Surface hydrophilic modification method of fluoropolymers

By contacting the surface of a fluoropolymer with an amine group and irradiating it with ultraviolet light, the problem of improving the hydrophilicity of the fluoropolymer surface without compromising mechanical properties and appearance in the prior art has been solved, and the effect of rapidly improving its hydrophilicity has been achieved.

CN123106961APending Publication Date: 2026-11-17BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610838574.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-09-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to easily and quickly improve the surface hydrophilicity of fluoropolymers without compromising their mechanical properties and appearance.

Method used

The hydrophilicity of a fluoropolymer is improved by contacting a compound with an amine group with the surface of the fluoropolymer and reacting it under ultraviolet light.

Benefits of technology

It rapidly reduces the water contact angle of fluoropolymer surfaces, improving surface hydrophilicity without compromising mechanical properties and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_16
    Figure SMS_16
  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

This invention relates to a method for surface hydrophilic modification of fluoropolymers. The modification method of this invention includes: contacting a compound having an amino group with the surface of the fluoropolymer and irradiating it with ultraviolet light; the compound having an amino group is at least one selected from the compounds represented by general formula (1), general formula (2), general formula (3), and general formula (4).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 202111069840.X, application date September 13, 2021, and invention title "Method for Surface Hydrophilic Modification of Fluoropolymers". Technical Field

[0002] This invention relates to a method for surface modification of fluoropolymers, and more particularly, to a method for surface hydrophilic modification of fluoropolymers. Background Technology

[0003] Fluoropolymers such as polytetrafluoroethylene (PTFE) hold a special place in the plastics industry due to their excellent chemical resistance, heat resistance, electrical insulation, and extremely low coefficient of friction. For example, these fluoropolymers are widely used in aerospace, petrochemicals, machinery, electronics, construction, textiles, and many other fields. However, due to their strong non-polarity and very low surface energy, fluoropolymers exhibit poor hydrophilicity and adhesiveness, limiting their applications, particularly in bonding, printing and dyeing, biocompatibility, and composites with other materials. Therefore, to improve surface wettability and compatibility with other materials, hydrophilic modification of the surface of fluoropolymers is often necessary to enable their wider utilization.

[0004] Currently, researchers both domestically and internationally have achieved certain results in modifying the hydrophilicity of fluoropolymer surfaces using methods such as wet chemical methods, plasma methods, irradiation methods, atomic layer deposition (ALD), and high-temperature melting methods. Non-patent literature 1 reports the use of chemical reagents to introduce reactive functional groups into fluoropolymers via wet chemical methods; however, this often leads to darkening of the fluoropolymer surface and even a decrease in its mechanical properties. Non-patent literature 2 reports the use of plasma methods to activate the fluoropolymer surface or graft selected monomers; however, this method usually causes aging of the fluoropolymer. Non-patent literature 3 reports the use of irradiation to form activated functional groups or initiate polymerization reactions on the fluoropolymer surface; however, this method requires expensive equipment and is considered to damage the polymer surface structure. Non-patent literature 4 reports the use of atomic layer deposition (ALD) to improve hydrophilicity by precisely controlling the deposition of uniform thin films on the substrate; however, due to its low growth rate, multiple depositions are usually required, and the process control is highly demanding. Non-patent literature 5 reports a high-temperature melting method, typically involving the embedding of adhesive fillers to modify fluoropolymers. However, the modified material exhibits poor dimensional stability and is difficult to maintain its shape. Non-patent literature 6 reports Hg-sensitized NH3 UV irradiation modification of fluoropolymers, but the process is cumbersome. Non-patent literature 7 reports a method for modifying perfluoroalkanes with alkylamines under UV irradiation; the equipment is simple, but the modification time is long and the modification efficiency is low.

[0005] Therefore, we seek a modification method that maximizes the preservation of the bulk physicochemical properties of fluoropolymers, is simple to operate, environmentally friendly, and has high modification efficiency.

