Antistatic and high wear-resistant polyurethane microporous elastomers, their preparation methods and applications
By introducing sulfonate-modified polyether ester polyols with side chains containing -SO3-Na+ into polyurethane materials and compounding them with imidazole ionic liquid antistatic agents, and by introducing a double-terminated monohydroxy organosilicon prepolymer into component B, the problems of decreased antistatic performance and poor wear resistance were solved, and the durability and wear resistance of antistatic polyurethane materials were improved.
Patent Information
- Application Number
- CN202611618660.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing antistatic polyurethane materials exhibit decreased antistatic properties after prolonged use, and the poor compatibility between silicone and polyurethane leads to a decline in wear resistance and mechanical properties.
A polyether ester polyol modified with sulfonate containing -SO3-Na+ in the side chain is compounded with an imidazole ionic liquid antistatic agent, and a double-terminated monohydroxy organosilicon prepolymer is introduced into component B to improve compatibility and wear resistance through chemical bonding.
It achieves improved durability of antistatic properties and enhanced wear resistance, with a dense and uniform microporous structure that maintains high mechanical properties.
Smart Images

Figure SMS_8 
Figure SMS_9
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyurethane polymer materials technology, specifically to antistatic and high-wear-resistant polyurethane microporous elastomers, their preparation methods, and applications. Background Technology
[0002] Polyurethane microporous elastomers possess characteristics such as low density, high specific strength, good resilience, and ease of molding, making them widely used in footwear manufacturing, automotive interiors, and cushioning and shock-absorbing materials. With increasingly stringent requirements for static electricity discharge in specialized protective equipment, electronics manufacturing workshops, and flammable and explosive environments, the demand for protective footwear with antistatic properties is gradually increasing. Simultaneously, as a friction component directly in contact with the ground, the wear resistance of the shoe sole directly affects its service life. Therefore, developing polyurethane microporous elastomers that combine durable antistatic properties with high wear resistance has significant engineering value.
[0003] Existing antistatic polyurethane materials are mostly prepared by adding external physical antistatic agents. Chinese patent application CN102977308A, published on March 20, 2013, discloses a two-component curable foamed polyurethane resin composition, a polyurethane molded body, and a shoe sole, which uses alkyl-substituted quaternary ammonium salts and alkyl-substituted imidazolium salts as antistatic agents. These small-molecule antistatic agents exist in a free state within the polyurethane matrix, mainly migrating to the material surface and absorbing moisture from the air to form a conductive layer. However, during wear, with sole wear, washing, or prolonged storage, the surface antistatic agent is easily lost, leading to a decline in antistatic performance over time, making it difficult to meet long-term antistatic requirements. Adding conductive fillers such as carbon black and carbon nanotubes can improve durability, but it limits the color of the shoe sole, and excessive inorganic fillers are prone to agglomeration, affecting foaming molding and mechanical properties.
[0004] To improve antistatic durability, existing technologies have attempted to introduce sulfonate structures into polyurethane systems. Chinese patent application CN119978304A, published on May 13, 2025, discloses a low-density, high-elasticity antistatic polyurethane foam material and its preparation method. Both the white and black components contain sulfonate polyester polyols. These sulfonate polyester polyols are formed by the dehydration condensation of dicarboxylic acids, alkali metal sulfonates, and diols to create hydroxyl-terminated macromolecules. The water absorption of sulfonates forms conductive channels, and migration is prevented by ester bonds. Chinese patent application CN117050287A, published on November 14, 2023, discloses a sulfonate polyether ester polyol, its preparation method, and its applications. The raw materials for its preparation include small-molecule diols, polyether diols, sulfonate diacids, and other diacids. While these documents disclose the general structure of sulfonate polyether ester polyols, they do not address their use in combination with imidazole ionic liquid antistatic agents, nor do they address further enhancing antistatic durability through the interaction between the two.
[0005] To improve wear resistance, existing technologies often incorporate organosilicon materials. Chinese patent application CN117106154A, published on November 24, 2023, discloses a low-temperature resistant and stain-resistant polyurethane shoe sole resin, its preparation method, and its application. Both components A and B contain terminal hydroxyl siloxanes, utilizing the low-temperature flexibility and hydrophobicity of the siloxane segments to improve low-temperature resistance and stain resistance. Chinese patent application CN121045501A, published on December 2, 2025, discloses a high-slip-resistant and durable polyurethane microporous shoe sole resin, its preparation method, and its application. It introduces polyether-modified siloxane and a benzyl-containing ester plasticizer into component A to improve slip resistance and durability. However, conventional polydimethylsiloxane has a significant polarity difference from polyurethane. If directly physically blended or simply introduced, phase separation easily occurs during molding, leading to a rough microporous structure, bubble collapse, or interlayer delamination, which ultimately reduces the overall mechanical properties. The aforementioned documents do not disclose the chemical bonding of the dual-terminated monohydroxy organosilicon prepolymer into the polyurethane backbone during the prepolymerization stage of component B, nor do they disclose the improvement of the compatibility between organosilicon and polyurethane matrix through octyl side groups.
[0006] In summary, while existing technologies have made some attempts in antistatic properties of sulfonates, antistatic properties of imidazole ionic liquids, and wear-resistant modification of organosilicon, they have not yet provided a polyurethane microporous elastomer solution that combines sulfonate-modified polyether ester polyols with imidazole ionic liquid antistatic agents and adds a bi-terminated monohydroxy organosilicon prepolymer to component B in steps, thereby simultaneously improving antistatic durability, wear resistance, and compatibility. Summary of the Invention
[0007] In view of the shortcomings of the prior art, the purpose of this invention is to provide an antistatic, high-wear-resistant polyurethane microporous elastomer. This is achieved by introducing side chains containing -SO3... - Na + The sulfonate-modified polyether ester polyol was combined with a physical antistatic agent to improve the antistatic durability; the introduction of a double-terminated monohydroxyl organosilicon prepolymer improved the wear resistance and the compatibility between organosilicon and polyurethane.
