A low-alkali expanded recycled aggregate block and its preparation method
By combining low-alkali cementitious components, modified recycled aggregates, and flame-retardant and smoke-suppressing fillers, along with carbon dioxide pre-carbonization and copolymer coating treatment, the problems of water absorption, interfacial bonding, low expansion stability, and flame retardancy and smoke suppression in recycled aggregate blocks are solved, and the performance is maintained after high temperature.
Patent Information
- Application Number
- CN202611273717.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have failed to effectively address the challenges of balancing water absorption control, interfacial bonding, low expansion stability, flame retardancy and smoke suppression, and performance retention at high temperatures in recycled aggregate blocks.
The combination of low-alkali cementitious components, modified recycled aggregates, flame-retardant and smoke-suppressing fillers, and chopped basalt fibers, along with carbon dioxide pre-carbonization treatment and coating treatment with phosphorus-nitrogen-silicon-carboxylate copolymers, combined with a semi-dry vibration compression molding process, creates a synergistic effect.
It improves the water absorption, interfacial bonding stability, flame retardant and smoke suppression effects, and structural integrity after high temperature of recycled aggregate blocks, thereby enhancing the resource utilization level of construction waste concrete.
Smart Images

Figure CN123106147A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building wall materials technology, specifically to a low-alkali expanded recycled aggregate block and its preparation method. Background Technology
[0002] Construction waste concrete, after being crushed, screened, and washed, can be used as recycled aggregate in concrete, mortar, or block products. Recycled aggregate typically contains a certain amount of attached old mortar, which may affect water absorption, interfacial bonding, and the volume stability of subsequent cement-based products. For recycled aggregate blocks, it is also necessary to consider semi-dry vibration molding, pore wall compaction, low expansion risk control, and flame-retardant and smoke-suppressing properties under fire conditions.
[0003] Chinese invention patent application CN121627329A describes a method for graded and sieved recycled aggregates, preparing a bissilane-modified solution of γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane, and using a graded pre-wetting-spraying composite modification method to treat the recycled aggregates. The recycled aggregate concrete is then prepared by combining it with a ternary composite admixture of slag powder, fly ash, and nano-silica. This method mainly focuses on the synergistic improvement of the performance of recycled aggregate concrete through bissilane coupling and mineral admixtures.
[0004] Chinese invention patent application CN120081610B describes a method for obtaining pretreated recycled aggregate by crushing, screening, and washing waste concrete. Nano-silica is then added to a modified acrylic emulsion to form a composite emulsion. The composite emulsion is mixed with the pretreated recycled aggregate and dried to obtain environmentally friendly recycled aggregate based on construction waste. This method primarily utilizes polymer emulsion film formation and nano-silica filling to improve aggregate porosity and water absorption.
[0005] Chinese invention patent application CN108793797A describes carbonizing recycled aggregate in a carbon dioxide atmosphere to obtain carbonized recycled aggregate for inhibiting alkali-aggregate reaction. Chinese invention patent application CN102321274B discloses obtaining a hydrotalcite-ammonium polyphosphate halogen-free flame retardant through anion exchange with ammonium polyphosphate using hydrotalcite as a raw material. The above technologies relate to the carbonization treatment of recycled aggregate and the preparation of ammonium polyphosphate-hydrotalcite flame retardants, respectively, but do not provide an overall design for the combination of the low-alkali cementitious system in semi-dry vibratory-pressed recycled aggregate blocks, the multifunctional group coating on the surface of recycled aggregate, the compatibility of flame-retardant fillers, and the gentle carbon dioxide curing process.
[0006] Therefore, it is still necessary to provide a recycled aggregate block suitable for block production lines and its preparation method, so as to achieve synergy between recycled aggregate surface pretreatment, low-alkali cementitious system, flame-retardant and smoke-suppressing filler and semi-dry vibration pressing process, thereby improving the overall performance of recycled aggregate blocks. Summary of the Invention
[0007] The purpose of this invention is to provide a low-alkali expansion recycled aggregate block and its preparation method, so as to improve the problem of recycling aggregate blocks being difficult to balance in terms of water absorption control, interfacial bonding, low expansion stability, flame retardancy and smoke suppression, and performance retention after high temperature.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a low-alkali expanded recycled aggregate block, which, by weight, comprises the following raw materials: 100 parts of low-alkali cementitious component, 260-420 parts of modified recycled aggregate, 3-10 parts of flame-retardant and smoke-suppressing filler, 0.2-1.2 parts of chopped basalt fiber, 0.2-1.0 parts of low-alkali polycarboxylate superplasticizer, and 25-38 parts of water; The low-alkali cementitious components include low-alkali cement, granulated blast furnace slag powder, fly ash, and silica fume and / or metakaolin. The modified recycled aggregate is a surface-modified aggregate formed by sequentially subjecting recycled aggregate to carbon dioxide pre-carbonization treatment and phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion coating treatment. The phosphorus-nitrogen-silicon-carboxylate copolymer contains repeating units derived from phosphate ester unsaturated monomers, carboxylic acid unsaturated monomers, amide unsaturated monomers, and hydrolyzable silane unsaturated monomers.
[0009] Furthermore, the low-alkali cementitious component comprises the following components in parts by weight: 45-65 parts of low-alkali silicate cement or low-alkali sulfoaluminate cement, 15-30 parts of S95 grade granulated blast furnace slag powder, 10-25 parts of Class II F fly ash, 2-8 parts of silica fume and / or metakaolin, and 0-5 parts of anhydrite; the total alkali content of the low-alkali cement, calculated as Na2Oeq, is not greater than 0.60%.
[0010] Furthermore, the recycled aggregate includes recycled fine aggregate and recycled coarse aggregate, wherein the particle size of the recycled fine aggregate is 0.15~4.75mm, the particle size of the recycled coarse aggregate is 5~15mm, and the mass ratio of the recycled fine aggregate to the recycled coarse aggregate is 1:(1.2~2.2).
[0011] Furthermore, the phosphate ester unsaturated monomer is at least one of 2-methacryloyloxyethyl phosphate, vinylphosphonic acid, or methacryloyloxyethyl phosphate; the carboxylic acid unsaturated monomer is acrylic acid and / or methacrylic acid; the amide unsaturated monomer is acrylamide and / or N-hydroxymethylacrylamide; and the hydrolyzable silane unsaturated monomer is γ-methacryloyloxypropyltrimethoxysilane and / or vinyltrimethoxysilane.
[0012] Furthermore, the phosphorus-nitrogen-silica-carboxylate copolymer aqueous dispersion is prepared from the following raw materials in parts by weight: 12-25 parts of 2-methacryloyloxyethyl phosphate, 5-12 parts of acrylic acid, 3-8 parts of acrylamide, 4-12 parts of γ-methacryloyloxypropyltrimethoxysilane, 1-4 parts of vinyltrimethoxysilane, 0.05-0.30 parts of ammonium persulfate, 60-90 parts of water, and 5-25 parts of ethanol; wherein the acrylic acid is partially neutralized with ammonia to make the pH of the system before polymerization 5.5-7.0; the dry basis weight of the coating layer formed by the phosphorus-nitrogen-silica-carboxylate copolymer on the surface of the recycled aggregate is 0.18-0.30% of the weight of the recycled aggregate.
