A thermoplastic polyester elastomer suitable for foaming, its preparation method and application

By adding zinc stearate, organic amide nucleating agents, and organic-inorganic hybrid titanium catalysts during the preparation of thermoplastic polyester elastomers, a dense crystalline structure is formed, which solves the problems of low melt strength and uneven cell structure of thermoplastic polyester elastomers in the supercritical foaming process, and realizes the preparation of high foaming ratio and low density foam materials.

CN123107052APending Publication Date: 2026-11-17XINJIANG BLUE RIDGE TUNHE CHEM IND JOINTSTOCK +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611076252.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing thermoplastic polyester elastomers have problems such as low melt strength, uneven cell structure, cracking and bulging, poor compression set retention, low delamination and tear strength, and poor resilience during supercritical foaming.

Method used

In the preparation of thermoplastic polyester elastomers, zinc stearate, organic amide nucleating agents, and organic-inorganic hybrid titanium catalysts are added. Through esterification and polycondensation reactions, a dense crystalline structure is formed, which improves melt strength and intrinsic viscosity. The synergistic effect enhances the stability and foaming effect of the material.

Benefits of technology

It effectively improves the melt strength and intrinsic viscosity of thermoplastic polyester elastomers, reduces bulk density, and solves the problems of cracking and bulging, poor compression set retention, uneven cell structure, low delamination tear strength and poor resilience in foamed materials, thus obtaining high foaming ratio, uniform closed-cell structure and low density foam materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention provides a foamed thermoplastic polyester elastomer, its preparation method, and its application, relating to the field of polymer materials technology. The preparation method includes the following steps: (1) using diols, diacids, and polyether ester polyols and / or polyethylene glycol as raw materials, an esterification reaction is carried out in the presence of an esterification catalyst to obtain an esterification product; (2) the esterification product, an organic amide nucleating agent, and zinc stearate are subjected to a polycondensation reaction in the presence of an organic-inorganic hybrid titanium catalyst; the organic amide nucleating agent is an aromatic diamide or a phenyltriamide nucleating agent. The preparation method of this invention is simple, and while reducing the melting point of the thermoplastic polyester elastomer, it can effectively improve the melt strength, intrinsic viscosity, and material crystallinity, and reduce the bulk density, thus solving the problems of cracking and bulging, poor compression set retention, uneven cell structure, low delamination tear strength, and poor resilience in foamed materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and in particular to a thermoplastic polyester elastomer suitable for foaming, its preparation method and application. Background Technology

[0002] Thermoplastic polyester elastomer (TPEE) is widely used in automotive cushioning components, cold chain packaging, track pads, and sports shoes due to its excellent low-temperature toughness, resilience, and processability. The preparation of lightweight TPEE materials through supercritical foaming is an important development direction for the industry.

[0003] TPEE elastomers have high melting points, low molecular weight, low intrinsic viscosity, and low melt strength. During supercritical foaming, supercritical fluids cannot easily penetrate between TPEE polymer chains, and cannot effectively encapsulate gas during depressurization, resulting in reduced performance of polyester elastomer foam materials, such as low expansion ratio, cracking and bulging, poor compression set retention, insufficient resilience, and uneven cell structure.

[0004] To lower the melting point and processing temperature of TPEE elastomers and improve rate performance, a common approach is to reduce crystallinity. This is often achieved by adding comonomers. For example, CN105778066A proposes a method for preparing low-melting-point polyesters, using diols and diacids as trimonomers and tetramonomers to perform secondary copolymerization modification with finished polyester PET products. CN109476869A proposes a method for preparing ester-based elastomer foamed molded bodies, in which isophthalic acid is added to the polyester hard segment to disrupt regularity.

[0005] Although the above methods can reduce crystallinity, too low crystallinity will reduce the strength of the material. The resulting TPEE elastomer has defects such as low melt strength, easy adhesion, and high bulk density. The foamed polyester elastomer material still has problems such as cracks and bulges, poor compression deformation retention, uneven cell structure, low delamination tear strength, and poor resilience.

[0006] In view of this, the present invention is hereby proposed. Summary of the Invention

[0007] This invention provides a thermoplastic polyester elastomer suitable for foaming, its preparation method, and its application. The preparation method can effectively improve melt strength and intrinsic viscosity, and reduce bulk density while lowering the melting point of the thermoplastic polyester elastomer. It solves the problems of cracking and bulging, poor compression set retention, uneven cell structure, low delamination tear strength, and poor resilience in foamed materials.

