Method for utilizing all components of plant straw, E NF Environmentally friendly wood adhesive, natural color paste and its preparation method and application
Through alkaline deconstruction and multi-reaction system technology, the low-solid content of ENF-grade environmentally friendly wood adhesives and natural pulp are directly used to prepare low-solid content ENF-grade environmentally friendly wood adhesives and natural pulp, solving the problems of plant straw utilization and adhesive performance, and achieving efficient and environmentally friendly growth All-component utilization of substance components and high-quality production of plywood.
Patent Information
- Application Number
- CN202410490368.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-04-23
AI Technical Summary
The existing technology cannot effectively utilize the entire component of plant straw, resulting in burning of straw or entering the river, causing environmental pollution. At the same time, the high solid content of traditional adhesives leads to increased costs and decreased viscosity, affecting the quality and environmental protection of plywood.
The alkaline method is used to deconstruct plant straw, and the ENF-grade environmentally friendly wood adhesive is directly used to prepare ENF-grade environmentally friendly wood adhesive. By gradually assembling the adhesive molecular structure under a multi-reaction system, combining phenol, urea and formaldehyde reactions, low-solid adhesives are prepared, and the The cellulose-rich solid residue is processed as a natural pulp and is used for paper manufacturing.
It realizes the high-value utilization of the entire component of plant straw, reduces the solid content and cost of adhesives, extends the opening period of plywood, improves the gluing performance and paper performance, and has no waste liquid discharge, which meets environmental protection requirements.
Smart Images

Figure CN118325118B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomass refining, and in particular relates to a method for utilizing all components of plant straw. NF Grade environmentally friendly wood adhesive, natural color pulp and preparation method and application thereof. Background Art
[0002] Since it is impossible to deal with a large amount of straw, people can only burn it or dump it into rivers to reduce the accumulation of straw. However, burning straw will cause air pollution and reduce air visibility; dumping straw into rivers will cause a large amount of organic matter to dissolve into the water, causing a large amount of dissolved oxygen in the water to be consumed, directly affecting the living environment of aquatic organisms and causing large-scale death of aquatic organisms.
[0003] At present, straw is the main raw material for many pulp and paper mills in my country, and the production method is basically based on the alkaline method. However, since grass crops contain silicates, the silicates become soluble in the alkaline solution during alkaline cooking, so the silicon in the crops basically goes into the black liquor, making the black liquor produced during the pulping process contain a high content of silicon, which hinders the recovery of alkali in the black liquor; at the same time, due to the high concentration of silicon, it is very difficult to filter lignin and hemicellulose; and the high silicon content of black liquor will also cause environmental pollution, so the treatment of black liquor is currently a very big dilemma in straw pulping.
[0004] The solid content of traditional adhesives used in the wood-based panel industry is more than 40%. However, high solid content adhesives increase the cost of use and also reduce the shelf life of adhesives. Low solid content adhesives generally lead to a decrease in adhesive viscosity, which makes coating difficult and causes waste due to excessive penetration of the adhesive into the wood. In addition, it affects the efficiency of hot pressing or secondary pressing, and even causes bubbling in the plywood due to the effect of moisture during the preparation of plywood. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for utilizing all components of plant straw. NF Environmentally friendly wood adhesive, natural color pulp and its preparation method and application, the technical problem to be solved is how to provide a method for utilizing all components of plant straw, directly using black liquor as raw material to prepare E NF The environmentally friendly wood adhesive is a kind of environmentally friendly wood adhesive. The adhesive is synthesized by gradually assembling the molecular structure of the adhesive in a multi-reaction system. The characteristics of the adhesive are that the black liquor does not need to be concentrated, and the hemicellulose in the black liquor does not need to be removed. The process steps are simple and the cost is saved. NF The environmentally friendly wood adhesive has a low solid content and still has good gluing performance when its mass solid content is as low as 25%.NF When the environmentally friendly wood adhesive is used to prepare multilayer boards, its opening period can be as long as 1.5 to 2 hours, which effectively overcomes the existing E NF The defect of the environmentally friendly wood adhesive product of grade 1 is short opening time after gluing; at the same time, the cellulose-rich solid residue decomposed by alkali method is processed into natural color pulp, and the natural color paper prepared with this natural color pulp has excellent performance; that is, the technical solution of the present invention has simple process, economical cost, good performance, can realize the full utilization of biomass components and no waste liquid discharge in the process, and has better practicality.
[0006] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. According to a method for utilizing all components of plant straw proposed by the present invention, the method comprises the following steps:
[0007] S11 deconstructs the plant straw by alkaline method to obtain a cellulose-rich solid residue and a black liquor containing hemicellulose and lignin; the weight solid content of the black liquor is 12-20%; the weight percentage of hemicellulose in the black liquor is 1-3%;
[0008] S12: processing the cellulose-rich solid residue into natural color pulp, polylactic acid or polyhydroxyalkanoate precursor; reacting the black liquor with phenol, urea and formaldehyde to prepare E NF Environmentally friendly wood adhesive.
[0009] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. NF The method for preparing a grade environmentally friendly wood adhesive comprises the following steps:
[0010] S21: deconstructing the plant straw by alkaline method, separating the solid and the liquid, and obtaining black liquor containing hemicellulose and lignin; weighing the raw materials according to a preset formula; the weight solid content of the black liquor is 12-20%; the weight percentage of hemicellulose in the black liquor is 1-3%;
[0011] S22: mixing the first batch of formaldehyde and the first batch of urea, and performing a first reaction under a first reaction condition to obtain a first product;
[0012] S23 adding phenol, carbonate and the black liquor to the first product, performing a second reaction under second reaction conditions to obtain a second product;
[0013] S24 adds a second batch of formaldehyde to the second product, and performs a third reaction under third reaction conditions to obtain a third product;
[0014] S25 cooling; adding the second batch of urea to the third product, performing a fourth reaction under the fourth reaction conditions to obtain a fourth product; cooling to obtain E NF Environmentally friendly wood adhesive.
[0015] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.
[0016] Preferably, in the aforementioned preparation method, the plant straw is selected from at least one of wheat straw, corn straw and rice straw, and has a length of 3 to 5 cm.