[0006] Existing technical documents

[0007] Non-patent literature 1: Wang SF et al., Applied Surface Science 256 (2010) 2293-2298

[0008] Non-patent literature 2: Yasuda H et al., Journal of Polymer Science Part A PolymerChemistry 15 (1977) 991-1019

[0009] Non-patent literature 3: Hidzir NM et al., Journal of Applied Polymer Science 132 (2015) 41482-41494

[0010] Non-patent literature 4: Xu Q et al., Journal of Membrane Science 415-416 (2012) 435-443

[0011] Non-patent literature 5: Ryan ME et al., Macromolecules 28 (1995) 1377-1382

[0012] Non-patent literature 6: J. Am et al., J. Am. Chem. Soc. 117 (1995) 10119-10120

[0013] Non-patent literature 7: Juan B et al., J. Fluorine Chem. 91 (1998) 49-54 Summary of the Invention

[0014] The problem the invention aims to solve

[0015] In view of the above-mentioned deficiencies in the art, the technical problem to be solved by the present invention is to provide a method for hydrophilizing the surface of fluoropolymers in a simple and rapid manner without degrading the mechanical properties and appearance of the fluoropolymers themselves.

[0016] Solution for solving the problem

[0017] According to the inventor's dedicated research, the above-mentioned technical problems can be solved by implementing the following technical solution:

[0018] [1]. A method for surface hydrophilic modification of a fluoropolymer, wherein the method comprises:

[0019] The compound with an amine group is brought into contact with the surface of a fluoropolymer and then irradiated with ultraviolet light;

[0020] The amino group-containing compound is selected from at least one of the following general formulas: (1), (2), (3), and (4).

[0021] General formula (1),

[0022] In general formula (1), R1 and R2 each independently represent a hydrogen atom, a C1-2 alkyl group, or a C1-4 hydroxyalkyl group. R1 and R2 are not both hydrogen atoms.

[0023] General formula (2),

[0024] In general formula (2), R3 represents C1-12 alkylene, Q represents -NH- or -O-, n1 represents 0 or 1, and n2 represents an integer from 1 to 10.

[0025] General formula (3),

[0026] In general formula (3), R4 represents H2C=CH-, H2C=C(CH3)-, or C1-12 alkyl, R5 represents a residue derived from C1-12 alkyl, R6 and R7 each independently represent a hydrogen atom or a C1-5 alkyl, and n3 represents 1 or 2.

[0027] General formula (4),

[0028] In general formula (4), R8 represents C1-5 alkyl, R9 represents C1-12 alkylene, and R 10 Indicates a direct bond or a C1-12 alkylene bond, R 11 and R 12 Each of these can be used independently to represent a hydrogen atom, a C1-5 alkyl group, or a phenyl group, and n4 represents an integer from 0 to 6.

[0029] [2]. The surface hydrophilic modification method of the fluoropolymer according to [1], wherein the fluoropolymer is a homopolymer or copolymer of fluoroolefin.

[0030] [3]. According to the surface hydrophilic modification method of the fluoropolymer described in [1] or [2], wherein,

[0031] In general formula (1), one of R1 and R2 is a hydrogen atom, or both R1 and R2 are C1-2 alkyl, or both R1 and R2 are C1-4 hydroxyalkyl.

[0032] In general formula (2), R3 represents C1-8 alkylene, Q represents -NH-, and n2 represents an integer from 1 to 6;

[0033] In general formula (3), R4 represents H2C=CH- or H2C=C(CH3)-, R5 represents residues derived from C1-8 alkyl groups, and R6 and R7 each independently represent hydrogen atoms or C1-2 alkyl groups;

[0034] In general formula (4), R8 represents C1-3 alkyl, R9 represents C1-6 alkylene, and R 10 Indicates a direct bond or a C1-6 alkylene group, R 11 and R 12 Each can be used independently to represent a hydrogen atom or a phenyl group, and n4 represents an integer from 0 to 4.

[0035] [4]. A method for surface hydrophilic modification of a fluoropolymer according to any one of [1] to [3], wherein a solution or dispersion containing the compound having an amine group is used to contact the surface of the fluoropolymer.

[0036] [5]. According to the surface hydrophilic modification method of the fluoropolymer described in [4], the solvent in the solution or dispersion containing the compound having an amino group is selected from at least one of water, sulfoxides, amides, ketones, and cyclic ethers.

[0037] [6]. The surface hydrophilic modification method of the fluoropolymer according to [4] or [5], wherein the content of the amine-containing compound in the solution or dispersion containing the amine-containing compound is 10 to 80 by weight.

[0038] [7]. A method for surface hydrophilic modification of fluoropolymers according to any one of [4] to [6], wherein the solution or dispersion containing the compound having an amine group further contains other hydrophilic monomers.

[0039] [8]. The surface hydrophilic modification method of the fluoropolymer according to any one of [1] to [7], wherein the intensity of the ultraviolet light irradiation is 5000~30000 μW / cm. 2 The irradiation time is 1 to 60 minutes.