[0008] Another objective of this invention is to provide a method for preparing an antistatic, highly abrasion-resistant polyurethane microporous elastomer. By first reacting a polyester polyol with an isocyanate, and then adding a reactive organosilicon prepolymer at a controlled temperature, the incorporation efficiency and dispersion uniformity of the organosilicon are improved.
[0009] A third objective of this invention is to provide an application of an antistatic, highly abrasion-resistant polyurethane microporous elastomer. By mixing components A and B in a specific ratio and then casting them into a mold, the antistatic durability and abrasion resistance of the shoe sole are improved.
[0010] This invention is achieved using the following technical solution: The antistatic, high-wear-resistant polyurethane microporous elastomer is composed of component A and component B in a mass ratio of 100:(60-91). Component A comprises the following raw materials in parts by weight: Polyester polyol a: 70-90 parts; Polyester polyol b: 5-20 parts; Sulfonate-modified polyether ester polyol: 5-10 parts; Chain extender: 5-10 parts; Foaming agent: 0.3-0.6 parts; Catalyst: 0.6-1.5 parts; Foaming agent: 0.2-0.6 parts; Antistatic agent: 2-5 parts; In component A, the sum of the mass fractions of polyester polyol a, polyester polyol b, and sulfonate-modified polyether ester polyol is 100 parts. Component B comprises the following raw materials in parts by weight: Polyester polyol a: 25-33 parts; Polyester polyol b: 4.5-11 parts; Reactive organosilicon: 0.5-2 parts; Isocyanate: 55-70 parts; The reactive organosilicon is a double-terminated monohydroxy organosilicon prepolymer.
[0011] Preferably, polyester polyol a is a linear polyester polyol with a functionality of 2 and a number-average molecular weight of 2000-3200 g / mol, obtained by reacting a small-molecule diol with adipic acid; and polyester polyol b is a branched polyester polyol with a functionality >2 and a number-average molecular weight of 1200-2000 g / mol, obtained by reacting a small-molecule diol and a small-molecule triol with adipic acid. This invention, by rationally combining linear polyester polyols with higher molecular weights and branched polyester polyols with lower molecular weights, provides matrix flexibility while utilizing the branched structure to construct a suitable cross-linking network, thus ensuring the initial mechanical strength and dimensional stability of the shoe sole material.
[0012] Preferably, the sulfonate-modified polyether ester polyol is prepared by an alkyd-acid condensation reaction of polytetrahydrofuran ether diol, adipic acid, and sodium isophthalic acid-5-sulfonate. Preferably, in the reaction system for preparing the sulfonate-modified polyether ester polyol, the ratio of the total molar number of hydroxyl groups to the total molar number of dicarboxylic acids is 1.9-2.2, the number-average molecular weight of the polytetrahydrofuran ether diol is 1000 g / mol, and the number-average molecular weight of the obtained sulfonate-modified polyether ester polyol is 1400-1800 g / mol, with -SO3-containing side chains. - Na +Ionic groups.
[0013] Component A contains an antistatic agent, which is an imidazole-based ionic liquid antistatic agent, and the imidazole-based ionic liquid has a cation of 1. Ethyl 3 Methylimidazolium cation, anion is ethyl sulfate anion (1 Ethyl 3 Ethyl methylimidazolium sulfate, CAS: 342573-75-5.
[0014] Preferably, the reactive organosilicon is a prepolymer of organosilicon with hydroxyl groups at both ends of the molecule and octyl side groups on the siloxane backbone, and its number-average molecular weight is about 1550 g / mol.
[0015] Preferably, the isocyanate is a mixture of 4,4-diphenylmethane diisocyanate (MDI) and carbodiimide-modified isocyanate (liquefied MDI); preferably, based on the total mass of the isocyanate mixture, MDI comprises 50-60 parts and carbodiimide-modified isocyanate comprises 5-10 parts. The introduction of liquefied MDI can effectively inhibit the crystallization of component B prepolymer at low temperatures and improve its storage stability. The -NCO content of component B is controlled between 16.35 wt.% and 21.8 wt.%, which matches well with the hydroxyl value of component A, ensuring the smooth progress of foaming and curing reactions.
[0016] This invention also provides a method for preparing the above-mentioned antistatic and high-wear-resistant polyurethane microporous elastomer, comprising the following steps: (1) Preparation of component A: The measured polyester polyol a, polyester polyol b, sulfonate modified polyether ester polyol, chain extender, foaming agent, catalyst, foaming agent and antistatic agent are put into the reaction vessel and stirred and mixed at atmospheric pressure and 40-60℃ for 1-2 hours to make the components evenly dispersed, thus obtaining component A. (2) Preparation of Component B: Measured amounts of polyester polyol a, polyester polyol b, and reactive organosilicon were vacuum-stirred and dehydrated at 110-120℃ for 1.5 hours (moisture content less than 0.05%). After dehydration, polyester polyol a and polyester polyol b were cooled, and the material temperature was controlled at 70℃. They were then added to measured amounts of isocyanate and reacted at 70-80℃ for 2-3 hours under nitrogen protection, followed by cooling to 65℃. Subsequently, measured amounts of dehydrated reactive organosilicon were added, and the mixture was reacted at 65-70℃ for 1-1.5 hours to obtain the prepolymer of Component B. In this step, due to the low reactivity of organosilicon and to avoid local overheating and side reactions, the temperature of the reactive organosilicon itself must not exceed 40℃ when it is added.
[0017] This invention also provides a molding method for the application of the above-mentioned resin in the preparation of polyurethane shoe soles: Component A and Component B are injected into the material tank of a low-pressure casting machine, the mold temperature is set to 45-60℃, and Component A and Component B are mixed at high speed through the mixing head of the casting machine at a mass ratio of 100:(60-91) and then injected into the mold. After curing for 2-4 minutes, the mold is opened to obtain an antistatic, high wear-resistant polyurethane microporous shoe sole.