[0013] Furthermore, the flame-retardant and smoke-suppressing filler is a 3-aminopropyltriethoxysilane-grafted ammonium polyphosphate intercalated Mg-Al layered bimetallic hydroxide, or a 3-aminopropyltriethoxysilane-grafted ammonium polyphosphate intercalated Mg-Al-Fe layered bimetallic hydroxide; the mass ratio of the layered bimetallic hydroxide, ammonium polyphosphate, and 3-aminopropyltriethoxysilane is 1:(0.6~1.8):(0.03~0.12).
[0014] Furthermore, the chopped basalt fibers have a length of 3-12 mm and a diameter of 8-20 μm; the low-alkali polycarboxylate superplasticizer is a polyether-type high-performance polycarboxylate superplasticizer; the blocks are hollow blocks with a hollowness of 25-45% and a pore wall thickness of 20-45 mm.
[0015] This invention also provides a method for preparing the above-mentioned low-alkali expanded recycled aggregate blocks, comprising the following steps: S1. Disperse the layered bimetallic hydroxide in a mixture of water and ethanol, add ammonium polyphosphate and adjust the pH to 4.0~6.0, stir at 60~80℃ for 2~6h, filter, wash and dry, and then react with 3-aminopropyltriethoxysilane to obtain flame retardant and smoke suppressant filler. S2. After removing impurities, crushing, screening and washing the construction waste concrete, recycled aggregate is obtained. S3. The recycled aggregate is placed in a carbon dioxide atmosphere for pre-carbonization treatment to obtain pre-carbonized recycled aggregate; S4. Phosphate ester unsaturated monomer, carboxylic acid unsaturated monomer, amide unsaturated monomer, hydrolyzable silane unsaturated monomer, initiator, water and ethanol are mixed and subjected to free radical copolymerization to obtain an aqueous dispersion of phosphorus nitrogen silicon-carboxylate copolymer. S5. Spray the phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion onto the surface of the pre-carbonized recycled aggregate and dry and cure it to obtain modified recycled aggregate; S6. The low-alkali cementitious component, the flame-retardant and smoke-suppressing filler and the short-cut basalt fiber are dry-mixed to obtain the first dry mix; the modified recycled aggregate is added to the first dry mix for secondary dry mixing, and then the low-alkali polycarboxylate superplasticizer and water are added for wet mixing to obtain the semi-dry block material. S7. The semi-dry block material is vibrated and pressed into shape, and after demolding, it is subjected to carbon dioxide mild curing and wet curing in sequence to obtain the low-alkali expansion recycled aggregate block.
[0016] Furthermore, in S3, the carbon dioxide volume fraction of the carbon dioxide-containing atmosphere is 5-30%, the relative humidity is 55-85%, the temperature is 20-45℃, and the pre-carbonization treatment time is 30-180 min; in S4, the free radical copolymerization temperature is 60-75℃, the reaction time is 1-3 h, and the solid content of the aqueous dispersion obtained after polymerization is 8-20%; in S5, the spraying amount of the phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion is 0.8-2.5% of the mass of the pre-carbonized recycled aggregate, and the drying and curing temperature is 50-80℃, and the time is 20-90 min.
[0017] Furthermore, in S6, the dry mixing time is 60-180s, the secondary dry mixing time is 60-120s, and the wet mixing time is 90-240s; during wet mixing, the first portion of water containing a low-alkali polycarboxylate superplasticizer is added first, followed by the remaining water, so that the moisture content of the semi-dry block material is 7-12%; in S7, the vibration molding pressure is 8-16MPa, and the vibration time is 20-60s; the carbon dioxide volume fraction for the mild carbon dioxide curing is 5-20%, the curing temperature is 20-45℃, the relative humidity is 60-90%, and the curing time is 1-6h; the relative humidity for the wet curing is not less than 90%, and the curing time is 3-28d.
[0018] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention, through continuous processing of carbon dioxide pre-carbonization and quaternary copolymer coating, helps to reduce water absorption of recycled aggregate and improve the interfacial bonding between the old mortar adhesion area and the new cementitious matrix; through the synergistic effect of phosphate esters, carboxylates, amides and hydrolyzable silane groups, it helps to improve the interfacial stability and water intrusion resistance of the coating layer; through the synergy of low-alkali cementitious system and modified recycled aggregate, it helps to reduce the risk of harmful expansion of recycled aggregate blocks.
[0019] 2. This invention utilizes aminosilane-grafted ammonium polyphosphate intercalated layered bimetallic hydroxides, which improves the flame-retardant and smoke-suppressing properties of the blocks while maintaining structural integrity at high temperatures. Through short-cut basalt fibers and a semi-dry vibration-pressing process, this invention enhances the crack resistance of the block's pore walls and its molding stability. This invention also improves the resource utilization level of construction waste concrete and is suitable for use in blocks for non-load-bearing interior partitions and fire-resistant partitions in buildings. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is a schematic diagram of the preparation process of a low-alkali expanded recycled aggregate block according to the present invention.
[0022] Figure 2 This is a schematic diagram of the structure of the modified recycled aggregate of the present invention. Detailed Implementation
[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] See Figure 1 As shown, in the preparation process of the low-alkali expansion recycled aggregate blocks of the present invention, waste construction concrete is subjected to impurity removal, crushing, screening, and washing to obtain recycled aggregate; the recycled aggregate is first subjected to carbon dioxide pre-carbonization treatment, and then coated with a phosphorus-nitrogen-silica-carboxylate copolymer aqueous dispersion to obtain modified recycled aggregate; subsequently, low-alkali cementitious components, flame-retardant and smoke-suppressing fillers, chopped basalt fibers, modified recycled aggregate, water-reducing agent, and water are mixed in sequence, and then subjected to vibration compression molding, mild carbon dioxide curing, and wet curing to obtain low-alkali expansion recycled aggregate blocks. This process reflects the process logic of first stabilizing the recycled aggregate interface and then performing semi-dry vibration compression molding.
[0025] See Figure 2 As shown, the modified recycled aggregate includes a recycled aggregate core, an old mortar attachment zone, a pre-carbonized zone, and a copolymer coating layer. The pre-carbonized zone is used to reduce the porosity of the old mortar; the copolymer coating layer is used to reduce water absorption and enhance the interfacial interaction between the recycled aggregate and the cementitious matrix.
[0026] Specifically, the low-alkali silicate cement used is grade 42.5 low-alkali silicate cement with Na2Oeq not exceeding 0.60%; the low-alkali sulfoaluminate cement used is grade 42.5 low-alkali sulfoaluminate cement; the granulated blast furnace slag powder used is grade S95 granulated blast furnace slag powder; the fly ash used is grade II F fly ash; the silica fume used is industrial silica fume with a silica content of not less than 90%; the metakaolin used is calcined metakaolin with an average particle size of 2~6μm; and the anhydrite used is industrial anhydrite powder with an anhydrous calcium sulfate content of not less than 80%.