[0017] Preferably, in the aforementioned preparation method, the alkaline deconstruction is to disperse the plant straw in an alkaline solution and heat it; the ratio of the plant straw, alkali and water is 1g:0.14-0.18g:3-50mL, the heating temperature is 150-180°C, and the heating time is 90-120min.
[0018] Preferably, in the aforementioned preparation method, the alkali solution is a sodium hydroxide solution or a potassium hydroxide solution.
[0019] Preferably, in the aforementioned preparation method, the molar ratio of phenol, urea and formaldehyde is 1.0:1.0-1.4:3.5-4.0; the mass ratio of phenol to black liquor is 1.0:1.3-9.0;
[0020] The first reaction conditions are pH 7.5-8.5, temperature 80-90°C, and time 50-70 min;
[0021] The second reaction conditions are pH 10-13, temperature 80-90°C, and time 50-70 min;
[0022] The third reaction condition is a temperature of 80-90°C and a time of 50-70 min;
[0023] The fourth reaction condition comprises a pH value of 10 to 13, a temperature of 60 to 70° C., and a time of 30 to 40 minutes.
[0024] Preferably, in the aforementioned preparation method, the first batch of formaldehyde accounts for 60-90% of the total formaldehyde; and the first batch of urea accounts for 75-95% of the total urea.
[0025] Preferably, in the aforementioned preparation method, the carbonate is sodium carbonate and / or potassium carbonate; and the added amount of the carbonate is 1 to 5% by mass of the added amount of the phenol.
[0026] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. NF The environmentally friendly wood adhesive is prepared by the above-mentioned preparation method.
[0027] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. NF Application of environmentally friendly wood adhesive in the manufacture of multilayer boards.
[0028] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.
[0029] Preferably, in the aforementioned application, before applying the glue, the E NF Grade environmentally friendly wood adhesive and flour are mixed in a mass ratio of 1:0.25-0.35, and the viscosity of the glue after mixing is 20000-50000mPa·s.
[0030] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. According to a method for preparing a natural color paste proposed by the present invention, it comprises the following steps:
[0031] S81 decomposes plant straw by alkaline method to obtain cellulose-rich solid residue;
[0032] S82: the cellulose-rich solid residue is decomposed into fibers, namely, natural color pulp.
[0033] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions: A natural color paste proposed in the present invention is prepared by the above-mentioned preparation method.
[0034] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions: According to the present invention, an application of the above-mentioned natural color pulp in the field of paper manufacturing is proposed.
[0035] By means of the above technical scheme, the present invention provides a method for utilizing all components of plant straw, E NF The environmentally friendly wood adhesive, natural color paste and its preparation method and application have at least the following advantages:
[0036] The method for utilizing all components of plant straw proposed in the present invention solves the problem that the straw cannot be fully utilized and a large amount of waste liquid will be generated. By utilizing the alkaline environment in papermaking black liquor and the structural characteristics of hemicellulose and lignin, the black liquor with low solid content obtained after decomposition of alkali liquor does not need to be concentrated or hemicellulose removed, but is directly used for preparing E paper with good performance. NFThe invention discloses a grade-environmentally friendly wood adhesive and when the mass solid content of the adhesive is as low as 25%, it still has good bonding performance and suitable coating viscosity; compared with the technical requirement of phenolic resin solid content ≥35% in GB / T 14732-2017 "urea-formaldehyde, phenol-formaldehyde and melamine-formaldehyde resins for wood industry adhesives", the mass solid content of the adhesive is greatly reduced, saving a lot of economic costs; at the same time, the cellulose-rich solid residue obtained after alkaline decomposition contains trace alkali, and the present invention further enzymatically hydrolyzes the cellulose-rich solid residue to obtain a salt-containing sugar solution by acid-base neutralization means, which is beneficial to the subsequent further microbial conversion of the sugar to obtain polylactic acid and polyhydroxyalkanoate precursors, laying a foundation for the high value of all components of straw and truly waste-free utilization.
[0037] Furthermore, the present invention E NF The raw material of the environmentally friendly wood adhesive is directly used as unconcentrated papermaking black liquor for feeding reaction, wherein the papermaking black liquor contains low molecular weight carbohydrates, for example, hemicellulose-based sugar molecular structure, which contains a large number of hydroxyl groups so that it can combine with water to form hydrogen bonds, and has good film-forming properties, which can prevent the loss of water in the board and prolong the opening period of the multilayer board; according to a large number of experiments, the use of the E NF When the environmentally friendly wood adhesive is used to glue the boards, its opening period can be as long as 1.5 to 2 hours, which is much longer than the E NF The opening period of the environmentally friendly wood adhesive is about 0.5h, which greatly prolongs the construction period of the plywood. In addition, the low molecular weight carbohydrates in the papermaking black liquor, for example, the hemicellulose-based sugar molecule structure, can form an acetal structure with free formaldehyde, thereby reducing the formaldehyde release of the multi-layer board. NF Environmentally friendly wood adhesive with extremely low formaldehyde emission. The formaldehyde emission of plywood made from it can even be as low as 0.003mg / m 3 , in line with ENF level limit requirements.
[0038] Furthermore, the present invention E NF The raw material of the environmentally friendly wood adhesive is papermaking black liquor from grass plant straw. Its composition is different from that of wood papermaking black liquor. Grass crops contain high content of silicon. The silicon element in the black liquor after pulping mainly exists in the form of sodium silicate. The effect of sodium silicate on the adhesive can make the cured adhesive layer present an island structure, thereby enhancing the performance of the adhesive to a certain extent.
[0039] Furthermore, the present invention allows the cellulose-rich solid residue obtained after alkali decomposition to be only decomposed into fibers, which can be used as high-performance natural color pulp after washing, and the natural color paper prepared therefrom has good comprehensive performance; the above simple and waste-free process can promote the high-value utilization of all components of plant straw biomass, and will not produce any pollutants. In the foreseeable future, it is expected to be used for the high-value green industrial application of all alkaline components of plant straw.
