Preparation method of reverse osmosis composite membrane and reverse osmosis composite membrane

By forming a graphene oxide layer on the substrate of the reverse osmosis membrane and performing interfacial polymerization, the problems of existing film surface roughness and poor anti-pollution performance are solved, the chlorine resistance and anti-pollution performance of the film are significantly improved, and the service life is extended .

CN119015903APending Publication Date: 2024-11-26CIMC ENRIC ENGINEERING TECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136311.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing reverse osmosis membrane has high surface roughness and poor anti-pollution performance, resulting in susceptibility to contamination and short service life.

Method used

The support is formed by vacuum suction filtration of graphene oxide suspension, and the interfacial polymerization is carried out on it. Hydrophilic polymer is added for cross-linking and copolymerization, controlling the polymerization reaction, reducing the release of diamine molecules, and improving the chlorine resistance of the membrane. Performance and anti-pollution properties.

Benefits of technology

It significantly improves the chlorine resistance and pollution resistance of the reverse osmosis composite membrane, extends the service life, and avoids the problem of rough surface of traditional membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015903A_ABST
    Figure CN119015903A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a reverse osmosis composite membrane and the reverse osmosis composite membrane. The preparation method of the reverse osmosis composite membrane comprises the following steps: providing a substrate, and carrying out hydrophilic pretreatment on the substrate; performing vacuum filtration on the graphene oxide suspension on the pretreated substrate to obtain a support body; carrying out interfacial polymerization reaction on a water phase and an organic phase which are prepared in advance on the support body; the water phase is a mixed water solution of diamine and a polymer, the polymer comprises at least one group of carboxyl, hydroxyl and amino, and the organic phase is a binary acyl chloride solution; and after the reaction is finished, drying in the air in the shade, and then carrying out heat treatment at 60-100 DEG C for 3-16 minutes to obtain the reverse osmosis composite membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite membranes, and in particular to a preparation method of a reverse osmosis composite membrane and the reverse osmosis composite membrane. Background Art

[0002] With the growth of population and the progress of industrialization, the lack of clean and safe water has become a key issue. Reverse osmosis membrane technology is widely used in the fields of seawater and brackish water desalination, wastewater treatment, pure water and ultrapure water preparation due to its advantages such as easy operation, high efficiency and energy saving, simple process and environmental friendliness. Most commercial reverse osmosis membranes are synthesized by interfacial polymerization on porous substrates to form a polyamide (PA) selective layer. Since the membrane formed by using m-phenylenediamine (MPD) solution usually has a leaf-like structure, the surface roughness is enhanced, making it more susceptible to contamination. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a reverse osmosis composite membrane and a reverse osmosis composite membrane, so as to solve the problems of large surface roughness and poor anti-pollution performance in the prior art.

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a reverse osmosis composite membrane, comprising the following steps:

[0005] Providing a substrate, and performing a hydrophilic pretreatment on the substrate;

[0006] vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support;

[0007] Conducting interfacial polymerization reaction of the pre-prepared aqueous phase and organic phase on the support; the aqueous phase is a mixed aqueous solution of diamine and polymer, the polymer includes at least one group of carboxyl, hydroxyl and amino, and the organic phase is a dibasic acid chloride solution;

[0008] After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat-treated at 60 to 100° C. for 3 to 16 minutes to obtain a reverse osmosis composite membrane.

[0009] In one embodiment, the diamine comprises at least one of m-phenylenediamine and hexamethylenediamine; and / or,

[0010] In the aqueous phase, the mass concentration of the diamine is 1-5%.

[0011] In one embodiment, the polymer comprises at least one of polyethyleneimine, polyethylene glycol, polyvinyl alcohol and polyacrylic acid; and / or,

[0012] In the water phase, the mass concentration of the polymer is 0.1-0.8%.

[0013] In one embodiment, the dibasic acid chloride comprises at least one of trimesoyl chloride and adipoyl chloride; and / or,

[0014] In the organic phase, the mass concentration of the dibasic acid chloride is 0.01-0.05%; and / or,

[0015] The solvent of the organic phase is n-hexane.