[0027] Recycled fine aggregate is obtained from construction waste concrete after impurity removal, crushing, screening and washing, with a particle size of 0.15~4.75mm, and raw material acceptance is carried out in accordance with GB / T 25176-2010; recycled coarse aggregate is obtained from construction waste concrete after impurity removal, crushing, screening and washing, with a particle size of 5~15mm, and raw material acceptance is carried out in accordance with GB / T 25177-2010; in the embodiment, the construction waste concrete is preferably derived from the crushed material of C30~C50 ordinary concrete components, and impurities such as wood chips, plastics, asphalt, bricks, steel bars and soil are removed.
[0028] The layered bimetallic hydroxide is industrial-grade Mg-Al hydrotalcite with a Mg / Al molar ratio of 2.0-2.5 and a D50 particle size of 2-5 μm; the ammonium polyphosphate is type II ammonium polyphosphate with a degree of polymerization of not less than 1000; the aminosilane is 3-aminopropyltriethoxysilane; the monomers of the phosphorus-nitrogen-silicon-carboxylate copolymer are 2-methacryloyloxyethyl phosphate, acrylic acid, acrylamide, γ-methacryloyloxypropyltrimethoxysilane, and vinyltrimethoxysilane; the initiator is ammonium persulfate; the pH adjuster is 25% ammonia water; and the solvents are deionized water and anhydrous ethanol.
[0029] The chopped basalt fibers are 6mm or 9mm in length and 13~15μm in diameter; the low-alkali polycarboxylate superplasticizer uses polyether-type polycarboxylate high-performance superplasticizer mother liquor with a solid content of about 40% and Na2Oeq not greater than 0.5%; tap water or deionized water is used.
[0030] Example 1: The preparation process of low-alkali expanded recycled aggregate blocks in this embodiment includes the following steps: First, prepare the flame-retardant and smoke-suppressing filler: Add 100 parts by weight of industrial-grade Mg-Al hydrotalcite to a mixture of 500 parts by weight of water and 500 parts by weight of ethanol, and stir for 30 min; add 120 parts by weight of type II ammonium polyphosphate, adjust the pH to 5.0 with 1 mol / L phosphoric acid solution, and stir at 70℃ for 4 h; after filtration, wash with water and ethanol until the filtrate is close to neutral, and dry at 70℃ for 8 h; disperse the obtained powder in ethanol, add 6 parts by weight of 3-aminopropyltriethoxysilane, react at 60℃ for 2 h, filter and dry at 70℃ to obtain aminosilane-grafted ammonium polyphosphate intercalated Mg-Al layered bimetallic hydroxide flame-retardant and smoke-suppressing filler.
[0031] Waste construction concrete is subjected to impurity removal, jaw crushing, impact crushing, magnetic separation, screening, and washing to obtain recycled fine aggregate with a particle size of 0.15~4.75mm and recycled coarse aggregate with a particle size of 5~15mm. The recycled fine aggregate and recycled coarse aggregate are blended at a mass ratio of 1:1.7 to obtain recycled aggregate.
[0032] The recycled aggregate was placed in a carbonization chamber and treated for 90 minutes under conditions of 15% carbon dioxide volume fraction, 70% relative humidity, and 30°C to obtain pre-carbonized recycled aggregate.
[0033] Preparation of an aqueous dispersion of a phosphorus-nitrogen-silicon-carboxylate copolymer: 18 parts by mass of 2-methacryloyloxyethyl phosphate, 8 parts by mass of acrylic acid, 5 parts by mass of acrylamide, 8 parts by mass of γ-methacryloyloxypropyltrimethoxysilane, 2 parts by mass of vinyltrimethoxysilane, 15 parts by mass of anhydrous ethanol, and 75 parts by mass of deionized water were added to a reaction vessel, and the pH was adjusted to 6.2 with 25% ammonia water; the temperature was raised to 65°C, 0.15 parts by mass of ammonium persulfate were added, and the reaction was maintained at this temperature for 2 hours to obtain an aqueous dispersion of a phosphorus-nitrogen-silicon-carboxylate copolymer with a solid content of about 12%.
[0034] The pre-carbonized recycled aggregate was placed in a rotating drum, and the above-mentioned aqueous dispersion was uniformly sprayed onto the aggregate surface at a spraying amount of 1.5% of the pre-carbonized recycled aggregate mass. After spraying, it was dried and cured at 65°C for 45 minutes to obtain modified recycled aggregate. The dry basis mass of the resulting coating layer was approximately 0.22% of the recycled aggregate mass.
[0035] Raw materials for preparing blocks: 100 parts by weight of low-alkali cementitious component consists of 55 parts by weight of 42.5 grade low-alkali silicate cement, 22 parts by weight of S95 grade granulated blast furnace slag powder, 18 parts by weight of Class II F fly ash, 4 parts by weight of silica fume, and 1 part by weight of anhydrite; based on 100 parts by weight of low-alkali cementitious component, 340 parts by weight of modified recycled aggregate, 6 parts by weight of flame retardant and smoke suppressant filler, 0.6 parts by weight of 6mm short-cut basalt fiber, 0.6 parts by weight of low-alkali polycarboxylate superplasticizer, and 31 parts by weight of water.
[0036] The low-alkali cementitious components, flame-retardant and smoke-suppressing fillers, and chopped basalt fibers were dry-mixed for 120 seconds to obtain the first dry mix. Modified recycled aggregate was added and dry-mixed for 90 seconds. The low-alkali polycarboxylate superplasticizer was dissolved in the first part of the water and added and wet-mixed for 90 seconds. The remaining water was added and wet-mixed for another 90 seconds to obtain a semi-dry block material with a moisture content of about 9.5%. The semi-dry block material was placed into a 390mm×190mm×190mm double-row hole hollow block mold and vibrated for 40 seconds under a pressure of 12MPa. After demolding, it was gently cured for 3 hours under the conditions of 10% carbon dioxide volume fraction, 30℃ temperature, and 75% relative humidity. Then it was wet-cured for 28 days under the condition of relative humidity not less than 90% to obtain low-alkali expanded recycled aggregate blocks.
[0037] Example 2: The preparation process of low-alkali expanded recycled aggregate blocks in this embodiment includes the following steps: The flame-retardant and smoke-suppressing filler was prepared according to the method of Example 1, but the mass ratio of Mg-Al hydrotalcite, ammonium type II polyphosphate and 3-aminopropyltriethoxysilane was adjusted to 1:1.4:0.07.
[0038] Waste concrete from construction is cleaned, crushed, screened, and washed to obtain recycled fine aggregate and recycled coarse aggregate. The recycled fine aggregate and recycled coarse aggregate are then blended at a mass ratio of 1:1.6 to obtain recycled aggregate.
[0039] The recycled aggregate was placed in a carbonization chamber and treated for 120 minutes under conditions of 20% carbon dioxide volume fraction, 75% relative humidity, and 35°C to obtain pre-carbonized recycled aggregate.