[0040] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The figure is a schematic diagram of the process flow of the method for utilizing all components of plant straws of the present invention. DETAILED DESCRIPTION
[0042] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a method for utilizing all components of plant straw according to the present invention in combination with the accompanying drawings and preferred embodiments. NF The environmentally friendly wood adhesive, natural color paste, preparation method and application thereof, and the specific implementation, structure, characteristics and efficacy thereof are described in detail below. In the following description, different "one embodiment" or "embodiment" do not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics of one or more embodiments may be combined in any suitable form.
[0043] The present invention provides a method for utilizing all components of plant straw, such as Figure 1 As shown, it includes the following steps:
[0044] First, the plant straw is decomposed by alkali method, and then solid-liquid separation is carried out, wherein the solid phase component obtained is cellulose-rich solid residue, and the liquid phase component is black liquor containing hemicellulose and lignin.
[0045] In the above steps, the plant straw is preferably at least one of wheat straw, corn straw and rice straw; this is because the above-mentioned plant straws are different from wood, and grass crops contain high content of silicon. The silicon in the black liquor obtained after pulping is mainly in the form of sodium silicate, which has a significant effect on the performance of the adhesive, and can make the cured adhesive layer present an island-like structure, thereby enhancing the performance of the adhesive to a certain extent. In order to facilitate the effect of alkaline deconstruction, the present invention preferably pre-treats the plant straw before feeding it. The specific operation is to simply cut and screen the straw fiber raw material, and control its length to about 3 to 5 cm, so that it can fully contact and react with the alkali solution during alkaline deconstruction.
[0046] In the above steps, the alkaline deconstruction can be carried out by using the conventional alkaline pretreatment process in the technical field, as long as it can achieve the full separation of the cellulose component from the lignin and hemicellulose components in the plant straw. In order to ensure the technical effect of the alkaline deconstruction and fully dissolve the lignin and hemicellulose, the preferred alkaline deconstruction of the present invention is to disperse the plant straw in an alkali solution and heat it; the alkali solution is preferably a sodium hydroxide solution or a potassium hydroxide solution, or a mixed solution of sodium hydroxide and potassium hydroxide; the temperature of the alkali solution heating is preferably 150 to 180°C, and the heating time is preferably 90 to 120 minutes; under this reaction condition, the speed of the alkali dissolution reaction can be faster, and the full dissolution of lignin and hemicellulose can be ensured, so that the two are fully separated from cellulose.
[0047] Furthermore, in order to better promote the alkali dissolution reaction, it is preferred to make the ratio of various materials under a better ratio condition. The present invention preferably has the ratio of the plant straw, alkali and water as 1g: 0.14-0.18g: 3-50mL.
[0048] In the above steps, the black liquor containing hemicellulose and lignin is the uniqueness of the present invention. The technical solution of the present invention is different from the conventional operation of the prior art. Specifically, the present invention does not concentrate the liquid phase components of the alkali solution deconstruction to keep it at a low solid content level. Specifically, the present invention limits the mass solid content of the black liquor to 12-20%; at the same time, the present invention does not remove hemicellulose from the liquid phase components of the alkali solution deconstruction, but limits the mass percentage of hemicellulose in the black liquor to 1-3%. Such a setting can make the process steps of the technical solution of the present invention simple, avoid the concentration treatment and hemicellulose removal treatment of the liquid phase components of the alkali solution deconstruction, so that the process steps are simple, the cost is economical, and the efficiency is improved.
[0049] Then the solid phase components and liquid phase components are digested and utilized respectively. The specific instructions are as follows:
[0050] On the one hand, the solid phase component obtained in the above steps, i.e., the cellulose-rich solid residue, is subjected to simple acid-base neutralization, and optionally, is subjected to physical grinding, crushing on a cell crusher and / or ball milling in a ball mill. The above-mentioned treatment methods can be used alone or in combination, so as to obtain a variety of cellulose-rich solid residues; then, the above-mentioned various cellulose-rich solid residues are added to a sodium acetate buffer, and cellulose hydrolase is added thereto, and the enzymatic hydrolysis conditions are: the amount of cellulose-rich solid residue is 300 mg, and the amount of cellulase is 0.15-0045 FPU; then, enzymatic hydrolysis is carried out at about 50° C. for about 72 hours, firstly, it is subjected to enzymatic saccharification to form a salt-containing glucose solution, and then the salt-containing glucose solution is subjected to microbial transformation to prepare polylactic acid and polyhydroxyalkanoate precursors; the digestion and utilization method of the above-mentioned cellulose-rich solid residue can be carried out using conventional process conditions in the technical field, and the present invention does not specifically limit it, but is only exemplified and does not constitute a specific limitation of the present invention. It can be seen from the performance tests of specific embodiments 1 to 3 of the present invention that the cellulose enzymatic hydrolysis rate in the above technical solution is as high as over 92%.
[0051] In addition, the cellulose-rich solid residue can be decomposed and washed to obtain natural color pulp, which can then be transported to a papermaking pool for papermaking to be processed into natural color paper. The papermaking process is a common industrial process and will not be described in detail in this application.
[0052] The process of processing the above-mentioned cellulose-rich solid residue into natural color pulp and natural color paper in the present invention shows that: as shown in Example 4, the cellulose-rich solid residue obtained by simple alkaline decomposition can be decomposed to obtain natural color pulp, which can also be used for the production of high-quality natural color paper, and the performance of paper made therefrom is higher than that of the natural color paper and bleached paper of the other two manufacturers on the market, as shown in Table 2 for details.