[0016] In one embodiment, the step of subjecting the pre-prepared aqueous phase and organic phase to interfacial polymerization on the support comprises the following:

[0017] First, add the water phase into the mold containing the support, leave it for 2 to 3 minutes, and then pour out the water phase;

[0018] Then, the organic phase is added into the above mold, left for 2 to 3 minutes, and then the organic phase is poured out.

[0019] In one embodiment, the substrate is made of polyacrylonitrile, cellulose acetate, polysulfone or polyethersulfone.

[0020] In one embodiment, the hydrophilization pretreatment of the substrate comprises the following steps:

[0021] The cut substrate is placed in a 1.2-1.6 mol / L NaOH solution at 40-50°C for 1.5-2 hours for hydrophilization pretreatment;

[0022] After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0023] In one embodiment, in the support, the thickness of the graphene oxide layer formed by the graphene oxide suspension is 100-200 nm.

[0024] In one embodiment, the concentration of the graphene oxide suspension is 0.01-0.25 mg / mL, and the ratio of the volume of the graphene oxide suspension to the area of ​​the substrate is (0.8-1.2): 1 mL / cm 2 .

[0025] The present invention also provides a reverse osmosis composite membrane, which is prepared by the above-mentioned preparation method.

[0026] It can be seen from the above technical solution that the advantages and positive effects of the present invention are:

[0027] The preparation method of the present invention comprises vacuum filtering a layer of GO membrane on a substrate, and then doping a polymer in the interfacial polymerization of diamine and diacyl chloride for cross-linking copolymerization, distributing the hydrophilic polymer on the substrate surface and in the transmission channel through in-situ cross-linking copolymerization, and since the GO membrane provides a clear interface, the release of diamine molecules is reduced, so the polymerization reaction can be effectively controlled, and the problem of the diamine solution protruding from the substrate to the diacyl chloride in the traditional interfacial polymerization causing the membrane surface to be rough is avoided. Therefore, the affinity of the reverse osmosis composite membrane to water is improved, the chlorination sites on the membrane are protected, the problem that the amide group is susceptible to chlorine attack is solved, and the chlorine resistance and anti-pollution performance of the reverse osmosis composite membrane are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic flow diagram of the method for preparing the reverse osmosis composite membrane in the present invention.

[0029] Figure 2 This is a graph showing the change in normalized flux over time of a sodium dodecyl sulfate (SDS) aqueous solution treated by the reverse osmosis composite membrane of Example 1 (operating conditions: 25±1° C., 1.0 MPa).

[0030] Figure 3 This is a graph showing the normalized flux variation over time of a dodecyltrimethylammonium bromide (DTAB) aqueous solution treated with the reverse osmosis composite membrane of Example 1 (operating conditions: 25±1° C., 1.0 MPa).

[0031] Figure 4 This is a graph showing the normalized flux variation over time of bovine serum albumin (BSA) aqueous solution treated by the reverse osmosis composite membrane of Example 1 (operating conditions: 25±1° C., 1.0 MPa). DETAILED DESCRIPTION

[0032] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions and illustrations therein are essentially used for illustration purposes rather than for limiting the present invention.

[0033] In order to further illustrate the principle and structure of the present invention, preferred embodiments of the present invention are now described in detail with reference to the accompanying drawings.

[0034] The invention provides a method for preparing a reverse osmosis composite membrane, wherein a layer of graphene oxide (usually represented by GO) membrane is vacuum filtered on a substrate, and dopants are added in interfacial polymerization for cross-linking copolymerization, thereby obtaining a reverse osmosis composite membrane with improved anti-pollution performance and service life.

[0035] Figure 1A schematic diagram showing a method for preparing a reverse osmosis composite membrane is shown in FIG. Figure 1 The method for preparing the reverse osmosis composite membrane comprises the following steps:

[0036] S1. Provide a substrate and perform hydrophilic pretreatment on the substrate.

[0037] The material of the substrate is polyacrylonitrile (PAN), cellulose acetate (CA), polysulfone (PSF) or polyethersulfone (PES).

[0038] The substrate is a film formed by the above materials.

[0039] The hydrophilization pretreatment of the substrate includes the following steps:

[0040] The cut substrate is placed in a 1.2-1.6 mol / L NaOH solution and subjected to a hydrophilic pretreatment at 40-50° C. for 1.5-2 h.

