A low-dielectric alkali-soluble resin and its preparation method, and a negative photoresist composition.
By copolymerizing fluorinated acrylate, long-chain alkyl acrylate and carboxylated acrylate monomers, a low-dielectric alkali-soluble resin was prepared, which solved the problem of high dielectric constant of OC photoresist, realized the application of low-dielectric materials in OLED touch layer, reduced parasitic capacitance and improved screen performance.
Patent Information
- Application Number
- CN202611286301.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing OC photoresist resins have high dielectric constants, which cannot meet the dielectric constant requirements between the driving electrode and the receiving electrode of the OLED touch layer. Furthermore, traditional OC photoresist materials introduce significant parasitic capacitance problems under the conditions of large-size and high-refresh-rate OLED screens.
A low-dielectric, alkali-soluble resin is formed by copolymerizing fluorinated acrylate, long-chain alkyl acrylate, and carboxyl acrylate monomers. The resin is then covalently bonded to the polymer molecular backbone. By adjusting the polarity and molecular density, a low-dielectric-negative photoresist composition is prepared.
It effectively reduces the dielectric constant of the resin to 2.5~2.9, meeting the performance requirements of the dielectric in the TP structure, reducing parasitic capacitance, simplifying the TP structure manufacturing process, and improving the brightness and resolution of the OLED screen.
Smart Images

Figure SMS_25 
Figure QLYQS_1 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, and relates to a low dielectric alkali-soluble resin and its preparation method, as well as a negative photoresist composition. Background Technology
[0002] Organic light-emitting diodes (OLEDs) have become the core of next-generation display technologies due to their advantages such as self-illumination, high contrast, and flexibility. In the integrated structure of OLED devices, touch functionality is typically achieved by directly fabricating capacitive touch sensors (TPs) on the display panel. Currently, SiNx is used as the dielectric material for capacitive touch sensors due to its high transmittance and mature manufacturing process. SiNx is a dielectric material with a high dielectric constant (6-8), high breakdown field strength, and low dielectric loss, exhibiting excellent performance in terms of power consumption and signal-to-noise ratio. However, as OLED screen sizes continue to increase and refresh rates continue to improve, the drawbacks of SiNx dielectric materials in existing TP structures become significant. The parasitic resistance R and parasitic capacitance C introduced by the TP layer electrode structure increase, leading to a significant increase in the RC time constant of the sensor node. Limited by the actual size of the TP structure, the parasitic capacitance C can be reduced by lowering the dielectric constant of the dielectric material. Therefore, replacing the existing SiNx with a low dielectric constant and optically transparent dielectric material is the best choice to improve the frame scanning frequency of the TP structure in large-size OLED modules. The dielectric constant of the OC (Over Coating) photoresist used in the TP layer (3.3~4.0) is lower than that of SiNx, making it a promising dielectric material for the TP structure and simplifying the fabrication process.
[0003] However, conventional OC photoresists use photosensitive phenolic resins, which have a high molecular weight and many polar groups, resulting in strong intermolecular forces. This leads to a relatively high dielectric constant in the thin film formed after photolithography, which does not meet the requirements of TP structure dielectrics (ε≤3.0).
[0004] Therefore, the present invention uses fluorinated acrylic monomers, acrylic monomers with flexible chains, and carboxyl-containing acrylic monomers to copolymerize and obtain a low dielectric alkali-soluble acrylic resin, and then prepares a low dielectric negative photoresist composition to solve the problems existing in the prior art. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a low-dielectric, alkali-soluble resin and its preparation method, as well as a negative photoresist composition. This addresses the problem that traditional OC photoresists, due to the high intrinsic polarity of photosensitive phenolic resins, have a high dielectric constant, failing to meet the dielectric constant requirements between the driving and receiving electrodes of the OLED touch layer. The invention replaces traditional photosensitive phenolic resins by thermally polymerizing low-dielectric monomers into a low-dielectric resin. Fluorinated acrylate monomers, long-chain alkyl acrylate monomers, and carboxyl acrylate monomers are free-radical copolymerized, thereby covalently bonding these three functional monomers to the same polymer backbone, forming a homogeneous and functionally integrated copolymer structure. By adjusting the polarity and molecular density at the molecular structure level of the low-dielectric resin, the dielectric constant of the resin is reduced, while also ensuring the alkali solubility of the photoresist resin.
