A method for producing 2,5-furandimethylamine from 2,5-furandiethanol
By using a supported catalyst in a fixed-bed reactor for hydroamination, the complex process and high cost of synthesizing 2,5-furandimethylamine in existing technologies have been solved, achieving efficient preparation of 2,5-furandimethylamine and improving production capacity and selectivity.
Patent Information
- Application Number
- CN202611443002.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for synthesizing 2,5-furandimethylamine suffer from problems such as cumbersome processes, complex reaction systems, high production costs, complex and difficult-to-separate catalysts, unavailable raw materials, and unsatisfactory product yields.
A supported catalyst, comprising active metal components Ni, Co, and Cu, and promoters Re, Zn, Ag, and Fe, was used. The support consisted of γ-Al₂O₃, SiO₂, and H-ZSM-5. 2,5-Furandimethylamine was prepared in a fixed-bed reactor via hydroamination. The reaction conditions were controlled as follows: 1.5–20 MPa, 120–220 °C, a molar ratio of liquid ammonia to 2,5-furandimethyl alcohol of 5–25:1, a molar ratio of hydrogen to 2,5-furandimethyl alcohol of 1–5:1, and a mass hourly space velocity (WHSV) of 0.2–3 h⁻¹.
The conversion rate of 2,5-furandimethylethanol reached over 95%, and the selectivity of 2,5-furandimethylamine reached over 90%, which simplified the process, reduced production costs, and improved production capacity.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organic synthesis and catalysis technology, and specifically relates to a method for producing 2,5-furandimethylamine from 2,5-furandiethanol. Background Technology
[0002] 2,5-Furfural dimethylamine, as an important bio-based diamine compound, has wide applications in the field of synthetic chemical engineering. It can be used as a building block in organic synthesis and has significant application value in the preparation of pharmaceuticals, coatings, antioxidants, and preservatives. The stable furan ring and symmetrical aminomethyl groups in the molecular structure of 2,5-furan dimethylamine make it an ideal monomer for the synthesis of polyamides, polyurethanes, and other polymer materials.
[0003] Currently, common raw materials for the synthesis of 2,5-furandimethylamine mainly include 5-hydroxymethylfurfural, 2,5-furandicarboxynitrile, 2,5-furandicarboxylic acid, and 2,5-furandiethanol.
[0004] In the synthesis of 2,5-furandimethylamine using 5-hydroxymethylfurfural as a raw material, patent document CN202110309620.3 discloses a one-pot, two-step process for synthesizing 2,5-furandimethylamine. In the first step, 5-hydroxymethylfurfural is oxidized and aminationd to generate an intermediate product under the action of a metal oxide catalyst and methylamine. In the second step, the intermediate product is converted into 2,5-furandimethylamine under the action of a supported Ni or Co catalyst and ammonia and hydrogen. This method uses readily available and simple raw materials and yields good results, but it involves two independent reaction steps, making the reaction system relatively complex. Furthermore, the use of the metal oxide catalyst, the developed supported catalyst, methylamine, and the solvent all increase production costs. Patent document CN201611088469.0 discloses a process for preparing 2,5-furandimethylamine from 2,5-furandicarboxynitrile via catalytic hydrogenation, which requires the use of a noble metal rhodium catalyst. Patent document CN202410007668.2 describes a process for the catalytic hydrogenation of 2,5-furandicarboxynitrile using relatively inexpensive Raney cobalt or Raney nickel catalysts. However, this process is a batch process, and the amounts of alkali additives, catalysts, and solvents used are relatively high. Patent document CN202410131186.8 explores the preparation of 2,5-furandimethylamine using the bio-based platform compound 2,5-furandicarboxylic acid as a substrate under a mixed atmosphere of Raney nickel catalyst and ammonia and hydrogen. Although the raw materials are readily available, the catalyst is inexpensive, and the conversion rate of the reaction raw materials is high, the product selectivity (maximum approximately 51%) still needs improvement. Patent document US2012232292A1 discloses a method for preparing primary amines via the amination reaction of alcohols using a homogeneous ruthenium-based catalyst, mentioning that 2,5-furandimethyl alcohol can be used as a raw material. However, this method relies on complex homogeneous noble metal catalysts.
