Oligomeric polyphenylene sulfide, polyphenylene sulfide resin, their preparation methods and applications

By controlling the molecular weight distribution and end-capping chlorine content, a high-temperature and corrosion-resistant polyphenylene sulfide resin was prepared, solving the problems of poor flowability and excessive chlorine content of PPS resin during high-temperature processing. This resin is suitable for the preparation of precision devices in the field of electronics and electrical appliances.

CN123107084APending Publication Date: 2026-11-17WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611498120.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PPS resins are prone to chain extension, cross-linking, or degradation during high-temperature processing or long-term use, resulting in poor flowability and excessive chlorine content, making it difficult to meet the environmental regulations in the electronics and electrical appliance industry.

Method used

By controlling the molecular weight distribution and end-capping chlorine content of low molecular weight polyphenylene sulfide, and by reacting specific low molecular weight polyphenylene sulfide with active thiol groups and halogen end groups, combined with appropriate feed ratios and polymerization processes, polyphenylene sulfide resins with narrow molecular weight distribution and low end-capping chlorine content can be prepared.

Benefits of technology

A polyphenylene sulfide resin with high temperature resistance, corrosion resistance, and good processing flowability was obtained, which is suitable for the preparation of high temperature precision components in the field of electronics and electrical appliances and meets environmental protection regulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107084A_ABST
    Figure CN123107084A_ABST
Patent Text Reader

Abstract

This application relates to the field of polymer synthesis technology, and particularly to oligomeric polyphenylene sulfide, polyphenylene sulfide resin, its preparation method, and its application. The oligomeric polyphenylene sulfide of this application has a weight-average molecular weight ≤8000 g / mol and a molar ratio of halogen-terminated to mercapto-terminated groups of (0.04-0.06):1. This oligomeric polyphenylene sulfide can be used to prepare polyphenylene sulfide resins with a narrow molecular weight distribution. The polyphenylene sulfide resin of this application has a halogen-terminated group content ≤300 ppm; a weight-average molecular weight of 20000 g / mol-40000 g / mol; and a mass percentage of components with a weight-average molecular weight in the range of 10000 g / mol-100000 g / mol ≥80%. This polyphenylene sulfide resin has a narrow molecular weight distribution, low end-capped chlorine content, good high-temperature resistance, and good processing fluidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer synthesis technology, and in particular to oligomeric polyphenylene sulfide, polyphenylene sulfide resin, preparation methods and applications thereof. Background Technology

[0002] Polyphenylene sulfide (PPS) is a high-performance thermoplastic engineering plastic. Its molecular backbone consists of alternating benzene rings and sulfur atoms, giving the material excellent heat resistance, dimensional stability, chemical stability, and intrinsic flame retardancy. Due to these properties, PPS has wide applications in the automotive, electronics, environmental filtration, and precision machinery industries, and is typically molded into various products through thermoforming methods such as injection molding and extrusion.

[0003] In recent years, with the rapid development of emerging industries such as new energy vehicles and humanoid robots, higher requirements have been placed on the performance of PPS resin. These applications often involve precision injection molding, which not only requires the resin to have excellent flowability in the molten state to fill complex thin-walled molds, but also demands that the products have stable mechanical properties and dimensional accuracy. Therefore, the development of PPS resin with low molecular weight and narrow molecular weight distribution has become a focus of industry attention. Low molecular weight ensures low melt viscosity, good flowability, and ease of processing; while a narrow molecular weight distribution means a uniform material composition, which can effectively avoid the uneven melting caused by high molecular weight components or the deterioration of mechanical properties caused by low molecular weight components, and is the key to ensuring the performance stability of products between batches.

[0004] Currently, the industrial production of PPS mainly employs a polycondensation reaction of sodium sulfide and p-dichlorobenzene in a polar solvent. Regardless of the raw material ratio, the resulting PPS resin molecular chains primarily consist of chlorine and mercapto groups at the end chains. These active end groups are prone to side reactions such as chain extension, cross-linking, or degradation during high-temperature processing or long-term use, leading to decreased material flowability and affecting the processing window. Furthermore, chlorine-containing salts embedded in the end groups and resin introduce residual chlorine. Chlorine may release corrosive hydrogen chloride gas in potential high-temperature failure scenarios in electronic and electrical products, endangering equipment safety. Moreover, most environmental regulations in the electronics and electrical fields (such as relevant EU requirements) have strict limits on the content of halogens such as bromine and chlorine (typically requiring chlorine content below 900 ppm and total halogens below 1500 ppm). Therefore, preparing PPS resin with low chlorine content is both a regulatory requirement and an essential requirement to ensure the safety of downstream applications.

[0005] To reduce the chlorine content of PPS, existing technologies have explored many approaches: (1) Adjusting the raw material ratio, changing the feeding procedure, or adding a phase transfer agent to reduce the end group chlorine content from the source. However, such methods often sacrifice the ability to control molecular weight, making it difficult to obtain products with low molecular weight and narrow distribution. Furthermore, a wider molecular weight distribution will reduce the thermal stability of the material. (2) Passivating the active end groups by adding end-capping agents (such as 4-phenylthio-phenylthiol or lorcabenzyl), or using mercapto-containing compounds to post-treat the resin. However, the end-capping agents used in the former are difficult to synthesize and costly, and it is difficult to achieve precise control of molecular weight distribution. The latter involves steps such as redissolution and high-temperature depolymerization, which are lengthy and cumbersome, and are not conducive to industrial promotion. (3) Using post-treatment methods such as vacuum distillation and solvent washing at the end of polymerization to remove volatile chlorine-containing components or free salts in the system. However, this method cannot eliminate chlorine atoms that are chemically bonded to the polymer chain ends, nor can it effectively remove inorganic salts that are tightly wrapped by the resin matrix. The dechlorination effect is limited.

[0006] Therefore, there is an urgent need to develop a polyphenylene sulfide resin with a narrow molecular weight distribution and low end-capped chlorine content. Summary of the Invention

[0007] Based on this, one or more embodiments of this application provide oligomeric polyphenylene sulfide, polyphenylene sulfide resin, preparation methods thereof, and applications. The oligomeric polyphenylene sulfide of this application can be used to prepare polyphenylene sulfide resins with outstanding flow properties, narrow molecular weight distribution, and excellent processing performance. The polyphenylene sulfide of this application has a narrow molecular weight distribution, low end-capped chlorine content, high temperature resistance, corrosion resistance, and good processing flowability.