[0008] A first aspect of the present invention provides a method for preparing a foamed thermoplastic polyester elastomer, comprising the following steps: (1) Using alcohol A, diacid and alcohol B as raw materials, an esterification reaction is carried out in the presence of an esterification catalyst to obtain an esterification product; wherein alcohol A is a diol and alcohol B is a polyether ester polyol and / or polyethylene glycol; (2) The esterification product, organic amide nucleating agent and zinc stearate are subjected to polycondensation reaction in the presence of an organic-inorganic hybrid titanium catalyst; The organic amide nucleating agent is an aromatic diamide and / or a phenyltriamide nucleating agent. The aromatic diamide nucleating agent is selected from at least one of N,N'-dicyclohexylterephthalamide and N,N'-dicyclohexyl-2,6-naphthalenediamide. The phenyltriamide nucleating agent is selected from at least one of 1,3,5-tris(2,2-dimethylpropamido)benzene, 1,3,5-tris(cyclohexylcarbamoyl)benzene and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)amidebenzene.

[0009] In the polycondensation reaction step of thermoplastic polyester elastomer preparation, this invention adds zinc stearate, an organic-inorganic hybrid titanium catalyst, and an organic amide nucleating agent. During polymerization, zinc stearate acts as a lubricant and catalyst, preventing the material from sticking to the stirring paddle, increasing the surface renewal rate of the material, accelerating the molecular weight increase, and improving the molecular weight. The organic amide nucleating agent promotes the formation of finer grains and a denser crystal structure. Although it increases crystallinity to some extent, the denser crystal structure still allows the thermoplastic polyester elastomer to maintain its low melting point, forming a finer and more uniform cell structure. This promotes the simultaneous improvement of intrinsic viscosity, melt index, and mechanical properties, while reducing bulk density. Simultaneously, the organic-inorganic hybrid titanium catalyst further increases the molecular weight and synergistically improves intrinsic viscosity. Furthermore, the lubricating effect of zinc stearate facilitates the dispersion of the organic-inorganic hybrid titanium catalyst and the organic amide nucleating agent, avoiding uneven polymerization and nucleation, further improving the stability of the material.

[0010] The synergistic effect of these three factors not only enhances the melt strength of thermoplastic polyester elastomers, enabling them to be effectively coated by the melt during supercritical fluid depressurization foaming, thus inhibiting cell wall rupture and preventing cracking and bulging, but also improves the melt flowability during foaming due to their high intrinsic viscosity. This helps to improve the penetration effect of supercritical fluids, forming a more uniform cell structure and endowing the cells with excellent reversible deformation capabilities. This results in high foaming ratio, uniform closed-cell structure, and low-density foam materials, improving the delamination tear strength, compression set retention rate, and resilience of thermoplastic polyester elastomer foam materials.

[0011] With the synergistic effect of zinc stearate, organic amide nucleating agents and organic-inorganic hybrid titanium catalysts, the reaction time can be shortened (especially the polycondensation time can be shortened from the conventional 6 hours to less than 3 hours), the end carboxyl content of the product can be reduced, and the molecular weight reduction caused by moisture and high temperature during the foaming process can be reduced, so that the foamed material can maintain better performance.

[0012] Furthermore, the mass ratio of the organic amide nucleating agent, the zinc stearate, and the organic-inorganic hybrid titanium catalyst is 3-5:1-2:1-3, preferably 3:1:1.5.

[0013] Preferably, the amount of the organic amide nucleating agent is 1000-4000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. If the amount of organic amide nucleating agent is too low, it cannot effectively exert the nucleating effect; if it is too high, it will cause poor dispersion and may lead to agglomeration.

[0014] Preferably, the amount of zinc stearate used is 400-1500 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. Too little zinc stearate will result in insufficient lubrication and slow liquid surface renewal; too much will hinder molecular weight growth and reduce the degree of polymerization.

[0015] Preferably, the amount of the organic-inorganic hybrid titanium catalyst is 500-2000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. Too low a dosage of the organic-inorganic hybrid titanium catalyst results in poor catalytic effect; too high a dosage leads to problems such as increased side reactions and higher costs.

[0016] Furthermore, the organic-inorganic hybrid titanium catalyst is selected from at least one of titanium-silicon composite catalysts, titanium-phosphorus-nitrogen composite catalysts, titanium ester catalysts modified with inorganic nanomaterials, and titanium-based polyester catalysts.