[0005] In summary, while there are diverse raw materials for the synthesis of 2,5-furandimethylamine in existing technologies, there are few production processes that utilize 2,5-furandimethylethanol as a raw material. Furthermore, existing reports have several shortcomings, mainly including: the use of expensive homogeneous or supported precious metal catalysts; difficulties in catalyst separation and recovery; the need for harsh reaction conditions such as high temperature and high pressure; unsatisfactory product yields or complex processes; and high raw material costs. 2,5-furandimethylethanol, on the other hand, is a stable raw material, and the catalytic reaction system for the preparation of 2,5-furandimethylamine via hydroamination is simple, with easily controllable reaction selectivity.
[0006] Therefore, developing a simple, mild, and industrially suitable method for synthesizing 2,5-furandimethylamine using 2,5-furandimethylethanol as a raw material is of great practical significance. Summary of the Invention
[0007] The purpose of this invention is to provide a method for preparing 2,5-furandimethylamine from 2,5-furandiethanol, in order to solve the problems mentioned in the background art regarding the preparation of 2,5-furandimethylamine, such as cumbersome processes, complex reaction systems, high production costs, difficulty in obtaining raw materials, or complex catalyst preparation and difficulty in subsequent separation and reuse.
[0008] To achieve the above objectives, the present invention provides a method for producing 2,5-furandimethylamine from 2,5-furandiethanol, comprising the following steps:
[0009] 2,5-furandimethylamine and liquid ammonia are introduced into a fixed-bed reactor packed with a supported catalyst and subjected to a hydroamination reaction under a hydrogen atmosphere. The reaction product is cooled and separated into gas and liquid components to obtain 2,5-furandimethylamine. The supported catalyst includes an active metal component, an additive, and a support. The active metal component is one or a combination of two of Ni, Co, and Cu. The additive is one or a combination of two of Re, Zn, Ag, and Fe. The support is selected from one or more of γ-Al₂O₃, SiO₂, and H-ZSM-5 molecular sieves.
[0010] In one specific embodiment, the reaction conditions for the hydroamination reaction are as follows: reaction system pressure is 1.5~20 MPa, reaction bed temperature is 120~220℃; the molar ratio of liquid ammonia to 2,5-furandiethanol is 5~25:1, the molar ratio of hydrogen to 2,5-furandiethanol is 1~5:1; and the mass hourly space velocity (HSV) of 2,5-furandiethanol is 0.2~3 h⁻¹. -1 The support is one of γ-Al2O3, SiO2, or H-ZSM-5.
[0011] In one specific embodiment, the active metal component accounts for 5-50% of the weight of the supported catalyst, the promoter accounts for 0.2-25% of the weight of the supported catalyst, and the remaining components of the supported catalyst are a support.
[0012] In one specific embodiment, the γ-Al₂O₃ support is a spherical support with a diameter of 0.8~5 mm and a specific surface area of 50~500 m². 2 / g, with a pore volume of 0.2~2mL / g and an average pore size of 7~15nm; the SiO2 support is a spherical support with a diameter of 1~5mm and a specific surface area of 100~800m². 2 / g, pore volume of 0.2~2mL / g, average pore size of 7~10nm; the silicon-to-aluminum ratio of the H-ZSM-5 support is 20~500, and the specific surface area is 250~500m². 2 / g, pore volume is 0.15~0.4mL / g, and average pore size is 3~6nm.
[0013] In one specific embodiment, the method for preparing the supported catalyst includes the following steps:
[0014] S1. Carrier pretreatment: Immerse the carrier in a weakly alkaline solution for 0.5 to 5 hours, and then dry it at 100 to 200°C for 2 to 4 hours.
[0015] S2. Active metal component loading: The support is impregnated in a mixed solution prepared by the excess impregnation method, which is composed of the precursor of the active metal component, the precursor of the auxiliary agent and the steric hindrance complexing agent. The impregnation time is 2 to 10 hours. After impregnation, the catalyst precursor is obtained.
[0016] S3. Drying and calcination: Dry the impregnated catalyst precursor at 80~150℃ for 4~12 hours, and then calcine at 300~600℃ for 2~8 hours.