[0053] On the other hand, the liquid-solid components obtained in the above steps, i.e., the black liquor containing hemicellulose and lignin, are directly used as raw materials to react with phenol, urea and formaldehyde to prepare E NF This step is the most critical innovation in the inventive concept of the present invention. Through the technical solution of the present invention, not only can the process steps of the technical solution of the present invention be simple, but also the concentration treatment of the liquid phase component of the alkali solution deconstruction and the removal of hemicellulose can be avoided, so that the process steps are simple, the cost is economical, and the efficiency is improved; more surprisingly, the E prepared by the technical solution of the present invention NF The environmentally friendly wood adhesive can still have good gluing performance and suitable coating viscosity when its mass solid content is as low as 25%; at the same time, the E NFWhen the environmentally friendly wood adhesive is used to glue the boards, its opening period can be as long as 1.5 to 2 hours, which is much longer than the E NF The environmentally friendly wood adhesive has an opening period of about 0.5h; the E NF The reason why the environmentally friendly wood adhesive has a long opening period is that there are low molecular weight carbohydrates in the papermaking black liquor, and the carbohydrates in the black liquor contain a large number of hydroxyl groups, which can form hydrogen bonds with water and have good film-forming properties, which can prevent the loss of water in the board and extend the opening period of the multilayer board. In addition, the presence of carbohydrates in the papermaking black liquor can also form acetal structures with free formaldehyde, thereby reducing the formaldehyde release of the multilayer board. NF Environmentally friendly wood adhesive with extremely low formaldehyde emission. The formaldehyde emission of plywood prepared by it can be as low as 0.003mg / m 3 , in accordance with E NF Level limit requirements.
[0054] The following is the preparation of E using black liquor as raw material NF The preparation method of the environmentally friendly wood adhesive is described in detail.
[0055] The present invention proposes an E NF Preparation method of environmentally friendly wood adhesive, as shown in the following Figure 1 As shown, it includes the following steps:
[0056] First, the plant straw is deconstructed by alkali method, and the solid-liquid separation is performed to obtain black liquor containing hemicellulose and lignin; the black liquor is low-solid content black liquor that has not been concentrated after alkali treatment, and its mass solid content is 12-20%; the mass percentage of hemicellulose in the black liquor is 1-3%; the black liquor used in this step is different from the treatment and application of black liquor in the prior art. The present invention does not concentrate the black liquor, nor remove the hemicellulose in the black liquor, but makes full use of the alkaline environment in the black liquor, as well as the structural characteristics of hemicellulose and lignin, and directly uses the black liquor as a raw material for E NF In the preparation of environmentally friendly wood adhesive, a low-solid content E NF Grade environmentally friendly wood adhesive; E prepared by the technical solution of the present invention NF The environmentally friendly wood adhesive has an extremely low solid content. When its mass solid content is as low as 25%, it still has good construction performance and bonding performance, and the formaldehyde emission is extremely low. The formaldehyde emission of the plywood prepared by it can even be as low as 0.003mg / m 3 ; Its solid content is far lower than the technical requirement of phenolic resin solid content ≥35% in GB / T14732-2017 "Urea-formaldehyde, phenol-formaldehyde and melamine-formaldehyde resins for wood industry adhesives", which greatly saves the cost of adhesives.
[0057] Secondly, raw materials are weighed according to a preset formula; the raw materials include formaldehyde, urea, phenol and carbonate in addition to the above-mentioned black liquor; wherein, formaldehyde adopts a formaldehyde solution with a mass concentration of 37%; carbonate acts as a catalyst and can be sodium carbonate and / or potassium carbonate; when the added amount of carbonate is 1-5% of the added amount of phenol by mass, the catalytic reaction effect is better; in the preparation process of the present invention, formaldehyde and urea are added in two batches, wherein the mass of the first batch of urea is 75-95% of the total mass of urea, and the mass of the first batch of formaldehyde is 60-90% of the total mass of formaldehyde; the present invention uses urea hydroxymethylation reaction as a starting point to generate hydroxymethyl urea; after adding papermaking black liquor, along with the hydroxymethylation process of lignin and hemicellulose, the generated hydroxymethylated substance is subjected to condensation reaction with the generated hydroxymethyl phenol under alkaline conditions, so as to achieve effective copolymerization at the molecular level and obtain a co-condensation resin with excellent performance. The present invention proposes a technical idea of gradually controlling the addition and condensation processes through multi-stage reactions in a multi-reaction system, gradually assembling the co-condensation resin molecules to synthesize an adhesive, which can better control the co-condensation of lignin, hemicellulose, phenol, urea and formaldehyde at the molecular level. The obtained co-condensation resin adhesive has stable properties, strength that meets the national Class I board strength requirements, extremely low formaldehyde emission, a wide range of applications, low adhesive production costs, and great commercial potential.
[0058] E NF The process steps of environmentally friendly wood adhesive are as follows:
[0059] The first step is to mix the first batch of formaldehyde and the first batch of urea, and carry out a first reaction under the first reaction conditions to obtain a first product. The reaction in this step is mainly a hydroxymethylation reaction of urea and formaldehyde to generate hydroxymethyl urea for the co-condensation in the subsequent step three; according to a large number of experimental verifications, the preferred first reaction conditions are pH 7.5-8.5, temperature 80-90°C, and time 50-70 minutes.
[0060] The second step is to add phenol, carbonate and the black liquor to the first product, so that it undergoes a second reaction under the second reaction conditions to obtain a second product. The reactions carried out in this step mainly include two types, one is the nucleophilic addition reaction between formaldehyde and phenol to generate hydroxymethylphenol, and the other is the nucleophilic addition reaction and aldol condensation reaction between formaldehyde and lignin and hemicellulose in the black liquor. The hydroxymethylphenol generated in this step and the products of the nucleophilic addition and aldol condensation reactions of lignin and hemicellulose are all used for the co-condensation in the subsequent step three; according to a large number of experimental verifications, the preferred second reaction conditions are pH 10-13, temperature 80-90°C, and time 50-70min.
[0061] The third step is to add a second batch of formaldehyde to the second product, so that it undergoes a third reaction under the third reaction conditions to obtain a third product. The reaction carried out in this step is mainly a co-condensation reaction between the monomers and oligomers, so that the molecular weight increases and the viscosity of the system increases; the oligomers described here include both the hydroxymethyl urea generated in the first reaction and the products of the nucleophilic addition and aldol condensation of hydroxymethyl phenol and formaldehyde with lignin generated in the second reaction; according to a large number of experimental verifications, the preferred third reaction conditions are a temperature of 80 to 90°C and a time of 50 to 70 minutes. Compared with the prior art, the present invention further simplifies the number of formaldehyde additions, and only adopts the method of adding formaldehyde twice. By adjusting the reaction temperature at each stage, the influence of carbohydrates in black liquor on the synthesis of co-condensation resin is reduced, so that formaldehyde can fully participate in hydroxymethylation and co-condensation reactions.