[0041] After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0042] S2. Vacuum-filter the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0043] Graphene oxide (GO) has a unique two-dimensional structure with a large number of oxygen-containing functional groups on its surface, which has great advantages in a variety of applications and in the preparation of separation membranes with excellent chemical stability and high permeability. There are two main separation mechanisms in GO membranes: separation through interlayer nanochannels and transmission through defects and pores. Since there are abundant functional groups on GO nanosheets, the hydrophilicity of the membrane surface can be improved, so it can be used as an excellent additive to improve the water flux and anti-fouling performance of the membrane.

[0044] Preferably, before vacuum filtering the graphene oxide suspension onto the pretreated substrate, the graphene oxide suspension is first subjected to ultrasonic treatment for 1 to 2 hours to disperse the graphene oxide suspension more evenly.

[0045] In the support, the thickness of the graphene oxide layer formed by the graphene oxide suspension is 100 to 200 nm.

[0046] Specifically, the concentration of the graphene oxide suspension is 0.01-0.25 mg / mL, and the ratio of the volume of the graphene oxide suspension to the area of ​​the substrate is (0.8-1.2): 1 mL / cm 2 .

[0047] S3, subjecting the prepared aqueous phase and organic phase to interfacial polymerization on the support. The aqueous phase is a mixed aqueous solution of diamine and dopant, the polymer includes at least one of carboxyl, hydroxyl and amino groups, and the organic phase is a dibasic acid chloride solution.

[0048] The diamine includes at least one of m-phenylenediamine and hexamethylenediamine, that is, the diamine can be any one of the above two, or a mixture of the two in any proportion.

[0049] The structural formula of m-Phenylenediamine (MPD) is It has two amine groups in its structure.

[0050] The structural formula of hexamethylenediamine (1,6-Diaminohexane) is It has two amine groups in its structure.

[0051] The polymer includes at least one of polyethyleneimine, polyethylene glycol, polyvinyl alcohol and polyacrylic acid, that is, the polymer can be any one of the above four, a mixture of any two in any proportion, a mixture of any three, or a mixture of any four.

[0052] The structural formula of polyethyleneimine (PEI) is It has an amino group in its structure.

[0053] Preferably, the PEI has a molecular weight of at least one of 600, 1700, 10,000 and 70,000.

[0054] The structural formula of polyethylene glycol (PEG) is It has hydroxyl groups in its structure.

[0055] Preferably, PEG has a molecular weight of at least one of 600, 800, 1000, 1500 and 2000.

[0056] The structural formula of polyvinyl alcohol (PVA) is It has hydroxyl groups in its structure.

[0057] Preferably, the PVA has a molecular weight of at least one of 9,000, 13,000, 23,000 and 31,000.

[0058] The structural formula of polyacrylic acid (PAA) is It has a carboxyl group in its structure.

[0059] Preferably, the PAA has a molecular weight of at least one of 2,000 and 450,000.

[0060] Therefore, the above polymer is a hydrophilic polymer.

[0061] The preparation method of the aqueous phase is: adding the diamine and the polymer into the aqueous solution, dissolving them, and stirring them evenly to form the aqueous phase.

[0062] The mass concentration of the diamine in the aqueous phase is 1-5%. The mass concentration of the polymer in the aqueous phase is 0.1-0.8%. The mass concentration of the diamine is calculated as follows: mass concentration of the diamine = mass of the diamine / (mass of the diamine + mass of the polymer + mass of the solvent deionized water).

[0063] The dibasic acid chloride includes at least one of trimesoyl chloride and adipoyl chloride, that is, the dibasic acid chloride can be any one of the above two types, or a mixture of the two in any proportion.

[0064] The structural formula of Trimesoyl chloride (TMC) is

[0065] The structural formula of adipoyl chloride is

[0066] The solvent in the organic phase is n-hexane.

[0067] The preparation method of the organic phase is to dissolve the dibasic acid chloride in a solvent, n-hexane, and stir it evenly, wherein the mass concentration of the dibasic acid chloride is 0.01-0.05%.

[0068] Taking the aqueous phase as PEI and MPD and the organic phase as TMC as an example, the reaction between the three is as follows:

[0069]

[0070] PEI is doped into the MPD and TMC interfacial polymerization for cross-linking copolymerization, and the hydrophilic polymer PEI is distributed on the PA membrane surface and in the transmission channel through in-situ cross-linking copolymerization.