[0017] In one specific embodiment, the steric hindrance complexing agent is selected from at least one of ethylenediaminetetraacetic acid, citric acid, or β-cyclodextrin; the weakly alkaline solution is ammonia or urea solution.
[0018] In one specific embodiment, the roasting atmosphere is one or a combination of two of air, H2, N2, NO, and Ar.
[0019] In one specific embodiment, the supported catalyst needs to be reduced in situ in a mixed atmosphere of hydrogen and nitrogen before being used in the hydroamylation reaction, with a reduction temperature of 200~500℃.
[0020] In one specific embodiment, the supported catalyst needs to be reduced in situ in a mixed atmosphere of hydrogen and nitrogen before being used in the hydroamylation reaction, with a reduction temperature of 300~400℃.
[0021] In one specific embodiment, the 2,5-furandiethanol is preheated to 100°C and melted into a liquid before being fed into the fixed-bed reactor.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The catalyst used in this invention has excellent selectivity: by pretreating the support, the acidic environment on the support surface is adjusted, avoiding byproducts from the polymerization of imine intermediates.
[0024] Meanwhile, a steric hindrance complexing agent is introduced during the impregnation process of the active metal component. This agent can complex with metal ions, allowing the metal ions to be uniformly loaded on the carrier and effectively inhibiting the aggregation of metal ions.
[0025] In addition, the introduction of metal additives significantly enhances the stability of the catalyst. Even under low hydrogen content conditions, the catalyst still exhibits good stability and effectively suppresses the side reactions caused by the hydrogenation of furan ring.
[0026] This invention utilizes a continuous process to prepare 2,5-furandimethylamine, significantly increasing production capacity compared to batch reactor processes. Furthermore, ammonia gas can be recovered and reused during the reaction, reducing ammonia emissions and the use of acidic wastewater.
[0027] In the hydroamination reaction of this invention, the conversion rate of 2,5-furandimethyl alcohol can reach over 95%, and the selectivity of 2,5-furandimethylamine can reach over 90%, providing a new technical route for the efficient preparation of bio-based diamines.
[0028] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The present invention will now be described in further detail. Detailed Implementation
[0029] The embodiments of the present invention will be described in detail below. The specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.
[0030] This invention provides a method for producing 2,5-furandimethylamine from 2,5-furandiethanol, comprising the following steps:
[0031] 2,5-furandiethanol is preheated and melted at 100°C, then mixed with liquid ammonia using a plunger pump and pumped into a fixed-bed reactor packed with a supported catalyst. Under a hydrogen atmosphere, the 2,5-furandiethanol feedstock and ammonia undergo a hydroamination reaction on the catalyst bed. The resulting liquid is cooled, and gas-liquid separation is performed to obtain the product. The supported catalyst is a heterogeneous supported catalyst, comprising an active metal component, an additive, and a support.
[0032] The reaction conditions are as follows:
[0033] The molar ratio of liquid ammonia to 2,5-furandiethanol is 5~25:1; preferably, the molar ratio is 10~15:1. The molar ratio of hydrogen to 2,5-furandiethanol is 1~5:1; preferably, the molar ratio is 1~2:1. The mass hourly space velocity (HSV) of 2,5-furandiethanol is 0.2~3 h⁻¹. -1 Preferably, the mass hourly space velocity (MSV) of 2,5-furandiethanol is 0.2–1 h⁻¹. -1 .
[0034] The reaction system pressure is 1.5~20MPa, preferably 12~18MPa; the reaction bed temperature is 120~220℃, preferably 160~200℃.
[0035] The active metal component in the supported catalyst is one or two of Ni, Co, and Cu, and accounts for 5-50% of the weight of the supported catalyst, preferably 10-30% by weight. The promoter in the supported catalyst is one or a combination of two of Mg, Re, Mo, Zn, Ru, Ag, and Fe, and accounts for 0.2-25% of the weight of the supported catalyst, preferably one or a combination of two of Re, Zn, Ag, and Fe, preferably 1-15% by weight.
