The stirring speed of the agitator in the reactor was adjusted to 500 rpm, and the mixture was stirred for 10 minutes.
[0043] S3, Introduce CO2 CO2 was introduced into the reactor at a carbon injection pressure of 2 MPa, the reactor pressure was 1 MPa, the stirring speed was 700 rpm, the reaction temperature was 30℃, and the reaction time was 30 min to obtain a carbon-fixed filling slurry. During the stirring process, the maximum carbon fixation amount of the material was measured to be 69.14 kg CO2 / t and the mineralization rate was 0.47 kg CO2 / (t·min).
[0044] S4, Casting Specimens The obtained carbon-fixed filling slurry is injected into a molding mold, and after being vibrated or allowed to stand to release air, it is molded to obtain a carbon-fixed filling material specimen.
[0045] S5, Demolding and Curing The obtained carbon-fixed filling material specimens were demolded and placed in a standard curing chamber for 28 days to obtain the enhanced carbon-fixed filling material. The compressive strength of the cured material was 13.35 MPa.
[0046] Example 2 was prepared using the same method as Example 1, except that the amount of sodium carbonate and the concentration and amount of triethanolamine were different. Example 3
[0047] A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization includes the following steps: S1, Raw material mixing 1. The cementitious material is composed of fly ash and cement. Based on the total mass of the cementitious material, the fly ash content is 80% and the cement content is 20%; the water-cement ratio of the cementitious material is 0.54. 2. The aggregate consists of fine aggregate, medium aggregate, and coarse aggregate. Based on the total mass of the aggregate, fine aggregate accounts for 30%, and medium and coarse aggregate each account for 35%. 3. The water-reducing agent is an external admixture, with the admixture dosage based on the total mass of the cementitious materials at 3%. 4. Converter steel slag and combined process red mud are used as high Ca / Mg auxiliary materials, with a mass ratio of 6:4; this compound auxiliary material is an external admixture, and the external admixture basis is the total mass of the cementitious materials and aggregate matrix, with an external admixture amount of 20%; All the above raw materials were put into the reactor and mixed. The temperature inside the reactor was set to 25°C and the pressure was set to 0 MPa. The stirring speed of the stirring paddle inside the reactor was adjusted to 500 rpm and stirred for 10 minutes. After mixing evenly, a solid carbon filling base slurry was obtained. The overall mass concentration of the slurry was controlled to be 79%.
[0048] S2, incorporating sodium carbonate and triethanolamine Sodium carbonate and triethanolamine were added to the obtained slurry. The amount of sodium carbonate added was 5% of the total mass of converter steel slag and combined process red mud, and the amount of triethanolamine added was 0.01 mol / L solution, which was 0.05% of the total mass of cementitious materials. The water content of the system was adjusted by adding an appropriate amount of clean water to ensure that the mass concentration of the modified slurry remained at 79%.
[0049] Pour the above materials into the reactor. Set the temperature inside the reactor to 25℃ and the pressure to 0MPa. Adjust the stirring speed of the stirring paddle inside the reactor to 500rpm and stir for 10min.
[0050] S3, Introduce CO2 CO2 was introduced into the reactor at a carbon injection pressure of 2 MPa, the reactor pressure was 1 MPa, the stirring speed was 700 rpm, the reaction temperature was 30℃, and the reaction time was 30 min to obtain a carbon-fixed filling slurry. During the stirring process, the maximum carbon fixation amount of the material was measured to be 67.88 kg CO2 / t and the mineralization rate was 0.48 kg CO2 / (t·min).
[0051] S4, Casting Specimens The obtained carbon-fixed filling slurry is injected into a molding mold, and after being vibrated or allowed to stand to release air, it is molded to obtain a carbon-fixed filling material specimen.
[0052] S5, Demolding and Curing The obtained carbon-fixed filling material specimens were demolded and placed in a standard curing chamber for 28 days to obtain the enhanced carbon-fixed filling material. The compressive strength of the cured material was 13.09 MPa.