[0062] The fourth step is to cool the reaction system to 60-70° C.; then add the second batch of urea to the third product to carry out a fourth reaction under fourth reaction conditions to obtain a fourth product; the reaction in this step is mainly a reaction between urea and free formaldehyde to generate low molecular weight substituted urea to reduce the content of free formaldehyde; according to a large number of experimental verifications, the preferred fourth reaction conditions are a pH value of 10-13 and a temperature time of 30-40 minutes.
[0063] Finally, cool down and get E NF Environmentally friendly wood adhesive.
[0064] In the above technical scheme, through a large number of experiments, it is preferred that the molar ratio of the raw materials phenol, urea and formaldehyde is 1.0:1.0-1.4:3.5-4.0, and the mass ratio of phenol to black liquor is 1.0:1.3-9.0. NF Grade environmentally friendly wood adhesive has better effect.
[0065] The present invention also proposes an E NF Grade environmentally friendly wood adhesive, which is prepared by the above-mentioned preparation method; the E NF The environmentally friendly wood adhesive has good construction performance and bonding performance when the solid content is as low as 25%, and the formaldehyde emission is extremely low. The formaldehyde emission of plywood prepared by it can even be as low as 0.003mg / m 3 ; Its solid content is far lower than the technical requirement of phenolic resin solid content ≥35% in GB / T 14732-2017 "Urea-formaldehyde, phenol-formaldehyde and melamine-formaldehyde resins for wood industry adhesives", which greatly saves the cost of adhesives.
[0066] The present invention also proposes a method according to the aforementioned E NFThe application of environmentally friendly wood adhesive in the field of multilayer board manufacturing. The multilayer board can be selected from plywood, particle board, fiberboard, high-end template, floor substrate and E NF Any type of furniture board can achieve good technical results.
[0067] Before gluing the above multilayer board, first NF Grade environmentally friendly wood adhesive and flour are mixed in a mass ratio of 1:0.25-0.35, and the viscosity of the glue solution after mixing is controlled to be 20000-50000 mPa·s. The technical purpose of such setting is not only to enable the adhesive to form a continuous and dense adhesive layer, but also not to affect its processing performance, and the adhesive has excellent leveling performance; in addition, the adhesive prepared by the present invention can be cured at 130°C, has the characteristics of short curing time, controllable viscosity, and excellent performance, and is suitable for the production of plywood, particleboard, fiberboard, etc.; in the subsequent embodiments and comparative examples, the hot pressing temperature of the plywood is 130°C, the hot pressing time is 1.5 min / mm, and the hot pressing pressure is 1 MPa, which will not affect the secondary pressing and hot pressing efficiency of the plywood.
[0068] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0069] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.
[0070] Example 1
[0071] 1) Simply cut the wheat straw fiber raw material to control its length to about 3 to 5 cm;
[0072] 2) Alkali deconstruction: Add 162g of sodium hydroxide and 5000mL of water to 1000g of straw raw material in step 1), heat to 160°C, and then keep warm for 90 minutes for reaction. After the reaction, a mixed slurry is obtained, and cellulose-rich solid residue and black liquor are obtained by filtration; wherein, the wheat straw black liquor of this embodiment has a mass solid content of 15.7%, an alkali amount of 0.5mol / L, a mass percentage of acid-insoluble lignin of 7.5%, a mass percentage of acid-soluble lignin of 0.29%, a mass percentage of ash of 6.11%, and a mass percentage of hemicellulose of 1.80%, wherein the ash includes other components such as silicon;
[0073] 3) Add 2 mol / L hydrochloric acid solution to the cellulose-rich solid residue obtained in step 2) and mix until the pH value is 7; add it to a sodium acetate buffer solution (pH=4.8) to form a cellulose-rich solid residue buffer solution with a solid-liquid ratio of 2 wt%; then add 0.15 FPU of cellulose hydrolase thereto and perform enzymatic hydrolysis at 50° C. for 72 h; detect the cellulose enzymatic hydrolysis rate in wt%, and the results are shown in Table 1;
[0074] 4) The black liquor obtained in step 2) is directly made into E NF Grade environmentally friendly wood adhesive, the specific steps are as follows:
[0075] 4-1) Add 13.4 g of urea and 51.1 g of formaldehyde solution into a reaction vessel equipped with a thermometer, a stirrer and a reflux device, mix well, adjust the pH to 7.5 with a 10% mass concentration of NaOH solution, slowly heat the reaction solution to 80° C., and react at a constant temperature for 50 min to obtain a first-stage reaction product;
[0076] 4-2) adding 28 g of phenol, 0.6 g of sodium carbonate and 145.6 g of wheat pulping black liquor to the reaction system, adjusting the pH of the reaction system to 12.0, and reacting at a constant temperature of 85° C. for 70 min to obtain a second-stage reaction product;
[0077] 4-3) adding 34 g of the second batch of formaldehyde to the second stage reaction product, and reacting at 80° C. for 50 min to obtain the third stage reaction product;
[0078] 4-4) The reaction system was cooled to 60° C., 4.4 g of the second batch of urea was added, the pH was adjusted to 10.0 with a 30% NaOH solution, and the reaction was continued at a constant temperature for 30 min to obtain a fourth-stage reaction product;
[0079] 4-5) Cooling the fourth stage reaction product to below 40° C. to obtain wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive, namely E NF Environmentally friendly wood adhesive.
[0080] 5) Preparation of multi-layer plywood:
[0081] Before gluing, the glue is mixed in a ratio of adhesive to flour of 1:0.25. After mixing, the viscosity is 20000mPa·s, and the opening period of the multilayer plywood is 1.7h. Hot pressing is carried out according to the following process conditions: the hot pressing temperature of the plywood is 130℃, the hot pressing time is 1.5min / mm, and the hot pressing pressure is 1MPa.
[0082] The various properties of the wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive in this embodiment were tested, and the results are listed in Table 1; the wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive prepared in this embodiment was used to press a poplar three-layer plywood, and its properties were tested, and the results are listed in Table 1.