[0036] The support in the supported catalyst is one or more of γ-Al₂O₃, θ-Al₂O₃, SiO₂, H-ZSM-5, or HY molecular sieve, preferably one of γ-Al₂O₃, SiO₂, or H-ZSM-5. The active metal component and additives are loaded onto the support by impregnation or precipitation, preferably by excess impregnation.
[0037] The γ-Al₂O₃ support is a spherical support with a diameter of 0.8–5 mm, preferably 2–4 mm. The specific surface area of the γ-Al₂O₃ support is 50–500 m². 2 / g, preferably, the specific surface area of the γ-Al2O3 support is 100~300m². 2 / g. The pore volume of the γ-Al2O3 support is 0.2~2mL / g, preferably 0.5~1mL / g.
[0038] The SiO2 support is a spherical support with a diameter of 1-5 mm, preferably 1.5-3 mm in diameter. The specific surface area of the SiO2 support is 100-800 m². 2 / g, preferably with a specific surface area of 200~300m². 2 / g. The pore volume of the SiO2 support is 0.2~2mL / g, preferably 1~2mL / g.
[0039] The silicon-to-aluminum ratio (SiO2 / Al2O3 molar ratio) of the H-ZSM-5 support is 20~500, preferably 30~80. The specific surface area of the H-ZSM-5 molecular sieve support is 250~500 m² / g. 2 / g, preferably with a specific surface area of 300~450m² 2 / g. The pore volume of the H-ZSM-5 molecular sieve support is 0.15~0.4mL / g, preferably 0.2~0.3mL / g.
[0040] The preparation method of the supported catalyst includes the following steps:
[0041] S1. Carrier Pretreatment: The carrier is immersed in a weakly alkaline solution for 0.5 to 5 hours, followed by drying. This pretreatment aims to adjust the surface pH of the carrier and suppress side reactions. The selected weakly alkaline solution is ammonia or urea solution, preferably ammonia. The drying temperature is 100 to 200°C, preferably 120 to 160°C.
[0042] S2. Loading of Active Metal Components: An excess impregnation method is used. The pretreated support is immersed in a mixed solution prepared from the precursor of the active metal component, the precursor of the auxiliary agent, and a sterically hindered complexing agent. The sterically hindered complexing agent is selected from at least one of ethylenediaminetetraacetic acid, citric acid, or β-cyclodextrin, and can form stable complexes with metal ions. The impregnation time is 2–10 hours, preferably 4–8 hours. After impregnation, excess solution is removed by filtration and then dried to obtain the catalyst precursor.
[0043] S3. Drying and Calcination: The impregnated catalyst precursor is dried at 80-150℃ for 4-12 hours, and then calcined at 300-600℃ for 2-8 hours, preferably at 350-500℃. The calcination atmosphere is one or a combination of two of air, H2, N2, NO, NO2, and Ar.
[0044] The prepared supported catalyst needs to be reduced in situ in a mixture of hydrogen and nitrogen before the reaction. The reduction temperature is 200~500℃, preferably 300~400℃. The gas flow rate is 200mL / min for hydrogen and 100mL / min for nitrogen. The reduction is carried out at atmospheric pressure for 5 hours.
[0045] Example 1
[0046] Preparation of Catalyst 1: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 12.88 g of Ni(NO₃)₂·6H₂O, 1.98 g of Co(NO₃)₂·6H₂O, and 0.29 g of NH₄ReO₄ were weighed and dissolved in 60 mL of deionized water. Then, 2.5 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.8 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution and stirred thoroughly for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 1.
[0047] 10g of the above catalyst was placed in a fixed-bed reactor and activated for 6 hours at atmospheric pressure, 380℃, hydrogen flow rate of 200mL / min, and nitrogen flow rate of 50mL / min. The reaction to produce 2,5-furandimethylamine from 2,5-furandiethanol was carried out at a reaction temperature of 180℃, a system pressure of 15MPa, and a feed mass hourly space velocity of 0.3h⁻¹ for 2,5-furandiethanol. -1 The molar ratio of liquid ammonia to 2,5-furandimethylethanol was 15:1, and the molar ratio of hydrogen to 2,5-furandimethylethanol was 1.5:1. After the reaction had been running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandimethylethanol was 98.5%, and the selectivity of 2,5-furandimethylamine was 95.3%.