[0018] The chain extender is one or two of ethylene glycol, diethylene glycol, and 1,4-butanediol.
[0019] The foam stabilizer is a polysiloxane-olefin oxide block copolymer, preferably DC2525 and DC193 from Air Products, Inc.
[0020] The catalyst is one of the tertiary amine catalysts DXD-07C and DXD-01C, preferably DXD-07C produced by Shandong Yinuowei Polyurethane Co., Ltd.; the foaming agent is water.
[0021] The antistatic agent is ethyl 1-ethyl-3-methylimidazolium sulfate, preferably ESD68 produced by Anhui Sancai Chemical Co., Ltd., CAS No.: 342573-75-5.
[0022] The dual-terminated monohydroxyl organosilicon prepolymer Silok® 8812F2 has a number-average molecular weight of 1550 g / mol and a functionality of 2. Silok® 8812F2 from Silok® is preferred. Its molecular structure is shown below: .
[0023] The isocyanate is a mixture of 4,4-diphenylmethane diisocyanate and carbodiimide-modified isocyanate, and the 4,4-diphenylmethane diisocyanate and carbodiimide-modified isocyanate can be mixed in any proportion.
[0024] This invention does not rely solely on traditional physical antistatic agents, but instead, through macromolecular structure design, introduces polyether / polyester flexible segments into the main chain and -SO3-containing segments into the side chains of component A. - Na + Sulfonate-modified polyether ester polyols with ionic groups. On the one hand, -SO3 - Na +The functional group itself can form a certain degree of ionic conductive channel (structural antistatic) within the polyurethane network. Furthermore, this macromolecular ionic group can generate strong ion-dipole interactions and electrostatic adsorption with small-molecule ionic liquid antistatic agents added to the formulation (such as 1-ethyl-3-methylimidazolium sulfate ethyl ester). This "chemical anchoring" effect effectively limits the rate at which small-molecule antistatic agents migrate to the material surface, overcoming the shortcomings of traditional physical antistatic agents that are easily washed away by water or rubbed off, thus achieving a stable and long-lasting antistatic effect.
[0025] This invention introduces a specific reactive organosilicon (a siloxane with dual-terminated monohydroxyl groups and an octyl side group on the main chain) into the B-component synthesis stage. First, the terminal hydroxyl groups react with isocyanate, introducing polysiloxane segments with extremely low surface energy into the polyurethane main chain via chemical bonds. During molding and curing, the siloxane segments tend to accumulate on the inner walls of micropores and the outer surface of the shoe sole, significantly reducing the surface friction coefficient and thus endowing the material with excellent friction-reducing and wear-resistant properties. Second, addressing the problem of macroscopic phase separation between organosilicon and polyurethane, this invention selects an organosilicon main chain with a long-chain aliphatic octyl side group. The nonpolar octyl side group acts as a "solvent" or "compatibility agent," reducing the interfacial tension between the siloxane segments and the polyester polyol and hard segment molecules. This allows the polysiloxane to achieve uniform dispersion at the microscale within the polyurethane matrix, avoiding pore collapse and mechanical property degradation caused by macroscopic phase separation.
[0026] Compared with the prior art, the beneficial effects of the present invention are: (1) Through the synergistic effect of sulfonate-modified polyol and physical antistatic agent, the polyurethane microporous elastomer of the present invention has excellent and long-lasting antistatic volume resistivity. Even after long-term friction and washing, its antistatic performance decay rate is still small, which meets the long-term protection requirements of special footwear.
[0027] (2) Introducing a double-terminated hydroxyl organosilicon prepolymer with octyl side groups allows the lubricating siloxane segments to be stably integrated into the polyurethane network through chemical bonds, which reduces the coefficient of friction and improves the DIN wear resistance of the finished product while avoiding precipitation and loss.
[0028] (3) It overcomes the problem of decreased mechanical properties caused by filler agglomeration or silicone oil phase separation in conventional modification methods. The introduction of octyl side groups improves microcompatibility. Combined with the compounding of linear and branched polyester polyols in the system, the resulting microporous elastomer has a dense and uniform cell structure, maintaining high tensile strength, tear strength and good flexural resistance. Detailed Implementation
[0029] The present invention will be further described below with reference to the embodiments and comparative examples. Unless otherwise specified, the raw materials used in the embodiments and comparative examples are all conventional commercial raw materials, and the process methods used are all conventional methods in the art unless otherwise specified. The parts involved in the raw materials in the embodiments and comparative examples are all parts by mass.
[0030] The raw materials used in the examples and comparative examples are described below: PE-25323: Polyester polyol a, functionality 2, number average molecular weight 3200 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2520: Polyester polyol a, functionality 2, number average molecular weight 2000 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2420: Polyester polyol a, functionality 2, number average molecular weight 2000 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2520F: Polyester polyol a, functionality 2, number average molecular weight 2000g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2520-03: Polyester polyol b, functionality 2.03, number average molecular weight 2000 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2512-04: Polyester polyol b, functionality 2.04, number average molecular weight 1200 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2325: Polyester polyol b, functionality 2.06, number average molecular weight 2000 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. PE-2517-06: Polyester polyol b, functionality 2.06, number average molecular weight 1700 g / mol, Shandong Yinuowei Polyurethane Co., Ltd. DC2525: Foaming agent, Air Products, Inc., USA; DC193: Foaming agent, Air Products, Inc., USA; Antistatic agent: ESD68, Anhui Sancai Chemical Co., Ltd.; DXD-07C: Catalyst, Shandong Yinuowei Polyurethane Co., Ltd.; MDI-100: 4,4-Diphenylmethane diisocyanate, Wanhua Chemical Group Co., Ltd.; CDMDI-100L: Carbodiimide-modified isocyanate, Wanhua Chemical Group Co., Ltd.; Bi-terminated monohydroxyl organosilicon prepolymer: Bi-terminated with hydroxyl groups, containing organosilicon, with a number average molecular weight of 1550 g / mol, purchased from Guangzhou Sloco New Materials Co., Ltd.