[0071] The step of performing interfacial polymerization reaction of the pre-prepared aqueous phase and organic phase on the support comprises the following:

[0072] First, add the water phase into the mold equipped with the support, leave it for 2 to 3 minutes, and then pour out the water phase.

[0073] Then, the organic phase is added into the above mold, left for 1 to 2 minutes, and then the organic phase is poured out.

[0074] S4. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat-treated at 60-100° C. for 3-16 minutes to obtain a reverse osmosis composite membrane.

[0075] The purpose of drying in the air is to evaporate the solvent n-hexane.

[0076] Heat treatment is to further remove n-hexane and make the entire membrane denser.

[0077] The present invention vacuum filters a layer of GO membrane on a substrate, then dopes a polymer in the interfacial polymerization of diamine and diacyl chloride for cross-linking copolymerization, and distributes the hydrophilic polymer on the substrate surface and in the transmission channel through in-situ cross-linking copolymerization. The addition of the hydrophilic polymer makes the GO membrane surface smoother, and as the polymer content increases, the hydrophilicity of the GO membrane surface gradually increases. After cross-linking copolymerization, the negative charge on the membrane surface decreases.

[0078] And because the GO membrane provides a clear interface and reduces the release of diamine molecules, the polymerization reaction can be effectively controlled, avoiding the problem of diamine solution protruding from the substrate to the diacyl chloride in traditional interfacial polymerization, resulting in a rough membrane surface. Therefore, the affinity of the reverse osmosis composite membrane to water is improved, the chlorination sites on the membrane are protected, the problem of amide groups being susceptible to chlorine attack is solved, and the chlorine resistance and anti-pollution performance of the reverse osmosis composite membrane are significantly improved.

[0079] The present application also provides a reverse osmosis composite membrane, which is prepared using the above-mentioned preparation method.

[0080] The inventors of the present application have achieved the preparation of an anti-pollution reverse osmosis composite membrane by strictly designing the content of each component and the parameters in each step. The method is introduced below through various embodiments.

[0081] Example 1

[0082] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0083] S11, placing the cut PAN substrate in a 1.5 mol / L NaOH solution at 45° C. for hydrophilization pretreatment for 1.5 h. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0084] S12, treating the graphene oxide suspension by ultrasound for 1 hour, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0085] The concentration of graphene oxide suspension is 0.05 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​substrate is 1.2:1 mL / cm 2 .

[0086] S13, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0087] The aqueous phase is a water solution of PEI and MPD, the molecular weight of PEI is 10000, the concentration of PEI is 0.4wt%, and the concentration of MPD is 2wt%. The organic phase is a TMC solution, the solvent is n-hexane, and the concentration of TMC is 0.025wt%.

[0088] Specifically, the water phase was first added into the mold equipped with the support, left for 3 minutes, and then the water phase was poured out.

[0089] Then, the organic phase was added into the above mold, left for 2 minutes, and then the organic phase was poured out.

[0090] S14. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat treated at 80° C. for 10 minutes to obtain a reverse osmosis composite membrane.

[0091] Example 2

[0092] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0093] S21, placing the cut CA substrate in a 1.2 mol / L NaOH solution at 40° C. for hydrophilic pretreatment for 2 h. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0094] S22, subjecting the graphene oxide suspension to ultrasonic treatment for 2 h, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0095] The concentration of graphene oxide suspension is 0.01 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​the substrate is 0.8:1 mL / cm 2 .

[0096] S23, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0097] The aqueous phase is an aqueous solution of PEG and hexamethylenediamine, the concentration of PEG is 0.1wt%, the concentration of hexamethylenediamine is 1wt%, and the organic phase is a solution of adipoyl chloride, the solvent is n-hexane, and the concentration of adipoyl chloride is 0.01wt%.

[0098] Specifically, the water phase was first added into the mold equipped with the support, left for 2.5 min, and then the water phase was poured out.

[0099] Then, the organic phase was added into the above mold, left for 2 minutes, and then the organic phase was poured out.

[0100] S24. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat treated at 100° C. for 3 minutes to obtain a reverse osmosis composite membrane.