[0017] Preferably, the titanium-silicon composite catalyst comprises at least one of titanium-silicon molecular sieves, mesoporous titanium-silicon materials, and amorphous titanium-silicon composite oxides.

[0018] Preferably, the titanium-phosphorus-nitrogen composite catalyst includes at least one of titanium-phosphorus-nitrogen oxides, titanium-oxygen phosphate, phosphorus-containing titanium-silicon-nitrogen oxides, carbon nitride-titanium phosphate composites, supported titanium phosphide, or titanium nitride.

[0019] Preferably, the inorganic nanomaterial-modified titanate catalyst includes at least one of oxide nanomaterial-modified titanium dioxide, metal nanoparticle-modified titanium dioxide, and carbon nanomaterial-modified titanium dioxide.

[0020] More preferably, the titanium dioxide modified with the oxide nanomaterial is selected from at least one of SiO2 / TiO2, Fe3O4 / TiO2, and Al2O3 / TiO2.

[0021] More preferably, the titanium dioxide modified with metal nanoparticles is selected from at least one of Au / TiO2, Ag / TiO2, and Pt / TiO2.

[0022] More preferably, the carbon nanomaterial-modified titanium dioxide is selected from at least one of graphene / TiO2 and carbon nanotube / TiO2.

[0023] Furthermore, the polycondensation reaction is carried out at a temperature of 230-240°C, a vacuum degree of less than 20 Pa, and a time of less than 3 hours, preferably 2-3 hours. At this temperature, the polycondensation reaction is more suitable for the organic-inorganic hybrid titanium catalyst, the organic amide nucleating agent, and zinc stearate to function effectively. If the temperature is too low, the reaction cannot proceed; if the temperature is too high, side reactions will be enhanced, and the effectiveness of the organic-inorganic hybrid titanium catalyst, the organic amide nucleating agent, and zinc stearate will be reduced or even rendered ineffective. Ultimately, this results in a low molecular weight product, poor color, and reduced melt strength during the foaming process.

[0024] Further, the diol is selected from at least one of 1,4-butanediol, ethylene glycol, cyclohexanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,5-pentanediol, and the diacid is selected from at least one of terephthalic acid, isophthalic acid, adipic acid and succinic acid.

[0025] Preferably, step (1) includes the following steps: S1. The diol, terephthalic acid, and esterification catalyst are mixed and esterification reaction is carried out to achieve an esterification rate of over 90% to obtain esterified product A. S2. The diol, isophthalic acid, and esterification catalyst are mixed and esterification reaction is carried out to achieve an esterification rate of over 90% to obtain esterified product B. S3. Mix the diol, adipic acid and / or succinic acid, and esterification catalyst to carry out an esterification reaction, so that the esterification rate reaches more than 90%, and obtain esterified product C. S4. After mixing the esterified compound A, the esterified compound B, and the esterified compound C, the polyether ester polyol and / or polyethylene glycol are added to carry out the esterification reaction, so that the esterification rate reaches more than 95%, and the esterified product is obtained.

[0026] In the above technical solution, during the esterification reaction, the regularity of the molecular chain can be changed by adding isophthalic acid and oxalic acid, thereby reducing the crystallinity and melting point and increasing the foaming ratio. Moreover, by adjusting the raw material combination and sequence of the esterification reaction, the present invention can accelerate the reaction speed and increase the molecular weight and intrinsic viscosity.

[0027] Polyether ester polyols (especially PTMEG) have poor thermal stability. If they remain in the pulping tank and esterification vessel for 1-2 hours, end-group degradation will produce substances that increase the b-value (yellowness). If added at the end of esterification, before the establishment of the high vacuum in the polycondensation reaction, the heating time of the polyether ester polyol is compressed to 30-45 minutes, significantly avoiding decomposition and increasing the molecular weight and intrinsic viscosity of the product, thereby improving the melt strength of TPEE during foaming. Simultaneously, adding it at the end of esterification also facilitates the formation of a strong and robust two-phase separation network, improving product color and soft segment integrity.

[0028] It should be noted that the order of steps S1-S3 in this invention can be flexibly adjusted according to actual process requirements. There is no strict sequential dependency between the steps, and any arrangement or combination can achieve the technical effect of this invention.

[0029] Preferably, the esterification catalyst is selected from at least one of tetrabutyl titanate, tetraisopropyl titanate, tetra(2-ethylhexyl) titanate, and titanium acetylacetonate.