[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a low-dielectric alkali-soluble resin, the chemical formula of which is shown in formula (1): Equation (1); In formula (1), R1 is H or methyl, R2 is a fluorine-containing group, R3 is a hydrocarbon group, and R4 is a hydrocarbon group or an ester-containing alkyl group; in molar ratio, x:y:z=(20~50):(0~40):(20~50).
[0007] Specifically, the weight-average molecular weight (Mw) of the low-dielectric alkali-soluble resin is 5000~13000, preferably 7500~12000.
[0008] Specifically, R2 is one of the following: straight-chain, branched fluorinated alkyl, fluorinated ether, and fluorinated aryl groups containing fluorine atoms.
[0009] Specifically, R3 is one of the following: a straight-chain alkane, a branched-chain alkane, or a cycloalkane containing six or more carbon atoms.
[0010] Secondly, the present invention provides a method for preparing a low-dielectric alkali-soluble resin, wherein a fluorinated acrylate monomer A, a long-chain alkyl acrylate monomer B, and a carboxyl acrylate monomer C are added to a solvent in a molar ratio of (20~50):(0~40):(20~50) and mixed, and then a free radical initiator is added to carry out a copolymerization reaction at a reaction temperature of 60~90℃, thereby obtaining the low-dielectric alkali-soluble resin as described in any one of claims 1 to 4.
[0011] Specifically, the solvent is one of tetrahydrofuran, propylene glycol methyl ether acetate, propylene glycol methyl ether, ethyl acetate, n-butyl acetate, isobutyl acetate, methyl propionate, methyl ethyl ketone, and 2-heptanone.
[0012] Specifically, the free radical initiator includes one of azobisisobutyronitrile (preferably AIBN), azobisisoheptanenitrile, azobisisobutylamidine hydrochloride, cyclohexanone peroxide, benzoyl peroxide, and persulfate.
[0013] Specifically, the chemical formula of the fluorinated acrylate monomer A is shown in formula (2): Equation (2); The fluorinated acrylate monomer A provides a low-polarity fluorinated functional group and is a key monomer for achieving low dielectric properties. The fluorinated acrylate monomer A is preferably a monomer represented by the following formulas A1 to A10: Equation (A1) Formula (A1) is trifluoroethyl acrylate, CAS: 407-47-6; Equation (A2) Formula (A2) is perfluoroalkyl ethyl acrylate, CAS: 65605-70-1; Formula (A3) Formula (A3) is 3-trifluoroacetoxy-1-adamantyl methacrylate, CAS: 1151809-20-9; Equation (A4) Formula (A4) is perfluorooctyl ethyl acrylate, CAS: 27905-45-9; Formula (A5) Formula (A5) is octafluoroamyl acrylate, CAS: 376-84-1; Formula (A6) Formula (A6) is 1H,1H,7H-dodecylfluoroheptyl acrylate, CAS: 2993-85-3; Formula (A7) Formula (A7) is tridecylfluorooctyl acrylate, CAS: 17527-29-6; Formula (A8) Formula (A8) is 1H,1H,9H-hexadecylfluoroacrylate nonyl ester, CAS: 4180-26-1; Formula (A9) Formula (A9) is 2,2,3,3,4,4,5,5,6,6,7,7,7-tridecylfluoroheptyl acrylate, CAS: 559-11-5; Formula (A10) Formula (A10) is 1H,1H-2,5-bis(trifluoromethyl)-3,6-dioxaundefluorononyl acrylate, CAS: 17559-01-2.