[0040] The effects of the invention

[0041] By implementing the above technical solutions, the present invention can achieve the following technical effects:

[0042] The modification method of the present invention, through the reaction of a specific amine-containing compound with fluorine atoms on the surface of a fluoropolymer under ultraviolet light irradiation, can rapidly and significantly reduce the surface energy of the fluoropolymer surface (reducing the water contact angle of the fluoropolymer surface to below 70° within 30 minutes, or even below 70° within 20 minutes), thereby improving the hydrophilicity of the fluoropolymer surface; however, the modification method of the present invention involves minimal changes to the substituents on the surface of the fluoropolymer, therefore, it does not degrade the mechanical properties and appearance of the fluoropolymer. Detailed Implementation

[0043] The present invention will now be described in detail. The descriptions of the technical features described below are based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0044] In this specification, the range of values ​​referred to as "value A to value B" refers to the range including the endpoint values ​​A and B.

[0045] In this specification, the numerical ranges referred to by "above" and "below" are ranges that include endpoint values.

[0046] In this specification, the numerical ranges indicated by "greater than" and "less than" refer to the ranges excluding endpoint values.

[0047] Unless otherwise specified, "%" in this instruction manual refers to weight percentage.

[0048] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.

[0049] In this specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes both the scenario in which the event occurs and the scenario in which the event does not occur.

[0050] In this specification, "(meth)acrylate" encompasses both "methacrylate" and "acrylate"; "(meth)acrylic acid" encompasses both "methacrylic acid" and "acrylic acid"; and "(meth)acrylamide" encompasses both "methacrylamide" and "acrylamide".

[0051] In this specification, "alkyl" or "alkylene" means a straight-chain, branched, or cyclic unsubstituted "alkyl" or "alkylene"; "hydroxyalkyl" means a straight-chain, branched, or cyclic "alkyl" or "alkylene" substituted with any number of hydroxyl groups.

[0052] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "implementation," etc., refer to specific elements (e.g., features, structures, properties, and / or characteristics) related to the described implementation that are included in at least one of the embodiments described herein, and may or may not be present in other embodiments. Furthermore, it should be understood that these elements may be combined in any suitable manner in various embodiments.

[0053] The method for surface hydrophilic modification of fluoropolymers of the present invention includes: contacting a compound having an amine group with the surface of the fluoropolymer and irradiating it with ultraviolet light.

[0054] In this invention, the amino-containing compound is selected from at least one of the following general formulas: (1), (2), (3), and (4).

[0055] General formula (1),

[0056] In general formula (1), R1 and R2 each independently represent a hydrogen atom, a C1-2 alkyl group, or a C1-4 hydroxyalkyl group. R1 and R2 are not both hydrogen atoms.

[0057] General formula (2),

[0058] In general formula (2), R3 represents C1-12 alkylene, Q represents -NH- or -O-, n1 represents 0 or 1, and n2 represents an integer from 1 to 10.

[0059] General formula (3),

[0060] In general formula (3), R4 represents H2C=CH-, H2C=C(CH3)-, or C1-12 alkyl, R5 represents a residue derived from C1-12 alkyl, R6 and R7 each independently represent a hydrogen atom or a C1-5 alkyl, and n3 represents 1 or 2.

[0061] General formula (4),

[0062] In general formula (4), R8 represents C1-5 alkyl, R9 represents C1-12 alkylene, and R 10 Indicates a direct bond or a C1-12 alkylene bond, R 11 and R 12 Each of these can be used independently to represent a hydrogen atom, a C1-5 alkyl group, or a phenyl group, and n4 represents an integer from 0 to 6.

[0063] The components and processes used in this invention will be described in more detail below.

[0064] <Compounds containing amine groups>

[0065] In this invention, to achieve the desired technical effects, the amine-containing compound is selected from at least one of the following general formulas: (1), (2), (3), and (4). By using these amine-containing compounds, the hydrophilicity of the fluoropolymer surface can be rapidly and significantly improved.

[0066] General formula (1)

[0067] In general formula (1), R1 and R2 each independently represent a hydrogen atom, a C1-2 alkyl group or a C1-4 hydroxyalkyl group, and R1 and R2 are not both hydrogen atoms.

[0068] In some preferred embodiments, from the viewpoint of enabling faster hydrophilic modification, it is preferred that one of R1 and R2 is a hydrogen atom, or that both R1 and R2 are C1-2 alkyl groups, or that both R1 and R2 are C1-4 hydroxyalkyl groups.