[0031] Sulfonate-modified polyether ester polyols: number average molecular weight of 1400g-1800g / mol, self-synthesized.
[0032] PTMG1000, manufacturer Mitsubishi Chemical Corporation; Adipic acid: Manufacturer: Shandong Hualu Hengsheng Chemical Co., Ltd.; Sodium isophthalic acid-5-sulfonate: Manufacturer: Weifang Derun Chemical Co., Ltd.; Tetrabutyl titanate: Manufacturer: Shandong Heruidong Fine Chemical Co., Ltd.
[0033] The preparation process of the sulfonate-modified polyether ester polyol used in the examples and comparative examples is shown below.
[0034] Sulfonate-modified polyether ester polyol a (number average molecular weight 1400±50 g / mol): The specific preparation steps for sulfonate-modified polyether ester polyol a (number average molecular weight of 1400 g / mol) are as follows: ① Add 93.382 kg of PTMG1000 melted at 80℃ to the reactor; add 5.706 kg of adipic acid, 0.912 kg of sodium isophthalic acid-5-sulfonate dried under vacuum at 110~120℃ to remove water of crystallization, and 0.012 kg of TNBT in sequence; purge the reactor with nitrogen to fully replace the air inside, and keep the reactor under nitrogen-sealed protection throughout the process.
[0035] ② Gradually increase the temperature to 185℃ and react under normal pressure. After more than 85% of the theoretical water output is separated, proceed to the vacuum polycondensation process.
[0036] ③ First, maintain a vacuum of -0.06~-0.07 MPa (low vacuum) for 1 hour; then increase the vacuum to -0.090~-0.098 MPa (high vacuum) and continue the polycondensation reaction for 5 hours until the system has an acid value of 0.9 mg KOH / g and a hydroxyl value of 80 mg KOH / g (corresponding to a number-average molecular weight of 1400 g / mol), then stop the reaction.
[0037] ④ Nitrogen gas is used to repressurize and break the vacuum, and the temperature is lowered to 100~120℃. The material is then filtered through a 200-mesh filter to obtain sulfonate-modified polyether ester polyol a.
[0038] The specific preparation steps for sulfonate-modified polyether ester polyol b (number average molecular weight of 1600 g / mol) are as follows: ① Add 92.760 kg of PTMG1000 melted at 70℃ to the reactor; add 6.236 kg of adipic acid, 0.992 kg of sodium isophthalic acid-5-sulfonate dried under vacuum at 110~120℃ to remove water of crystallization, and 0.012 kg of TNBT in sequence; purge the reactor with nitrogen to fully replace the air inside, and keep the reactor under nitrogen-sealed protection throughout the process.
[0039] ② Gradually increase the temperature to 195℃ and react under normal pressure. After more than 85% of the theoretical water output is separated, proceed to the vacuum polycondensation process.
[0040] ③ First, maintain a vacuum of -0.06~-0.07 MPa (low vacuum) for 1.5h; then increase the vacuum to -0.090~-0.098 MPa (high vacuum) for condensation reaction for 3h, until the system acid value reaches 0.85mgKOH / g and the hydroxyl value reaches 70.1mgKOH / g (corresponding to a number average molecular weight of 1600g / mol), then stop the reaction.
[0041] ④ Nitrogen gas is used to repressurize and break the vacuum, and the temperature is lowered to 100~120℃. The material is then filtered through a 200-mesh filter to obtain sulfonate-modified polyether ester polyol b.
[0042] The specific preparation steps for sulfonate-modified polyether ester polyol C (number average molecular weight of 1800 g / mol) are as follows: ① Add 92.421 kg of PTMG1000 melted at 60℃ to the reactor; add 6.535 kg of adipic acid, 1.044 kg of sodium isophthalic acid-5-sulfonate dried under vacuum at 110~120℃ to remove water of crystallization, and 0.012 kg of TNBT in sequence; purge the reactor with nitrogen to fully replace the air inside, and keep the reactor under nitrogen protection throughout the process.
[0043] ② Gradually increase the temperature to 190℃ and react under normal pressure. After more than 85% of the theoretical water output is separated, proceed to the vacuum polycondensation process.
[0044] ③ First, maintain a vacuum of -0.06~-0.07 MPa (low vacuum) for 2 hours; then increase the vacuum to -0.090~-0.098 MPa (high vacuum) for 4 hours of polycondensation reaction, until the acid value of the system reaches 0.78 mg KOH / g and the hydroxyl value reaches 62.3 mg KOH / g (corresponding to a number average molecular weight of 1800 g / mol), and then stop the reaction.
[0045] ④ Nitrogen gas is used to repressurize and break the vacuum, and the temperature is lowered to 100~120℃. The material is then filtered through a 200-mesh filter to obtain sulfonate-modified polyether ester polyol c.
[0046] Example 1 The preparation method of the aforementioned antistatic and high abrasion-resistant polyurethane microporous shoe sole resin includes the following steps: (1) Preparation of component A: According to the mass parts, start stirring and add 70 parts of PE-25323, 20 parts of PE-2520-03, 10 parts of sulfonate modified polyether ester polyol a, 8 parts of ethylene glycol, 0.4 parts of DC2525, 2 parts of ESD68, 1.2 parts of DXD-07C and 0.3 parts of water into the reactor in sequence. After stirring at 40°C for 2 hours, component A is obtained. (2) Preparation of component B: According to the mass parts, 50 parts of MDI-100 and 5 parts of CDMDI-100L were added to the reactor. The reactor was stirred and the 33 parts of PE-2420 and 10 parts of PE-2325 that had been dehydrated were cooled to 70°C and added to the reactor. Under nitrogen protection, the temperature was slowly raised to 80°C. After reacting for 2 hours, the temperature was lowered to 65°C and 2 parts of the dehydrated organosilicon prepolymer Silok® 8812F2 (the temperature of the organosilicon prepolymer should not exceed 40°C) were added. The reaction was carried out at 65°C for 1.5 hours to obtain component B with a -NCO content of 16.35wt.%.