[0014] Specifically, the chemical formula of the long-chain alkyl acrylate monomer B is shown in formula (3): Equation (3); The long-chain alkyl acrylate monomer B introduces low-density alkyl side chains, which reduces the inter-chain forces of the polymer, increases the molecular chain spacing and the free volume of the material, thus helping to reduce the resin density. This not only helps to further reduce the dielectric constant, but also improves the flexibility of the material. The long-chain alkyl acrylate monomer B is preferably a monomer represented by the following formulas B1 to B8: Formula (B1) Formula (B1) is isooctadecyl acrylate, CAS: 93841-48-6; Formula (B2) Formula (B2) is octadecyl methacrylate, CAS: 32360-05-7; Formula (B3) Formula (B3) is octadecyl acrylate, CAS: 4813-57-4; Equation (B4) Formula (B4) is hexadecyl acrylate, CAS: 13402-02-3; Formula (B5) Formula (B5) is tetradecyl acrylate, CAS: 21643-42-5; Formula (B6) Formula (B6) is dodecyl acrylate, CAS: 2156-97-0; Formula (B7) Formula (B7) is isodecyl acrylate, CAS: 1330-61-6; Formula (B8) Formula (B8) is isononyl acrylate, CAS: 51952-49-9.
[0015] Specifically, the chemical formula of the carboxyl-containing acrylate monomer C is shown in formula (4): Equation (4); The carboxyl-containing acrylate monomer C, by introducing carboxyl groups, ensures that the resulting acrylic resin is alkali-soluble, guaranteeing the photoresist's developability (the non-exposed areas of the photolithographic pattern are washed away by the alkaline developer), which is a basic requirement for photoresist resins. The carboxyl-containing acrylate monomer C is preferably represented by the following formulas C1 and C2: Formula (C1) Formula (C1) is carboxyethyl acrylate, CAS: 24615-84-7; Formula (C2) Formula (C2) is mono-2-(methacryloyloxy)ethyl maleate, CAS: 51978-15-5.
[0016] Thirdly, the present invention provides a negative photoresist composition, wherein, by weight, the raw materials of the negative photoresist composition include at least: 15-30 parts of a low dielectric alkali-soluble resin, 5-10 parts of a UV-crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS, purchased from DIC), 5-10 parts of a UV crosslinking agent, 0.1-5 parts of an adhesion promoter, 1-3 parts of a photoinitiator, 0.01-0.5 parts of a leveling agent, and 50-80 parts of a solvent.
[0017] Specifically, the UV crosslinking agent is a multifunctional acrylate monomer selected from one of pentaerythritol triacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane triacrylate.
[0018] Specifically, the adhesion promoter includes a silane coupling agent, including one of 3-(methacryloyloxy)propyltrimethoxysilane, methacryloyloxypropyltriethoxysilane, and 3-methacryloyloxypropylmethyldimethoxysilane.
[0019] Specifically, the photoinitiator includes oxime ester photoinitiators, and the oxime ester photoinitiator includes any one or both of OXE-01 and OXE-02. OXE-01 is 1-(4-phenylthiophenyl)-octane-1,2-dione-2-benzoic acid oxime ester (CAS No.: 253585-83-0), and OXE-02 is 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]acetophenone 1-(O-acetyl oxime) (CAS No.: 478556-66-0).
[0020] Specifically, the leveling agent is preferably an organosilicon or a fluorosurfactant. This includes RS-75 and EFS-321 sold by DIC; and BYK-300, BYK-301, BYK-306, BYK-310, BYK-313, BYK-320, BYK-366P, BYK-368P, and BYK-370 sold by BYK.
[0021] Specifically, the solvent is one of 3-methoxybutanol, diacetone alcohol, methyl ethyl ketone, cyclohexanone, N-methyl-2-pyrrolidone, diethylene glycol ethyl methyl ether, propylene glycol methyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, 3-methoxybutyl acetate, 3-methoxy-3-butyl acetate, and propylene glycol methyl ether acetate. For health and environmental reasons, propylene glycol methyl ether acetate is preferred.
[0022] Fourthly, the present invention provides an application of a negative photoresist composition, wherein the negative photoresist composition is subjected to slit coating / spin coating, vacuum desolventizing, pre-baking, exposure, development, and then heat post-treatment to form a colorless and transparent film with a target pattern.