[0069] General formula (2)

[0070] In general formula (2), R3 represents C1 to 12 alkylene, Q represents -NH- or -O-, n1 represents 0 or 1, and n2 represents an integer from 1 to 10.

[0071] In some preferred embodiments, from the viewpoint of enabling faster hydrophilic modification, R3 preferably represents C1-8 alkylene, more preferably C1-6 alkylene, and even more preferably C1-4 alkylene.

[0072] In some preferred embodiments, from the same point of view, Q preferably represents -NH-, and n1 represents 0 or 1.

[0073] In some preferred embodiments, from the same point of view, n2 preferably represents an integer from 1 to 6, and more preferably an integer from 1 to 4.

[0074] General formula (3),

[0075] In general formula (3), R4 represents H2C=CH-, H2C=C(CH3)- or C1-12 alkyl, R5 represents residues derived from C1-12 alkyl, R6 and R7 each independently represent hydrogen atoms or C1-5 alkyl, and n3 represents 1 or 2.

[0076] In some preferred embodiments, from the viewpoint of enabling faster hydrophilic modification, R4 preferably represents H2C=CH- or H2C=C(CH3)-. Additionally, when R4 represents H2C=CH- or H2C=C(CH3)-, the amine-containing compound represented by general formula (3) may or may not undergo polymerization using R4.

[0077] In some preferred embodiments, from the same point of view, R5 preferably represents residues derived from C1 to 8 alkyl groups, more preferably residues derived from C1 to 6 alkyl groups, and even more preferably residues derived from C1 to 4 alkyl groups.

[0078] In some preferred embodiments, from the same point of view, R6 and R7 preferably each independently represent a hydrogen atom or a C1-2 alkyl group, more preferably, R6 and R7 are not both hydrogen atoms.

[0079] General formula (4),

[0080] In general formula (4), R8 independently represents C1-5 alkyl groups, R9 represents C1-12 alkylene groups, and R... 10 Indicates a direct bond or a C1-12 alkylene bond, R 11 and R 12 Each of these can be used independently to represent a hydrogen atom, a C1-5 alkyl group, or a phenyl group, and n4 represents an integer from 0 to 6.

[0081] In some preferred embodiments, from the viewpoint of enabling faster hydrophilic modification, R8 preferably represents each of the C1-3 alkyl groups independently, and more preferably represents each of the C1-2 alkyl groups.

[0082] In some preferred embodiments, from the same point of view, R9 preferably represents C1-12 alkylene, more preferably C1-6 alkylene, and even more preferably C1-4 alkylene.

[0083] In some preferred embodiments, from the same viewpoint, R 10 Preferably, it represents a direct bond or a C1-12 alkylene group; more preferably, it represents a direct bond or a C1-6 alkylene group; and even more preferably, it represents a direct bond or a C1-3 alkylene group.

[0084] In some preferred embodiments, from the same viewpoint, R 11 and R 12 Preferably, each is independently represented by a hydrogen atom or a phenyl group.

[0085] In some preferred embodiments, from the same viewpoint, n4 preferably represents an integer from 0 to 4, and more preferably an integer from 0 to 2. Further, in some more preferred embodiments, when n4 is 0 or 1, R 10 Indicates C1-3 alkylene groups; when n4 is 2, R 10 This indicates a direct key.

[0086] In some particularly preferred embodiments, from the viewpoint of further achieving the desired technical effects of the invention, the compound having an amino group is preferably selected from at least one of methylamine, ethylamine, methyl ethylamine, diethylamine, monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, methanol ethanolamine, ethylenediamine, propylenediamine, butanediamine, tetraethylenehexamine, triethylenetetramine, diethylenetriamine, dimethylaminomethyl methacrylate, dimethylaminoethyl methacrylate, methylaminoethyl methacrylate, tert-butylaminoethyl methacrylate, compounds represented by the following general formula (4-1), compounds represented by the following general formula (4-2), and compounds represented by the following general formula (4-3):

[0087] General formula (4-1),

[0088] In general formula (4-1), R8 independently represents methyl or ethyl, R 10 n represents ethylidene or propyleneide, and n4 represents 0 or 1;

[0089] General formula (4-2),

[0090] In general formula (4-2), R8 independently represents either methyl or ethyl;

[0091] General formula (4-3),

[0092] In general formula (4-3), R8 independently represents methyl or ethyl.