[0048] Example 2
[0049] Preparation of Catalyst 2: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 14.86 g of Ni(NO₃)₂·6H₂O, 3.8 g of Cu(NO₃)₂·3H₂O, and 0.58 g of NH₄ReO₄ were weighed and dissolved in 60 mL of deionized water. Then, 2.0 g of β-cyclodextrin was added as a complexing agent to prepare an impregnation solution. 15.6 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution and stirred thoroughly for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined in air at 450 °C for 4 hours to obtain Catalyst 2.
[0050] 10g of the above-mentioned catalyst 2 was placed in a fixed-bed reactor. The activation method and reaction conditions for the preparation of 2,5-furandimethylamine were the same as in Example 1. After the reaction was running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandimethylamine was 96.4%, and the selectivity of 2,5-furandimethylamine was 93.7%.
[0051] Example 3
[0052] Preparation of Catalyst 3: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 14.86 g of Ni(NO₃)₂·6H₂O, 2.89 g of Fe(NO₃)₃·9H₂O, and 0.91 g of Zn(NO₃)₂·6H₂O were weighed and dissolved in 60 mL of deionized water. Then, 2.0 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.6 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution, stirred thoroughly, and impregnated for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 3.
[0053] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions for the preparation of 2,5-furandimethylamine were the same as in Example 1. After the reaction was running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandimethylamine was 91.3%, and the selectivity of 2,5-furandimethylamine was 85.4%.
[0054] Example 4
[0055] Preparation of Catalyst 4: 20 g of SiO2 support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 14.86 g of Ni(NO3)2·6H2O and 0.63 g of AgNO3 were weighed and dissolved in 60 mL of deionized water. Then, 2.0 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.6 g of the pretreated SiO2 support was added to the impregnation solution, stirred thoroughly, and impregnated for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours in a mixture of hydrogen and nitrogen to obtain Catalyst 4.
[0056] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions for the preparation of 2,5-furandimethylamine were the same as in Example 1. After the reaction was running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandimethylamine was 97.4%, and the selectivity of 2,5-furandimethylamine was 92.8%.
[0057] Example 5
[0058] Preparation of Catalyst 5: 20 g of H-ZSM-5 support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 11.41 g of Cu(NO3)3·3H2O and 0.63 g of AgNO3 were weighed and dissolved in 60 mL of deionized water. Then, 2.0 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.6 g of the pretreated H-ZSM-5 support was added to the impregnation solution, stirred thoroughly, and impregnated for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours in air to obtain catalyst 5.
[0059] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions for the preparation of 2,5-furandimethylamine were the same as in Example 1. After the reaction was running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandimethylamine was 62.4%, and the selectivity of 2,5-furandimethylamine was 71.5%.
[0060] Comparative Example 1
[0061] Preparation of Catalyst 6: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 12.88 g of Ni(NO₃)₂·6H₂O, 1.98 g of Co(NO₃)₂·6H₂O, and 0.29 g of NH₄ReO₄ were weighed and dissolved in 60 mL of deionized water to prepare an impregnation solution. 16.8 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution and stirred thoroughly for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 6.
[0062] The preparation method is basically the same as in Example 1, except that no complexing agent is added to the impregnation solution.
[0063] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions were the same as in Example 1. After the reaction ran stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandiethanol was 67.0%, and the selectivity of 2,5-furandimethylamine was 90.2%.
[0064] Comparative Example 2
[0065] Preparation of Catalyst 7: Weigh 14.86 g of Ni(NO3)2·6H2O, 3.8 g of Cu(NO3)2·3H2O, and 0.58 g of NH4ReO4, dissolve them in 60 mL of deionized water, and then add 2.0 g of β-cyclodextrin as a complexing agent to prepare an impregnation solution. Add 15.6 g of γ-Al2O3 support to the impregnation solution, stir thoroughly, and impregnate for 3 hours. Filter, dry the obtained catalyst precursor at 110 °C for 5 hours, and then calcine it in air at 450 °C for 4 hours to obtain Catalyst 7.
[0066] The preparation method is basically the same as in Example 2, except that the γ-Al2O3 support is not pretreated with alkaline solution and is used directly for impregnation.