[0040] Preparation of an aqueous dispersion of a phosphorus-nitrogen-silicon-carboxylate copolymer: 22 parts by mass of 2-methacryloyloxyethyl phosphate, 9 parts by mass of acrylic acid, 6 parts by mass of acrylamide, 9 parts by mass of γ-methacryloyloxypropyltrimethoxysilane, 2 parts by mass of vinyltrimethoxysilane, 18 parts by mass of anhydrous ethanol, and 72 parts by mass of deionized water were added to a reaction vessel, and the pH was adjusted to 6.0 with 25% ammonia water; the temperature was raised to 68°C, 0.18 parts by mass of ammonium persulfate were added, and the reaction was maintained at this temperature for 2.5 h to obtain an aqueous dispersion with a solid content of about 15%.
[0041] The above-mentioned aqueous dispersion was sprayed onto the surface of the pre-carbonized recycled aggregate at a dosage of 1.8% of the pre-carbonized recycled aggregate mass, and dried and cured at 70°C for 60 minutes to obtain modified recycled aggregate. The dry basis mass of the resulting coating layer was approximately 0.30% of the recycled aggregate mass.
[0042] The low-alkali cementitious component, with 100 parts by weight, consists of 50 parts by weight of 42.5 grade low-alkali sulfoaluminate cement, 25 parts by weight of S95 grade granulated blast furnace slag powder, 17 parts by weight of Class II F fly ash, 6 parts by weight of metakaolin, and 2 parts by weight of anhydrite; based on 100 parts by weight of the low-alkali cementitious component, it also includes 330 parts by weight of modified recycled aggregate, 7 parts by weight of flame-retardant and smoke-suppressing filler, 0.8 parts by weight of 9mm short-cut basalt fiber, 0.7 parts by weight of low-alkali polycarboxylate superplasticizer, and 30 parts by weight of water.
[0043] Low-alkali cementitious components, flame-retardant and smoke-suppressing fillers, and chopped basalt fibers were dry-mixed for 150 seconds, modified recycled aggregate was added and dry-mixed again for 100 seconds, and then wet-mixed twice with water for a total of 200 seconds to obtain semi-dry block material with a moisture content of about 9.0%. The semi-dry block material was put into a 390mm×190mm×190mm double-row hole hollow block mold and vibrated for 45 seconds under a pressure of 13MPa. After demolding, it was gently cured for 4 hours under the conditions of 12% carbon dioxide volume fraction, 35℃ temperature, and 80% relative humidity, and then wet-cured for 28 days to obtain low-alkali expansion recycled aggregate blocks.
[0044] Example 3: The preparation process of low-alkali expanded recycled aggregate blocks in this embodiment includes the following steps: The flame-retardant and smoke-suppressing filler was prepared according to the method of Example 1, but the mass ratio of Mg-Al hydrotalcite, ammonium type II polyphosphate and 3-aminopropyltriethoxysilane was adjusted to 1:0.6:0.03.
[0045] Waste concrete from construction is cleaned, crushed, screened, and washed to obtain recycled fine aggregate and recycled coarse aggregate. The recycled fine aggregate and recycled coarse aggregate are then blended at a mass ratio of 1:1.2 to obtain recycled aggregate.
[0046] The recycled aggregate was placed in a carbonization box and treated for 30 minutes under the conditions of 5% carbon dioxide volume fraction, 55% relative humidity, and 20℃ to obtain pre-carbonized recycled aggregate.
[0047] Preparation of an aqueous dispersion of a phosphorus-nitrogen-silicon-carboxylate copolymer: 12 parts by mass of 2-methacryloyloxyethyl phosphate, 5 parts by mass of acrylic acid, 3 parts by mass of acrylamide, 4 parts by mass of γ-methacryloyloxypropyltrimethoxysilane, 1 part by mass of vinyltrimethoxysilane, 5 parts by mass of anhydrous ethanol, and 60 parts by mass of deionized water were added to a reaction vessel, and the pH was adjusted to 5.5 with 25% ammonia water. The temperature was raised to 60°C, and 0.05 parts by mass of ammonium persulfate were added. The reaction was maintained at this temperature for 1 hour to obtain an aqueous dispersion with a solid content of about 8%.
[0048] The above-mentioned aqueous dispersion was sprayed onto the surface of the pre-carbonized recycled aggregate at a spraying amount of 0.8% of the mass of the pre-carbonized recycled aggregate, and dried and cured at 50°C for 20 minutes to obtain modified recycled aggregate; the dry basis mass of the resulting coating layer was approximately 0.08% of the mass of the recycled aggregate.
[0049] One hundred parts by weight of the low-alkali cementitious component consists of 65 parts by weight of 42.5 grade low-alkali silicate cement, 15 parts by weight of S95 grade granulated blast furnace slag powder, 15 parts by weight of Class II F fly ash, and 5 parts by weight of silica fume. One hundred parts by weight of the low-alkali cementitious component also includes 260 parts by weight of modified recycled aggregate, 3 parts by weight of flame-retardant and smoke-suppressing filler, 0.2 parts by weight of 6mm chopped basalt fiber, 0.2 parts by weight of low-alkali polycarboxylate superplasticizer, and 25 parts by weight of water.
[0050] Low-alkali cementitious components, flame-retardant and smoke-suppressing fillers, and chopped basalt fibers were dry-mixed for 60 seconds, modified recycled aggregate was added and dry-mixed again for 60 seconds, and then water was added twice and wet-mixed for a total of 90 seconds to obtain semi-dry block material with a moisture content of about 7.0%. The semi-dry block material was put into a 390mm×190mm×190mm double-row hole hollow block mold, vibrated and pressed under 8MPa pressure for 20 seconds, demolded, and gently cured for 1 hour under the conditions of 5% carbon dioxide volume fraction, 20℃ temperature, and 60% relative humidity, and then wet-cured for 28 days to obtain low-alkali expansion recycled aggregate blocks.
[0051] Example 4: The preparation process of low-alkali expanded recycled aggregate blocks in this embodiment includes the following steps: The flame-retardant and smoke-suppressing filler was prepared according to the method of Example 1, but the mass ratio of Mg-Al hydrotalcite, ammonium type II polyphosphate and 3-aminopropyltriethoxysilane was adjusted to 1:1.8:0.12.
[0052] Waste concrete from construction is cleaned, crushed, screened, and washed to obtain recycled fine aggregate and recycled coarse aggregate. The recycled fine aggregate and recycled coarse aggregate are then blended at a mass ratio of 1:2.2 to obtain recycled aggregate.
[0053] The recycled aggregate was placed in a carbonization chamber and treated for 180 minutes under conditions of 30% carbon dioxide volume fraction, 85% relative humidity, and 45℃ to obtain pre-carbonized recycled aggregate.
[0054] Preparation of an aqueous dispersion of a phosphorus-nitrogen-silicon-carboxylate copolymer: 25 parts by mass of 2-methacryloyloxyethyl phosphate, 12 parts by mass of acrylic acid, 8 parts by mass of acrylamide, 12 parts by mass of γ-methacryloyloxypropyltrimethoxysilane, 4 parts by mass of vinyltrimethoxysilane, 25 parts by mass of anhydrous ethanol, and 90 parts by mass of deionized water were added to a reaction vessel, and the pH was adjusted to 7.0 with 25% ammonia water; the temperature was raised to 75°C, 0.30 parts by mass of ammonium persulfate was added, and the reaction was maintained at this temperature for 3 hours to obtain an aqueous dispersion with a solid content of about 20%.