[0093] In this invention, there are no particular restrictions on the form of the amine-containing compound that comes into contact with the fluoropolymer. The amine-containing compound can be applied directly to the fluoropolymer, or it can be applied to the fluoropolymer in the form of a solution or dispersion (especially preferably, in the form of a solution).

[0094] In some preferred embodiments, the amine-containing compound is applied to the fluoropolymer in the form of a solution or dispersion, i.e., a solution or dispersion containing the amine-containing compound is brought into contact with the surface of the fluoropolymer. This is because the inventors have found that, compared to the direct application of the amine-containing compound, the amine-containing compound in solution or dispersion form (particularly preferably, solution form) can achieve the hydrophilic modification effect more quickly and effectively.

[0095] In this invention, there are no particular limitations on the solvent used in the solution or dispersion containing the compound with an amino group, as long as it can dissolve or disperse the compound with an amino group of this invention. In some preferred embodiments, in order to better obtain the desired technical effect of this invention, the solvent is preferably at least one selected from water, sulfoxides, amides, ketones, and cyclic ethers. This is because the inventors have found that when the solvent in the above-mentioned preferred embodiments is used as the solvent in the solution or dispersion containing the compound with an amino group of this invention, the hydrophilic modification reaction under ultraviolet light irradiation can be carried out more easily.

[0096] There are no particular restrictions on the type of water used as a solvent, but deionized water is preferred.

[0097] Examples of sulfoxide solvents include, but are not limited to: dimethyl sulfoxide, trimethyl sulfoxide, tetramethyl sulfoxide, monochloro sulfoxide, dichloro sulfoxide, trichloro sulfoxide, monobromo sulfoxide, dibromo sulfoxide, tribromo sulfoxide, disulfide sulfoxide, etc.

[0098] Examples of amide solvents include, but are not limited to, acetamide, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0099] Examples of ketone solvents include, but are not limited to: acetone, butanone, pentanone, methyl ethyl ketone, methyl isopropanone, methyl isobutyl ketone, n-pentanone, cyclopentanone, n-hexanone, cyclohexanone, isophorone, diacetone alcohol, etc.

[0100] Examples of cyclic ethers include, but are not limited to: tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-oxocyclopentane, dioxane, etc.

[0101] In some more preferred embodiments, the solvent is more preferably at least one selected from deionized water, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, acetone, butanone, and dioxane.

[0102] In this invention, there is no particular limitation on the concentration of the amino-containing compound in the solution or dispersion containing the amino-containing compound. In some preferred embodiments, the content of the amino-containing compound in the solution or dispersion is preferably 10-80% by weight. For embodiments using solution or dispersion form, when the content of the amino-containing compound is less than 10% by weight, the effect of hydrophilic modification tends to decrease; when the content of the amino-containing compound is greater than 80% by weight, the effect of hydrophilic modification also tends to decrease. In some more preferred embodiments, the content of the amino-containing compound in the solution or dispersion is more preferably 15-75% by weight, even more preferably 20-70% by weight, and even more preferably 22-70% by weight.

[0103] In some preferred embodiments, in addition to compounds with amine groups, the solutions or dispersions containing compounds with amine groups may also contain other hydrophilic monomers, such as monomers with hydroxyl groups, monomers with amide groups, monomers with nitrogen-containing heterocycles, monomers with phosphate groups, monomers with sulfonic acid groups, and monomers with carboxyl groups. The inventors have discovered that when compounds with amine groups react with the surface of fluoropolymers under ultraviolet light to generate free radicals, other hydrophilic monomers can react with the generated free radicals and then graft onto the surface of the fluoropolymer, thereby obtaining further improved modification effects.

[0104] Examples of monomers having hydroxyl groups include, but are not limited to, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, vinyl alcohol, and allyl alcohol.

[0105] Examples of monomers having an amide group include, but are not limited to, (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide.

[0106] Examples of monomers having nitrogen-containing heterocycles include, but are not limited to, N-vinyl-2-pyrrolidone, N-vinyl-2-piperidinone, N-vinyl-2-caprolactam, N-vinylpiperazine, N-vinylpyrrole, or N-vinylimidazolium, and (meth)acryloylmorpholine, etc.

[0107] Examples of monomers having a phosphate group include, but are not limited to, 2-hydroxyethylacryloyl phosphate.

[0108] Examples of monomers having a sulfonic acid group include, but are not limited to, sodium vinyl sulfonate.

[0109] Examples of monomers having a carboxyl group include, but are not limited to, (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid, and their anhydrides (e.g., anhydride-containing monomers such as maleic anhydride and itaconic anhydride).