[0023] Specifically, the negative photoresist composition is first coated onto a substrate (glass, silicon wafer, silicon nitride substrate, quartz substrate, Ti-containing glass substrate, or ITO film substrate) using a slit coater, spin coater, or roller coater. Then, the solvent is removed by VCD (vacuum solvent removal) for 120 seconds, followed by pre-baking to further remove the solvent, thereby forming a thin film with a thickness of 2~10μm, preferably 2~4μm; the pre-baking temperature is 70~100℃ and the baking time is 2~5 minutes. The obtained film is then subjected to UV exposure to obtain a colorless and transparent film with the target pattern. A mask with a specific pattern is mounted on an exposure machine and cross-linked and cured by UV irradiation. The film surface is then covered with a developing solution in a developing machine to dissolve unexposed areas. After development, the pattern is washed out with deionized water, and the surface is dried with nitrogen gas. The developing solution can be an aqueous solution of potassium hydroxide or sodium hydroxide, an aqueous solution of tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide, choline, or other quaternary ammonium hydroxides, or an alkaline aqueous solution of amines such as ethanolamine, propylamine, or ethylenediamine. TMAH developing solution is preferred.
[0024] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects: 1. This invention utilizes copolymerization of fluorinated acrylic monomers, long-chain alkyl acrylate monomers, and carboxyl acrylic monomers to prepare a low-dielectric, alkali-soluble resin. By introducing low-dielectric fluorinated functional groups and long-chain alkyl side chains into the resin side chains, a synergistic effect of polarity control and free volume adjustment is achieved, effectively reducing the resin's dielectric constant. The resulting negative photoresist material has a dielectric constant ε reduced to 2.5~2.9 (1MHz), meeting the performance requirement of ε≤3.0 for TP structure dielectrics. Compared to traditional acrylic phenolic resin systems, the dielectric performance of the photoresist (ε approximately 3.3~4.0) is significantly improved, and it is significantly lower than the SiNx dielectric material commonly used in existing TP layers. This material can replace SiNx as the dielectric layer of capacitive touch sensors, effectively reducing parasitic capacitance C, decreasing the RC time constant of sensor nodes, and overcoming the technical bottleneck of the TP structure frame scanning frequency being limited by dielectric materials in large-size, high-refresh-rate OLED modules.
[0025] 2. This invention introduces carboxyl groups into the resin molecular structure, thereby achieving low dielectric properties while imparting alkali solubility to the resin. This ensures the photolithography and development capabilities of the photoresist material, making it compatible with existing standard photolithography processes for OLED panels and meeting the process requirements for OC photoresist. It solves the problem of balancing low dielectric modification with photolithography performance.
[0026] 3. The low-dielectric material of the present invention belongs to the OC photoresist system and can be directly used as the dielectric layer of the TP structure. It does not require an additional independent deposition process for the SiNx dielectric layer, which simplifies the fabrication process of the TP structure and reduces the process complexity and preparation cost.
[0027] 4. The polymer film prepared by this invention also possesses the advantage of low refractive index; at a wavelength of 550 nm, the refractive index n can be reduced to 1.43~1.49, which is lower than that of traditional acrylic phenolic resin system photoresist materials (n approximately 1.51~1.53). This negative photoresist material can be combined with high refractive index OC photoresist materials to construct MLP (Micro Lens Panel) structures, effectively enhancing the light extraction efficiency of OLEDs and thus improving screen display brightness. Detailed Implementation
[0028] Exemplary embodiments will now be described in detail. The embodiments described below are not representative of all embodiments consistent with this invention. Rather, they are merely examples consistent with some aspects of the invention as detailed in the appended claims.
[0029] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to embodiments.
[0030] Preparation Example 1 This preparation example provides a method for preparing a low-dielectric, alkali-soluble resin, as detailed below: Trifluoroethyl acrylate (A2), isooctadecyl acrylate (B1), and carboxyethyl acrylate (C1) were added to propylene glycol methyl ether acetate solvent in a molar ratio of 30:20:20, and then azobisisobutyronitrile (AIBN) was added. The mixture was heated and stirred at 80°C under nitrogen protection to carry out the polymerization reaction. The reaction was stopped after the carbon-carbon double bonds in the reaction system disappeared by infrared detection. The resulting solution was then added dropwise to petroleum ether for precipitation, filtered, and then dissolved in acetone. The petroleum ether was then precipitated again, and this process was repeated three times. Finally, the mixture was placed in a vacuum drying oven at 30°C for 24 hours to obtain the desired low-dielectric alkali-soluble resin M1. The molecular weight (Mw) of the low-dielectric alkali-soluble resin M1 is 7500, and the dispersion index (PDI) is 2.2.