[0067] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions were the same as in Example 1. After the reaction ran stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandiethanol was 81.2%, and the selectivity of 2,5-furandimethylamine was 72.7%.
[0068] Comparative Example 3
[0069] Preparation of Catalyst 8: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 12.88 g of Ni(NO₃)₂·6H₂O was weighed and dissolved in 60 mL of deionized water, and then 2.5 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.8 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution, stirred thoroughly, and impregnated for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 8.
[0070] The preparation method is basically the same as in Example 1, except that no other additives are added.
[0071] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions were the same as in Example 1. After the reaction was running stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandiethanol was 75.1%, and the selectivity of 2,5-furandimethylamine was 67.5%.
[0072] Comparative Example 4
[0073] Preparation of Catalyst 9: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 12.88 g of Ni(NO₃)₂·6H₂O and 1.98 g of Co(NO₃)₂·6H₂O were weighed and dissolved in 60 mL of deionized water. Then, 2.5 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.8 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution and stirred thoroughly for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 9.
[0074] It is basically the same as Example 1, except that the auxiliary agent NH4ReO4 is not added.
[0075] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions were the same as in Example 1. After the reaction ran stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandiethanol was 85.4%, and the selectivity of 2,5-furandimethylamine was 91.1%.
[0076] Comparative Example 5
[0077] Preparation of Catalyst 10: 20 g of γ-Al₂O₃ support was weighed and immersed in 200 mL of 10% ammonia solution, and stirred at room temperature for 3 hours. After filtration, it was washed with deionized water until neutral and dried at 120 °C for 6 hours to obtain the pretreated support. 12.88 g of Ni(NO₃)₂·6H₂O and 0.29 g of NH₄ReO₄ were weighed and dissolved in 60 mL of deionized water. Then, 2.5 g of ethylenediaminetetraacetic acid was added as a complexing agent to prepare an impregnation solution. 16.8 g of the pretreated γ-Al₂O₃ support was added to the impregnation solution and stirred thoroughly for 3 hours. After filtration, the obtained catalyst precursor was dried at 110 °C for 5 hours and then calcined at 450 °C for 4 hours under NO atmosphere to obtain Catalyst 10.
[0078] It is basically the same as Example 1, except that Co(NO3)2·6H2O was not added.
[0079] 10g of the above catalyst was placed in a fixed-bed reactor. The activation method and reaction conditions were the same as in Example 1. After the reaction ran stably for 50 hours, samples were taken for analysis. The conversion rate of 2,5-furandiethanol was 91.7%, and the selectivity of 2,5-furandimethylamine was 93.2%.
[0080] Investigation of reaction process conditions:
[0081] Based on the catalyst in Example 1, the effects of different reaction conditions on the reaction results were investigated, and the results are shown in Table 1.
[0082] Table 1. Effect of different reaction conditions on the hydroamination of 2,5-furandimethyl.
[0083] As shown in Table 1, the preferred reaction conditions are: temperature 180℃, pressure 12~18MPa, and space velocity 0.2~0.5h. -1 The ammonia / alcohol molar ratio is 12~18:1, and the hydrogen / alcohol molar ratio is 2~1:1. Within this range, high conversion and selectivity can be obtained.
[0084] Catalyst stability test:
[0085] Under the conditions of Example 1, catalyst 1 was subjected to a long-term stability test for 400 hours. The results showed that after 400 hours of reaction, the conversion rate of 2,5-furandimethylethanol remained above 90.1%, and the selectivity of 2,5-furandimethylamine remained above 91.4%, indicating that the catalyst exhibited excellent stability.
[0086] Table 2. Catalyst stability test.
[0087] By comprehensively controlling the reaction temperature, pressure, space velocity, and feed ratio, the conversion rate of 2,5-furandimethylethanol can reach over 95%, and the selectivity of 2,5-furandimethylamine can reach over 90%, providing a new technical route for the efficient preparation of bio-based diamines.