[0047] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:91 and then injected into a mold at 45°C. The mold is opened after 3 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0048] Example 2 The preparation method of the aforementioned antistatic and high abrasion-resistant polyurethane microporous shoe sole resin includes the following steps: (1) Preparation of component A: According to the mass parts, start stirring and add 90 parts of PE-25323, 5 parts of PE-2520-03, 5 parts of sulfonate modified polyether ester polyol b, 10 parts of ethylene glycol, 0.3 parts of DC2525, 5 parts of ESD68, 0.8 parts of DXD-07C and 0.6 parts of water into the reactor in sequence. After stirring at 50°C for 1.5h, component A is obtained. (2) Preparation of component B: According to the mass fraction, 60 parts of MDI-100 and 10 parts of CDMDI-100L were added to the reactor. The reactor was stirred and the 25 parts of PE-2520F and 4.5 parts of PE-2517-06 that had been dehydrated were added to the reactor after cooling to 70°C. Under nitrogen protection, the temperature was slowly raised to 70°C and reacted for 3 hours. Then the temperature was lowered to 65°C and 0.5 parts of the dehydrated organosilicon prepolymer Silok® 8812F2 (the temperature of the organosilicon prepolymer should not exceed 40°C) were added. The reaction was carried out at 70°C for 1 hour to obtain component B with a -NCO content of 21.8 wt.%.
[0049] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:79 and then injected into a mold at 50°C. The mold is opened after 4 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0050] Example 3 The preparation method of the aforementioned antistatic and high abrasion-resistant polyurethane microporous shoe sole resin includes the following steps: (1) Preparation of component A: According to the mass parts, start stirring and add 83 parts of PE-25323, 12 parts of PE-2520-03, 5 parts of sulfonate modified polyether ester polyol a, 5 parts of ethylene glycol, 0.6 parts of DC2525, 3 parts of ESD68, 1.5 parts of DXD-07C and 0.2 parts of water into the reactor in sequence. After stirring at 60°C for 1 hour, component A is obtained. (2) Preparation of component B: According to the mass fraction, add 50 parts of MDI-100 and 5 parts of CDMDI-100L to the reactor, turn on the reactor and stir. Add 33 parts of PE-2420 and 10 parts of PE-2325 that have been dehydrated to 70°C to the reactor. Under nitrogen protection, slowly raise the temperature to 80°C and react for 2 hours. Then, lower the temperature to 65°C and add 2 parts of the dehydrated organosilicon prepolymer Silok® 8812F2 (the temperature of the organosilicon prepolymer should not exceed 40°C). React at 65°C for 1.5 hours to obtain component B with a -NCO content of 16.35 wt.%.
[0051] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:66 and then injected into a mold at 50°C. The mold is opened after 4 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0052] Example 4 The preparation method of the aforementioned antistatic and high abrasion-resistant polyurethane microporous shoe sole resin includes the following steps: (1) Preparation of component A: According to the mass parts, start stirring and add 80 parts of PE-2520, 12 parts of PE-2512-04, 8 parts of sulfonate modified polyether ester polyol c, 8 parts of 1,4-butanediol, 0.5 parts of DC2525, 3 parts of ESD68, 1.2 parts of DXD-07C and 0.4 parts of water into the reactor in sequence. After stirring at 60°C for 1 hour, component A is obtained. (2) Preparation of component B: According to the mass fractions, 53 parts of MDI-100 and 7 parts of CDMDI-100L were added to the reactor. The reactor was stirred and the 28 parts of PE-2520F and 11 parts of PE-2517-06 that had been dehydrated were cooled to 70°C and added to the reactor. Under nitrogen protection, the temperature was slowly raised to 80°C and reacted at 80°C for 2 hours. Then the temperature was lowered to 65°C and 1 part of the dehydrated organosilicon prepolymer Silok® 8812F2 (the temperature of the organosilicon prepolymer should not exceed 40°C) was added. The reaction was carried out at 65°C for 1.5 hours to obtain component B with a -NCO content of 18.09 wt.%.
[0053] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:73 and then injected into a mold at 60°C. The mold is opened after 2 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0054] Example 5 The preparation method of the aforementioned antistatic and high abrasion-resistant polyurethane microporous shoe sole resin includes the following steps: (1) Preparation of component A: According to the mass parts, start stirring and add 85 parts of PE-2520, 10 parts of PE-2512-04, 5 parts of sulfonate modified polyether ester polyol a, 5 parts of ethylene glycol, 0.6 parts of DC2525, 5 parts of ESD68, 1.2 parts of DXD-07C and 0.5 parts of water into the reactor in sequence. After stirring at 40°C for 2 hours, component A is obtained. (2) Preparation of component B: According to the mass fraction, 60 parts of MDI-100 and 10 parts of CDMDI-100L were added to the reactor. The reactor was stirred and the 25 parts of PE-2520F and 4.5 parts of PE-2517-06 that had been dehydrated were cooled to 70°C and added to the reactor. Under nitrogen protection, the temperature was slowly raised to 70°C and reacted at 70°C for 3 hours. Then the temperature was lowered to 65°C and 0.5 parts of the dehydrated organosilicon prepolymer Silok® 8812F2 (the temperature of the organosilicon prepolymer should not exceed 40°C) were added. The reaction was carried out at 70°C for 1 hour to obtain component B with a -NCO content of 21.8 wt.%.
[0055] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:60 and then injected into a mold at 60°C. The mold is opened after 2 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0056] Comparative Example 1 Compared to Example 1, this comparative example omits the Silok®8812F2 reactive silicone prepolymer in component B, which belongs to the traditional pure polyurethane system. The rest of the formulation, preparation process, and molding process are completely consistent with Example 1.