[0055] The above-mentioned aqueous dispersion was sprayed onto the surface of the pre-carbonized recycled aggregate at a spraying amount of 2.5% of the mass of the pre-carbonized recycled aggregate, and dried and cured at 80°C for 90 min to obtain modified recycled aggregate; the dry basis mass of the resulting coating layer was approximately 0.45% of the mass of the recycled aggregate.
[0056] 100 parts by weight of the low-alkali cementitious component consists of 45 parts by weight of 42.5 grade low-alkali silicate cement, 30 parts by weight of S95 grade granulated blast furnace slag powder, 17 parts by weight of Class II F fly ash, and 8 parts by weight of metakaolin. 100 parts by weight of the low-alkali cementitious component also includes 420 parts by weight of modified recycled aggregate, 10 parts by weight of flame-retardant and smoke-suppressing filler, 1.2 parts by weight of 9mm short-cut basalt fiber, 1.0 part by weight of low-alkali polycarboxylate superplasticizer, and 38 parts by weight of water.
[0057] The low-alkali cementitious components, flame-retardant and smoke-suppressing fillers, and chopped basalt fibers were dry-mixed for 180 seconds, then modified recycled aggregate was added and dry-mixed again for 120 seconds. Finally, water was added twice and wet-mixed for a total of 240 seconds to obtain semi-dry block material with a moisture content of about 12.0%. The semi-dry block material was placed into a 390mm×190mm×190mm double-row hole hollow block mold and vibrated under a pressure of 16MPa for 60 seconds. After demolding, it was gently cured for 6 hours under the conditions of 20% carbon dioxide volume fraction, 45℃ temperature, and 90% relative humidity, and then wet-cured for 28 days to obtain low-alkali expansion recycled aggregate blocks.
[0058] Comparative Example 1: This comparative example is an unmodified recycled aggregate comparative example. Except that the recycled aggregate is not subjected to carbon dioxide pre-carbonization treatment, nor is it coated with phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion treatment, but is directly used after impurity removal, crushing, screening and water washing, the other raw material types, dosages, mixing order, vibration compression molding, carbon dioxide mild curing and wet curing conditions are the same as in Example 1.
[0059] Comparative Example 2: This comparative example is a comparative example lacking carbon dioxide precarbonation. Except that the recycled aggregate was not precarbonized with carbon dioxide and was directly coated with the phosphorus-nitrogen-silica-carboxylate copolymer aqueous dispersion of Example 1, all other conditions were the same as in Example 1.
[0060] Comparative Example 3: This comparative example is a comparative example lacking quaternary copolymer coating. Except that the recycled aggregate was only subjected to carbon dioxide pre-carbonization treatment as in Example 1 and was not coated with the phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion, all other conditions were the same as in Example 1.
[0061] Comparative Example 4: This comparative example is a comparative example lacking the phosphate ester monomer. Except that 2-methacryloyloxyethyl phosphate was not added when preparing the copolymer aqueous dispersion, and the solid content was adjusted to be close to that of Example 1 by equal mass of acrylic acid and water, all other conditions were the same as in Example 1.
[0062] Comparative Example 5: This comparative example is a comparative example lacking the amide monomer. Except that acrylamide was not added when preparing the copolymer aqueous dispersion, and the solid content of the system was adjusted to be close to that of Example 1 with an equal mass of deionized water, all other conditions were the same as in Example 1.
[0063] Comparative Example 6: This comparative example is a comparative example lacking flame-retardant and smoke-suppressing filler. Except for the absence of flame-retardant and smoke-suppressing filler, all other conditions are the same as in Example 1.
[0064] Comparative Example 7: This comparative example is a comparative example lacking a low-alkali cementitious system. Except for replacing the low-alkali cementitious component in Example 1 with 100 parts by weight of P·O 42.5 ordinary Portland cement, and omitting the addition of granulated blast furnace slag powder, fly ash, silica fume, and anhydrite, all other conditions are the same as in Example 1.
[0065] Comparative Example 8: This comparative example is a flame-retardant and smoke-suppressing filler without aminosilane grafting. Except for the ammonium polyphosphate intercalated Mg-Al layered bimetallic hydroxide not being grafted with 3-aminopropyltriethoxysilane, all other conditions are the same as in Example 1.
[0066] Comparative Example 9: This comparative example has a lower dry basis weight of the coating layer than the range comparative example. Except for reducing the amount of phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion sprayed so that the dry basis weight of the coating layer is about 0.03% of the weight of the recycled aggregate, all other conditions are the same as in Example 1.
[0067] Comparative Example 10: This comparative example has a higher dry basis weight of the coating layer than the range comparative example. Except for increasing the amount of phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion sprayed so that the dry basis weight of the coating layer is approximately 0.70% of the weight of the recycled aggregate, all other conditions are the same as in Example 1.
[0068] Comparative Example 11: This comparative example is a comparative example of insufficient carbon dioxide pre-carbonization. Except for adjusting the carbon dioxide pre-carbonization conditions to 3% carbon dioxide volume fraction, 50% relative humidity, 20°C, and 15 min treatment, all other conditions are the same as in Example 1.
[0069] Comparative Example 12: This comparative example is a carbon dioxide pre-carbonization over-comparison example. Except for adjusting the carbon dioxide pre-carbonization conditions to 50% carbon dioxide volume fraction, 90% relative humidity, 50°C, and 300 min, all other conditions are the same as in Example 1.
[0070] Comparative Example 13: This comparative example uses a lower-range comparative example with a flame-retardant and smoke-suppressing filler content. Except for adjusting the flame-retardant and smoke-suppressing filler content to 1 part by mass, all other conditions are the same as in Example 1. This comparative example is used to demonstrate the rationality of the lower limit of the flame-retardant and smoke-suppressing filler content.
[0071] Comparative Example 14: This comparative example uses a higher amount of flame-retardant and smoke-suppressing filler than the range comparative example. Except for adjusting the amount of flame-retardant and smoke-suppressing filler to 15 parts by weight, all other conditions are the same as in Example 1.
[0072] Comparative Example 15: This comparative example is for cases with insufficient vibration compression. Except for adjusting the vibration compression molding pressure to 4 MPa and the vibration time to 10 s, all other conditions are the same as in Example 1.
[0073] Test example: The 28-day compressive strength was tested according to GB / T 4111-2013 "Test Methods for Concrete Blocks and Bricks"; the test objects were 390mm×190mm×190mm hollow blocks cured for 28 days; 6 blocks were tested in each group, the compressive strength of each block was recorded, and the average value was calculated; the point values in the performance data table are the average values.
[0074] The 24-hour water absorption rate was determined according to GB / T 4111-2013 "Test Methods for Concrete Blocks and Bricks"; the test objects were block specimens cured to 28 days; 3 blocks were tested in each group. After the specimens were dried to constant weight, they were soaked in water for 24 hours. After being taken out, the surface water was wiped off in a uniform manner, and the water absorption rate was weighed and calculated; the point values in the performance data table are average values.