[0101] Example 3

[0102] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0103] S31, placing the cut PSF substrate in a 1.4 mol / L NaOH solution at 50° C. for hydrophilization pretreatment for 1.5 h. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0104] S32, treating the graphene oxide suspension by ultrasound for 1.5 h, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0105] The concentration of graphene oxide suspension is 0.25 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​substrate is 1:1 mL / cm 2 .

[0106] S33, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0107] The aqueous phase is a water solution of PVA and MPD, the concentration of PVA is 0.8wt%, the concentration of MPD is 5wt%, and the organic phase is a solution of adipoyl chloride, the solvent is n-hexane, and the concentration of adipoyl chloride is 0.05wt%.

[0108] Specifically, the water phase was first added into the mold equipped with the support, left for 2 minutes, and then the water phase was poured out.

[0109] Then, the organic phase was added into the above mold, left for 1 min, and then the organic phase was poured out.

[0110] S34. After the reaction is completed, the membrane is placed in the air to dry in the shade, and then heat treated at 60° C. for 16 minutes to obtain a reverse osmosis composite membrane.

[0111] Example 4

[0112] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0113] S41, placing the cut PES substrate in a 1.3 mol / L NaOH solution at 48° C. for hydrophilization pretreatment for 1.6 h. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0114] S42, treating the graphene oxide suspension by ultrasound for 2 hours, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0115] The concentration of graphene oxide suspension is 0.15 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​the substrate is 1.1:1 mL / cm 2 .

[0116] S43, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0117] The aqueous phase is a PAA and MPD aqueous solution, the PAA concentration is 0.5wt%, the MPD concentration is 4wt%, and the organic phase is a adipoyl chloride solution, the solvent is n-hexane, and the adipoyl chloride concentration is 0.04wt%.

[0118] Specifically, the water phase was first added into the mold equipped with the support, left for 3 minutes, and then the water phase was poured out.

[0119] Then, the organic phase was added into the above mold, left for 2 minutes, and then the organic phase was poured out.

[0120] S44. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat treated at 70° C. for 13 minutes to obtain a reverse osmosis composite membrane.

[0121] Example 5

[0122] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0123] S51, placing the cut PSF substrate in a 1.6 mol / L NaOH solution at 46° C. for hydrophilic pretreatment for 2 hours. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0124] S52, treating the graphene oxide suspension by ultrasound for 1.2 h, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0125] The concentration of graphene oxide suspension is 0.1 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​the substrate is 0.9:1 mL / cm 2 .

[0126] S53, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0127] The aqueous phase is an aqueous solution of PEI, PVA and MPD. The molecular weight of PEI is 70,000, the concentration of PEI is 0.3wt%, the concentration of PVA is 0.3wt%, and the concentration of MPD is 3wt%. The organic phase is a TMC solution, the solvent is n-hexane, and the concentration of TMC is 0.03wt%.

[0128] Specifically, the water phase was first added into the mold equipped with the support, left for 3 minutes, and then the water phase was poured out.

[0129] The organic phase was then added into the above mold, left for 1.5 min, and then the organic phase was poured out.

[0130] S54. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat treated at 90° C. for 6 minutes to obtain a reverse osmosis composite membrane.

[0131] Example 6

[0132] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0133] S61, placing the cut PAN substrate in a 1.5 mol / L NaOH solution at 42° C. for hydrophilization pretreatment for 2 hours. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0134] S62, treating the graphene oxide suspension by ultrasound for 1.8 h, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0135] The concentration of graphene oxide suspension is 0.2 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​the substrate is 1.05:1 mL / cm 2 .

[0136] S63, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0137] The aqueous phase is an aqueous solution of PEI, MPD and hexamethylenediamine. The molecular weight of PEI is 1700, the concentration of PEI is 0.2wt%, the concentration of MPD is 2wt%, and the concentration of hexamethylenediamine is 1wt%. The organic phase is a TMC solution, the solvent is n-hexane, and the concentration of TMC is 0.015wt%.

[0138] Specifically, the water phase was first added into the mold equipped with the support, left for 3 minutes, and then the water phase was poured out.

[0139] Then, the organic phase was added into the above mold, left for 2 minutes, and then the organic phase was poured out.