[0008] One or more embodiments of this application provide oligomeric polyphenylene sulfides having a weight-average molecular weight ≤8000 g / mol;

[0009] The components of the oligomeric polyphenylene sulfide include different cyclic polyphenylene sulfides and linear polyphenylene sulfides;

[0010] The different linear polyphenylene sulfides each independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the number of moles of halogen elements contained in each halogen end group is X1, the sum of the number of moles of sulfur elements contained in each mercapto end group is X2, the sum of the mass of halogen elements contained in each halogen end group is Y1, and the sum of the mass of sulfur elements contained in each mercapto end group is Y2.

[0011] The mass of the oligomeric polyphenylene sulfide is Z1;

[0012] X1:X2=(0.04-0.06):1;

[0013] 0.8%≤(Y1+Y2) / Z1≤1.5%.

[0014] In some embodiments, the cyclic polyphenylene sulfide comprises structural units of formula (I) repeated in a number of 2-20;

[0015] The linear polyphenylene sulfide comprises structural units of formula (Ⅰ) with a repeating number of 10-75;

[0016] (I).

[0017] In some embodiments, the molecular weight distribution of the oligomeric polyphenylene sulfide is 2.5 to 4.0.

[0018] In some embodiments, the linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the oligomeric polyphenylene sulfide.

[0019] The preparation method of oligomeric polyphenylene sulfide according to one or more embodiments of this application includes the following steps:

[0020] Organic solvent A, sulfur source A and alkali metal hydroxide A are mixed and dehydrated to obtain mixture A;

[0021] The mixture A, dihaloaromatic compound A, and organic solvent B are mixed in a sealed container, and the resulting reaction solution A is subjected to a first-stage gradient temperature increase. The first-stage gradient temperature increase program includes: 0-60 min, from 20℃-40℃ to 220℃-225℃; 60 min-90 min, from 220℃-225℃ to 230℃; 90 min-150 min, from 230℃ to 240℃.

[0022] After the first stage of gradient heating is completed, dihaloaromatic compound B and organic solvent C are added and mixed within 60 min, while the resulting reaction solution B is subjected to a second stage of gradient heating. The program for the second stage of gradient heating includes: heating from 240℃ to 250℃ in 150 min to 240 min.

[0023] In some embodiments, the molar amount of sulfur in sulfur source A is X1 mol;

[0024] The sum of the molar amounts of dihaloaromatic compound A and dihaloaromatic compound B is X2mol;

[0025] The sum of the molar amounts of organic solvent A, organic solvent B, and organic solvent C is X3 mol;

[0026] X1:X2:X3=1:(0.75-0.95):(1.7-3).

[0027] One or more embodiments of this application also provide a polyphenylene sulfide resin having a weight-average molecular weight of 20,000 g / mol to 40,000 g / mol.

[0028] The polyphenylene sulfide resin comprises different cyclic polyphenylene sulfide and linear polyphenylene sulfide, wherein the sum of the masses of the components with a weight-average molecular weight in the range of 10,000 g / mol to 100,000 g / mol is Y3.

[0029] The different linear polyphenylene sulfides each independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the mass of chlorine elements contained in each halogen end group is Y4;

[0030] The mass of the polyphenylene sulfide resin is Z2;

[0031] Y3 / Z2 ≥ 80%;

[0032] Y4 / Z2≤0.03%.

[0033] In some embodiments, the cyclic polyphenylene sulfide comprises structural units of formula (I) repeated in a number of 2-20;

[0034] The linear polyphenylene sulfide comprises structural units of formula (Ⅰ) with a repeating number of 25-400;

[0035] (I).

[0036] In some embodiments, the polyphenylene sulfide resin has a molecular weight distribution of 4.0-6.0.

[0037] In some embodiments, the melt index of the polyphenylene sulfide resin at 315°C / 5Kg is 500-1500 g / 10min.

[0038] In some embodiments, the linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the polyphenylene sulfide resin.

[0039] The preparation method of polyphenylene sulfide resin according to one or more embodiments of this application includes the following steps:

[0040] The first organic solvent, sulfur source and alkali metal hydroxide are mixed and dehydrated to obtain the first mixture;

[0041] The first mixture, the dihalo aromatic compound, and the second organic solvent are mixed in a sealed container. The resulting first reaction solution is heated to 225°C-230°C and kept at that temperature for a reaction. The pressure inside the sealed container is increased to X1MPa and then begins to decrease.

[0042] After the pressure inside the sealed container is reduced to X2MPa, oligomeric polyphenylene sulfide and a third organic solvent are added to the sealed container and mixed. The resulting second reaction solution is heated from 225℃-230℃ to 250℃-270℃, and then heating is stopped; X2 / X1×100% = 90%-98%; the oligomeric polyphenylene sulfide is the oligomeric polyphenylene sulfide described above, or the oligomeric polyphenylene sulfide prepared by the preparation method described above;

[0043] The reaction liquid in the sealed container is cooled and then subjected to solid-liquid separation to obtain the polyphenylene sulfide resin.

[0044] In some embodiments, the heat preservation reaction lasts for 90-300 minutes; and / or,

[0045] Within 30 minutes after the pressure inside the sealed container decreases to X2MPa, the oligomeric polyphenylene sulfide and the third organic solvent are added to the sealed container.

[0046] In some embodiments, the process of heating the resulting first reaction solution to 225°C-230°C includes:

[0047] The temperature was increased from 20℃-40℃ to 220℃ in 0-60 minutes.

[0048] The temperature is increased from 220℃ to 225℃-230℃ over 60-90 minutes; and / or,

[0049] The procedure for heating the resulting second reaction solution from 225℃-230℃ to 250℃-270℃ includes:

[0050] The temperature was increased from 225℃-230℃ to 240℃-245℃ in 0-60 minutes.

[0051] The temperature was increased from 240℃-245℃ to 250℃-270℃ over a period of 60-300 minutes.

[0052] One or more embodiments of this application also provide the application of the polyphenylene sulfide resin described herein or the polyphenylene sulfide resin prepared by the described method in the preparation of high-temperature resistant materials.

[0053] The polyphenylene sulfide resin of this application has the advantages of narrow molecular weight distribution and low end-capped chlorine content, good high temperature resistance, and excellent processing fluidity, and can be used to prepare high temperature precision devices in the field of electronics and electrical appliances.