[0030] Preferably, the polyether ester polyol is selected from at least one of polytetramethylene ether diols with a number average molecular weight of 1000-2000.

[0031] More preferably, the polyether ester polyol is selected from at least one of polytetramethylene ether glycol with a number average molecular weight of 1000, polytetramethylene ether glycol with a number average molecular weight of 1800, and polytetramethylene ether glycol with a number average molecular weight of 2000.

[0032] Further, in step S1, the molar ratio of the diol to terephthalic acid is 1.0-2.0:1, the amount of the esterification catalyst is 250-1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer, and preferably the esterification temperature is 200-230℃, the time is 1-2h, and the pressure is 60-80KPa.

[0033] Further, in step S2, the molar ratio of the diol and isophthalic acid is 1.0~2.0:1, and the amount of the esterification catalyst is 250-1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230℃, the time is 1-2h, and the pressure is 60-80KPa.

[0034] Further, in step S3, the molar ratio of the diol to adipic acid and / or succinic acid is 1.0~2.0:1, and the amount of the esterification catalyst is 250-1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230℃, the time is 1-2h, and the pressure is 60-80KPa.

[0035] Further, in step S4, the amount of polyether ester polyol and / or polyethylene glycol used is 30-50% of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230℃, the time is 0.5-1h, and the pressure is 60-80KPa.

[0036] During the esterification reaction, parameters such as temperature and pressure must be strictly controlled to ensure that the esterification reaction can proceed normally. The raw material ratio must also be strictly controlled to ensure that the basic parameters such as melting point and hardness of the final product meet the requirements.

[0037] Further, during the polycondensation reaction in step (2), antioxidants and / or crosslinking agents are added. The antioxidants include a primary antioxidant and a secondary antioxidant. The primary antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, 2,6-di-tert-butyl-4-cresol, and 4,4'-di(α,α-dimethylbenzyl)diphenylamine, and is used in an amount of 500-5000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. The secondary antioxidant is selected from at least one of tris(2,4-di-tert-butylphenyl) phosphite and dioctadecyl thiodipropionate, and is used in an amount of 500-5000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer.

[0038] Furthermore, the crosslinking agent is selected from at least one of glycerol, pentaerythritol, triglycidyl isocyanurate (TGIC), triallyl isocyanurate (TAIC), and trimethylolpropane (TMP), and is used in an amount of 200-800 ppm. The crosslinking agent can reduce the carboxyl content of the product, accelerate the polymerization rate, and improve the melt strength of the material during the foaming process; the antioxidant can improve the heat resistance of the final product.

[0039] In a second aspect, the present invention provides a thermoplastic polyester elastomer suitable for foaming prepared by the above-described preparation method.

[0040] Preferably, the thermoplastic polyester elastomer has a melting point of 145±2℃, a crystallinity of 14±2%, an intrinsic viscosity of 1.83±0.2dl / g, a terminal carboxyl group content of 18±2mol / t, and a number-average molecular weight of 100,000-110,000.

[0041] A third aspect of the present invention provides a thermoplastic polyester elastomer suitable for foaming prepared by the above-described preparation method, or the application of the above-described thermoplastic polyester elastomer suitable for foaming in the preparation of foamed materials.

[0042] In a fourth aspect, the present invention provides a polyester elastomer foam material, which is prepared by using a thermoplastic polyester elastomer suitable for foaming obtained by the above preparation method or the above-mentioned thermoplastic polyester elastomer suitable for foaming as raw material, mixing with a supercritical fluid and performing supercritical foaming.

[0043] Preferably, the supercritical fluid includes supercritical nitrogen or supercritical carbon dioxide.

[0044] Furthermore, the parameters of the supercritical foaming include: temperature of 120-130℃, pressure of 15-18MPa, pressure holding time of 60-80min, and pressure relief rate of 5-15MPa / s.

[0045] The beneficial effects of the present invention on a foamed thermoplastic polyester elastomer, its preparation method, and its application include at least the following: The preparation method of the present invention is simple. During the polycondensation process, zinc stearate, organic amide nucleating agents, and organic amide nucleating agents are added. While lowering the melting point of the thermoplastic polyester elastomer, the melt strength and intrinsic viscosity can be effectively improved, and the bulk density can be reduced. This solves the problems of cracking and bulging, poor compression set retention, uneven cell structure, low delamination tear strength, and poor resilience in foamed materials. Detailed Implementation

[0046] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0047] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field, or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.