[0140] S64. After the reaction is completed, the membrane is placed in the air to dry in the shade, and then heat treated at 75°C for 12 minutes to obtain a reverse osmosis composite membrane.

[0141] Comparative Example 1

[0142] The method for preparing the reverse osmosis composite membrane in this embodiment comprises the following steps:

[0143] S71, placing the cut PAN substrate in a 1.5 mol / L NaOH solution at 45° C. for hydrophilization pretreatment for 1.5 h. After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

[0144] S72, subjecting the graphene oxide suspension to ultrasonic treatment for 1 hour, and then vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support.

[0145] The concentration of graphene oxide suspension is 0.05 mg / mL, and the ratio of the volume of graphene oxide suspension to the area of ​​substrate is 1.2:1 mL / cm 2 .

[0146] S73, subjecting the pre-prepared aqueous phase and organic phase to an interfacial polymerization reaction on a support.

[0147] The aqueous phase is an MPD aqueous solution, the concentration of MPD is 2wt%, the organic phase is a TMC solution, the solvent is n-hexane, and the concentration of TMC is 0.025wt%.

[0148] Specifically, the water phase was first added into the mold equipped with the support, left for 3 minutes, and then the water phase was poured out.

[0149] Then, the organic phase was added into the above mold, left for 2 minutes, and then the organic phase was poured out.

[0150] S74. After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat treated at 60° C. for 16 minutes to obtain a reverse osmosis composite membrane.

[0151] Comparative Example 2

[0152] FR12-8040 reverse osmosis composite membrane from Wharton Technology Co., Ltd.

[0153] The reverse osmosis composite membranes prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were respectively tested for NaCl flux and NaCl rejection. The test results are shown in Table 1.

[0154] Among them, the detection method of NaCl flux is as follows:

[0155] The reverse osmosis composite membranes of Examples 1 to 6 and Comparative Examples 1 to 2 were cut into pieces with an effective area of ​​7.065 cm2 For the test sample, the raw material liquid 500mg / L NaCl solution is pressurized by a high-pressure constant flow pump at a flow rate of 10mL / min and then enters the above-mentioned reverse osmosis composite membrane. The concentrated water flows back to the feed tank, and the operating pressure is 1.0MPa. The feed tank is placed in a constant temperature water tank to stabilize the temperature during operation at 25±1°C. The operating pressure during the reverse osmosis process is controlled by a back pressure valve on the membrane interception side. The reverse osmosis system is run for 3h before testing to ensure that the membrane mass transfer process reaches a stable state, and then samples are taken every hour. The test lasts for four hours, and the volume of the permeate is measured four times to take the average value.

[0156] The flux is calculated by the formula F = V / At, where F is the flux, V is the volume of the permeate solution in L, and A is the permeate membrane area in m 2 , t represents the penetration time, the unit is h.

[0157] The NaCl retention rate is tested as follows: the conductivity of the permeate and the raw material solution is measured using a conductivity meter. f )×100% to calculate the interception rate, R is the interception rate (%), C f and Cp are the electrical conductivities of the feed solution and the permeate, respectively.

[0158] Table 1 Performance of reverse osmosis composite membrane

[0159] Examples and Comparative Examples <![CDATA[NaCl flux (L m -2 h -1 )]]> NaCl retention rate (%) Example 1 3.2 97.45 Example 2 2.9 97.21 Example 3 3.1 96.74 Example 4 2.5 96.46 Example 5 2.3 95.39 Example 6 2.1 95.79 Comparative Example 1 1.9 92.75 Comparative Example 2 1.8 93.82

[0160] It can be seen from Table 1 that the separation performances of Examples 1 to 6 are all better than those of the comparative example.

[0161] The reverse osmosis composite membranes prepared in Example 1 and Comparative Example 1 were evaluated by normalizing the flux J / J0 during the treatment of sodium dodecyl sulfate (SDS) aqueous solution, dodecyltrimethylammonium bromide (DTAB) aqueous solution and bovine serum albumin (BSA) aqueous solution.