[0053] Example 3 was prepared using the same method as Example 1, except that the amount of sodium carbonate and the concentration and amount of triethanolamine were different. Example 4
[0054] A method for preparing carbon-fixing filler materials by triethanolamine-enhanced sodium carbonate cyclic mineralization includes the following steps: S1, Raw material mixing 1. Precursors: The mass ratio of coal gangue, blast furnace slag, and fly ash is 4:5:1; 2. Water glass is an external additive component, with the external additive base being the total mass of the precursor, and the external additive amount being 10%. 3. Calcium carbide slag is an external admixture component, with the admixture standard being the total mass of the precursor and the admixture amount being 5%; 4. Converter steel slag and combined process red mud are used as high Ca / Mg auxiliary materials, with a mass ratio of 8:2; the total mass of the precursor is used as the external addition basis, and the external addition amount is 25%; the unified water-cement ratio of the system is set at 0.6 mL / g.
[0055] Weigh all raw materials according to the above ratio and put them into the reaction vessel. Set the reaction vessel temperature to 25℃, the pressure inside the vessel to 0MPa, and the stirring speed to 500rpm. Stir continuously for 10 minutes. After mixing evenly, a carbon-fixed filling base slurry is obtained. The overall mass concentration of the slurry is controlled to be 79%.
[0056] S2, Modification and regulation by adding sodium carbonate and triethanolamine The base slurry prepared by S1 was mixed with modifying and enhancing components sodium carbonate and triethanolamine. The amount of sodium carbonate added was 5% of the total mass of converter steel slag and combined process red mud, and the amount of triethanolamine added was 0.05 mol / L solution, at 0.03% of the total mass of the precursors. The moisture content of the system was adjusted by adding an appropriate amount of water to ensure that the mass concentration of the modified slurry remained at 79%.
[0057] The modified slurry was transferred into a reactor and stirred for 10 minutes at 25°C, 0 MPa, and 500 rpm to ensure that the modified components were uniformly combined with the base slurry.
[0058] S3, Atmospheric-Pressure Coupled CO2 Mineralization Reaction After the modification and stirring were completed, the process parameters of the reactor were adjusted: reaction temperature 25℃, stirring speed 800rpm, CO2 gas was introduced into the reactor, carbon injection pressure was controlled at 1.5MPa, the reaction pressure inside the reactor was stabilized at 1.2MPa, and the mineralization reaction was carried out under constant temperature and pressure for 30min to obtain a carbon-fixed filling slurry synergistically enhanced by triethanolamine-sodium carbonate.
[0059] The mineralization reaction process was characterized by real-time testing. The maximum total carbon sequestration of the modified system was 69.82 kg CO2 / t, and the mineralization reaction rate was 0.46 kg CO2 / (t·min).
[0060] S4, Specimen casting The carbon-fixing filler slurry, which has undergone S3 mineralization reaction, is rapidly injected into a molding mold. The air bubbles inside the slurry are eliminated by vibration and static venting. The slurry is then leveled and molded to obtain a preliminary specimen of the modified mineralized carbon-fixing filler material.
[0061] S5, standard maintenance yields finished materials. After the specimens were allowed to set initially, they were demolded and placed in a standard curing chamber for constant temperature and humidity curing for 28 days. The final product was a triethanolamine-enhanced sodium carbonate circulating mineralization-enhanced carbon-fixing filling material. After curing, the uniaxial compressive strength of the specimens reached 14.76 MPa.
[0062] The raw materials and proportions of the coal-based solid waste cemented backfill in Example 4 are different from those in Example 1. The dosage of high Ca / Mg content auxiliary materials is different. The dosage of sodium carbonate and the concentration and dosage of triethanolamine are also different. The carbon injection pressure, the pressure inside the reactor, the reaction temperature and the speed of the agitator are also different.