[0048] Raw material information: Tetrabutyl titanate: Titanium content: 13.5%-14.4%, chloride ion: ≤50mg / Kg, color number: ≤100, density: 0.990-1.010g / cm³ 3 Manufacturer: Shandong Jianbang New Materials; Organic amide nucleating agent: N,N'-dicyclohexyl terephthalamide, whiteness: ≥90, particle size: 10μm, non-volatile content (105℃): ≥98.5%, manufacturer: Chenghe Technology, brand: TMB-5; Organic-inorganic hybrid titanium catalyst: titanium-based polyester catalyst, titanium content: 2.5%; density: 1.08-1.12 g / cm³ 3 Moisture content: ≤0.3%, thermal decomposition temperature: ≥265℃, manufacturer: Shanghai Huiyi New Material Technology Co., Ltd., grade: DH-HyTi; Polytetramethylene ether glycol: PTMEG-1000, melting point: 28-32℃, average molecular weight: 950-1050g / mol, hydroxyl value: 112.2-114.5mgKOH / g, moisture: ≤100mg / Kg. Manufacturer: Xinjiang Lanshan Tunhe Technology Co., Ltd., brand name: PTMEG-1000.

[0049] Example 1 This embodiment provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are as follows: (1) 2.6 kg of 1,4-butanediol (BDO), 3 kg of terephthalic acid (PTA) and 9 g of tetrabutyl titanate were added to a 10 L esterification reactor and esterification reaction was carried out at 230 °C and 60 kPa. After 2 h of reaction, the esterification rate reached 90% and esterified product A was obtained. (2) Add 0.325 kg BDO, 0.28 kg isophthalic acid and 0.9 g tetrabutyl titanate to a 3 L esterification reactor and carry out esterification reaction at 230 °C and 60 kPa. After 1.5 h of reaction, the esterification rate reaches 90% and esterified product B is obtained. (3) Add 0.286 kg BDO, 0.28 kg adipic acid and 0.9 g tetrabutyl titanate to a 3 L esterification reactor and carry out esterification reaction at 230 °C and 60 kPa. After 1.5 h of reaction, the esterification rate reaches 90% and esterification product C is obtained. (4) Ester A, ester B and ester C were sent to a 20L esterification reactor and 3.33kg of polytetramethylene ether glycol (PTMEG) was added. The esterification reaction was further carried out at 230℃ and 60Kpa. After esterification for 0.5h, the esterification rate reached 95% and the esterified product was obtained. (5) The esterification product is mixed with 20g of N,N'-dicyclohexyl terephthalamide, 10g of titanium-based polyester catalyst, 7g of zinc stearate, 20g of antioxidant B215, and 300g of glycerol and sent to a 20L polycondensation reactor for polycondensation reaction. After reacting for 3h at a temperature of 230℃ and a vacuum of 20pa, a polyester elastomer suitable for foaming is obtained.

[0050] This embodiment also discloses a method for preparing a polyester elastomer foam material, the steps of which are as follows: (1) Pretreatment: The polyester elastomer is vacuum dried at 80°C for 4 hours to remove moisture and prevent hydrolysis from causing a decrease in melt strength; the dried polyester elastomer is then injection molded into a shoe blank, and after stress relief, it is placed in a high-pressure reactor with a circulation system. (2) Supercritical carbon dioxide fluid foaming: Supercritical carbon dioxide fluid is used as a foaming agent for foaming. The foaming temperature is 125℃, the pressure is 17MPa, and the holding time is 70min, so that CO2 can be fully dissolved and diffused to reach saturation concentration. (3) Depressurization: Quickly open the pressure relief valve and reduce the pressure inside the vessel to atmospheric pressure at a pressure relief rate of 10 MPa / s to obtain the foamed sample; (4) After shaping and cooling, the foamed sample is taken out and placed at room temperature to cool; (5) Degassing: Place at room temperature for 24-48 hours to allow residual CO2 to slowly escape, avoiding dimensional shrinkage, and obtain polyester elastomer foam material.

[0051] Example 2 This embodiment provides a method for preparing a foamed thermoplastic polyester elastomer. The steps are basically the same as those in Example 1, except that in step (5), 8g of N,N'-dicyclohexyl terephthalamide, 4g of titanium-based polyester catalyst, and 2.6g of zinc stearate are used.

[0052] This embodiment also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Embodiment 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this embodiment.