[0054] The method for preparing polyphenylene sulfide resin of this application involves adding specific low molecular weight polyphenylene sulfide at an appropriate time during polymerization. The oligomer with extremely low chlorine content can react with active thiol groups and halogen-terminated groups, thereby effectively controlling the end-capping chlorine content. In addition, by adjusting the oligomer structure and feeding ratio, a large number of oligomers are linked to the original polyphenylene sulfide chain, thereby effectively controlling the molecular weight distribution and obtaining the aforementioned polyphenylene sulfide resin with a narrow molecular weight distribution and low end-capping chlorine content. Attached Figure Description

[0055] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0056] Figure 1 This is a process flow diagram for the preparation of the oligomeric polyphenylene sulfide of this application.

[0057] Figure 2 This is a process flow diagram for the preparation of the polyphenylene sulfide resin of this application. Detailed Implementation

[0058] The present application is further described below with reference to embodiments and examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Furthermore, it should be understood that after reading the teachings of this application, those skilled in the art can make various alterations or modifications to this application, and these equivalent forms also fall within the protection scope of the appended claims.

[0059] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0060] The terms "and / or," "or / and," and "and / or" as used herein include any one of two or more related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations encompass any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that, in this application, the technical solution undoubtedly includes solutions connected by "logical AND," and also undoubtedly includes solutions connected by "logical OR." For example, "A and / or B" includes three parallel solutions: A, B, and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, a technical solution that is connected by "logical OR"), as well as any and all combinations of A, B, C, and D, that is, combinations of any two or three of A, B, C, and D, and also combinations of all four of A, B, C, and D (that is, a technical solution that is connected by "logical AND").

[0061] In this document, terms such as "preferred," "better," and "more preferred" are merely descriptions of implementation methods or examples that achieve better results, and should be understood as not constituting a limitation on the scope of protection of this application.

[0062] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0063] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0064] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, optional numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval points to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges may be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.

[0065] In this application, mass can be a well-known unit of mass in the chemical industry, such as μg, mg, g, or kg.

[0066] In this application, "%" represents a percentage, referring to the proportion of mass; however, the percentage of a solution, unless otherwise specified, refers to the number of grams of solute contained in 100 mL of the solution; the percentage of alcohol refers to the proportion of volume at 20°C. Furthermore, the following symbols may be used as needed: %(g / g) indicates the number of grams of solute contained in 100 g of solution; %(mL / mL) indicates the number of milliliters of solute contained in 100 mL of solution; %(mL / g) indicates the number of milliliters of solute contained in 100 g of solution; %(g / mL) indicates the number of grams of solute contained in 100 mL of solution.

[0067] In this article, ppm means parts per million, 1ppm = 0.0001%, 8000ppm = 0.8%, and other values ​​follow the same logic.

[0068] One or more embodiments of this application provide an oligomeric polyphenylene sulfide with a weight-average molecular weight ≤8000g / mol;

[0069] The composition of this oligomeric polyphenylene sulfide includes different cyclic polyphenylene sulfides and linear polyphenylene sulfides;

[0070] The different linear polyphenylene sulfides each independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the number of moles of halogen elements contained in each halogen end group is X1, the sum of the number of moles of sulfur elements contained in each mercapto end group is X2, the sum of the mass of halogen elements contained in each halogen end group is Y1, and the sum of the mass of sulfur elements contained in each mercapto end group is Y2.

[0071] The mass of the oligomeric polyphenylene sulfide is Z1;

[0072] X1:X2=(0.04-0.06):1;

[0073] 0.8%≤(Y1+Y2) / Z1≤1.5%.

[0074] In oligomeric polyphenylene sulfides, both cyclic polyphenylene sulfides and linear polyphenylene sulfides independently contain the structural unit shown in formula (Ⅰ);

[0075] (I).

[0076] The number of repetitions of the structural unit shown in Equation (I) can be 2-75, for example 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 40, 50, 60, 70, 75, or any value or range between any two of the above values.

[0077] In some embodiments, the cyclic polyphenylene sulfide comprises structural units of formula (I) repeated in a number of 2-20, for example 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, or any number or range between any two of the above values.

[0078] In some embodiments, the linear polyphenylene sulfide comprises structural units of formula (I) repeated in a number of 10-75, for example 10, 15, 20, 25, 30, 40, 50, 60, 70, 75, or any number or range between any two of the above values.

[0079] In some embodiments, the weight-average molecular weight of the oligomeric polyphenylene sulfide is 1000-8000 g / mol, and more particularly 4000-8000 g / mol, for example 1000 g / mol, 2000 g / mol, 3000 g / mol, 4000 g / mol, 5000 g / mol, 6000 g / mol, 7000 g / mol, 8000 g / mol, etc.

[0080] In some embodiments, the molar ratio represented by X1:X2 can be selected from (0.04-0.06):1, for example, it can be 0.04:1, 0.045:1, 0.05:1, 0.055:1, 0.06:1, or any value or range between any two of the above values.

[0081] In some embodiments, the mass percentage represented by (Y1+Y2) / Z1 can be selected from 0.8% to 1.5%, for example, it can be 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, or any value or range between any two of the above values.

[0082] There is no particular limitation on the mass percentage of the sum of the sulfur elements contained in each mercapto end group in the oligomeric polyphenylene sulfide. In some embodiments, the percentage represented by Y2 / Z1 can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any value or range between any two of the above values.

[0083] In some embodiments, the molecular weight distribution of the oligomeric polyphenylene sulfide is 2.5-4.0, for example 2.5, 3.0, 3.5, 4.0, etc.

[0084] In some embodiments, the linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the oligomeric polyphenylene sulfide, for example, 95%-99%, such as 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, etc.

[0085] The preparation method of oligomeric polyphenylene sulfide according to one or more embodiments of this application includes the following steps:

[0086] S11. Mix organic solvent A, sulfur source A and alkali metal hydroxide A, and dehydrate them to obtain mixture A;

[0087] S12. Mix the mixture A, dihaloaromatic compound A, and organic solvent B in a sealed container, and subject the resulting reaction solution A to a first-stage gradient temperature increase; the first-stage gradient temperature increase program includes: 0-60 min, from 20℃-40℃ to 220℃-225℃; 60 min-90 min, from 220℃-225℃ to 230℃; 90 min-150 min, from 230℃ to 240℃;

[0088] S13. After the first stage of gradient heating is completed, add dihaloaromatic compound B and organic solvent C within 60 min, and simultaneously perform a second stage of gradient heating on the resulting reaction solution B. The program for the second stage of gradient heating includes: heating from 240℃ to 250℃ from 150 min to 240 min.

[0089] In the above embodiments, there are no particular limitations on the type of organic solvent A. Amide polar solvents such as N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), and dimethylacetamide (DMAc), sulfoxide / sulfone solvents such as dimethyl sulfoxide (DMSO), dimethyl sulfone, and other commonly used solvents in the art can be selected.