[0031] Preparation Example 2 The difference between this preparation example and Preparation Example 1 is that the fluorinated acrylate monomer A is perfluorooctyl ethyl acrylate (A4), the long-chain alkyl acrylate monomer B is octadecyl acrylate (B3), and the molar ratio of the three is 20:30:20. The low dielectric alkali soluble resin M2 prepared has a molecular weight Mw of 8500 and a dispersion index PDI of 2.2.
[0032] Preparation Example 3 The difference between this preparation example and Preparation Example 1 is that the fluorinated acrylate monomer A is 1H,1H,7H-dodecylfluoroheptyl acrylate (A6), the long-chain alkyl acrylate monomer B is tetradecyl acrylate (B5), and the carboxyl acrylate monomer C is mono-2-(methacryloyloxy)ethyl maleate (C2). The molar ratio of the three is 30:40:25. The resulting low dielectric alkali-soluble resin M3 has a molecular weight Mw of 8000 and a dispersion index PDI of 2.3.
[0033] Preparation Example 4 The difference between this preparation example and Preparation Example 1 is that the fluorinated acrylate monomer A is 1H,1H,7H-dodecylfluoroheptyl acrylate (A6), the long-chain alkyl acrylate monomer B is tetradecyl acrylate (B5), and the carboxyl acrylate monomer C is mono-2-(methacryloyloxy)ethyl maleate (C2). The molar ratio of the three is 30:30:30. The resulting low dielectric alkali-soluble resin M4 has a molecular weight Mw of 9000 and a dispersion index PDI of 2.1.
[0034] Preparation Example 5 The difference between this preparation example and Preparation Example 1 is that the fluorinated acrylate monomer A is 1H,1H,9H-hexadecylfluoroacrylate nonyl acrylate (A8), the long-chain alkyl acrylate monomer B is isodecyl acrylate (B7), and the carboxyl acrylate monomer C is mono-2-(methacryloyloxy)ethyl maleate (C2). The molar ratio of the three is 40:20:20. The resulting low dielectric alkali-soluble resin M5 has a molecular weight Mw of 9500 and a dispersion index PDI of 2.4.
[0035] Preparation Example 6 The difference between this preparation example and Preparation Example 1 is that the fluorinated acrylate monomer A is 1H,1H,9H-hexadecylfluoroacrylate nonyl ester (A8), and the carboxyl acrylate monomer C is maleic acid mono-2-(methacryloyloxy)ethyl ester (C2), with a molar ratio of 50:50. The resulting low dielectric alkali-soluble resin M6 has a molecular weight Mw of 12000 and a dispersion index PDI of 2.5.
[0036] Comparative Example 1 The difference between this comparative example and preparation example 1 is that the long-chain alkyl acrylate monomer B is tetradecyl acrylate (B5), and the carboxyl acrylate monomer C is mono-2-(methacryloyloxy)ethyl maleate (C2), with a molar ratio of 20:30. The resulting low-dielectric alkali-soluble resin D1 has a molecular weight Mw of 7500 and a dispersion index PDI of 2.3.
[0037] Comparative Example 2 The difference between this comparative example and preparation example 1 is that the fluorinated acrylate monomer A is 1H,1H,7H-dodecylfluoroheptyl acrylate (A6), the long-chain alkyl acrylate monomer B is tetradecyl acrylate (B5), and the carboxyl acrylate monomer C is mono-2-(methacryloyloxy)ethyl maleate (C2). The molar ratio of the three is 60:20:20. The resulting low dielectric alkali-soluble resin D2 has a molecular weight Mw of 8000 and a dispersion index PDI of 2.4.
[0038] Example 1 This embodiment provides an application of a negative photoresist composition, as detailed below: The negative photoresist composition, by weight, comprises the following raw materials: 30 parts of low-dielectric alkali-soluble resin (M1), 5 parts of UV-crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 10 parts of UV crosslinking agent, 5 parts of adhesion promoter, 2 parts of photoinitiator, 0.1 parts of leveling agent, and 70 parts of solvent. The above raw materials are added to a brown glass bottle and stirred until uniformly dispersed. The mixture is then filtered through a 0.2 μm pore size filter membrane to obtain the negative photoresist composition.