[0053] Example 3 This embodiment provides a method for preparing a foamed thermoplastic polyester elastomer. The steps are basically the same as those in Example 1, except that in step (5), there are 32g of N,N'-dicyclohexyl terephthalamide, 16g of titanium-based polyester catalyst, and 10.6g of zinc stearate.

[0054] This embodiment also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Embodiment 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this embodiment.

[0055] Example 4 This embodiment provides a method for preparing a foamed thermoplastic polyester elastomer. The steps are basically the same as those in Example 1, except that in step (5), 25g of N,N'-dicyclohexyl terephthalamide, 3g of titanium-based polyester catalyst, and 10g of zinc stearate are used.

[0056] This embodiment also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Embodiment 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this embodiment.

[0057] Example 5 This embodiment provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are as follows: (1) 3.211 kg of 1,4-butanediol (BDO), 3 kg of terephthalic acid (PTA), 0.28 kg of isophthalic acid, 0.28 kg of adipic acid, 3.33 kg of polytetramethylene ether glycol (PTMEG), and 10.8 g of tetrabutyl titanate were added to a 20 L esterification reactor and esterified at 230 °C and 60 kPa. After 3 h of reaction, the esterification rate reached 90%, and the esterified product was obtained. (2) 20g of N,N'-dicyclohexyl terephthalamide, 10g of titanium-based polyester catalyst, 7g of zinc stearate, 20g of antioxidant B215, and 300g of glycerol were added to the esterified product in (1) and polycondensation reaction was carried out at a temperature of 230℃ and a vacuum of 20pa. After 3h of reaction, a polyester elastomer suitable for foaming was obtained.

[0058] This embodiment also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Embodiment 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this embodiment.

[0059] Comparative Example 1 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that N,N'-dicyclohexyl terephthalamide is not added in step (5).

[0060] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0061] Comparative Example 2 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that zinc stearate is not added in step (5).

[0062] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0063] Comparative Example 3 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that a titanium-based polyester catalyst is not added in step (5).

[0064] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0065] Comparative Example 4 This comparative example provides a method for preparing a foamable thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that N,N'-dicyclohexyl terephthalamide and zinc stearate are not added.

[0066] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0067] Comparative Example 5 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that: no titanium-based polyester catalyst and zinc stearate are added.

[0068] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0069] Comparative Example 6 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that N,N'-dicyclohexyl terephthalamide and titanium-based polyester catalyst are not added.

[0070] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0071] Comparative Example 7 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that N,N'-dicyclohexyl terephthalamide is replaced by a sorbitol-based nucleating agent (manufacturer and brand name Millad 3988).

[0072] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0073] Comparative Example 8 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that zinc stearate is replaced by zinc acetate.

[0074] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0075] Comparative Example 9 This comparative example provides a method for preparing a foamed thermoplastic polyester elastomer, the steps of which are basically the same as those in Example 1, except that the titanium-based polyester catalyst is replaced by tetrabutyl titanate in equal mass.

[0076] This comparative example also discloses a method for preparing a polyester elastomer foam material, the steps of which are the same as in Example 1, except that the thermoplastic polyester elastomer suitable for foaming used is the thermoplastic polyester elastomer prepared in this comparative example.

[0077] Experimental Example 1 The present invention measured the melt index, melting point, crystallinity, molecular weight, intrinsic viscosity, melt strength, terminal carboxyl group content, and hardness of the foamed thermoplastic polyester elastomers prepared in the examples and comparative examples. The measurement methods are as follows: Melt index: ISO 868 (2.16 kg, 190 °C); Melting point: ISO 11357-3; Crystallinity: ISO 11357-3; Hardness: ISO 868; Molecular weight: GB / T 1040.1-2025; Intrinsic viscosity: GB / T 14190-2017; Tensile strength: GB / T 21863-2008; Terminal carboxyl group content: GB / T 14190-2017.

[0078] The results are shown in Table 1: As shown in Table 1, the intrinsic viscosity and molecular weight of the thermoplastic polyester elastomers prepared in Examples 1-5 are higher than those in Comparative Examples 1-9, while the end carboxyl group content is generally lower than that in Comparative Examples 1-9. Moreover, although the crystallinity of Example 1 is higher than that of Comparative Example 1, its melting point is not significantly different from that of Comparative Example 1. This indicates that organic amide nucleating agents can promote the formation of dense crystals in materials, thereby improving the crystallinity to a certain extent while maintaining the low melting point characteristics. Under the synergistic effect of organic amide nucleating agents, zinc stearate, and organic-inorganic hybrid titanium catalysts, thermoplastic polyester elastomers can maintain low melting point characteristics while effectively increasing molecular weight and intrinsic viscosity and reducing end carboxyl group content.