[0083] Example 2
[0084] 1) Simply cut the corn straw fiber raw material to control its length to about 3 to 5 cm;
[0085] 2) Alkali deconstruction: Add 180g sodium hydroxide and 5000mL water to 1000g straw raw material in step 1), heat to 160°C, and then keep warm for 90 minutes for reaction. After the reaction, a mixed slurry is obtained, and cellulose-rich solid residue and black liquor are obtained by filtration; wherein, the corn black liquor of this embodiment has a mass solid content of 12.00%, an alkali content of 0.35mol / L, a mass percentage of acid-insoluble lignin of 5.5%, a mass percentage of acid-soluble lignin of 0.18%, a mass percentage of ash of 5.10%, and a mass percentage of hemicellulose of 1.22%, wherein the ash includes other components such as silicon;
[0086] 3) Add 2 mol / L hydrochloric acid solution to the cellulose-rich solid residue obtained in step 2) and mix to make the pH value 7; grind it in a mortar for 20 minutes; add it to a sodium acetate buffer solution (pH=4.8) to form a cellulose-rich solid residue buffer solution with a solid-liquid ratio of 2 wt%; then add 0.15 FPU of cellulose hydrolase thereto, and perform enzymatic hydrolysis at 50° C. for 72 hours; detect the cellulose enzyme hydrolysis rate, unit wt%, the results are shown in Table 1;
[0087] 4) The black liquor obtained in step 2) is directly made into E NF Grade environmentally friendly wood adhesive, the specific steps are as follows:
[0088] 4-1) Add 17.9 g of urea and 63 g of formaldehyde solution into a reaction vessel equipped with a thermometer, a stirrer and a reflux device, mix well, adjust the pH to 7.5 with a 10% mass concentration of NaOH solution, slowly heat the reaction solution to 90° C., and react at a constant temperature for 70 minutes to obtain a first-stage reaction product;
[0089] 4-2) adding 28 g of phenol, 0.5 g of potassium carbonate and 36.4 g of corn pulping black liquor to the reaction system, adjusting the pH of the reaction system to 10.0, and reacting at a constant temperature of 85° C. for 60 min to obtain a second-stage reaction product;
[0090] 4-3) adding 27 g of the second batch of formaldehyde to the second stage reaction product, and reacting at 90° C. for 50 min to obtain the third stage reaction product;
[0091] 4-4) The reaction system was cooled to 60° C., 3.7 g of the second batch of urea was added, the pH was adjusted to 12.5 with a 30% NaOH solution, and the reaction was continued at a constant temperature for 30 min to obtain a fourth-stage reaction product;
[0092] 4-5) Cooling the fourth stage reaction product to below 40° C. to obtain corn pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive, namely E NF Environmentally friendly wood adhesive.
[0093] 5) Preparation of multi-layer plywood:
[0094] Before gluing, the glue is mixed in a ratio of adhesive to flour of 1:0.28. After mixing, the viscosity is 33000mPa·s, and the opening period of the multilayer plywood is 2h. Hot pressing is carried out according to the following process conditions: the hot pressing temperature of the plywood is 130℃, the hot pressing time is 1.5min / mm, and the hot pressing pressure is 1MPa.
[0095] The various properties of the corn pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive in this embodiment were tested, and the results are listed in Table 1; the corn pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive prepared in this embodiment was used to press a poplar three-layer plywood, and its properties were tested, and the results are listed in Table 1.
[0096] Example 3
[0097] 1) Simply cut the rice straw fiber raw material to control its length to about 3 to 5 cm;
[0098] 2) Alkali deconstruction: Add 140g sodium hydroxide and 3000mL water to 1000g straw raw material in step 1), heat to 180°C, and then keep warm for 90 minutes to react. After the reaction, a mixed slurry is obtained, and cellulose-rich solid residue and black liquor are obtained by filtration; wherein, the straw black liquor of this embodiment has a mass solid content of 18.2%, an alkali content of 0.6mol / L, a mass percentage of acid-insoluble lignin of 9.00%, a mass percentage of acid-soluble lignin of 0.35%, a mass percentage of ash of 6.55%, and a mass percentage of hemicellulose of 2.3%, wherein the ash includes other components such as silicon;
[0099] 3) The cellulose-rich solid residue obtained in step 2) was subjected to simple acid-base neutralization, and then crushed by a cell crusher to reduce the fiber viscosity; the residue was added to a sodium acetate buffer solution (pH=4.8) to form a cellulose-rich solid residue buffer solution with a solid-liquid ratio of 2 wt%; 0.15 FPU of cellulose hydrolase was added thereto, and the solution was hydrolyzed at 50° C. for 72 h; the cellulose hydrolysis rate was detected, and the results were shown in Table 1 in wt%;
[0100] 4) The black liquor obtained in step 2) is directly made into E NF Grade environmentally friendly wood adhesive, the specific steps are as follows:
[0101] 4-1) Add 22.7 g of urea and 72 g of formaldehyde solution into a reaction vessel equipped with a thermometer, a stirrer and a reflux device, mix well, adjust the pH to 8.0 with a 10% mass concentration of KO H solution, slowly heat the reaction solution to 85° C., and react at a constant temperature for 60 min to obtain a first-stage reaction product;
[0102] 4-2) adding 28 g of phenol, 1.4 g of sodium carbonate and 204.4 g of rice straw pulping black liquor to the reaction system, adjusting the pH of the reaction system to 11.0, and reacting at a constant temperature of 80° C. for 50 min to obtain a second-stage reaction product;
[0103] 4-3) adding 18 g of the second batch of formaldehyde to the second stage reaction product, and reacting at 85° C. for 70 min to obtain a third stage reaction product;
[0104] 4-4) The reaction system was cooled to 70° C., 2.5 g of the second batch of urea was added, the pH was adjusted to 11.0 with a 30% NaOH solution, and the reaction was continued at a constant temperature for 30 min to obtain a fourth-stage reaction product;
[0105] 4-5) Cooling the fourth stage reaction product to below 40° C. to obtain a straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive, namely, E of the present invention. NF Environmentally friendly wood adhesive.