[0090] In some embodiments, organic solvent A is N-methyl-2-pyrrolidone (NMP), which has a high boiling point, good solubility for reactants and oligomers, and excellent chemical stability in the preparation method of this application.

[0091] In the above embodiments, sulfur source A is selected from alkali metal sulfides, alkali metal hydrosulfides (hydrsulfides), or mixtures thereof, including but not limited to sodium sulfide, sodium hydrosulfide, potassium sulfide, and potassium hydrosulfide. Preferably, sulfur source A is sodium hydrosulfide (NaSH), which can be added in the form of an aqueous solution with a concentration of 40wt% to 65wt%.

[0092] In the above embodiments, alkali metal hydroxide A is selected from sodium hydroxide, potassium hydroxide, or a mixture thereof, preferably sodium hydroxide (NaOH), and is used to adjust the pH value of the system and promote the nucleophilic substitution reaction.

[0093] In the above embodiments, dihaloaromatic compound A and dihaloaromatic compound B are each independently selected from para-dihalobenzene, m-dihalobenzene, or mixtures thereof, wherein the halogen atom is selected from chlorine, bromine, or iodine. Preferably, both dihaloaromatic compound A and para-dihaloaromatic compound B are para-dichlorobenzene (p-DCB), and they may be the same or different.

[0094] In some embodiments, the molar amount of sulfur in sulfur source A is X1 mol; the sum of the molar amounts of dihaloaromatic compound A and dihaloaromatic compound B is X2 mol; the sum of the molar amounts of organic solvent A, organic solvent B and organic solvent C is X3 mol; X1:X2:X3 = 1:(0.75-0.95):(1.7-3), for example, can be selected from 1:0.75:1.7, 1:0.75:1.8, 1:0.75:2, 1:0.75:2.2, 1:0.75:2.4, 1:0.75:2.5, 1:0.75:3, 1:0.8:1.7, 1:0.8:1.8, 1:0.8:2, 1:0.8:2.2, 1 :0.8:2.4, 1:0.8:2.5, 1:0.8:3, 1:0.85:1.7, 1:0.85:1.8, 1:0.85:2, 1:0.85:2.2, 1:0.85:2.4, 1:0.85:2.5, 1:0.85:3, 1:0.9:1.7, 1:0.9:1.8, 1:0.9:2, 1:0.9:2.2, 1:0.9:2.4, 1:0.9:2.5, 1:0.9:3, 1:0.95:1.7, 1:0.95:1.8, 1:0.95:2, 1:0.95:2.2, 1:0.95:2.4, 1:0.95:2.5, 1:0.95:3, etc.

[0095] Generally, dehydration treatment, besides removing water, results in the loss of some organic solvent A and sulfur source. Calculated by mass or moles, the loss of organic solvent A is approximately 15%-30%, for example, 15%-30% of organic solvent A is distilled off with the water. The sulfur loss rate is approximately 1%-3%, for example, 1%-3% of the sulfur element is lost in the form of H2S during dehydration. However, these losses are already included in the overall calculation, and in specific implementation methods, calculations are based on the initial feed amount.

[0096] In some embodiments, the molar ratio of alkali metal hydroxide A to sulfur source A is in the range of 0.85-1.05:1, for example, 1:1; further, the molar ratio of organic solvent A to sulfur source A is in the range of 1-3:1, for example, 1.4:1; when the loss rate of organic solvent A is 15% to 30%, a molar ratio of 1-2:1 is beneficial to control the content of organic solvent in the reaction system within a suitable range.

[0097] In some embodiments, the molar amount of dihaloaromatic compound A relative to sulfur source A is 0.8:1 to 1.2:1 (e.g., 0.8:1, 1:1, 1.2:1, etc.); the molar amount of dihaloaromatic compound B is 5% to 30% of the molar amount of dihaloaromatic compound A (e.g., 5%, 10%, 15%, 20%, 25%, 30%, etc.).

[0098] The dehydration process is carried out under inert gas protection, with a heating temperature of 100℃~200℃, preferably 150℃~180℃, and a dehydration time of 1h~4h, until the water content in the system drops to an acceptable range for the reaction (e.g., below 500ppm). During the dehydration process, the water in the system is removed by azeotropic distillation with the organic solvent, while alkali metal hydroxide A reacts in situ with some of the hydrides in sulfur source A to generate sulfide active species.

[0099] In some embodiments, the sealed container is a pressure-resistant reactor, and the reaction is carried out under autogenous pressure. During the first and second gradient heating processes, the pressure of the reaction system is controlled within the range of 0.5 MPa to 2.5 MPa.

[0100] In the above embodiments, the dihaloaromatic compound B and organic solvent C are added at an appropriate time, such as 60 minutes, in order to supplement the dihaloaromatic compound monomer in the later stage of polymerization, so as to adjust the end group structure, molecular weight distribution or further improve the degree of polymerization of the oligomeric polyphenylene sulfide.

[0101] Organic solvent B and organic solvent C may be the same or different, and each is independently selected from the same type as organic solvent A, preferably both being N-methyl-2-pyrrolidone (NMP).

[0102] After the second stage of gradient heating is completed, the resulting reaction solution is cooled to room temperature at a rate of 0.5-10℃ / min.

[0103] In some embodiments, the reaction is stopped after reaching 250°C, and the temperature is first lowered to 140°C-160°C (e.g., 140°C, 150°C, 160°C) at a rate of 0.5-1°C / min (e.g., 0.5°C / min, 0.8°C / min, 1°C / min, etc.), and then lowered to room temperature (usually 20°C-40°C) at a rate of 2-10°C / min (e.g., 2°C / min, 5°C / min, 6°C / min, 8°C / min, 10°C / min, etc.).

[0104] After cooling to room temperature, the product undergoes solid-liquid separation, washing, and drying to obtain oligomeric polyphenylene sulfide resin. The washing process includes sequential washing with deionized water, an organic solvent (such as acetone or NMP), and then with deionized water to remove residual salts and unreacted monomers.

[0105] In some embodiments, the drying temperature is 100℃~150℃ (e.g., 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, etc.), and the drying time is 6h~24h (e.g., 6h, 8h, 10h, 12h, 16h, 20h, 24h, etc.).

[0106] In some embodiments, the average particle size of the solid obtained after drying is 50 μm-100 μm, and the bulk density is 0.15-0.2 g / cm³. 3 .