[0039] The UV crosslinking agent used is pentaerythritol triacrylate; the adhesion promoter used is 3-(methacryloyloxy)propyltrimethoxysilane; the photoinitiator used is OXE-01; the leveling agent used is BYK-310 from BYK; and the solvent used is propylene glycol methyl ether acetate.
[0040] A negative photoresist composition was spin-coated onto a silicon nitride substrate. After vacuum desolventizing for 2 minutes using a VCD, the composition was further desolventized by preheating at 85°C for 2 minutes on a hot stage, resulting in a film with a thickness of 2-4 μm. The negative photoresist composition was exposed using a GHI mixed-line exposure machine (mercury lamp light source) with a 2-40 μm square / gap pattern mask. Then, it was developed using an aqueous solution of tetramethylammonium hydroxide (2.38% TMAH developer), rinsed with deionized water, and finally, the developed film (patterned) was placed in an oven at 80-90°C for 60 minutes for further curing, resulting in a colorless and transparent film with the target pattern.
[0041] Example 2 The difference between this embodiment and Embodiment 1 is that it contains 20 parts of low dielectric alkali-soluble resin (M2), 10 parts of UV crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 5 parts of UV crosslinking agent, 0.1 parts of adhesion promoter, 1 part of photoinitiator, 0.5 parts of leveling agent, and 60 parts of solvent.
[0042] The UV crosslinking agent used is trimethylolpropane triacrylate; the adhesion promoter used is methacryloyloxypropyltriethoxysilane; the photoinitiator used is OXE-01; the leveling agent used is BYK-310 from BYK; and the solvent used is propylene glycol methyl ether acetate.
[0043] Example 3 The difference between this embodiment and Embodiment 1 is that it contains 15 parts of low dielectric alkali-soluble resin (M3), 5 parts of UV crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 8 parts of UV crosslinking agent, 1 part of adhesion promoter, 1.5 parts of photoinitiator, 0.2 parts of leveling agent, and 70 parts of solvent.
[0044] The UV crosslinking agent used is pentaerythritol tetraacrylate; the adhesion promoter used is 3-methacryloyloxypropylmethyldimethoxysilane; the photoinitiator used is OXE-01 (1 part) and OXE-02 (0.5 parts); the leveling agent used is BYK-313 from BYK Company; and the solvent used is propylene glycol methyl ether acetate.
[0045] Example 4 The difference between this embodiment and Embodiment 1 is that 15 parts of low dielectric alkali-soluble resin (M4), 5 parts of UV crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 10 parts of UV crosslinking agent, 4 parts of adhesion promoter, 2 parts of photoinitiator, 0.01 parts of leveling agent, and 80 parts of solvent are used.
[0046] The UV crosslinking agent used is dipentaerythritol pentaacrylate; the adhesion promoter used is 3-(methacryloyloxy)propyltrimethoxysilane; the photoinitiator used is OXE-01; the leveling agent used is BYK-320 from BYK; and the solvent used is propylene glycol methyl ether acetate.
[0047] Example 5 The difference between this embodiment and Embodiment 1 is that it contains 15 parts of low dielectric alkali-soluble resin (M5), 8 parts of UV crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 7 parts of UV crosslinking agent, 3 parts of adhesion promoter, 1.5 parts of photoinitiator, 0.3 parts of leveling agent, and 70 parts of solvent.
[0048] The UV crosslinking agent used is trimethylolpropane triacrylate ethoxylate; the adhesion promoter used is 3-(methacryloyloxy)propyltrimethoxysilane; the photoinitiator used is OXE-01; the leveling agent used is BYK-320 from BYK; and the solvent used is propylene glycol methyl ether.
[0049] Example 6 The difference between this embodiment and Embodiment 1 is that 15 parts of low dielectric alkali-soluble resin (M6), 10 parts of UV crosslinkable alkali-soluble resin (LUXYDIR V-5000-ZS), 5 parts of UV crosslinking agent, 3 parts of adhesion promoter, 3 parts of photoinitiator, 0.3 parts of leveling agent, and 50 parts of solvent are used.