[0106] 5) Preparation of multi-layer plywood:
[0107] Before gluing, the glue was mixed in a ratio of adhesive to flour of 1:0.32. The viscosity after mixing was 42000 mPa·s, and the opening period of the multilayer plywood was 1.9 h. Hot pressing was carried out according to the following process conditions: the hot pressing temperature of the plywood was 130°C, the hot pressing time was 1.5 min / mm, and the hot pressing pressure was 1 MPa.
[0108] The various properties of the straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive in this embodiment were tested, and the results are listed in Table 1; the straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive prepared in this embodiment was used to press a poplar three-layer plywood, and its properties were tested, and the results are listed in Table 1.
[0109] Example 4
[0110] 1) Simply cut the wheat straw fiber raw material to control its length to about 3 to 5 cm;
[0111] 2) Alkali deconstruction: Add 162g of sodium hydroxide and 3000mL of water to 1000g of straw raw material in step 1), heat to 150°C, and then keep warm for 120min to react. After the reaction, a mixed slurry is obtained, and cellulose-rich solid residue and black liquor are obtained by filtration; wherein, the wheat straw black liquor of this embodiment has a solid content of 20.00%, an alkali content of 0.65mol / L, an acid-insoluble lignin content of 9.20%, an acid-soluble lignin content of 0.37%, an ash content of 7.43%, and a hemicellulose content of 3.00%, wherein the ash includes other components such as silicon;
[0112] 3) Wash the cellulose-rich solid residue obtained in step 2) to obtain natural color pulp; then use the natural color paper production line to produce natural color paper, and the natural color paper sample is numbered as C1. At the same time, wheat straw bleached paper and bamboo pulp natural color paper purchased from two other manufacturers on the market are used as controls, numbered as K1 and K2, and paper performance tests are carried out under the same conditions. The specific results are shown in Table 2;
[0113] 4) The black liquor obtained in step 2) is directly made into E NF Grade environmentally friendly wood adhesive, the specific steps are as follows:
[0114] 4-1) Add 23.94 g of urea and 85.41 g of formaldehyde solution into a reaction vessel equipped with a thermometer, a stirrer and a reflux device, mix well, adjust the pH to 8.5 with a 10% mass concentration of NaOH solution, slowly heat the reaction solution to 90° C., and react at this temperature for 50 min to obtain a first-stage reaction product;
[0115] 4-2) adding 28 g of phenol, 0.4 g of potassium carbonate and 252 g of wheat pulping black liquor to the reaction system, adjusting the pH of the reaction system to 13.0, and reacting at a constant temperature of 90° C. for 60 min to obtain a second-stage reaction product;
[0116] 4-3) adding 9.49 g of the second batch of formaldehyde to the second stage reaction product, and reacting at 80° C. for 60 min to obtain the third stage reaction product;
[0117] 4-4) The reaction system was cooled to 65° C., 1.26 g of the second batch of urea was added, the pH was adjusted to 13.0 with a 30% NaOH solution, and the reaction was continued at a constant temperature for 40 min to obtain a fourth-stage reaction product;
[0118] 4-5) Cooling the fourth stage reaction product to below 40° C. to obtain wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive, namely E NF Environmentally friendly wood adhesive.
[0119] 5) Preparation of multi-layer plywood:
[0120] Before gluing, the glue is mixed in a ratio of adhesive to flour of 1:0.35. After mixing, the viscosity is 50000 mPa·s, and the opening period of the multilayer plywood is 1.5 h. Hot pressing is carried out according to the following process conditions: the hot pressing temperature of the plywood is 130°C, the hot pressing time is 1.5 min / mm, and the hot pressing pressure is 1 MPa.
[0121] The various properties of the wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive in this embodiment were tested, and the results are listed in Table 1; the wheat straw pulping black liquor-phenol-urea-formaldehyde co-condensation resin adhesive prepared in this embodiment was used to press a poplar three-layer plywood, and its properties were tested, and the results are listed in Table 1.
[0122] Table 1 Performance test data of each embodiment
[0123]
[0124] Table 2 Performance results of the natural paper in Example 4 and the natural paper and bleached paper on the market
[0125]
[0126]
[0127] In the above embodiment, E NF The solid content, viscosity and pH of the environmentally friendly wood adhesive are tested in accordance with the requirements of GB / T 14074-2017.
[0128] In the above embodiment, the plywood used is a poplar three-layer plywood, and the glue content of the veneer is 280-316g / m 2 The hot pressing temperature is 130°C, the hot pressing pressure is 1MPa, and the hot pressing time is 90s / mm.
[0129] Testing of the above plywood: The pressed plywood was placed at room temperature for 5 to 7 days before testing. The bonding strength of the adhesives prepared in Examples 1 to 4 was measured according to GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels"; the formaldehyde emission was tested according to the climate chamber method specified in GB / T 39600-2021 "Classification of formaldehyde emission of wood-based panels and their products".
[0130] In the above embodiment, the method for detecting the opening period of the multilayer board is to apply the mixed adhesive to the single board, i.e., the assembly, and the maximum time that the single board can be left before the adhesive dries.
[0131] In the above examples, the results of the cellulose hydrolysis rate were calculated by measuring the monosaccharide content using high performance liquid chromatography.
[0132] It can be seen from the test data in Table 1 that the enzymatic saccharification rate of the plant straw cellulose-rich solid residue provided by the present invention is higher than 90%, which can achieve effective utilization of the cellulose-rich solid residue; in addition, the obtained plant straw cellulose-rich solid residue can also be used to prepare natural paper, and its various properties are higher than those of commercially available natural paper and bleached paper, which can achieve effective utilization and diversified utilization of cellulose-rich solid residue. NF The environmentally friendly wood adhesive has good performance even when the solid content is as low as 25%, which can not only make the black liquor fully utilized, but also avoid the process of black liquor concentration and hemicellulose removal, and can also greatly save the raw material cost of the adhesive, and has good economic value; and the E NF The environmentally friendly wood adhesive is mixed with flour to a suitable viscosity and then applied by brushing. It has good construction performance and an opening period of up to 1.5 to 2 hours, which is very conducive to glue mixing construction. The plywood prepared by it has a bonding strength that meets the standard requirements of Class II boards (≥0.7MPa) specified in GB / T 9846-2004 "General Technical Conditions for Ordinary Plywood"; the formaldehyde emission of the prepared plywood is <0.0025mg / m 3 , with excellent environmental protection.