[0107] One or more embodiments of this application also provide a polyphenylene sulfide resin having a weight-average molecular weight of 20,000 g / mol to 40,000 g / mol;

[0108] The components of polyphenylene sulfide resin include different cyclic polyphenylene sulfide and linear polyphenylene sulfide, wherein the sum of the masses of the components with a weight average molecular weight in the range of 10,000 g / mol to 100,000 g / mol is Y3.

[0109] Different linear polyphenylene sulfides have end groups that independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the mass of chlorine elements contained in each halogen end group is Y4.

[0110] The mass of the polyphenylene sulfide resin is Z2;

[0111] Y3 / Z2 ≥ 80%;

[0112] Y4 / Z2≤0.03%.

[0113] Both cyclic polyphenylene sulfide and linear polyphenylene sulfide independently contain the structural unit shown in formula (Ⅰ);

[0114] (I).

[0115] In polyphenylene sulfide resin, the number of repetitions of the structural unit shown in formula (I) can be 2-400, for example 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 50, 100, 150, 200, 250, 300, 350, 400, or any value or range between any two of the above values.

[0116] In some embodiments, the cyclic polyphenylene sulfide comprises structural units of formula (I) repeated in a number of 2-20, for example 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, or any number or range between any two of the above values.

[0117] In some embodiments, the linear polyphenylene sulfide comprises structural units of formula (I) in a repeating number of 25-400, for example 25, 30, 50, 100, 150, 200, 250, 300, 350, 400, or any number or range between any two of the above values.

[0118] In some embodiments, the weight-average molecular weight of the polyphenylene sulfide resin is 20,000 g / mol to 40,000 g / mol, for example, it can be 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, etc.

[0119] In some embodiments, the mass percentage represented by Y3 / Z2 is ≥80%, and can be 80%-99.9%, for example, it can be 80%, 85%, 90%, 95%, 99%, 99.5%, 99.9%, or any value or range between any two of the above values.

[0120] In some embodiments, the mass percentage represented by Y4 / Z2 is ≤0.03%, which can be selected from 0.005% to 0.03%, for example, it can be 0.005%, 0.01%, 0.02%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, or any value or range between any two of the above values.

[0121] In some embodiments, the molecular weight distribution of the polyphenylene sulfide resin is 4.0-6.0, for example 4.0, 4.5, 5.0, 5.5, 6.0, etc.

[0122] In some embodiments, the melt index of the polyphenylene sulfide resin at 315°C / 5Kg is 500-1500 g / 10min, for example, it can be 500 g / 10min, 800 g / 10min, 1000 g / 10min, 1200 g / 10min, 1400 g / 10min, 1500 g / 10min, etc.

[0123] In some embodiments, the linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the polyphenylene sulfide resin, for example, 95%-99.9%, such as 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, etc.

[0124] The preparation method of polyphenylene sulfide resin according to one or more embodiments of this application includes the following steps:

[0125] S21. The first organic solvent, sulfur source and alkali metal hydroxide are mixed and dehydrated to obtain the first mixture;

[0126] S22. The first mixture, the dihalo aromatic compound and the second organic solvent are mixed in a sealed container. The resulting first reaction solution is heated to 225℃-230℃ and kept at that temperature for a reaction. The pressure inside the sealed container increases to X1MPa and then begins to decrease.

[0127] S23. After the pressure inside the sealed container is reduced to X2MPa, add oligomeric polyphenylene sulfide and a third organic solvent to the sealed container and mix. Heat the resulting second reaction solution from 225℃-230℃ to 250℃-270℃ and stop heating; X2 / X1 ×100% = 90%-98%; the oligomeric polyphenylene sulfide is the oligomeric polyphenylene sulfide described above, or the oligomeric polyphenylene sulfide prepared by the preparation method described above;

[0128] S24. The reaction liquid in the sealed container is cooled down and then subjected to solid-liquid separation to obtain the polyphenylene sulfide resin.

[0129] In the above embodiments, the type of the first organic solvent is not particularly limited. Amide polar solvents such as N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), and dimethylacetamide (DMAc), sulfoxide / sulfone solvents such as dimethyl sulfoxide (DMSO) and dimethyl sulfone, and other commonly used solvents in the art can be selected. The second and third organic solvents can be the same or different, each independently selected from the same type as the first organic solvent, preferably both being N-methyl-2-pyrrolidone (NMP).

[0130] In the above embodiments, the sulfur source is selected from alkali metal sulfides, alkali metal hydrosulfides (hydrsulfides), or mixtures thereof, including but not limited to sodium sulfide, sodium hydrosulfide, potassium sulfide, and potassium hydrosulfide. Preferably, the sulfur source is sodium hydrosulfide (NaSH), which can be added in the form of an aqueous solution with a concentration of 40wt% to 65wt%, such as 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, and 65wt%.

[0131] In the above embodiments, the alkali metal hydroxide is selected from sodium hydroxide, potassium hydroxide, or a mixture thereof, preferably sodium hydroxide (NaOH), and is used to adjust the pH value of the system and promote the nucleophilic substitution reaction.

[0132] In the above embodiments, the dihaloaromatic compound is selected from p-dihalobenzene, m-dihalobenzene, or mixtures thereof, wherein the halogen atom is selected from chlorine, bromine, or iodine. Preferably, the dihaloaromatic compound is p-dichlorobenzene (p-DCB).

[0133] The steps and effects of the dehydration treatment are described above. In some embodiments, the molar ratio of alkali metal hydroxide to sulfur source is in the range of 0.85-1.05:1, for example, 1:1; further, the molar ratio of first organic solvent to sulfur source is in the range of 1-3:1, for example, 1.4:1; when the loss rate of first organic solvent is 15% to 30%, a molar ratio of 1-2:1 is beneficial for controlling the content of organic solvent in the reaction system within a suitable range.

[0134] In some embodiments, the molar ratio of the dihaloaromatic compound to the sulfur source is 0.8:1 to 1.2:1 (e.g., 0.8:1, 1:1, 1.2:1, etc.), and the molar ratio of the oligomeric polyphenylene sulfide to the dihaloaromatic compound is 100g:20-25mol (e.g., 100g:20mol, 100g:22mol, 100g:25mol, etc.).

[0135] Understandably, in the steps of the above embodiments, in the step of simultaneously adding a dihaloaromatic compound (e.g., a dihaloaromatic compound) and an organic solvent (e.g., a second organic solvent), the organic solvent is typically used to fully dissolve the dihaloaromatic compound. When adding it, the dihaloaromatic compound can be dissolved in the corresponding organic solvent first. The mass ratio of the dihaloaromatic compound to the organic solvent can be 0.5:1 to 1.5:1 (e.g., 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, etc.) or other ranges that allow for the formation of a solution. The solution may also include necessary additives such as lithium acetate, and the amount of additive added is in accordance with the general practice in the art.