[0063] Comparative Example 1 S1, Raw material mixing 1. The cementitious material is composed of fly ash and cement. Based on the total mass of the cementitious material, the fly ash content is 80% and the cement content is 20%; the water-cement ratio of the cementitious material is 0.54. 2. The aggregate consists of fine aggregate, medium aggregate, and coarse aggregate. Based on the total mass of the aggregate, fine aggregate accounts for 30%, and medium and coarse aggregate each account for 35%. 3. The water-reducing agent is an external admixture, with the admixture dosage based on the total mass of the cementitious materials at 3%. 4. Converter steel slag and combined process red mud are used as high Ca / Mg auxiliary materials with a mass ratio of 6:4. This compound auxiliary material is an external admixture, and the external admixture basis is the total mass of the matrix of cementitious materials and aggregates, with an external admixture amount of 20%.
[0064] All the above raw materials were put into the reactor and mixed. The temperature inside the reactor was set to 25°C and the pressure was set to 0 MPa. The stirring speed of the stirring paddle inside the reactor was adjusted to 500 rpm and stirred for 10 minutes. After mixing evenly, a solid carbon filling base slurry was obtained. The overall mass concentration of the slurry was controlled to be 79%.
[0065] S2. Prepare unmineralized blank control specimens and determine background performance. The uniform base slurry obtained in S1 was directly injected into the molding mold, compacted, allowed to stand and degas, and then molded at room temperature to obtain an unmineralized blank control specimen. This control group did not add sodium carbonate or triethanolamine, nor did it introduce external CO2. It was molded and naturally cured only in air at room temperature and pressure, and was used to deduct the background carbon fixation value caused by the original carbonates of the raw materials and natural carbonization in the air.
[0066] After 28 days of standard curing, the following results were obtained: the background carbon fixation of the unmineralized control specimen was 24.27 kg CO2 / t, the natural mineralization rate was 0.33 kg CO2 / (t·min), and the uniaxial compressive strength after 28 days was 12.0 MPa.
[0067] Experimental Example 1 The carbon fixation amount of Examples 1-4 was determined using a thermogravimetric analyzer. Multiple parallel samples were designed, and the reaction was terminated at different time points (e.g., 5 min, 10 min, 15 min, 25 min, and 30 min) during the mineralization reaction. The carbon fixation amount at each time point was measured, and carbon fixation amount-time curves were plotted to calculate the mineralization rate. Each group of samples was tested three times, and the average value was taken.
[0068] Cubic specimens of carbon-fixed filling material were prepared and cured in a standard curing room at 20±2℃ and 90±5% humidity for 24 hours before demolding. They were then cured under the same conditions for another 28 days. After reaching the specified curing age, the specimens were placed vertically at the center of the central base of the press. Initially, manual loading was used to ensure the pressure surface of the press was in parallel contact with the specimen surface, guaranteeing stable contact. Then, the process was switched to computer-controlled displacement loading mode, where pressure was applied at a rate of 0.1 kN / s until failure, and the loading data were recorded. Three specimens were tested at each curing age, and the average value was taken.
[0069] 1. Real-time testing and characterization of the mineralization reaction process: The maximum total carbon fixation in Example 1 was 68.08 kg CO2 / t, and the mineralization reaction rate was 0.46 kg CO2 / (t·min); after curing, the uniaxial compressive strength of the specimen reached 13.11 MPa.
[0070] 2. Real-time testing and characterization of the mineralization reaction process: The maximum total carbon fixation in Example 2 was 69.14 kg CO2 / t, and the mineralization reaction rate was 0.47 kg CO2 / (t·min); after curing, the uniaxial compressive strength of the specimen reached 13.35 MPa.
[0071] 3. Real-time testing and characterization of the mineralization reaction process: The maximum total carbon fixation in Example 3 was 67.88 kg CO2 / t, and the mineralization reaction rate was 0.48 kg CO2 / (t·min); after curing, the uniaxial compressive strength of the specimen reached 13.09 MPa.