[0110] In some further preferred embodiments, the other hydrophilic monomer is more preferably selected from at least one of monomers having an amide group, monomers having a nitrogen-containing heterocycle, monomers having a sulfonic acid group, and monomers having a carboxyl group.

[0111] In some particularly preferred embodiments, the other hydrophilic monomers are particularly preferably (meth)acrylamide or (meth)acrylic acid or their anhydrides.

[0112] In this invention, there is no particular limitation on the concentration of other hydrophilic monomers in the solution or dispersion containing the compound having an amino group. In some preferred embodiments, the content of other hydrophilic monomers in the solution or dispersion containing the compound having an amino group is preferably 10 to 30% by weight.

[0113] Furthermore, without impairing the effects of the present invention, the solution or dispersion containing the amine-containing compound may also contain any other components, such as surfactants, thickeners (e.g., starch, cellulose, etc.), viscosity reducers, antioxidants, pH adjusters, leveling agents, plasticizers, chain transfer agents, polymerization inhibitors, etc. These other components may be used alone or in combination of two or more.

[0114] Fluoropolymers

[0115] In this invention, the fluoropolymer is a high molecular weight compound containing fluorine atoms, and there is no particular limitation on the specific type. In some preferred embodiments, the fluoropolymer is preferably a homopolymer or copolymer of fluoroolefins.

[0116] In this invention, fluoroolefins are olefins in which one or more hydrogen atoms are replaced by fluorine atoms. Examples of fluoroolefins include, but are not limited to, CF2=CF2, CF2=CFCl, CF2=CHF, CH2=CF2, CF2=CFCF3, CF2=CHCF3, CF3CH=CHF, CF3CF=CH2, etc.

[0117] In this invention, the copolymer of fluoroolefins can be a copolymer between different fluoroolefins, or a copolymer of fluoroolefins with other comonomers. Furthermore, there are no particular limitations on the comonomers, as long as they can copolymerize with the fluoroolefins.

[0118] Furthermore, in this invention, the modification method of this invention can be applied whenever the surface of the fluoropolymer requires hydrophilic modification. In other words, there are no particular limitations on the form of the fluoropolymer; it can be a molded article containing the fluoropolymer (including various molded articles such as films and molding products made of resin or elastomers), or a coating containing the fluoropolymer.

[0119] <Hydrophilic modification process>

[0120] In this invention, there are no particular limitations on the method of applying the solvent containing the amine-group compound (coating method), and application methods commonly used in the art can be employed. Examples of application methods include, but are not limited to: drop application, dip coating, spin coating, bar coating, doctor blade coating, curtain coating, screen printing coating, spray coating, slot coating, etc. These methods can be used alone or in combination of two or more.

[0121] In this invention, the conditions for ultraviolet irradiation generally vary depending on the type of amine-containing compound, the type of solvent, the concentration of the amine-containing compound, and the type of fluoropolymer used, and are not particularly limited. Typically, the ultraviolet irradiation intensity is preferably 5000–30000 μW / cm². 2 More preferably 10000~20000 μW / cm 2 The irradiation time is 1 to 60 minutes, more preferably 2 to 20 minutes.

[0122] In this invention, the irradiation device for ultraviolet light irradiation can be any of the devices known in the art, such as high-pressure mercury lamps, low-pressure mercury lamps, contact aligners, mirror projectors, stepper exposure machines, etc.

[0123] In this invention, after irradiation with ultraviolet light, the fluorinated polymer can be subjected to any treatment known in the art, such as washing or drying, as needed. Each of these treatments can be performed using methods known in the art.

[0124] In some specific implementations, the washing process can be performed using a washing solvent. Examples of washing solvents include, but are not limited to, water (e.g., deionized water), alcohol solvents (e.g., methanol, ethanol, isopropanol, etc.), or mixtures of aqueous organic solvents such as any combination thereof.

[0125] In some specific implementations, the drying process can be carried out by conventional methods in the art (e.g., oven drying, air drying, freeze drying, etc.).

[0126] In some particularly specific implementations, after irradiation with ultraviolet light, the surface of the fluoropolymer is ultrasonically cleaned with deionized water and then dried in a vacuum oven.

[0127] Example

[0128] The present invention is described in detail below by way of embodiments; however, the scope of this application is not limited to these embodiments. Unless otherwise stated, in the following text, "parts" means "parts by weight" and "%" means "% by weight".