[0136] In some embodiments, the duration of the heat preservation reaction is 90 min to 300 min, for example, it can be 90 min, 100 min, 120 min, 150 min, 200 min, 220 min, 250 min, 300 min, etc.

[0137] In some embodiments, within 30 minutes after the pressure inside the sealed container decreases to X2 MPa, the oligomeric polyphenylene sulfide and the third organic solvent are added to the sealed container.

[0138] In some embodiments, the process of heating the resulting first reaction solution to 225°C-230°C includes:

[0139] The temperature was increased from 20℃-40℃ to 220℃ in 0-60 minutes.

[0140] The temperature was increased from 220℃ to 225℃-230℃ over 60-90 minutes.

[0141] In some embodiments, the process of heating the resulting second reaction solution from 225°C-230°C to 250°C-270°C includes:

[0142] The temperature was increased from 225℃-230℃ to 240℃-245℃ in 0-60 minutes.

[0143] The temperature was increased from 240℃-245℃ to 250℃-270℃ over a period of 60-300 minutes.

[0144] One or more embodiments of this application also provide the application of the polyphenylene sulfide resin described herein or the polyphenylene sulfide resin prepared by the described method.

[0145] Compositions can be prepared using this polyphenylene sulfide resin. Depending on the intended use, other resin components can be used without limitation, including various engineering plastics and conventional resins with good compatibility with polyphenylene sulfide resin. Furthermore, various additives, such as flame retardants, weather resistant agents, and fillers, can be added to the above resin compositions as needed to meet the processing and usage requirements of industrial applications, especially in the electronics and electrical appliance industries. Typical composite materials prepared using the polyphenylene sulfide resin of this application can be fiber-reinforced composites. These can be composites reinforced with short-cut fibers or long-fiber fibers.

[0146] The polyphenylene sulfide resin of this application has the advantages of narrow molecular weight distribution and low end-capped chlorine content, and good high-temperature resistance. In some embodiments, it is used to prepare high-temperature resistant materials. The polyphenylene sulfide resin of this application also has excellent processing fluidity, and in some embodiments, it is used in the preparation of high-temperature resistant precision devices in the field of electronics and electrical appliances.

[0147] The following are some specific examples.

[0148] For experimental parameters not specified in the following specific embodiments, please refer to the guidelines provided in this application, or consult experimental manuals or other known experimental methods in the field, or refer to the manufacturer's recommended experimental conditions. Raw materials and reagents not mentioned can be obtained commercially, or can be prepared by those skilled in the art using known methods.

[0149] In the following examples, NMP refers to N-methylpyrrolidone; p-DCB refers to p-dichlorobenzene; all raw materials and reagents are commercially available products with a purity of over 99%.

[0150] Example 1

[0151] This embodiment provides a method for synthesizing the oligomeric polyphenylene sulfide of this application, including the following steps:

[0152] A 10-liter autoclave was filled with 1500 g (15.1 mol) of NMP, 2000 g (21.6 mol) of sodium hydrosulfide aqueous solution (NaSH: purity 60.5 wt%), and 1129 g (20.3 mol) of sodium hydroxide (NaOH: purity 72%). After purging the autoclave with nitrogen, the temperature was increased from 100 °C to 200 °C at a rate of 1.0 °C / min while stirring at 200 rpm. The resulting distillate contained 1000 g of water (H2O), 302 g of NMP, and 13 g of hydrogen sulfide (H2S).

[0153] After the above dehydration process, the contents of the autoclave are cooled to 185°C. Then, 2500g (17.0mol) of p-DCB, 2900g (29.3mol) of NMP, and 59g (0.2mol) of an aqueous solution of lithium acetate (an auxiliary agent) are added to a closed system. The temperature is raised from room temperature (20-40°C); from 0-60 min, the temperature is raised from 20-40°C to 220-225°C; from 60-90 min, the temperature is raised from 220-225°C to 230°C; and from 90-150 min, the temperature is raised from 230°C to 240°C.

[0154] 400 g (2.7 mol) of pDCB and 500 g (5.0 mol) of NMP were added and mixed over 60 min, and the temperature was increased from 240 °C to 250 °C over 150-240 min; the reaction was stopped after reaching 250 °C and the temperature was lowered. The conversion rate of the polymerized p-DCB was 96%.

[0155] The cooling process included: cooling to 150°C at a rate of 1°C / min, then cooling to room temperature at a rate of 5°C / min; diluting with 4000g NMP; centrifuging; washing the resulting solid with acetone and deionized water, followed by washing with an acetic acid solution; drying the washed solid to obtain granular PPS. The average particle size was 80μm, and the bulk density was 0.18g / cm³. 3 The performance test results are shown in Table 2.

[0156] Example 2

[0157] This embodiment provides a method for synthesizing the low-chlorine grade polyphenylene sulfide of this application, including the following steps:

[0158] A 10-liter autoclave was filled with 3000 g (30.3 mol) of NMP, 2000 g (21.6 mol) of sodium hydrosulfide aqueous solution (NaSH: purity 60.5 wt%), and 1212 g (21.8 mol) of sodium hydroxide (NaOH: purity 72%). After purging the autoclave with nitrogen, the temperature was increased from 100 °C to 200 °C at a rate of 1.0 °C / min while stirring at 200 rpm. The resulting distillate contained 1020 g of water (H2O), 345 g of NMP, and 10 g of hydrogen sulfide (H2S).

[0159] After the above dehydration process, the contents of the autoclave are cooled to 185°C. Then, 3300g (22.4mol) of p-DCB, 2500g (25.2mol) of NMP, and 59g (0.2mol) of an aqueous solution of lithium acetate are added to a closed system. The temperature is raised from room temperature (20-40°C); from 0-60 min, the temperature is raised from 20-40°C to 220°C; from 60-90 min, the temperature is raised from 220°C to 225°C; and from 90-150 min, the temperature is held constant at 225°C.

[0160] During the isothermal process, the system pressure was detected to gradually increase from 0.3-0.4 MPa until it reached the maximum pressure of 0.65 MPa, after which it began to slowly decrease. After decreasing to 0.63 MPa, 500 g of polyphenylene sulfide oligomer solution (containing 400 g (4.0 mol) of NMP and 100 g of oligomeric polyphenylene sulfide, which had been preheated to 230 °C) was added to the closed system and the addition was completed within 30 min.