[0079] Experiment Example 2 The present invention measured the drop ball rebound performance, delamination tear strength, compression set retention, and cell structure of the polyester elastomer foam materials prepared in the examples and comparative examples. The measurement methods are as follows: Rebound: Measured according to ISO 8307.

[0080] Delamination tear strength: determined with reference to GB / T 3903.29.

[0081] Compression set: GB / T 6669.

[0082] Hardness: Measured according to ASTM D2240.

[0083] The results are shown in Table 2: As shown in Table 2, the tensile strength, delamination tear strength, and resilience of the polyester elastomer foam materials prepared in Examples 1-5 are all higher than those in Comparative Examples 1-9, while the compression set is lower than that in Comparative Examples 1-9. This indicates that the synergistic effect of zinc stearate and the organic-inorganic hybrid titanium catalyst can effectively improve the performance of thermoplastic polyester elastomers, enhance their foaming effect, and obtain foam materials with high foaming ratio, uniform closed-cell structure, and low density. This improves the tensile strength, delamination tear strength, compression set, and resilience of the thermoplastic polyester elastomer foam materials.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing foamed thermoplastic polyester elastomers, characterized in that, Includes the following steps: (1) Using alcohol A, diacid and alcohol B as raw materials, esterification reaction is carried out in the presence of esterification catalyst to obtain esterification product; Alcohol A is a diol, and alcohol B is a polyether ester polyol and / or polyethylene glycol; (2) The esterification product, organic amide nucleating agent and zinc stearate are subjected to polycondensation reaction in the presence of an organic-inorganic hybrid titanium catalyst; The organic amide nucleating agent is an aromatic diamide and / or a triphenyl amide nucleating agent. The aromatic diamide nucleating agent is selected from at least one of N,N'-dicyclohexylterephthalamide and N,N'-dicyclohexyl-2,6-naphthalenediamide. The triphenyl amide nucleating agent is selected from at least one of 1,3,5-tris(2,2-dimethylpropamido)benzene, 1,3,5-tris(cyclohexylcarbamoyl)benzene and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)amidebenzene.

2. The method for preparing foamed thermoplastic polyester elastomers according to claim 1, characterized in that, The mass ratio of the organic amide nucleating agent, the zinc stearate, and the organic-inorganic hybrid titanium catalyst is 3-5:1-2:1-3; Preferably, the amount of the organic amide nucleating agent is 1000-4000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; Preferably, the amount of zinc stearate used is 400-1500 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; Preferably, the amount of the organic-inorganic hybrid titanium catalyst is 500-2000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer.

3. The method for preparing foamed thermoplastic polyester elastomers according to claim 1 or 2, characterized in that, The organic-inorganic hybrid titanium catalyst is selected from at least one of titanium-silicon composite catalysts, titanium-phosphorus-nitrogen composite catalysts, inorganic nanomaterial-modified titanate catalysts, and titanium-based polyester catalysts. Preferably, the titanium-silicon composite catalyst comprises at least one of titanium-silicon molecular sieves, mesoporous titanium-silicon materials, and amorphous titanium-silicon composite oxides; Preferably, the titanium-phosphorus-nitrogen composite catalyst comprises at least one of titanium-phosphorus-nitrogen oxides, titanium-oxygen phosphate, phosphorus-containing titanium-silicon-nitrogen oxides, carbon nitride-titanium phosphate composites, supported titanium phosphide, or titanium nitride. Preferably, the inorganic nanomaterial-modified titanate catalyst includes at least one of oxide nanomaterial-modified titanium dioxide, metal nanoparticle-modified titanium dioxide, and carbon nanomaterial-modified titanium dioxide.

4. The method for preparing a foamed thermoplastic polyester elastomer according to any one of claims 1-3, characterized in that, The polycondensation reaction is carried out at a temperature of 230-240℃, a vacuum degree of less than 20Pa, and a time of less than 3 hours.