[0057] (1) Preparation of component A: According to the mass parts, start stirring and add 70 parts of PE-25323, 20 parts of PE-2520-03, 10 parts of sulfonate modified polyether ester polyol a, 8 parts of ethylene glycol, 0.4 parts of DC2525, 2 parts of ESD68, 1.2 parts of DXD-07C and 0.3 parts of water into the reactor in sequence. After stirring at 40°C for 2 hours, component A is obtained. (2) Preparation of component B: According to the mass fraction, add 50 parts of MDI-100 and 5 parts of CDMDI-100L to the reactor, turn on the reactor and stir. Add 33 parts of PE-2420 and 10 parts of PE-2325 (after dehydration) to the reactor after cooling to 70°C. Under nitrogen protection, slowly raise the temperature to 80°C and react at 80°C for 2 hours. Then, cool down to 65°C and keep the temperature constant for 1.5 hours (without adding organosilicon prepolymer) to obtain component B with a -NCO content of 16.80 wt.%.
[0058] The application of the aforementioned antistatic, high abrasion-resistant polyurethane microporous sole resin includes the following steps: Components A and B are injected into the material tank of a low-pressure casting machine. Components A and B are quickly mixed at a mass ratio of 100:90 and then injected into a mold at 45°C. The mold is opened after 3 minutes to obtain an antistatic, high-wear-resistant polyurethane microporous shoe sole.
[0059] Comparative Example 2 Compared to Example 4, this comparative example uses conventional common polyether polyol C2140 (Yantai Wanhua Chemical Co., Ltd., functionality 2) instead of the sulfonate ionic polyether polyol c synthesized in this invention. The molecular chain chemical bond ionic conductive structure is eliminated, and only the physical antistatic agent is retained. The rest of the formulation and process are completely the same.
[0060] (1) Preparation of component A: According to the mass parts, start stirring and add 80 parts of PE-2520, 12 parts of PE-2512-04, 8 parts of C2140, 8 parts of 1,4-butanediol, 0.5 parts of DC2525, 3 parts of ESD68, 1.2 parts of DXD-07C and 0.4 parts of water into the reactor in sequence. After stirring at 60°C for 1 hour, component A is obtained. (2) Preparation of component B: The preparation of component B with an NCO content of 18.09 wt.% was completely consistent with Example 4; (3) Molding process: completely consistent with Example 4, 100:73 ratio of mixing, 60℃ mold, 2min mold opening molding.
[0061] Comparative Example 3 Compared to Example 2, this comparative example changed the way silicone was added. 0.5 parts of Silok®8812F2 silicone prepolymer were directly mixed into the polyol system of component A (traditional blending process), and bonding was not performed in the prepolymer stage of component B. The rest of the formulation, process, NCO content and molding parameters were completely the same.
[0062] (1) Preparation of component A: According to the mass parts, start stirring and add 90 parts of PE-25323, 5 parts of PE-2520-03, 5 parts of sulfonate modified polyether ester polyol b, 10 parts of ethylene glycol, 0.3 parts of DC2525, 5 parts of ESD68, 0.8 parts of DXD-07C, 0.6 parts of water and 0.5 parts of dehydrated Silok®8812F2 into the reactor in sequence. After stirring at 50°C for 1.5h, component A is obtained. (2) Preparation of component B: The addition of organosilicon was omitted, and the rest was the same as in Example 2, to obtain component B with an NCO content of 21.9 wt.%; (3) Molding process: completely consistent with Example 2, 100:78 ratio, 50℃ mold, 4min mold opening.
[0063] Comparative Example 4 Compared to Example 5, this comparative example completely removes the self-synthesized sulfonate-modified polyether ester polyol and replaces it with an equal amount of conventional polyester polyol. It achieves antistatic properties solely by relying on a high amount of physical antistatic agent, which is a traditional antistatic PU shoe sole formulation. The rest of the process is completely identical.
[0064] (1) Preparation of component A: According to the mass parts, start stirring and add 90 parts of PE-2520, 10 parts of PE-2512-04, 5 parts of ethylene glycol, 0.6 parts of DC2525, 5 parts of ESD68, 1.2 parts of DXD-07C and 0.5 parts of water into the reactor in sequence. After stirring at 40°C for 2 hours, component A is obtained. (2) Preparation of component B: The preparation was completely consistent with Example 5, and component B with an NCO content of 21.8 wt.% was obtained; (3) Molding process: completely consistent with Example 5, 100:60 ratio, 60℃ mold, 2min mold opening.
[0065] The performance of the polyurethane shoe soles prepared in Examples 1-5 and Comparative Examples 1-4 was tested, and the test results are shown in Tables 1-2: The density of the product was tested in accordance with GB / T 6343-2009, and the hardness was tested in accordance with GB / T 3903.4-2017; the tensile strength, elongation, right-angle tear strength, and flexural strength were tested in accordance with GB / T 20991-2007.
[0066] The shoe upper used in the examples and comparative examples is a leather upper. The peel strength between the upper and the polyurethane sole is tested according to EN ISO 20344:2021+A1:2024, 5.2 standard. The requirements are: if the sole material is not damaged during the test, the peel strength is >4.0 N / mm; if the sole material is damaged, the peel strength is at least 3.0 N / mm.
[0067] Abrasion resistance testing was conducted using the DIN abrasion resistance test, determined according to ISO 4649:2017 standard. Specific test parameters were as follows: the material was cut into cylindrical specimens with a diameter of 16 mm. Under a load of 10 N, the specimens were moved 40 m on a rotating roller (covered with #60 grit sandpaper). The mass loss of the specimens was recorded and converted to volumetric abrasion loss (mm³) based on the specimen density. Each group of samples was tested five times, and the arithmetic mean was taken.