[0075] The 28-day drying shrinkage was determined according to GB / T 4111-2013 "Test Methods for Concrete Blocks and Bricks"; three specimens were tested in each group, and the drying shrinkage value was recorded; the point values in the performance data table are average values.
[0076] The 14-day rapid alkali-silica reaction expansion rate was determined according to the relevant methods for alkali-silica reaction in GB / T 50082-2024 "Standard for Test Methods of Long-Term Performance and Durability of Concrete". To ensure comparability among groups, mortar rod specimens were prepared using the same cementitious system, modified recycled fine aggregate, and water-cement conditions as the blocks, with 3 specimens per group. 80℃, 1mol / L NaOH solution, and 14 days of age were used as uniform rapid evaluation conditions, and the length change rate was recorded. If the testing institution uses the specific sample size and age nodes specified in the standard, the testing institution's method should prevail, and consistency should be maintained across all groups. The point values in the performance data table are average values.
[0077] The peak heat release rate was determined according to ISO 5660-1:2015; samples were cut from the wall region of the block cavity, with dimensions of 100mm × 100mm × 25mm, and conditioned for 48 hours at 23±2℃ and 50±5% relative humidity before testing; the thermal radiation flux was 50kW / m². 2 Place them horizontally, test for 20 minutes, with 3 pieces per group, and record the peak heat release rate (pHRR); the point values in the performance data table are average values.
[0078] Smoke density was tested according to GB / T 8627-2007 "Test Method for Smoke Density of Building Materials under Combustion or Decomposition"; samples were cut from the wall area of the block hole, with 3 samples per group, and the maximum smoke density Dsmax was recorded; the point values in the performance data table are average values.
[0079] The residual compressive strength retention rate after 600℃ was evaluated using the internally controlled high-temperature mechanical evaluation method. Six solid auxiliary specimens (100mm×100mm×100mm) were prepared simultaneously with the semi-dry material from the same batch of blocks in each group. The compressive strength of three specimens was measured directly at 28 days of age, while the other three specimens were placed in a muffle furnace and heated to 600±10℃ at a rate of 5℃ / min. After holding at this temperature for 2 hours, the specimens were cooled to room temperature with the furnace and then their compressive strength was measured. The residual compressive strength retention rate is the ratio of the average compressive strength after high-temperature treatment to the average compressive strength without high-temperature treatment. The point values in the performance data table are average values.
[0080] The specific test results are shown in the table below: Analysis of experimental results: Example 1 showed a 28-day compressive strength of 12.2 MPa, a 24-hour water absorption rate of 8.5%, a 14-day rapid ASR expansion rate of 0.065%, a 28-day drying shrinkage of 0.48 mm / m, and a pHRR of 39 kW / m. 2 The smoke density Dsmax is 36, and the residual compressive strength retention rate after 600℃ is 69%.
[0081] Example 2 showed a 28-day compressive strength of 13.0 MPa, a 24-hour water absorption rate of 7.8%, a 14-day rapid ASR expansion rate of 0.055%, a 28-day drying shrinkage of 0.42 mm / m, and a pHRR of 34 kW / m. 2 The smoke density Dsmax is 30, and the residual compressive strength retention rate after 600℃ is 72%. Compared with Example 1, Example 2 has a better range in terms of pre-carbonization degree, phosphate ester monomer ratio, dry basis weight of coating layer, and amount of flame retardant and smoke suppressing filler. Therefore, it has better performance in terms of low expansion, water absorption control, flame retardancy and smoke suppression, and high-temperature performance.
[0082] Example 3 showed a 28-day compressive strength of 9.5 MPa, a 24-hour water absorption rate of 10.7%, a 14-day rapid ASR expansion rate of 0.092%, and a pHRR of 52 kW / m³. 2 The smoke density Dsmax was 54, and the residual compressive strength retention rate after 600℃ was 61%. Example 3 still falls within the scope of the claims, but the carbon dioxide pre-carbonization, dry basis quality of the coating layer, amount of flame retardant and smoke-suppressing filler, and vibration and compression conditions are all at the lower limit, so it is generally weaker than Example 1 and Example 2.
[0083] Example 4 showed a 28-day compressive strength of 10.8 MPa, a 24-hour water absorption rate of 8.1%, a 14-day rapid ASR expansion rate of 0.060%, and a pHRR of 35 kW / m³. 2 The smoke density (Dsmax) was 31, and the residual compressive strength retention rate after 600℃ was 67%. Example 4 showed a similar trend in flame retardancy, smoke suppression, and low expansion as Example 2, but its compressive strength and drying shrinkage were lower. This trend indicates that high aggregate content, high coating content, and high filler content are beneficial for flame retardancy, smoke suppression, and low expansion control, but may lead to trade-offs in water demand, interface softening, or compaction.
[0084] Example 1 and Comparative Example 1 were used to verify the necessity of surface modification of recycled aggregate. Comparative Example 1, without carbon dioxide pre-carbonization and quaternary copolymer coating, had a 28-day compressive strength of 7.3 MPa, a 24-hour water absorption rate of 14.6%, a 14-day rapid ASR expansion rate of 0.158%, a 28-day drying shrinkage of 0.74 mm / m, and a residual compressive strength retention rate of 47% after 600℃. Compared with Example 1, Comparative Example 1 was significantly weaker in terms of strength, water absorption, expansion, drying shrinkage, and high-temperature performance, indicating that when recycled aggregate is directly used in blocks, the porosity and weak interface of the old mortar will affect the overall performance of the blocks.
[0085] Example 1 and Comparative Example 2 were used to verify the contribution of carbon dioxide precarbonation. Comparative Example 2, without carbon dioxide precarbonation, had a 28-day compressive strength of 10.7 MPa, a 24-hour water absorption rate of 9.9%, and a 14-day rapid ASR expansion rate of 0.098%. Comparative Example 2 was still superior to Comparative Example 1 due to its quaternary copolymer coating, but its water absorption rate and expansion rate were both higher than those of Example 1. This indicates that carbon dioxide precarbonation is beneficial in first reducing the porosity and alkaline calcium phase fluctuations of the old mortar, and then forming a synergistic effect with the subsequent coating layer.
[0086] Example 1 and Comparative Example 3 were used to verify the contribution of the quaternary copolymer coating layer. Comparative Example 3 underwent only carbon dioxide pre-carbonization, and its 28-day compressive strength was 9.6 MPa, 24-hour water absorption rate was 11.8%, 14-day rapid ASR expansion rate was 0.112%, and 28-day drying shrinkage was 0.64 mm / m. Comparative Example 3 shows that simple carbon dioxide pre-carbonization can bring some improvement, but without the phosphorus-nitrogen-silica-carboxylate copolymer coating layer, water absorption control, interfacial bonding, and volume stability are insufficient.
[0087] Example 1 and Comparative Example 4 were used to verify the contribution of unsaturated monomers in phosphate esters. Comparative Example 4, lacking 2-methacryloyloxyethyl phosphate, exhibited a 14-day rapid ASR (Automatic Stress Reduction) of 0.087%, higher than the 0.065% of Example 1; its 28-day compressive strength was 11.0 MPa, also lower than the 12.2 MPa of Example 1. This trend suggests that phosphate ester monomers are beneficial for enhancing interfacial stability through calcium ion coordination and contribute to controlling the risk of low swelling.