[0129] Example 1

[0130] A 30wt% N,N-dimethylformamide (DMF) solution of ethylamine was dropped onto the surface of polytetrafluoroethylene (PTFE), and the solution was then subjected to illumination with a high-pressure mercury lamp at an intensity of 20,000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 60 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0131] Example 2

[0132] A 20wt% DMF solution of ethylamine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp at an intensity of 20000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 60 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0133] Example 3

[0134] A 10 wt% DMF solution of ethylamine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp under an illumination intensity of 20000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 60 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0135] Example 4

[0136] A 50 wt% dioxane solution of diethanolamine was dropped onto a surface containing polyvinylidene fluoride, and the solution was then applied under a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 Irradiate with ultraviolet light for 10 minutes; after the reaction is complete, remove the polyvinylidene fluoride, ultrasonically clean the surface with deionized water for 30 minutes, and then dry it in a vacuum oven at 60℃ to obtain surface-modified polyvinylidene fluoride.

[0137] Example 5

[0138] A 60 wt% deionized aqueous solution of diethylamine was added dropwise to a surface containing polyvinylidene fluoride, and the mixture was then exposed to light using a high-pressure mercury lamp at an intensity of 20000 μW / cm². 2 Irradiate with ultraviolet light for 30 minutes; after the reaction is complete, remove the polyvinylidene fluoride, ultrasonically clean the surface with deionized water for 60 minutes, and then dry it in a vacuum oven at 60°C to obtain surface-modified polyvinylidene fluoride.

[0139] Example 6

[0140] A 60wt% DMF solution of ethylenediamine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp under an illumination intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0141] Example 7

[0142] A 60 wt% DMF solution of triethylenetetramine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0143] Example 8

[0144] A 60 wt% DMF solution of diethylenetriamine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0145] Example 9

[0146] A 20wt% DMF solution of dimethylaminoethyl methacrylate (DMAEMA) was dropped onto the surface of polytetrafluoroethylene (PTFE), and the solution was then subjected to a high-pressure mercury lamp under an illumination intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0147] Example 10

[0148] A 40 wt% DMF solution of DMAEMA was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to a high-pressure mercury lamp under an illumination intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0149] Example 11

[0150] Add 15 wt% acrylamide relative to the total weight of the ethylenediamine DMF solution to prepare a mixed solution (acrylamide content is 13 wt% relative to the total weight of the mixed solution). Drop this mixed solution onto a polytetrafluoroethylene surface and expose it to a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 17 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0151] Example 12

[0152] To prepare a mixed solution, 20 wt% acrylic acid (relative to the total weight of the solution) was added to a 60 wt% DMF solution of ethylenediamine to form a mixed solution (acrylic acid content was 17 wt% relative to the total weight of the mixed solution). This mixed solution was then dropped onto a polytetrafluoroethylene (PTFE) surface and exposed to light using a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 17 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0153] Example 13

[0154] To prepare a mixed solution, 15 wt% acrylic acid (relative to the total weight of the solution) was added to a 60 wt% DMF solution of ethylenediamine to form a mixed solution (acrylic acid content of 13 wt% relative to the total weight of the mixed solution). This mixed solution was then dropped onto a polytetrafluoroethylene (PTFE) surface and exposed to light using a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 17 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0155] Example 14

[0156] A 60 wt% DMF solution of triethylenetetramine was dropped onto the surface of a perfluoroethylene-propylene copolymer, and the mixture was then exposed to light from a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The reaction was subjected to ultraviolet light irradiation for 17 minutes. After the reaction was completed, the perfluoroethylene propylene copolymer was taken out, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain the surface-modified ethylene propylene copolymer.

[0157] Example 15

[0158] Ethylenediamine was directly added dropwise to the surface of polytetrafluoroethylene and then subjected to a high-pressure mercury lamp at an intensity of 15000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 20 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0159] Example 16

[0160] A 70 wt% N,N-dimethylacetamide solution of N-2-aminoethyl-3-aminopropyltrimethoxysilane was dropped onto the surface of polytetrafluoroethylene, and the solution was subjected to illumination with a high-pressure mercury lamp at an intensity of 20000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 60 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0161] Comparative Example 1

[0162] A deionized aqueous solution was dropped onto the surface of polytetrafluoroethylene and then exposed to light from a high-pressure mercury lamp at an intensity of 5000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 30 minutes. Then it was dried in a vacuum oven at 60°C to obtain polytetrafluoroethylene as a control.