[0050] The UV crosslinking agent used is dipentaerythritol hexaacrylate; the adhesion promoter used is 3-(methacryloyloxy)propyltrimethoxysilane; the photoinitiator used is OXE-02; the leveling agent used is BYK-370 from BYK; and the solvent used is 3-methoxybutylacetic acid ester.
[0051] Comparative Example 1 The difference between this comparative example and Example 1 is that the low dielectric alkali-soluble resin used in this comparative example is the low dielectric alkali-soluble resin (D1) prepared in the comparative example.
[0052] Comparative Example 2 The difference between this comparative example and Example 1 is that the low dielectric alkali-soluble resin used in this comparative example is the low dielectric alkali-soluble resin (D2) prepared in the comparative example.
[0053] Comparative Example 3 The difference between this comparative example and Example 1 is that this comparative example does not contain a low dielectric alkali-soluble resin.
[0054] Comparative Example 4 The difference between this comparative example and Example 1 is that 40 parts of low dielectric alkali-soluble resin (M1) were added to this comparative example.
[0055] Comparative Example 5 The difference between this comparative example and Example 3 is that this comparative example does not contain a UV-crosslinkable alkali-soluble resin.
[0056] Comparative Example 6 The difference between this comparative example and Example 3 is that 15 parts of a UV-crosslinkable alkali-soluble resin were added to this comparative example.
[0057] To further verify the effectiveness of the technical solution provided by the present invention, the following performance tests were performed on the films prepared in the above embodiments and comparative examples: (1) Dielectric constant: A 10cm×10cm×4μm (width×length×thickness) thin film was prepared on an ITO glass substrate. Except for the absence of a mask, the sample was prepared according to the method for forming the curing pattern. Then, a 100nm thick silver electrode of a specific area was vacuum-deposited on the surface of the thin film using an evaporation machine. The capacitance value was tested using an Agilent 4294A precision impedance analyzer at a test frequency of 1MHz. The dielectric constant was calculated using the following formula: ε = (C×d)⁄(ε0×S), where C, d, and S are the capacitance, thickness, and electrode area of the material, respectively; ε0 represents the vacuum dielectric constant, ε0 = 8.854×10 -12 F / m.
[0058] (2) Adhesion: Use a utility knife to score the film into a grid; apply 3M transparent tape to the grid and apply force to ensure the tape adheres firmly to the coating surface and the scored areas; visually inspect the coating peeling phenomenon and degree on the substrate to determine its ASTM level; the ASTM levels are as follows: The cut edges of 5B are smooth, and there is no peeling at the edges of the grid. 4B The peeling area within the edge grid zone is ≤ grid percentage; Within Zone 3B, the area of peeling within the gridded areas is greater than 5% to 15%; Within Zone 2B, the area of peeling within the gridded areas is greater than 15% to 35%; Within Zone 1B, the area of peeling within the gridded areas is greater than 35% to 65%; Within zone 0B, the peeling area within the gridded area is greater than 65%.
[0059] (3) Refractive index: A 5cm×5cm×1.5μm (width×length×thickness) thin film was formed on the upper surface of the glass substrate. Except for not using a mask, the sample was prepared according to the method of forming the curing pattern. An ellipsometer was used for testing and fitting. The wavelength corresponding to the refractive index value was selected as 550nm.
[0060] (4) Transmittance: A 5cm×5cm×2μm (width×length×thickness) thin film was formed on the upper surface of the glass substrate. Except for not using a mask, the sample was prepared according to the method of forming the curing pattern. The transmittance of the cured film in the visible light range of 380nm~800nm was measured by a UV-Vis spectrophotometer (U-3900Hitachi). The wavelength corresponding to the transmittance value was selected as 550nm.
[0061] (5) Resolution: The patterned photoresist film after photolithography is tested using a scanning electron microscope (SEM) to observe and measure the minimum linewidth CD (Critical Dimension) to evaluate its resolution capability; the minimum feature size that can be clearly and completely reproduced within ±10% of the mask design size is the resolution.
[0062] The test results are shown in Table 1.