[0068] Surface resistivity (Ω): Tested according to GB / T 2439-2001; Surface resistivity after water washing: Samples (100mm×100mm×4mm) were prepared for Examples 1-5 and Comparative Examples 1-4. They were soaked and washed 50 times in distilled water at room temperature, with each soaking lasting 10 minutes. After each wash, the samples were allowed to drain naturally. After all the washing was completed, the samples were placed in a 60℃ constant temperature oven to dry for 30 minutes, and then placed in a standard constant temperature and humidity environment to stand for 24 hours to ensure that the moisture and stress inside the samples were completely balanced. The surface resistance values under normal conditions and after washing were measured respectively.
[0069] Cell structure: visual inspection Product dimensional stability: The change in sample size was tested after the mold was opened and cooled for 24 hours.
[0070] Mechanical property retention rate after thermo-oxidative aging: Dumbbell-shaped standard samples were prepared and placed in a hot air aging chamber at a temperature of 80℃±2℃ for continuous aging for 72 hours. Immediately after aging, the samples were removed and placed in a standard constant temperature and humidity environment (temperature 23℃±2℃, relative humidity 50%±5%) for 24 hours to eliminate thermal stress and temperature / humidity differences. The tensile strength, elongation, and right-angle tear strength of the samples before and after aging were tested to calculate the mechanical property retention rate. Simultaneously, the surface of the samples was visually inspected for defects such as blooming and precipitation.
[0071] The performance test data of the products in Examples 1-5 are shown in Table 1.
[0072] The performance test data of Comparative Examples 1-4 are shown in Table 2.
[0073] Table 1: Performance test data of products from Examples 1-5
[0074] Table 2: Performance test data of Comparative Examples 1-4
[0075] The product density of Examples 1-5 of this invention is 502-521 kg / m³. 3 With a hardness of Shore C 62-80, the tensile strength of the products can reach 3.8-4.7MPa, the elongation is not less than 415%, the right angle tear strength is maintained at 16.1-18KN / m, and the flexural resistance at room temperature can reach more than 150,000 cycles without cracking or breakage, showing good toughness and fatigue bending resistance.
[0076] In this embodiment of the invention, the surface resistivity of the sample under normal conditions is stably controlled at 2.8 × 10⁻⁶. 6 ~4.3×10 7 After 50 accelerated water washing tests at room temperature, the surface resistivity of the sample in the example remained within the same order of magnitude, without any sudden change in magnitude, and remained stable at 4.5 × 10⁻⁶ Ω. 6 ~6.9×10 7 Ω, with no order-of-magnitude abrupt change, low surface resistance, good conductivity, and durable and strong antistatic properties. Comparative Examples 2 and 4 used conventional polyether / polyester polyols instead of ionic polyether ester polyols, relying solely on physical antistatic agents to achieve antistatic effects. Initially, the surface resistance increased, and the conductivity slightly decreased. Especially after 50 accelerated washing tests at room temperature, the surface resistance increased further, and the antistatic properties deteriorated significantly. This invention addresses this by chemically bonding -SO3 to the polyurethane molecular chain segments. - Na +The ionic groups construct a stable intrinsic ionic conductive network, which, together with the physical antistatic agent, forms a dual system of "chemically bonded long-lasting conductivity + physically uniform electrostatic conduction". This solves the problems of poor water resistance, easy migration and performance degradation of traditional single physical antistatic systems, and has long-lasting and stable antistatic capability, which can meet the safety requirements of electronic and flammable and explosive working conditions.
[0077] This invention, tested by DIN abrasion resistance, shows a significant reduction in wear volume. Compared to Comparative Example 1 without silicone modification, the reduction in wear is more pronounced. Comparative Example 1, lacking reactive silicone prepolymer, exhibits high frictional heat generation and wear. Comparative Example 3, employing a traditional physical blending process of silicone component A, shows a slight improvement in short-term wear resistance, but the poor compatibility between silicone and the polyurethane matrix leads to easy accumulation and precipitation on the surface, resulting in decreased wear resistance after long-term friction, and precipitation and blooming defects appearing on the sample surface. This invention chemically bonds the dual-terminated monohydroxyl silicone prepolymer Silok®8812F2 into the polyurethane molecular backbone during the prepolymerization stage of component B. Stable siloxane flexible segments are uniformly distributed within the material and at the friction interface, effectively reducing the interfacial friction coefficient and buffering frictional stress, thus improving the material's wear resistance without sacrificing the matrix's mechanical and adhesive properties.
[0078] Analysis of thermo-oxidative aging stability data showed that after thermo-oxidative aging at 80℃ for 72 hours, the tensile and tear mechanical properties of the sample samples retained ≥90%, and there was no blooming, precipitation, or cracking on the sample surface, indicating excellent appearance and performance stability. Comparative Examples 2 and 4, containing only free small-molecule antistatic agents and lacking compounded ionic polyether ester polyols, easily migrated to the surface and precipitated during thermo-oxidative aging, resulting in obvious whitening and blooming on the sample surface. Their mechanical property retention rate was only 65%–75%, indicating poor aging stability.
[0079] Mechanism conclusion: The ionic polyether ester polyol chemical bonding modification system has no free migratable small molecules, the organosilicon segments are stably bonded to the molecular chain, and with the addition of physical antistatic agents, it is not easy to migrate and precipitate under high temperature aging. The material has a stable cross-linking structure and excellent heat and oxygen aging resistance and long-term use stability.
[0080] The samples in this invention exhibit uniform and dense foam cells with high pore size consistency, free from defects such as large pores, voids, and broken holes. Furthermore, the soles and uppers of these samples demonstrate high peel strength and stable bonding interfaces. In contrast, the physically blended organosilicon system in Comparative Example 3 shows a continuous enrichment of silicon segments on the material surface, significantly reducing the surface energy of the sole and resulting in a decrease in the bonding strength between the upper and sole, making it prone to delamination and separation during use.