[0161] Starting from the point where the addition is complete: 0-60 min, the temperature is increased from 225℃ to 240℃; 60-300 min, the temperature is increased from 240℃ to 255℃; after reaching 255℃, the reaction is stopped and the temperature is lowered. The conversion rate of p-DCB after polymerization is 92%.

[0162] The cooling process included: cooling to 150°C at a rate of 1°C / min, then cooling to room temperature at a rate of 5°C / min; diluting with 4000g NMP; centrifuging; washing the resulting solid with acetone and deionized water, followed by washing with an acetic acid solution; drying the washed solid to obtain granular PPS. The average particle size was 480μm, and the bulk density was 0.38g / cm³. 3 The performance test results are shown in Table 2.

[0163] Example 3

[0164] The difference between Example 3 and Example 2 is that the amount of p-DCB fed after dehydration is 3350g (22.8mol), while the other conditions are exactly the same as in Example 2.

[0165] Example 4

[0166] The difference between Example 4 and Example 2 is that the amount of p-DCB fed after dehydration is 3200g (21.8mol), while the other conditions are exactly the same as in Example 2.

[0167] Comparative Example 1

[0168] A 10-liter autoclave was filled with 3000g (30.3mol) of NMP, 2000g (21.6mol) of sodium hydrosulfide aqueous solution (NaSH: purity 60.5wt%), and 1212g (21.8mol) of sodium hydroxide (NaOH: purity 72%). After purging the autoclave with nitrogen, the temperature was increased from 100℃ to 200℃ at a rate of 1.0℃ / min while stirring at 200 rpm. The resulting distillate contained 980g of water (H2O), 23g of NMP, and 11g of hydrogen sulfide (H2S).

[0169] After the above dehydration process, the contents of the autoclave were cooled to 185°C. Then, 3200g (21.8mol) of p-DCB, 2500g (25.2mol) of NMP, and 59g (0.2mol) of an aqueous solution of lithium acetate were added to a closed system. The temperature was increased from room temperature (20-40°C); from 0-60 min, the temperature was increased from 20-40°C to 220°C; from 60-90 min, the temperature was increased from 220°C to 225°C; from 90-150 min, the temperature was held at 225°C. After the holding time was completed, the timing was restarted. From 0-60 min, the temperature was increased from 225°C to 240°C; from 60-300 min, the temperature was increased from 240°C to 255°C; the reaction was stopped after reaching 255°C, and the temperature was then lowered. The conversion rate of the polymerized p-DCB was 96%.

[0170] The cooling process included: cooling to 150°C at a rate of 1°C / min, then cooling to room temperature at a rate of 5°C / min; diluting with 4000g NMP; centrifuging; washing the resulting solid with acetone and deionized water, followed by washing with an acetic acid solution; drying the washed solid to obtain granular PPS. The average particle size was 480μm, and the bulk density was 0.38g / cm³. 3 .

[0171] The structural performance of the products prepared in the examples and comparative examples was tested, and the test results are shown in Table 1.

[0172] Molecular weight was determined using volume exclusion chromatography-high temperature system with 1-chloronaphthalene as the organic solvent.

[0173] Melting point and crystallization temperature were determined using a differential scanning calorimeter (DSC). 4.5-5.5 mg of PPS resin was heated to 340°C at a heating rate of 20°C / min, held at that temperature for 5 min, and then cooled to 40°C at a cooling rate of 10°C / min for measurement.

[0174] Melt index is calculated by monitoring the outflow volume of resin at 315℃ / 5kg for 5 minutes, while thermal stability is the ratio of the outflow volume after holding the sample in the melt indexer for 5 minutes to the data without holding for 5 minutes.

[0175] Total chlorine content was determined according to EN14582:2007, using oxygen bomb combustion ICP. The proportion of covalently bonded chlorine was determined using XPS.

[0176] Test method for the proportion of linear polymer chains in low-chlorinated polyphenylene sulfide: Take a certain mass of polyphenylene sulfide sample A, add dichloromethane at a mass ratio of 15 times, stir and reflux at 40℃ for 15h, collect the clear liquid, concentrate it, add methanol for precipitation, separate the cyclic oligomer powder obtained by precipitation, dry and weigh it, the mass is B, and the linearity = 1-B / A.

[0177] Table 1. Structural and property characterization of polyphenylene sulfide in the examples and comparative examples

[0178]

[0179] The polymers in the examples and comparative examples were thoroughly dried in a vacuum oven at 150°C before extrusion and injection molding to obtain heat-treated polymers. 59.6 parts (by mass) of the heat-treated polymer, 40 parts (by mass) of glass fiber (13 μm in diameter), and 0.4 parts (by mass) of pentaerythritol tetrastearate (PETS) were mixed and melt-kneaded using a twin-screw extruder to prepare PPS resin compositions. Each composition was injection molded into samples, and their tensile and flexural strengths were measured.

[0180] Corrosion test method: 4 grams of PPS resin were placed in a glass test tube with an outer diameter of 21 mm and a length of 200 mm. Then, a SUS304H stainless steel foil corrosion test piece (50 μm thick, 18 mm wide, and 160 mm long) was placed in the test tube and sealed with a silicone rubber perforated sponge plug. The test piece was heated at 280°C for 3 hours using a constant temperature bath. After heat treatment, it was left at room temperature for approximately 12 hours, and then the corrosion status of the test piece was visually observed. The evaluation of the metal corrosion resistance of PPS resin is divided into the following four stages.

[0181] Metal corrosion judgment criteria: A: No corrosion, corrosion area <0.1%; B: Slight corrosion, corrosion area <0.5%; C: Corrosion present, corrosion area 0.5%-1%; D: Severe corrosion, corrosion area >1%.

[0182] Thermal stability test method: The test was conducted using a capillary rheometer (GOTTFERT RG20, Germany) at a temperature of 310℃ and an L / D ratio of 30 / 1. After the sample was added, it was melted and kept at this temperature in the sample chamber for a certain period of time. The thermal stability of the product was determined by the ratio of the melt viscosity measured after 30 minutes of holding at this temperature to that measured after 5 minutes of holding at this temperature, i.e., MV30 / MV5.

[0183] Molding time refers to the total time of a single injection molding process, including the demolding time of the part.

[0184] Tensile strength and flexural strength shall be in accordance with GB / T 1040.1 / 2 and GB / T 9341.

[0185] Table 2. Application performance characterization of the examples and comparative examples

[0186]

[0187] In Table 2, the oligomers from Example 1 were not included in the molding test.