[0088] Example 1 and Comparative Example 5 were used to verify the contribution of the amide unsaturated monomer. Comparative Example 5 lacked acrylamide, and its 28-day drying shrinkage was 0.58 mm / m, higher than that of Example 1 (0.48 mm / m); its residual compressive strength retention after 600°C was 66%, lower than that of Example 1 (69%). This data trend indicates that the amide group has an auxiliary contribution to the toughness of the coating layer, interfacial crack resistance, and structural integrity after high temperature.
[0089] Example 1 and Comparative Example 6 were used to verify the contribution of the flame-retardant and smoke-suppressing filler. Comparative Example 6, without the addition of aminosilane-grafted APP-LDH flame-retardant and smoke-suppressing filler, had a 28-day compressive strength of 12.5 MPa, slightly higher than Example 1, but a pHRR of 68 kW / m². 2 The smoke density Dsmax was 70, and the residual compressive strength retention rate after 600℃ was 54%. This indicates that the main function of flame-retardant and smoke-suppressing filler is not to improve the compressive strength at room temperature, but to reduce heat release and smoke density, and improve strength retention after high temperature.
[0090] Example 1 and Comparative Example 7 were used to verify the contribution of the low-alkali cementitious system. Comparative Example 7 used 100 parts by weight of P·O 42.5 ordinary Portland cement, which had a 28-day compressive strength of 12.8 MPa, but a 14-day rapid ASR expansion rate of 0.122% and a 28-day drying shrinkage of 0.61 mm / m. These data trends suggest that while ordinary Portland cement systems may have higher room-temperature strength, the low-alkali composite cementitious system is more beneficial in reducing the risk of harmful expansion and improving volume stability.
[0091] Example 1 and Comparative Example 8 were used to verify the contribution of aminosilane grafting. Comparative Example 8 used ungrafted aminosilane APP-LDH, which had a 28-day compressive strength of 11.5 MPa and a pHRR of 45 kW / m. 2 The smoke density Dsmax was 44, and the residual compressive strength retention rate after 600℃ was 63%. Compared with Example 1, Comparative Example 8 still had a certain flame retardant and smoke suppression effect, but the strength retention, heat release and smoke density indicators were weaker, indicating that aminosilane grafting helps to improve the dispersibility and interfacial compatibility of APP-LDH in cement-based systems.
[0092] Example 1, along with Comparative Examples 9 and 10, were used to verify the rationality of the dry basis mass range of the coating layer. The dry basis mass of the coating layer in Comparative Example 9 was approximately 0.03%, with a water absorption rate of 11.1% and a 14-day rapid ASR expansion rate of 0.105%, indicating insufficient coating continuity when the coating amount is too low. The dry basis mass of the coating layer in Comparative Example 10 was approximately 0.70%, with a water absorption rate of 7.9% and a 14-day rapid ASR expansion rate of 0.058%. However, its 28-day compressive strength was 10.5 MPa, its 28-day drying shrinkage was 0.67 mm / m, and its smoke density (Dsmax) was 52, indicating that while excessive organic coating is beneficial for reducing water absorption and expansion, it may lead to an overly soft interface, increased drying shrinkage, and increased smoke density. Therefore, controlling the dry basis mass of the coating layer within the range of 0.18% to 0.30% is reasonable.
[0093] Example 1, along with Comparative Examples 11 and 12, were used to verify the rationality of the carbon dioxide pre-carbonation window. Comparative Example 11 showed insufficient pre-carbonation, with a 24-hour water absorption rate of 9.3% and a 14-day rapid ASR expansion rate of 0.097%, indicating that insufficient carbonation resulted in inadequate adjustment of the old mortar porosity and alkaline calcium phase. Comparative Example 12 showed excessive pre-carbonation, with a 24-hour water absorption rate of 8.2% and a 14-day rapid ASR expansion rate of 0.064%, but a 28-day compressive strength of 10.2 MPa and a residual compressive strength retention rate of 62% after 600℃, indicating that excessive carbonation may lead to embrittlement of the aggregate surface or subsequent interfacial bonding fluctuations. Therefore, a carbon dioxide volume fraction of 5–30%, relative humidity of 55–85%, temperature of 20–45℃, and treatment time of 30–180 min is a more reasonable process window.
[0094] Example 1, along with Comparative Examples 13 and 14, were used to verify the rationality of the dosage range of the flame-retardant and smoke-suppressing filler. Comparative Example 13 used 1 part by mass of filler, and its pHRR was 59 kW / m³. 2 The smoke density (Dsmax) was 61, and the residual compressive strength retention rate after 600℃ was 57%, indicating that the filler's contribution to flame retardancy and smoke suppression was insufficient when the filler content was below the specified range. Comparative Example 14 used 15 parts by mass of filler, and its pHRR was 32 kW / m³. 2 The smoke density (Dsmax) is 28, indicating good flame retardancy and smoke suppression performance. However, the 28-day compressive strength drops to 10.1 MPa, and the 24-hour water absorption rate rises to 9.5%, suggesting that excessive filler content increases water demand and weakens compaction and room-temperature mechanical properties. Therefore, a range of 3-10 parts by weight for flame retardant and smoke-suppressing filler is reasonable.
[0095] Example 1 and Comparative Example 15 were used to verify the necessity of semi-dry vibration molding conditions. Comparative Example 15 had a vibration pressure of 4 MPa and a vibration time of 10 s. Its 28-day compressive strength was 7.9 MPa, its 24-hour water absorption rate was 13.2%, its 28-day drying shrinkage was 0.70 mm / m, and its residual compressive strength retention rate after 600°C was 50%. These data trends indicate that the beneficial effects of the present invention not only come from the formulation components but also depend on suitable vibration molding conditions for semi-dry block materials. Insufficient vibration pressure and vibration time result in insufficient compaction of the block pore walls, affecting water absorption, drying shrinkage, and strength retention after high temperatures.
[0096] In summary, carbon dioxide pre-carbonization and quaternary copolymer coating synergistically reduce the risk of water absorption and expansion; phosphate esters, carboxylates, amides, and hydrolyzable silane monomers jointly improve interfacial stability; the low-alkali gelling system reduces the risk of harmful expansion; aminosilane grafted APP-LDH improves flame retardancy, smoke suppression, and high-temperature strength retention; and reasonable coating amount, pre-carbonization window, flame retardant filler dosage, and vibration and compression conditions jointly ensure the comprehensive performance of the blocks.
[0097] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
[0098] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A low-alkali expanded recycled aggregate block, characterized in that, By weight, it includes the following raw materials: 100 parts of low-alkali cementitious component, 260-420 parts of modified recycled aggregate, 3-10 parts of flame retardant and smoke suppressant filler, 0.2-1.2 parts of chopped basalt fiber, 0.2-1.0 parts of low-alkali polycarboxylate superplasticizer, and 25-38 parts of water; The low-alkali cementitious components include low-alkali cement, granulated blast furnace slag powder, fly ash, and silica fume and / or metakaolin. The modified recycled aggregate is a surface-modified aggregate formed by sequentially subjecting recycled aggregate to carbon dioxide pre-carbonization treatment and phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion coating treatment. The phosphorus-nitrogen-silicon-carboxylate copolymer contains repeating units derived from phosphate ester unsaturated monomers, carboxylic acid unsaturated monomers, amide unsaturated monomers, and hydrolyzable silane unsaturated monomers.