[0088] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions and substitutions can be made without departing from the inventive concept, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A method for preparing 2,5-furandimethylamine from 2,5-furandiethanol, characterized in that, Includes the following steps: 2,5-furandimethylamine and liquid ammonia are introduced into a fixed-bed reactor packed with a supported catalyst and subjected to a hydroamination reaction under a hydrogen atmosphere. The reaction product is cooled and separated into gas and liquid components to obtain 2,5-furandimethylamine. The supported catalyst includes an active metal component, an additive, and a support. The active metal component is one or a combination of two of Ni, Co, and Cu. The additive is one or a combination of two of Re, Zn, Ag, and Fe. The support is selected from one or more of γ-Al₂O₃, SiO₂, and H-ZSM-5 molecular sieves.
2. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, The reaction conditions for the hydroamination reaction are as follows: reaction system pressure is 1.5~20 MPa, reaction bed temperature is 120~220℃; the molar ratio of liquid ammonia to 2,5-furandiethanol is 5~25:1, the molar ratio of hydrogen to 2,5-furandiethanol is 1~5:1; and the mass hourly space velocity (HSV) of 2,5-furandiethanol is 0.2~3 h⁻¹. -1 The support is one of γ-Al2O3, SiO2, or H-ZSM-5.
3. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, The active metal component accounts for 5-50% of the weight of the supported catalyst, the promoter accounts for 0.2-25% of the weight of the supported catalyst, and the remaining components of the supported catalyst are the support.
4. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, The γ-Al₂O₃ support is a spherical support with a diameter of 0.8–5 mm and a specific surface area of 50–500 m². 2 / g, with a pore volume of 0.2~2mL / g and an average pore size of 7~15nm; the SiO2 support is a spherical support with a diameter of 1~5mm and a specific surface area of 100~800m². 2 / g, pore volume of 0.2~2mL / g, average pore size of 7~10nm; the silicon-to-aluminum ratio of the H-ZSM-5 support is 20~500, and the specific surface area is 250~500m². 2 / g, pore volume is 0.15~0.4mL / g, and average pore size is 3~6nm.
5. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, The preparation method of the supported catalyst includes the following steps: S1. Carrier pretreatment: Immerse the carrier in a weakly alkaline solution for 0.5 to 5 hours, and then dry it at 100 to 200°C for 2 to 4 hours. S2. Active metal component loading: The support is impregnated in a mixed solution prepared by the excess impregnation method, which is composed of the precursor of the active metal component, the precursor of the auxiliary agent and the steric hindrance complexing agent. The impregnation time is 2 to 10 hours. After impregnation, the catalyst precursor is obtained. S3. Drying and calcination: Dry the impregnated catalyst precursor at 80~150℃ for 4~12 hours, and then calcine at 300~600℃ for 2~8 hours.
6. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 5, characterized in that, The steric hindrance complexing agent is selected from at least one of ethylenediaminetetraacetic acid, citric acid, or β-cyclodextrin; the weakly alkaline solution is ammonia or urea solution.
7. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 5, characterized in that, The roasting atmosphere is one or a combination of two of the following: air, H2, N2, NO, and Ar.
8. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, Before being used in the hydrogen amination reaction, the supported catalyst needs to be reduced in situ in a mixed atmosphere of hydrogen and nitrogen at a reduction temperature of 200~500℃.
9. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 8, characterized in that, Before being used in the hydroamylation reaction, the supported catalyst needs to be reduced in situ in a mixed atmosphere of hydrogen and nitrogen at a reduction temperature of 300-400°C.
10. The method for producing 2,5-furandimethylamine from 2,5-furandiethanol according to claim 1, characterized in that, The 2,5-furandiethanol is preheated to 100°C and melted into a liquid before being fed into the fixed-bed reactor.
Citation Information
Patent Citations
Method for synthesizing 2,5-dimethylamino furan through catalytic hydrogenation of 2,5-dicyanofuran
CN108129426A
A method for preparing 2,5-bis(aminomethyl)furan
CN113149937B
Method for preparing 2, 5-furandimethylamine from 2, 5-furandicarbonitrile
CN120247843A
Method for preparing 2, 5-furandimethylamine from 2, 5-furandicarboxylic acid
CN120398802A
Process for the preparation of primary amines by homogeneously catalyzed alcohol amination
US20120232292A1