[0188] The technical features of the above-described embodiments and examples can be combined in any suitable manner. For the sake of brevity, not all possible combinations of the technical features in the above-described embodiments and examples are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0189] The embodiments described above merely illustrate several implementation methods of this application and should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Furthermore, it should be understood that after reading the above teachings, those skilled in the art can make various alterations or modifications to this application, and the equivalent forms obtained also fall within the protection scope of this application. It should also be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided in this application through logical analysis, reasoning, or limited experimentation are all within the protection scope of the appended claims. Therefore, the protection scope of this patent application should be determined by the appended claims, and the specification can be used to interpret the content of the claims.

Claims

1. An oligomeric polyphenylene sulfide, characterized in that, The weight-average molecular weight of the oligomeric polyphenylene sulfide is ≤8000 g / mol; The components of the oligomeric polyphenylene sulfide include different cyclic polyphenylene sulfides and linear polyphenylene sulfides; The different linear polyphenylene sulfides each independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the number of moles of halogen elements contained in each halogen end group is X1, the sum of the number of moles of sulfur elements contained in each mercapto end group is X2, the sum of the mass of halogen elements contained in each halogen end group is Y1, and the sum of the mass of sulfur elements contained in each mercapto end group is Y2. The mass of the oligomeric polyphenylene sulfide is Z1; X1:X2=(0.04-0.06):1; 0.8%≤(Y1+Y2) / Z1≤1.5%.

2. The oligomeric polyphenylene sulfide according to claim 1, characterized in that, The cyclic polyphenylene sulfide comprises structural units of formula (Ⅰ) repeated in a number of 2-20; The linear polyphenylene sulfide comprises structural units of formula (Ⅰ) with a repeating number of 10-75; (I); and / or, The oligomeric polyphenylene sulfide has a molecular weight distribution of 2.5-4.0; and / or, The linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the oligomeric polyphenylene sulfide.

3. The method for preparing oligomeric polyphenylene sulfide according to claim 1 or 2, characterized in that, Includes the following steps: Organic solvent A, sulfur source A and alkali metal hydroxide A are mixed and dehydrated to obtain mixture A; Mix the mixture A, dihaloaromatic compound A and organic solvent B in a sealed container, and subject the resulting reaction solution A to a first-stage gradient temperature increase. The first gradient temperature program includes: 0-60 min, from 20℃-40℃ to 220℃-225℃; 60 min-90 min, from 220℃-225℃ to 230℃; 90 min-150 min, from 230℃ to 240℃; After the first stage of gradient heating is completed, dihaloaromatic compound B and organic solvent C are added and mixed within 60 min, while the resulting reaction solution B is subjected to a second stage of gradient heating. The program for the second stage of gradient heating includes: heating from 240℃ to 250℃ in 150 min to 240 min.

4. The preparation method according to claim 3, characterized in that, The molar amount of sulfur in sulfur source A is M1 mol; The sum of the molar amounts of the dihaloaromatic compound A and the dihaloaromatic compound B is M2mol; The sum of the molar amounts of organic solvent A, organic solvent B, and organic solvent C is M3mol; M1:M2:M3=1:(0.75-0.95):(1.7-3).

5. A polyphenylene sulfide resin, characterized in that, The weight-average molecular weight of the polyphenylene sulfide resin is 20,000 g / mol to 40,000 g / mol. The polyphenylene sulfide resin comprises different cyclic polyphenylene sulfide and linear polyphenylene sulfide, wherein the sum of the masses of the components with a weight-average molecular weight in the range of 10,000 g / mol to 100,000 g / mol is Y3. The different linear polyphenylene sulfides each independently include one or more of halogen end groups and mercapto end groups, wherein the sum of the mass of chlorine elements contained in each halogen end group is Y4; The mass of the polyphenylene sulfide resin is Z2; Y3 / Z2 ≥ 80%; Y4 / Z2≤0.03%.

6. The polyphenylene sulfide resin according to claim 5, characterized in that, The cyclic polyphenylene sulfide comprises structural units of formula (Ⅰ) repeated in a number of 2-20; The linear polyphenylene sulfide comprises structural units of formula (Ⅰ) with a repeating number of 25-400; (I); and / or, The polyphenylene sulfide resin has a molecular weight distribution of 4.0-6.0; and / or, The polyphenylene sulfide resin has a melt index of 500-1500 g / 10min at 315℃ / 5Kg; and / or, The linear polyphenylene sulfide accounts for ≥95% of the mass percentage of the polyphenylene sulfide resin.

7. The method for preparing the polyphenylene sulfide resin according to claim 5 or 6, characterized in that, Includes the following steps: The first organic solvent, sulfur source and alkali metal hydroxide are mixed and dehydrated to obtain the first mixture; The first mixture, the dihalo aromatic compound, and the second organic solvent are mixed in a sealed container. The resulting first reaction solution is heated to 225°C-230°C and kept at that temperature for a reaction. The pressure inside the sealed container is increased to X1MPa and then begins to decrease. After the pressure inside the sealed container is reduced to X2 MPa, oligomeric polyphenylene sulfide and a third organic solvent are added to the sealed container and mixed. The resulting second reaction solution is heated from 225℃-230℃ to 250℃-270℃, and then heating is stopped; X2 / X1 ×100% = 90%-98%; the oligomeric polyphenylene sulfide is the oligomeric polyphenylene sulfide according to claim 1 or 2, or the oligomeric polyphenylene sulfide prepared by the preparation method according to claim 3 or 4; The reaction liquid in the sealed container is cooled and then subjected to solid-liquid separation to obtain the polyphenylene sulfide resin.

8. The preparation method according to claim 7, characterized in that, The duration of the heat preservation reaction is 90 min-300 min; and / or, Within 30 minutes after the pressure inside the sealed container decreases to X2MPa, the oligomeric polyphenylene sulfide and the third organic solvent are added to the sealed container.

9. The preparation method according to claim 7 or 8, characterized in that, The procedure for heating the resulting first reaction solution to 225℃-230℃ includes: The temperature was increased from 20℃-40℃ to 220℃ in 0-60 minutes. The temperature is increased from 220℃ to 225℃-230℃ over 60-90 minutes; and / or, The procedure for heating the resulting second reaction solution from 225℃-230℃ to 250℃-270℃ includes: The temperature was increased from 225℃-230℃ to 240℃-245℃ in 0-60 minutes. The temperature was increased from 240℃-245℃ to 250℃-270℃ over a period of 60-300 minutes.

10. The use of the polyphenylene sulfide resin according to claim 5 or 6 or the polyphenylene sulfide resin prepared by the preparation method according to any one of claims 7-9 in the preparation of high-temperature resistant materials.