[0063] Table 1 As shown in Table 1, the films corresponding to Examples 1 to 6 have low refractive index, low dielectric constant, and high light transmittance. Meanwhile, the adhesion is acceptable (3B to 4B), and the lithographic pattern has good resolution.
[0064] Conversely, Comparative Example 1's resin D1 is free of fluorine (F), resulting in higher dielectric and refractive indices. Comparative Example 2's low-dielectric, alkali-soluble resin has a high F content, leading to lower overall resin chain polarity, incompatibility with other acrylate monomers, hazy film surface, and reduced light transmittance. Simultaneously, low polarity weakens the interaction between the film and substrate molecules, worsening adhesion. Furthermore, a high F content makes the material more hydrophobic, hindering developer (TMAH aqueous solution) wetting and resulting in decreased resolution. Comparative Example 3's formulation is free of low-dielectric, alkali-soluble resin, resulting in higher dielectric and refractive indices. Comparative Example 4 has a high proportion of low-dielectric, alkali-soluble resin. Similar to Comparative Example 2, the low polarity of resin M1, when added in excess, leads to incompatibility with other acrylate monomers, causing film surface haze, affecting light transmittance, and also worsening resolution and adhesion. Comparative Example 5 lacked the UV-crosslinkable alkali-soluble resin V-5000-ZS, resulting in poor curing and adhesion. Furthermore, its reduced alkali solubility led to decreased resolution. Comparative Example 6, with its higher content of the UV-crosslinkable alkali-soluble resin V-5000-ZS, exhibited a higher dielectric constant and refractive index.
[0065] In summary, the thin film prepared by this invention has a low refractive index, a low dielectric constant, and a high transmittance. It also has acceptable adhesion, and the pattern after photolithography has good resolution, fully meeting the requirements for use in TP structure dielectrics.
[0066] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.
[0067] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A low-dielectric, alkali-soluble resin, characterized in that, Its chemical formula is shown in formula (1): Equation (1); In formula (1), R1 is H or methyl, R2 is a fluorine-containing group, R3 is a hydrocarbon group, and R4 is a hydrocarbon group or an ester-containing alkyl group; in molar ratio, x:y:z=(20~50):(0~40):(20~50).
2. The low-dielectric alkali-soluble resin according to claim 1, characterized in that, The weight-average molecular weight (Mw) of the low-dielectric alkali-soluble resin is 5000~13000.
3. The low-dielectric alkali-soluble resin according to claim 1, characterized in that, R2 is one of the following: straight-chain, branched fluorinated alkyl, fluorinated ether, or fluorinated aryl containing fluorine atoms.
4. The low-dielectric alkali-soluble resin according to claim 1, characterized in that, R3 is one of straight-chain alkanes, branched-chain alkanes, and cycloalkanes.
5. A method for preparing a low-dielectric, alkali-soluble resin, characterized in that, By copolymerizing fluorinated acrylate monomer A, long-chain alkyl acrylate monomer B, and carboxyl acrylate monomer C in a molar ratio of (20~50):(0~40):(20~50), a low dielectric alkali-soluble resin as described in any one of claims 1 to 4 is obtained.
6. The preparation method according to claim 5, characterized in that, The chemical formula of the fluorinated acrylate monomer A is shown in formula (2): Equation (2).
7. The preparation method according to claim 5, characterized in that, The chemical formula of the long-chain alkyl acrylate monomer B is shown in formula (3): Equation (3).
8. The preparation method according to claim 5, characterized in that, The chemical formula of the carboxyl-containing acrylate monomer C is shown in formula (4): Equation (4).
9. A negative photoresist composition, characterized in that, By weight, the raw materials include: 15-30 parts of the low dielectric alkali-soluble resin according to any one of claims 1 to 4, 5-10 parts of the alkali-soluble resin capable of UV crosslinking, 5-10 parts of the UV crosslinking agent, 0.1-5 parts of the adhesion promoter, 1-3 parts of the photoinitiator, 0.01-0.5 parts of the leveling agent, and 50-80 parts of the solvent.
10. The application of a negative photoresist composition, characterized in that, Based on the negative photoresist composition of claim 9, a colorless and transparent film with a target pattern is formed by slit coating / spin coating, vacuum desolventizing, pre-baking, exposure, development, and then heat post-treatment.