2. The low-alkali expanded recycled aggregate block according to claim 1, characterized in that, The low-alkali cementitious component comprises the following components in parts by weight: 45-65 parts of low-alkali silicate cement or low-alkali sulfoaluminate cement, 15-30 parts of S95 grade granulated blast furnace slag powder, 10-25 parts of Class II F fly ash, 2-8 parts of silica fume and / or metakaolin, and 0-5 parts of anhydrite.
3. The low-alkali expanded recycled aggregate block according to claim 1, characterized in that, The recycled aggregate includes recycled fine aggregate and recycled coarse aggregate. The particle size of the recycled fine aggregate is 0.15~4.75mm, the particle size of the recycled coarse aggregate is 5~15mm, and the mass ratio of the recycled fine aggregate to the recycled coarse aggregate is 1:(1.2~2.2).
4. The low-alkali expanded recycled aggregate block according to claim 1, characterized in that, The phosphate ester unsaturated monomer is at least one of 2-methacryloyloxyethyl phosphate, vinylphosphonic acid, or methacryloyloxyethyl phosphate; the carboxylic acid unsaturated monomer is acrylic acid and / or methacrylic acid; the amide unsaturated monomer is acrylamide and / or N-hydroxymethylacrylamide; and the hydrolyzable silane unsaturated monomer is γ-methacryloyloxypropyltrimethoxysilane and / or vinyltrimethoxysilane.
5. A low-alkali expanded recycled aggregate block according to claim 4, characterized in that, The phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion is prepared from the following raw materials in parts by weight: 12-25 parts of 2-methacryloyloxyethyl phosphate, 5-12 parts of acrylic acid, 3-8 parts of acrylamide, 4-12 parts of γ-methacryloyloxypropyltrimethoxysilane, 1-4 parts of vinyltrimethoxysilane, 0.05-0.30 parts of ammonium persulfate, 60-90 parts of water, and 5-25 parts of ethanol; wherein the acrylic acid is partially neutralized with ammonia to make the pH of the system before polymerization 5.5-7.0; the dry basis weight of the coating layer formed by the phosphorus-nitrogen-silicon-carboxylate copolymer on the surface of recycled aggregate is 0.18-0.30% of the weight of recycled aggregate.
6. The low-alkali expanded recycled aggregate block according to claim 1, characterized in that, The flame-retardant and smoke-suppressing filler is a 3-aminopropyltriethoxysilane-grafted ammonium polyphosphate intercalated Mg-Al layered bimetallic hydroxide, or a 3-aminopropyltriethoxysilane-grafted ammonium polyphosphate intercalated Mg-Al-Fe layered bimetallic hydroxide; the mass ratio of the layered bimetallic hydroxide, ammonium polyphosphate and 3-aminopropyltriethoxysilane is 1:(0.6~1.8):(0.03~0.12).
7. The low-alkali expanded recycled aggregate block according to claim 1, characterized in that, The chopped basalt fibers have a length of 3-12 mm and a diameter of 8-20 μm; the low-alkali polycarboxylate superplasticizer is a polyether-type high-performance polycarboxylate superplasticizer.
8. A method for preparing low-alkali expanded recycled aggregate blocks, characterized in that, The method for preparing a low-alkali expanded recycled aggregate block according to any one of claims 1 to 7 comprises the following steps: S1. Disperse the layered bimetallic hydroxide in a mixture of water and ethanol, add ammonium polyphosphate and adjust the pH to 4.0~6.0, stir at 60~80℃ for 2~6h, filter, wash and dry, and then react with 3-aminopropyltriethoxysilane to obtain flame retardant and smoke suppressant filler. S2. After removing impurities, crushing, screening and washing the construction waste concrete, recycled aggregate is obtained. S3. The recycled aggregate is placed in a carbon dioxide atmosphere for pre-carbonization treatment to obtain pre-carbonized recycled aggregate; S4. Phosphate ester unsaturated monomer, carboxylic acid unsaturated monomer, amide unsaturated monomer, hydrolyzable silane unsaturated monomer, initiator, water and ethanol are mixed and subjected to free radical copolymerization to obtain an aqueous dispersion of phosphorus nitrogen silicon-carboxylate copolymer. S5. Spray the phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion onto the surface of the pre-carbonized recycled aggregate and dry and cure it to obtain modified recycled aggregate; S6. The low-alkali cementitious component, the flame-retardant and smoke-suppressing filler and the short-cut basalt fiber are dry-mixed to obtain the first dry mix; the modified recycled aggregate is added to the first dry mix for secondary dry mixing, and then the low-alkali polycarboxylate superplasticizer and water are added for wet mixing to obtain the semi-dry block material. S7. The semi-dry block material is vibrated and pressed into shape, and after demolding, it is subjected to carbon dioxide mild curing and wet curing in sequence to obtain the low-alkali expansion recycled aggregate block.
9. The method for preparing low-alkali expanded recycled aggregate blocks according to claim 8, characterized in that, In S3, the carbon dioxide volume fraction of the carbon dioxide atmosphere is 5-30%, the relative humidity is 55-85%, the temperature is 20-45℃, and the pre-carbonization treatment time is 30-180 min; in S4, the free radical copolymerization temperature is 60-75℃, the reaction time is 1-3 h, and the solid content of the aqueous dispersion obtained after polymerization is 8-20%; in S5, the spraying amount of the phosphorus-nitrogen-silicon-carboxylate copolymer aqueous dispersion is 0.8-2.5% of the mass of the pre-carbonized recycled aggregate, and the drying and curing temperature is 50-80℃, and the time is 20-90 min.
10. A method for preparing low-alkali expanded recycled aggregate blocks according to claim 8, characterized in that, In S6, the dry mixing time is 60-180s, the secondary dry mixing time is 60-120s, and the wet mixing time is 90-240s. During wet mixing, the first portion of water containing a low-alkali polycarboxylate superplasticizer is added first, followed by the remaining water, so that the moisture content of the semi-dry block material is 7-12%. In S7, the vibration molding pressure is 8-16MPa, and the vibration time is 20-60s. The carbon dioxide volume fraction for the mild carbon dioxide curing is 5-20%, the curing temperature is 20-45℃, the relative humidity is 60-90%, and the curing time is 1-6h. The relative humidity for the wet curing is not less than 90%, and the curing time is 3-28d.
Citation Information
Patent Citations
Hydrotalcite-ammonium polyphosphate halogen-free flame retardant and preparation method thereof
CN102321274B
Method for preparing carbonized recycled aggregate with function of inhibiting alkali-aggregate reaction
CN108793797A
A recycled environmental protection aggregate based on construction waste and its preparation method
CN120081610B
Method for improving performance of recycled aggregate concrete
CN121627329A