5. The method for preparing a foamed thermoplastic polyester elastomer according to any one of claims 1-4, characterized in that, The diol is selected from at least one of 1,4-butanediol, ethylene glycol, cyclohexanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and 1,5-pentanediol, and the dicarboxylic acid is selected from at least one of terephthalic acid, isophthalic acid, adipic acid, and succinic acid. Preferably, step (1) includes the following steps: S1. The diol, terephthalic acid, and esterification catalyst are mixed and esterification reaction is carried out to achieve an esterification rate of over 90% to obtain esterified product A. S2. The diol, isophthalic acid, and esterification catalyst are mixed and esterification reaction is carried out to achieve an esterification rate of over 90% to obtain esterified product B. S3. Mix the diol, adipic acid and / or succinic acid, and esterification catalyst to carry out an esterification reaction, so that the esterification rate reaches more than 90%, and obtain esterified product C. S4. After mixing the esterified A, the esterified B, and the esterified C, add the polyether ester polyol and / or polyethylene glycol to carry out an esterification reaction, so that the esterification rate reaches more than 95%, and obtain the esterified product. Preferably, the esterification catalyst is selected from at least one of tetrabutyl titanate, tetraisopropyl titanate, tetra(2-ethylhexyl) titanate, and titanium acetylacetonate; Preferably, the polyether ester polyol is selected from at least one of polytetramethylene ether diols with a number average molecular weight of 1000-2000.

6. The method for preparing foamed thermoplastic polyester elastomers according to claim 5, characterized in that, In step S1, the molar ratio of the diol to terephthalic acid is 1.0-2.0:1, the amount of the esterification catalyst is 250-1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer, and preferably the esterification temperature is 220-230℃, the time is 1-2h, and the pressure is 60-80KPa. Alternatively, in step S2, the molar ratio of the diol to isophthalic acid is 1.0-2.0:1, and the amount of the esterification catalyst is 250-1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230°C, the time is 1-2 h, and the pressure is 60-80 kPa. Alternatively, in step S3, the mass ratio of the diol to adipic acid and / or succinic acid is 1.0~2.0:1, and the amount of the esterification catalyst is 250~1000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230℃, the time is 1-2h, and the pressure is 60-80KPa. Alternatively, in step S4, the amount of polyether ester polyol and / or polyethylene glycol used is 30-50% of the theoretical mass yield of the thermoplastic polyester elastomer; preferably, the esterification temperature is 220-230℃, the time is 0.5-1h, and the pressure is 60-80KPa.

7. The method for preparing a foamed thermoplastic polyester elastomer according to any one of claims 1-6, characterized in that, During the polycondensation reaction in step (2), antioxidants and / or crosslinking agents are added. The antioxidants include primary antioxidants and secondary antioxidants. The primary antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, 2,6-di-tert-butyl-4-cresol, and 4,4'-di(α,α-dimethylbenzyl)diphenylamine, and is used at an amount of 500-5000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. The secondary antioxidant is selected from at least one of tris(2,4-di-tert-butylphenyl) phosphite and dioctadecyl thiodipropionate, and is used at an amount of 500-5000 ppm of the theoretical mass yield of the thermoplastic polyester elastomer. Preferably, the crosslinking agent is selected from at least one of glycerol, pentaerythritol, triglycidyl isocyanurate (TGIC), triallyl isocyanurate (TAIC), and trimethylolpropane (TMP), and is used in an amount of 200-800 ppm of the theoretical mass yield of the thermoplastic polyester elastomer.

8. A thermoplastic polyester elastomer suitable for foaming, prepared by the method according to any one of claims 1-7.

9. The application of the thermoplastic polyester elastomer suitable for foaming prepared by the preparation method according to any one of claims 1-7, or the thermoplastic polyester elastomer suitable for foaming according to claim 8, in the preparation of foamed materials.

10. A polyester elastomer foam material, characterized in that, The thermoplastic polyester elastomer suitable for foaming, prepared by any one of the preparation methods of claims 1-7 or the thermoplastic polyester elastomer suitable for foaming as described in claim 8, is mixed with a supercritical fluid and subjected to supercritical foaming. Preferably, the supercritical fluid includes supercritical nitrogen or supercritical carbon dioxide; Preferably, the parameters of the supercritical foaming include: temperature of 120-130℃, pressure of 15-18MPa, pressure holding time of 60-80min, and pressure relief rate of 5-15MPa / s.

Citation Information

Patent Citations

  • Low-melting-point copolyester and preparing method thereof

    CN105778066A

  • Molded foam of ester-based elastomer, uses thereof, and expanded beads of ester-based elastomer

    CN109476869A