[0072] 4. Real-time testing and characterization of the mineralization reaction process: The maximum total carbon fixation in Example 4 was 69.82 kg CO2 / t, and the mineralization reaction rate was 0.46 kg CO2 / (t·min); after curing, the uniaxial compressive strength of the specimen reached 14.76 MPa.
[0073] 5. The carbon fixation amount of the unmineralized control specimen was 24.27 kg CO2 / t, the natural mineralization rate was 0.33 kg CO2 / (t·min), and the 28-day uniaxial compressive strength was 12.0 MPa.
[0074] Example test results show that sodium carbonate continuously removes Ca from the solution by rapidly precipitating calcium carbonate. 2+ This process disrupts the thermodynamic equilibrium of calcium silicate dissolution, creating a strong driving force that continuously promotes the dissolution of the calcium silicate phase in steel slag and red mud, thus completely overcoming the kinetic bottleneck of traditional mineralization. Example test results show that triethanolamine, as a weakly basic organic amine, can accept H+ released during the CO2 hydrolysis and dissociation process. + Promotes the conversion of CO2 to HCO3 - / CO3 2- Conversion; simultaneously, its chelation effect can promote the dissolution of calcium-containing phases in solid waste, increasing the Ca content in the system. 2+ The concentration of CaCO3 is increased, thereby accelerating the formation of CaCO3 precipitate and ultimately improving the mineralization rate of the carbon-fixed filling material.
[0075] The results of the case tests show that sodium carbonate and triethanolamine played an important role in the subsequent curing stage. Compared with the unmineralized control specimen, the compressive strength was improved, and the phenomenon of early reaction inhibition was alleviated.
[0076] The test results show that the carbon fixation amount of the carbon-fixing filling material based on triethanolamine-enhanced sodium carbonate cyclic mineralization in Example 2 of this invention is 69.14 kg CO2 / t, the mineralization rate is 0.47 kg CO2 / (t·min), and the uniaxial compressive strength is 13.35 MPa after a curing period of 28 days. Both the carbon fixation performance and mechanical properties have good application potential.
[0077] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization, characterized in that, Includes the following steps: S1. Mixing raw materials: Steel slag, red mud and coal-based solid waste cementitious filling material are placed in a reaction vessel, water is added and stirred to make the solid particles uniformly dispersed in the liquid phase to obtain the initial filling slurry; S2. Adding sodium carbonate and triethanolamine: Add sodium carbonate and triethanolamine to the obtained initial filling slurry, and continue stirring until the two are evenly dispersed in the initial filling slurry to form a filling slurry to be carbonized containing sodium carbonate and triethanolamine; the amount of sodium carbonate is 2-5% of the total mass of steel slag and red mud; the amount of triethanolamine is 0.02-0.05% of the total mass of cementitious materials; S3. Introduce CO2: Introduce CO2 gas into the obtained carbonized filling slurry to obtain solid carbonized filling slurry; S4. Cast the specimen, demold and cure to obtain the carbon-fixed filling material.
2. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, The carbon injection pressure during CO2 introduction is 0.5~2.5 MPa.
3. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, In step S1, stir for 5-10 minutes, then add water and continue stirring for 5-10 minutes to ensure that the solid particles are uniformly dispersed in the liquid phase.
4. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, In step S2, continue stirring for 5-10 minutes until the two are evenly dispersed in the filling slurry.
5. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, In step S3, during the introduction of CO2, the mixture is stirred at a speed of 300-1000 rpm for 20-30 minutes to carry out the reaction.
6. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 5, characterized in that, In step S3, the pressure inside the reactor is 1.0~1.5MPa, and the reaction temperature is 25~65℃.
7. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, The steel slag is one of the following: converter steel slag, open-hearth steel slag, and electric furnace steel slag.
8. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, The red mud is one of the following: Bayer process red mud, sintering process red mud, and combined process red mud.
9. The method for preparing carbon-fixing filling materials by triethanolamine-enhanced sodium carbonate cyclic mineralization according to claim 1, characterized in that, The mass ratio of steel slag to red mud is 9~4:1~6.
Citation Information
Patent Citations