[0133] It can be seen from the test data in Table 2 that the plant straw cellulose-rich solid residue provided by the present invention is deflagrated, that is, it becomes natural color pulp after washing, and is used to prepare natural color paper. Compared with the natural color paper and bleached paper purchased on the market, the natural color paper has excellent comprehensive performance, especially in terms of folding endurance, ring crush, ring crush strength index, burst resistance, tensile strength and tensile index, thereby achieving effective utilization of the cellulose-rich solid residue.
[0134] From the above, it can be seen that the present invention obtains a cellulose-rich solid residue that is easily hydrolyzed and saccharified by enzymes and can be used to prepare high-performance natural color pulp and natural color paper, and a black liquor for high performance and low formaldehyde release through a simple alkaline deconstruction; the adhesive prepared using the black liquor has good performance when used in the production and manufacture of multilayer boards; at the same time, the pulping black liquor, a by-product of biomass refining, is also reasonably utilized; in the entire utilization process, not only the high-value utilization of all components of biomass is achieved, but also no waste liquid is discharged, which has great economic, social and sustainable development benefits.
[0135] The technical features in the claims and / or the specification of the present invention may be combined, and the combination is not limited to the combination obtained by reference in the claims. The technical solution obtained by combining the technical features in the claims and / or the specification is also within the protection scope of the present invention.
[0136] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for utilizing all components of plant straw, characterized in that: It includes the following steps: S11 alkaline decomposition of plant straw to obtain cellulose-rich solid residue and black liquor containing hemicellulose and lignin; the plant straw is selected from at least one of wheat straw, corn straw and rice straw; the mass solid content of the black liquor is 12-20%; the mass percentage of hemicellulose in the black liquor is 1-3%; S12: processing the cellulose-rich solid residue into natural color pulp, polylactic acid or polyhydroxyalkanoate precursor; reacting the black liquor with phenol, urea and formaldehyde to prepare E NF Grade environmentally friendly wood adhesive; It includes the following steps: Mixing the first batch of formaldehyde and the first batch of urea, and performing a first reaction under first reaction conditions to obtain a first product; the first batch of formaldehyde accounts for 60-90% of the total formaldehyde; the first batch of urea accounts for 75-95% of the total urea; the first reaction conditions are pH 7.5-8.5, temperature 80-90° C., and time 50-70 min; Add phenol, carbonate and the black liquor to the first product, and carry out a second reaction under second reaction conditions to obtain a second product; the second reaction conditions have a pH value of 10 to 13, a temperature of 80 to 90° C., and a time of 50 to 70 min; the mass ratio of the phenol to the black liquor is 1.0:1.3 to 9.0; the molar ratio of the phenol, urea and formaldehyde is 1.0:1.0 to 1.4:3.5 to 4.0; Adding a second batch of formaldehyde to the second product, and performing a third reaction under third reaction conditions to obtain a third product; the third reaction conditions are a temperature of 80 to 90° C. and a time of 50 to 70 min; Cooling; adding the second batch of urea to the third product, and performing a fourth reaction under the fourth reaction conditions to obtain a fourth product; the fourth reaction conditions have a pH value of 10 to 13, a temperature of 60 to 70° C., and a time of 30 to 40 min; cooling to obtain E NF Environmentally friendly wood adhesive.
2. A kind of E NF The method for preparing a grade environmentally friendly wood adhesive is characterized in that: It includes the following steps: S21: deconstructing the plant straw by alkaline method, separating the solid and the liquid, and obtaining black liquor containing hemicellulose and lignin; weighing the raw materials according to a preset formula; the weight solid content of the black liquor is 12-20%; the weight percentage of hemicellulose in the black liquor is 1-3%; S22: mixing the first batch of formaldehyde and the first batch of urea, and performing a first reaction under first reaction conditions to obtain a first product; the first batch of formaldehyde accounts for 60-90% of the total formaldehyde; the first batch of urea accounts for 75-95% of the total urea; the first reaction conditions are pH 7.5-8.5, temperature 80-90° C., and time 50-70 min; S23: adding phenol, carbonate and the black liquor to the first product, and performing a second reaction under second reaction conditions to obtain a second product; the second reaction conditions have a pH value of 10 to 13, a temperature of 80 to 90° C., and a time of 50 to 70 min; the mass ratio of the phenol to the black liquor is 1.0:1.3 to 9.0; the molar ratio of the phenol, urea and formaldehyde is 1.0:1.0 to 1.4:3.5 to 4.0; S24 adds a second batch of formaldehyde to the second product, and performs a third reaction under third reaction conditions to obtain a third product; the third reaction conditions are a temperature of 80 to 90° C. and a time of 50 to 70 min; S25 cooling; adding the second batch of urea to the third product, carrying out a fourth reaction under the fourth reaction conditions to obtain a fourth product; the fourth reaction conditions have a pH value of 10 to 13, a temperature of 60 to 70° C., and a time of 30 to 40 min; cooling to obtain E NF Environmentally friendly wood adhesive.
3. The preparation method according to claim 2, characterized in that: The length of the plant straw is 3 to 5 cm; the alkaline deconstruction is to disperse the plant straw in an alkaline solution and heat it; the ratio of the plant straw, the alkali and the water is 1 g: 0.14 to 0.18 g: 3 to 50 mL, the heating temperature is 150 to 180° C., and the heating time is 90 to 120 min.
4. The preparation method according to claim 2, characterized in that: The carbonate is sodium carbonate and / or potassium carbonate; the added amount of the carbonate is 1-5% of the added amount of the phenol by mass.
5. A kind of E NF Grade environmentally friendly wood adhesive, characterized in that: The invention is prepared by the preparation method according to any one of claims 2 to 4.
6. An E according to claim 5 NF Application of environmentally friendly wood adhesive in the manufacture of multilayer boards.
Citation Information
Cited By
Resin and gluing composition comprising it
FR3172508A1
Resin and sizing composition comprising same
WO2026176048A1