[0163] Comparative Example 2

[0164] A 20wt% N,N-dimethylformamide solution of n-butylamine was dropped onto the surface of polytetrafluoroethylene, and the solution was then subjected to illumination with a high-pressure mercury lamp at an intensity of 20000 μW / cm². 2 The polytetrafluoroethylene was irradiated with ultraviolet light for 30 minutes. After the reaction was completed, the polytetrafluoroethylene was removed, and the surface was ultrasonically cleaned with deionized water for 60 minutes. Then it was dried in a vacuum oven at 60°C to obtain surface-modified polytetrafluoroethylene.

[0165] The products processed in the above embodiments and comparative examples were tested as follows.

[0166] hydrophilic properties

[0167] The hydrophilicity was evaluated by conducting water contact angle tests on the surface of the product during the hydrophilic modification process and on the surface of the product immediately after treatment. The results are shown in Table 1. The water contact angle was measured using a contact angle meter.

[0168] In this invention, the water contact angle of the unmodified fluoropolymer surfaces is approximately 120°. The greater the change in water contact angle between the modified and unmodified fluoropolymer surfaces, the better the modification effect.

[0169] Hydrophilic properties stability

[0170] After the treated product was left for 50 days, the water contact angle test was performed on the surface of the treated product as described above to evaluate the stability of the hydrophilic properties. The results are shown in Table 1.

[0171] Generally, the less change there is in the water contact angle obtained on the surface of a freshly treated product in terms of "hydrophilic properties," the better the modification effect.

[0172] Table 1

[0173]

[0174] As can be seen from Table 1, each embodiment of the present invention can reduce the water contact angle of the fluoropolymer surface to below 70° within 30 minutes, and even within 20 minutes, without deteriorating the mechanical properties and appearance of the fluoropolymer.

Claims

1. A method for surface hydrophilic modification of a fluoropolymer, characterized in that, The method includes: A solution or dispersion containing an amine-group compound is brought into contact with the surface of a fluoropolymer, and then irradiated with ultraviolet light. Within 30 minutes, the water contact angle of the fluoropolymer surface is reduced to below 70°. The intensity of the ultraviolet light irradiation is 10,000~30,000 μW / cm². 2 The irradiation time is 1 to 60 minutes; The content of the amino-containing compound in the solution or dispersion is 10-50% by weight. The compound having an amino group is at least one selected from compounds represented by the following general formula (1) and compounds represented by the following general formula (4): General formula (1), In general formula (1), R1 and R2 each independently represent a hydrogen atom, a C1-2 alkyl group, or a C1-4 hydroxyalkyl group. R1 and R2 are not both hydrogen atoms. General formula (4), In general formula (4), R8 represents C1-5 alkyl, R9 represents C1-12 alkylene, and R 10 Indicates a direct bond or a C1-12 alkylene bond, R 11 and R 12 Each of these can be used independently to represent a hydrogen atom, a C1-5 alkyl group, or a phenyl group, and n4 represents an integer from 0 to 6.

2. The surface hydrophilic modification method for fluoropolymers according to claim 1, characterized in that, The fluoropolymer is a homopolymer or copolymer of fluoroolefins.

3. The method for surface hydrophilic modification of fluoropolymers according to claim 1 or 2, characterized in that, In general formula (1), one of R1 and R2 is a hydrogen atom, or both R1 and R2 are C1-2 alkyl groups, or both R1 and R2 are C1-4 hydroxyalkyl groups; In general formula (4), R8 represents C1-3 alkyl, R9 represents C1-6 alkylene, and R 10 Indicates a direct bond or a C1-6 alkylene group, R 11 and R 12 Each can be used independently to represent a hydrogen atom or a phenyl group, and n4 represents an integer from 0 to 4.

4. The method for surface hydrophilic modification of fluoropolymers according to claim 1 or 2, characterized in that, The solvent in the solution or dispersion containing the compound having an amino group is at least one selected from water, sulfoxides, amides, ketones, and cyclic ethers.

5. The method for surface hydrophilic modification of fluoropolymers according to claim 1 or 2, characterized in that, The content of the amino-containing compound in the solution or dispersion containing the amino-containing compound is 15 to 50% by weight.

6. The method for surface hydrophilic modification of fluoropolymers according to claim 1 or 2, characterized in that, The solution or dispersion containing the amine-containing compound also contains other hydrophilic monomers.

7. The method for surface hydrophilic modification of fluoropolymers according to claim 1 or 2, characterized in that, The intensity of the ultraviolet light irradiation is 15000~30000μW / cm. 2 The irradiation time is 2 to 20 minutes.