[0162] The test method is as follows: first feed with 500mg / L NaCl aqueous solution, and after stabilization, add pollutants to the feed solution to make the concentration of pollutants 50-200mg / L. The pollutants mainly include electronegative sodium dodecyl sulfate (SDS), positive dodecyl trimethyl ammonium bromide (DTAB) and neutral bovine serum albumin (BSA). After the pollution test is completed, the pressure is released, and the polluted membrane is cleaned with deionized water as the feed liquid, and then the permeation flux of the composite membrane is measured with 500mg / L NaCl aqueous solution as the feed liquid. Samples are taken every hour during the experiment.

[0163] Record the data and process them to obtain Figure 2 , Figure 3 and Figure 4 .

[0164] Figure 2 The normalized flux of sodium dodecyl sulfate (SDS) aqueous solution treated in Example 1 and Comparative Example 1 varies with time. Figure 2 It can be seen that PEI cross-linking copolymerization modification improves the membrane's resistance to anion pollution.

[0165] Figure 3 The normalized flux of dodecyltrimethylammonium bromide (DTAB) aqueous solution treated in Example 1 and Comparative Example 1 varies with time. Figure 3 It can be seen that PEI cross-linking copolymerization modification improves the membrane's resistance to cationic fouling.

[0166] Figure 4 The normalized flux of bovine serum albumin (BSA) aqueous solution treated in Example 1 and Comparative Example 1 is shown as a function of time. Figure 4 It can be seen that PEI cross-linking copolymerization modification improves the membrane's resistance to protein fouling.

[0167] Although the present invention has been described with reference to several typical embodiments, it should be understood that the terms used are illustrative and exemplary, rather than restrictive. Since the present invention can be embodied in a variety of forms without departing from the spirit or essence of the invention, it should be understood that the above embodiments are not limited to any of the foregoing details, but should be interpreted broadly within the spirit and scope defined by the appended claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the appended claims.

Claims

1. A method for preparing a reverse osmosis composite membrane, characterized in that: The following steps are involved: Providing a substrate, and performing a hydrophilic pretreatment on the substrate; vacuum filtering the graphene oxide suspension onto the pretreated substrate to obtain a support; Conducting interfacial polymerization reaction of the pre-prepared aqueous phase and organic phase on the support; the aqueous phase is a mixed aqueous solution of diamine and polymer, the polymer includes at least one group of carboxyl, hydroxyl and amino, and the organic phase is a dibasic acid chloride solution; After the reaction is completed, the mixture is placed in the air to dry in the shade, and then heat-treated at 60 to 100° C. for 3 to 16 minutes to obtain a reverse osmosis composite membrane.

2. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The diamine comprises at least one of m-phenylenediamine and hexamethylenediamine; and / or, In the aqueous phase, the mass concentration of the diamine is 1-5%.

3. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The polymer comprises at least one of polyethyleneimine, polyethylene glycol, polyvinyl alcohol and polyacrylic acid; and / or, In the water phase, the mass concentration of the polymer is 0.1-0.8%.

4. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The dibasic acid chloride comprises at least one of trimesoyl chloride and adipoyl chloride; and / or, In the organic phase, the mass concentration of the dibasic acid chloride is 0.01-0.05%; and / or, The solvent of the organic phase is n-hexane.

5. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The step of subjecting the pre-prepared aqueous phase and organic phase to interfacial polymerization on the support comprises the following: First, add the water phase into the mold containing the support, leave it for 2 to 3 minutes, and then pour out the water phase; Then, the organic phase is added into the above mold, left for 2 to 3 minutes, and then the organic phase is poured out.

6. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The material of the substrate is polyacrylonitrile, cellulose acetate, polysulfone or polyethersulfone.

7. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The hydrophilization pretreatment of the substrate comprises the following steps: The cut substrate is placed in a 1.2-1.6 mol / L NaOH solution at 40-50°C for 1.5-2 hours for hydrophilization pretreatment; After the pretreatment, the surface of the substrate is cleaned with deionized water and stored in deionized water for later use.

8. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: In the support, the thickness of the graphene oxide layer formed by the graphene oxide suspension is 100-200 nm.

9. The method for preparing a reverse osmosis composite membrane according to claim 1, characterized in that: The concentration of the graphene oxide suspension is 0.01-0.25 mg / mL, and the ratio of the volume of the graphene oxide suspension to the area of ​​the substrate is (0.8-1.2): 1 mL / cm 2 .

10. A reverse osmosis composite membrane, characterized in that: The method is described in any one of claims 1 to 9.