[0081] This invention constructs a long-lasting ion-conducting network by independently synthesizing ionic polyether ester polyols, and achieves a stable antistatic effect by compounding physical antistatic agents; by chemically bonding a double-terminated monohydroxy organosilicon prepolymer through component B, the wear resistance is improved without sacrificing the material's mechanical, adhesive, and molding properties. This invention solves the defects of existing polyurethane microporous shoe soles, such as easy failure of antistatic properties, inability to balance wear resistance and adhesion, and poor molding stability, and is suitable for antistatic shoe soles.
Claims
1. An antistatic, high-wear-resistant polyurethane microporous elastomer, characterized in that, It is composed of component A and component B in a mass ratio of 100:(60-91); Component A comprises the following raw materials in parts by weight: Polyester polyol a: 70-90 parts; Polyester polyol b: 5-20 parts; Sulfonate-modified polyether ester polyol: 5-10 parts; Chain extender: 5-10 parts; Foaming agent: 0.3-0.6 parts; Catalyst: 0.6-1.5 parts; Foaming agent: 0.2-0.6 parts; Antistatic agent: 2-5 parts; In component A, the sum of the mass fractions of polyester polyol a, polyester polyol b, and sulfonate-modified polyether ester polyol is 100 parts. Component B comprises the following raw materials in parts by weight: Polyester polyol a: 25-33 parts; Polyester polyol b: 4.5-11 parts; Reactive organosilicon: 0.5-2 parts; Isocyanate: 55-70 parts; The reactive organosilicon is a double-terminated monohydroxy organosilicon prepolymer.
2. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that: The polyester polyol a is a polyester polyol with a functionality of 2 and a number-average molecular weight of 2000-3200 g / mol, obtained by reacting a small molecule diol with adipic acid; the polyester polyol b is a branched polyester polyol with a functionality >2 and a number-average molecular weight of 1200-2000 g / mol, obtained by reacting a small molecule diol and a small molecule triol with adipic acid.
3. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 2, characterized in that: The small molecule diol is one or two of ethylene glycol, diethylene glycol, and 1,4-butanediol; the small molecule triol is one of glycerol and trimethylolpropane.
4. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that: The sulfonate-modified polyether ester polyol is prepared by an alkyd-acid condensation reaction of polytetrahydrofuran ether diol, adipic acid, and sodium isophthalic acid-5-sulfonate. In the reaction system for preparing this sulfonate-modified polyether ester polyol, the ratio of total hydroxyl moles to total carboxylic acid moles is 1.9-2.
2. The number-average molecular weight of the polytetrahydrofuran ether diol is 1000 g / mol, and the number-average molecular weight of the obtained sulfonate-modified polyether ester polyol is 1400-1800 g / mol, with -SO3-containing side chains. - Na + Ionic groups.
5. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that: The chain extender is one or two of ethylene glycol, diethylene glycol, and 1,4-butanediol; the foaming agent is a polysiloxane-oxidized olefin block copolymer; the catalyst is a tertiary amine catalyst; and the foaming agent is water.
6. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that, The antistatic agent is an imidazole-based ionic liquid antistatic agent, and the imidazole-based ionic liquid has a cation of 1. Ethyl 3 The cation of methylimidazolium is ethyl sulfate anion.
7. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that: The reactive organosilicon is a prepolymer of organosilicon with hydroxyl groups at both ends of the molecule and octyl side groups on the siloxane backbone, and its number average molecular weight is 1550 g / mol.
8. The antistatic, high-wear-resistant polyurethane microporous elastomer according to claim 1, characterized in that: The isocyanate is a mixture of 4,4-diphenylmethane diisocyanate and carbodiimide-modified isocyanate; based on the total mass of the isocyanate mixture, 4,4-diphenylmethane diisocyanate is 50-60 parts and carbodiimide-modified isocyanate is 5-10 parts; the -NCO content of component B is 16.35 wt.% - 21.8 wt.%.
9. A method for preparing the antistatic, high-wear-resistant polyurethane microporous elastomer according to any one of claims 1-8, characterized in that, Includes the following steps: (1) Preparation of component A: The polyester polyol a, polyester polyol b, sulfonate modified polyether ester polyol, chain extender, foam leveler, catalyst, foaming agent and antistatic agent are put into the reaction vessel and stirred at atmospheric pressure and 40-60℃ for 1-2 hours to obtain component A. (2) Preparation of component B: The polyester polyol a, polyester polyol b and reactive organosilicon were vacuum stirred and dehydrated at 110-120℃ for 1.5 hours; After dehydration, polyester polyol a and polyester polyol b are added to a metered amount of isocyanate at a controlled temperature of 70°C. The mixture is then reacted at 70-80°C for 2-3 hours under nitrogen protection, followed by cooling to 65°C. Subsequently, a metered amount of dehydrated reactive organosilicon is added, and the mixture is reacted at 65-70°C for 1-1.5 hours to obtain component B. When adding the reactive organosilicon, the material temperature should not exceed 40°C.
10. An application of the antistatic, high-abrasion-resistant polyurethane microporous elastomer according to any one of claims 1-8 in the preparation of polyurethane shoe soles, characterized in that, The process includes the following steps: injecting component A and component B into the material tank of a low-pressure casting machine, mixing component A and component B at a mass ratio of 100:(60-91), and then injecting the mixture into a mold at 45-60℃. After 2-4 minutes, the mold is opened to obtain the final product.
Citation Information
Patent Citations
Bi-component cured foam polyurethane resin composition, polyurethane molding body and sole
CN102977308A
Sulfonate polyether ester polyol as well as preparation method and application thereof
CN117050287A
Low-temperature-resistant and dirt-resistant polyurethane sole resin as well as preparation method and application thereof
CN117106154A
Low-density high-elasticity antistatic polyurethane foam material and preparation method thereof
CN119978304A
Resin for polyurethane microporous sole with high slip resistance and durability as well as preparation method and application of resin
CN121045501A